Superconducting quantum chip and preparation method thereof

By using air bridge patches instead of electrical connection patches in superconducting quantum chips, the problems of parasitic junctions and ion beam etching damage in traditional processes are solved, enabling the fabrication of high-performance and low-cost superconducting quantum chips.

CN121152553APending Publication Date: 2025-12-16SHENZHEN SPINQ TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511274820.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-09-05
Publication Date
2025-12-16

Smart Images

  • Figure CN121152553A_ABST
    Figure CN121152553A_ABST
Patent Text Reader

Abstract

The invention discloses a superconducting quantum chip and a preparation method thereof. The preparation method of the superconducting quantum chip comprises the following steps: preparing a bottom layer circuit on a substrate; preparing a Josephson junction on the substrate on which the bottom circuit is prepared; spin-coating a first photoresist on the substrate on which the bottom circuit and the Josephson junction are prepared and baking; spin-coating a second photoresist and baking the second photoresist; aligning the first mask with the Josephson junction, and performing exposure and development to form a hollow pattern of the bridge pier in the first photoresist and the second photoresist; pier metal is evaporated on the hollowed-out pattern of the pier through electron beam evaporation; spin-coating sacrificial layer photoresist on the substrate on which the pier metal is evaporated, and baking the sacrificial layer photoresist; aligning a second mask with the Josephson junction, and performing exposure and development to remove a non-air bridge region in the sacrificial layer; etching the global etching oxide layer by using an ion beam, and etching the deposited metal material in a non-air bridge area by using inductively coupled plasma to form an air bridge patch; and removing the photoresist and stripping to obtain the superconducting quantum chip.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the field of superconducting quantum technology, and in particular to a superconducting quantum chip and a preparation method thereof. BACKGROUND

[0002] In the field of quantum computing, a superconducting quantum chip is a core component of a superconducting quantum computer. The superconducting quantum computer relies on the superconducting quantum chip to realize logical gate operation. The superconducting quantum chip generally includes a substrate, and a bottom layer circuit and a quantum bit formed on the substrate, wherein the quantum bit includes a Josephson junction, and the bottom layer circuit includes a transmission line (the transmission line includes a control line and a read line), a resonant cavity, and the like.

[0003] Currently, the superconducting quantum chip manufactured by the traditional process generally adopts a method of first manufacturing a bottom layer circuit on a substrate (a wafer), and then manufacturing a Josephson junction connected to the bottom layer circuit by using a double-angle evaporation method. This method has the problems of parasitic junction and Ion Beam Etching (IBE) damage to the substrate, which limits the low-temperature performance of the superconducting quantum chip to some extent. In order to solve this problem, researchers have invented a patch process. In the preparation process of the related process, a two-step method is used to manufacture the Josephson junction, that is, a structure part of the Josephson junction is first prepared by using a double-angle evaporation method, and then a patch (a Josephson junction patch) for electrically connecting the Josephson junction and the bottom layer circuit is manufactured by performing photoetching and evaporation once again. This method can effectively avoid the generation of parasitic junctions, and also reduce the damage of IBE to the substrate near the junction area to some extent. SUMMARY

[0004] In order to improve the performance of the superconducting quantum chip and increase the selection space of the superconducting quantum chip preparation method, the present application provides a superconducting quantum chip preparation method and related products.

[0005] In a first aspect, an embodiment of the present application provides a preparation method of a Josephson junction in a superconducting quantum chip, comprising: manufacturing a bottom layer circuit on a substrate; manufacturing a Josephson junction on the substrate on which the bottom layer circuit has been manufactured; spinning a first photoresist on the substrate on which the bottom layer circuit and the Josephson junction have been manufactured and baking; spinning a second photoresist on the substrate on which the first photoresist has been coated and baking; aligning a first mask plate to the Josephson junction, and exposing and developing the first photoresist and the second photoresist to form a hollow pattern of a bridge pier in the first photoresist and the second photoresist; evaporating a bridge pier metal in the hollow pattern of the bridge pier by using electron beam evaporation to connect the bottom layer circuit and the Josephson junction; A sacrificial photoresist layer is spin-coated onto a substrate containing evaporated bridge pier metal and then baked. Align the second mask with the Josephson junction to expose and develop the sacrificial layer to remove non-air bridge regions in the sacrificial layer; The oxide layer is etched globally using an ion beam, and the deposited metal material in the non-air bridge area is etched away using inductively coupled plasma to form air bridge patches. The adhesive is removed and peeled off to obtain the superconducting quantum chip.

[0006] In one embodiment, before spin-coating the sacrificial photoresist onto the substrate with the evaporated bridge pier metal and baking, the above method further includes: The substrate with the evaporated bridge pier metal is placed in a hexamethyldisilazane pretreatment device and thickened using hexamethyldisilazane vapor.

[0007] In one embodiment, the debonding and peeling to obtain a superconducting quantum chip includes: The etched substrate is immersed in an N-methylpyrrolidone solution to remove all remaining photoresist, resulting in a superconducting quantum chip.

[0008] In one embodiment, fabricating the underlying circuitry on the substrate includes: A negative photoresist is coated onto the substrate and then baked. The third mask is aligned with the substrate to expose the negative photoresist; The exposed negative photoresist is subjected to generalized exposure and development to form a bottom layer circuit pattern on the negative photoresist; Superconducting metal is deposited onto the underlying circuit pattern using electron beam evaporation. The substrate with the superconducting metal deposited on it is immersed in a stripping solution to remove the negative photoresist and obtain the bottom layer circuit.

[0009] In one embodiment, the process of coating the substrate with negative photoresist and baking it includes: Negative photoresist is spin-coated onto the substrate at a first rotational speed; The negative photoresist is thinned using the second rotation speed to achieve the target photoresist thickness; The negative photoresist is baked in a hot plate.

[0010] In one embodiment, the negative photoresist is AZ 5214E ​​photoresist; after exposing the negative photoresist, the method further includes: The exposed negative photoresist is then post-baked.

[0011] In one embodiment, after developing the negative photoresist, the method further includes hardening the negative photoresist.

[0012] In one embodiment, the method of stripping the negative photoresist from the substrate on which the superconducting metal has been deposited, comprises: heating the stripping solution to a preset temperature range, and immersing the substrate on which the superconducting metal has been deposited into the heated stripping solution for a preset time period to strip the negative photoresist.

[0013] In one embodiment, after the method of stripping the negative photoresist from the substrate on which the superconducting metal has been deposited to obtain the bottom layer circuit, the method further comprises: replacing the fresh stripping solution, and immersing the substrate from which the negative photoresist has been stripped into the fresh stripping solution for a preset time period; sequentially rinsing the substrate from which the negative photoresist has been stripped with pure acetone solution, isopropyl alcohol solution and deionized water; blowing dry with nitrogen.

[0014] In one embodiment, the method of preparing the bottom layer circuit on the substrate, comprises: depositing superconducting metal on the substrate; spin-coating positive photoresist on the substrate on which the superconducting metal has been deposited; aligning the fourth mask to the substrate, and exposing and developing the positive photoresist; etching the superconducting metal on the developed substrate to obtain the bottom layer circuit; stripping the remaining positive photoresist.

[0015] In one embodiment, the method of depositing superconducting metal on the substrate, comprises: depositing superconducting metal by electron beam evaporation or controlled sputtering.

[0016] In one embodiment, the method of etching the superconducting metal on the developed substrate to obtain the bottom layer circuit, comprises: etching the superconducting metal on the developed substrate by inductively coupled plasma etching or reactive ion etching to obtain the bottom layer circuit.

[0017] In one embodiment, the method of stripping the remaining positive photoresist, comprises: ashing the substrate on which the bottom layer circuit has been prepared by plasma to remove the remaining positive photoresist; cleaning the substrate from which the positive photoresist has been removed in acetone solution, and removing the residual positive photoresist by ultrasonic oscillation of the acetone solution.

[0018] In one embodiment, before the method of preparing the bottom layer circuit on the substrate, the method further comprises: cleaning the substrate.

[0019] In one embodiment, the method of fabricating a Josephson junction on the substrate with prepared bottom layer circuit comprises: spinning a third photoresist on the substrate with prepared bottom layer circuit and baking; spinning a fourth photoresist on the substrate with prepared bottom layer circuit and baking; exposing, developing and fixing the third photoresist and the fourth photoresist to form a cross-shaped gap's hollow pattern in the third photoresist and the fourth photoresist; the cross-shaped gap comprises a first gap and a second gap intersecting each other; depositing a bottom superconducting metal layer in the first gap at a first angle by electron beam evaporation; in-situ oxidizing the surface of the bottom superconducting metal layer to form an in-situ oxidation layer; depositing a top superconducting metal layer in the second gap at a second angle by electron beam evaporation; the top superconducting metal layer intersects the bottom superconducting metal layer with prepared in-situ oxidation layer; stripping the remaining third photoresist and fourth photoresist to obtain a Josephson junction.

[0020] In one embodiment, the method of exposing the third photoresist and the fourth photoresist comprises: exposing the third photoresist and the fourth photoresist at a Josephson junction core junction area using a first preset dose of exposure amount on an electron beam lithography device with preset voltage and beam current; and exposing the third photoresist and the fourth photoresist at a peripheral electrode area outside the Josephson junction core junction area using a second preset dose of exposure amount.

[0021] In one embodiment, the method of developing the exposed third photoresist and the fourth photoresist comprises: using a developer mixed by methyl isobutyl ketone: isopropyl alcohol = 1:3 ratio to develop the exposed part of the exposed third photoresist and the fourth photoresist according to a set time.

[0022] In one embodiment, after the method of developing the exposed third photoresist and the fourth photoresist, the method further comprises: immersing the developed substrate into an isopropyl alcohol solution for a preset duration to remove the developer of the third photoresist and the fourth photoresist; blowing dry with nitrogen.

[0023] In one embodiment, the method of fixing the third photoresist and the fourth photoresist comprises: lightly etching the developed substrate using plasma to remove residual developer of the third photoresist and the fourth photoresist.

[0024] In one embodiment, peeling off the third photoresist and the fourth photoresist to obtain the Josephson junction comprises: placing the substrate on which the bottom superconducting metal layer and the top superconducting metal layer are deposited into an N-methylpyrrolidone solution for a preset time period to remove the remaining third photoresist and fourth photoresist, and obtaining the Josephson junction.

[0025] In one embodiment, peeling off the third photoresist and the fourth photoresist to obtain the Josephson junction comprises: placing the substrate on which the bottom superconducting metal layer and the top superconducting metal layer are deposited into an acetone solution for a preset time period to remove the remaining fourth photoresist; placing the substrate on which the fourth photoresist is removed into a toluene solution for a preset time period, and oscillating the toluene solution with ultrasound to remove the remaining third photoresist, and obtaining the Josephson junction.

[0026] In one embodiment, the above method further comprises, in the process of removing the remaining fourth photoresist and removing the remaining third photoresist, oscillating the acetone solution and / or the toluene solution with megasonic waves.

[0027] In one embodiment, after the step of peeling off the remaining third photoresist and fourth photoresist to obtain the Josephson junction, the above method further comprises: rinsing the substrate on which the third photoresist and the fourth photoresist are removed with isopropyl alcohol solution or deionized water to remove organic matter; blowing dry with nitrogen.

[0028] In one embodiment, the third photoresist is methyl methacrylate; the fourth photoresist is polymethyl methacrylate.

[0029] In a second aspect, an embodiment of the present application provides a superconducting quantum chip, which is prepared according to the method for preparing a superconducting quantum chip as described above.

[0030] The above technical solutions provided by the embodiments of the present application have at least the following beneficial effects: The preparation method of the superconducting quantum chip provided by the embodiment of the application directly replaces the electrical connection patch with an air bridge patch, uses the air bridge structure for interconnection isolation as the connection structure of the Josephson junction below or nearby, retains the advantages of the patch process, avoids parasitic junctions and reduces IBE damage to the substrate, and does not reduce the low-temperature performance of the chip. Before or at the same time as the key step of air bridge production (usually plating / depositing bridge metal, releasing the sacrificial layer), the metallized area (i.e., the future "pier") below can be defined as the patch area. After the air bridge patch is produced, the area below the bridge body, from which the sacrificial layer is etched and released, naturally forms a low-loss air gap (air) "isolation layer", which protects the underlying material from IBE damage in the subsequent Josephson junction layer and provides electrical isolation integrated with the air bridge structure.

[0031] The preparation method of the superconducting quantum chip provided by the embodiment of the application directly replaces the electrical connection patch with an air bridge patch, covers the area predetermined as the patch, and the air bridge structure (bridge body) itself becomes the most effective mask to protect the underlying material from IBE damage in the subsequent Josephson junction layer. Only the piers (metal through holes / pad areas) used to support the air bridge need to be exposed for IBE etching (for defining the connection circuit). IBE damage is thus localized to these small-area pier contact areas, minimizing IBE damage to the substrate. When the ion beam etches the oxide layer globally, the Josephson junction itself and its immediately adjacent (usually qubit loop) high-sensitivity areas are located in a relatively distant area of the air bridge. Due to the presence of photoresist, the substrate in these areas is protected to the greatest extent, almost completely isolating the direct and main scattering damage sources of IBE. Therefore, the substrate interface damage caused by IBE can be limited to a small-area region of the electrical connection point (pier), greatly protecting the key device area (especially the high-Q Josephson junction and its underlying substrate interface), and minimizing the dielectric loss caused by IBE damage, thereby significantly improving the coherence time of the superconducting quantum bit and improving the performance of the superconducting quantum chip.

[0032] The preparation method of the superconducting quantum chip provided by the embodiment of the application realizes low-capacitance and low-loss electrical isolation at the cross-interconnection by using the air bridge patch. The bridge body surrounded by air provides a superior dielectric environment (low dielectric constant of air) for the Josephson junction patch area below and the signal line spanning above, which protects the Josephson junction while maintaining the low parasitic capacitance and low interconnection loss required for high-performance interconnection, thereby improving the performance of the superconducting quantum chip.

[0033] Compared with a two-step patch process, the preparation method of the superconducting quantum chip provided in the embodiment of the application saves the additional steps required for special deposition, lithography and etching of the dielectric patch layer, at least reduces one mask and one lithography and etching cycle, simplifies the process procedure, significantly reduces the manufacturing cost and period, improves the process efficiency, and improves the yield and fault tolerance of the wafer.

[0034] Additional features and advantages of the application will be set forth in the description that follows, and in part will be apparent from the description, or can be learned by practice of the application. The objectives and other advantages of the application will be realized and attained by the structure particularly pointed out in the written description and claims hereof as well as the appended drawings.

[0035] The technical solutions of the application will be further described in detail below with reference to the drawings and examples. BRIEF DESCRIPTION OF DRAWINGS

[0036] The accompanying drawings are included to provide a further understanding of the application and are incorporated in and constitute a part of this specification, illustrate embodiments of the application and serve to explain the principles of the application, and should not be considered limiting of the application. In the drawings: Figure 1 A flow chart of the preparation method of the superconducting quantum chip in the embodiment of the application; Figure 2 A schematic diagram of preparing the bottom layer circuit on the substrate in the embodiment of the application; Figure 3 A schematic diagram of preparing the bottom layer circuit and the Josephson junction on the substrate in the embodiment of the application; Figure 4 A schematic diagram of the hollow pattern of the bridge pier lithographically defined on both ends of the Josephson junction and the bottom layer circuit in the embodiment of the application; Figure 5 A schematic diagram of preparing the air bridge patch to connect the Josephson junction and the bottom layer circuit in the embodiment of the application. DETAILED DESCRIPTION

[0037] Exemplary embodiments of the present disclosure will be described more fully hereinafter with reference to the accompanying drawings. While example embodiments of the present disclosure are shown in the drawings, it is understood that the present disclosure can be embodied in various forms without being limited by the embodiments set forth herein. Rather, these embodiments are provided so that the present disclosure can be more thoroughly and completely understood, and so that the scope of the present disclosure can be conveyed completely to those skilled in the art.

[0038] In the description of the present application, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", "far", "near", "front", "back", and the like indicate the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the devices or elements referred to must have a particular orientation, be constructed and operated in a particular orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first", "second", "third" are only for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0039] In the description of the present application, it should be noted that unless otherwise explicitly specified and limited, the terms "mounting", "connection", "connection" should be understood broadly, for example, it can be fixedly connected, or it can be detachably connected, or integrally connected; it can be mechanically connected, or it can be electrically connected; it can be directly connected, or it can be indirectly connected through an intermediate medium; it can be the communication inside two elements. For those skilled in the art, the specific meaning of the above terms in the present application can be understood according to the specific circumstances.

[0040] Josephson junction: or superconducting tunnel junction. It is an important component in superconducting quantum chips, which can be used to build superconducting quantum bits, and together with other superconducting elements to form a superconducting circuit. Josephson junction is usually composed of two layers of superconducting material (superconducting metal layer) with a very thin insulating layer (in-situ oxidation layer) in between, showing a microstructure similar to "sandwich".

[0041] Josephson junction patch: a connection structure in a superconducting quantum chip that connects Josephson junctions and the underlying circuit required for connection.

[0042] Parasitic junction: other Josephson junctions brought about during the preparation of Josephson junctions.

[0043] Sacrificial layer: in the lift-off technique, in order to lift off the deposited material in the non-defined area, a photoresist is applied on the substrate in the non-defined area; during the lift-off, this layer of photoresist dissolves in a specific solution, and at the same time, the material deposited on its upper layer is also lifted off, and this layer of photoresist is called the sacrificial layer.

[0044] Air bridge: also known as air bridge, is a circuit structure that realizes the cross-connection of planar circuit in a three-dimensional bridge type.

[0045] Pier: the area left on the underlying circuit structure for the air bridge and Josephson junction to contact the underlying circuit.

[0046] Bridge support: the part on the air bridge used to connect the Josephson junction and the underlying circuit.

[0047] Bridge: The part of the bridge body connecting two bridge supports.

[0048] Air bridge patch: An air-bridge connection structure in a superconducting quantum chip that connects a Josephson junction and an underlying line required for connection.

[0049] Coherence time: A measure of how long a quantum system can maintain its quantum coherence, including the energy relaxation time T1 and the dephasing time T2. T1 represents the average time for a quantum bit to spontaneously decay from an excited state (|1>) to a ground state (|0>). T2 represents the time required for the relative phase information of a superposition state of a quantum bit (such as |0> + |1>) to become completely randomized and unpredictable.

[0050] Undercut: In a double-layer resist process, after the photoresist of the upper layer is exposed and developed, the lower layer resist continues to etch in the developing solution, and a horizontally expanding structure with a narrow upper part and a wide lower part is formed.

[0051] Pre-baking: One of the basic steps of the photolithography process, also known as soft baking. That is, at a certain temperature, the solvent in the photoresist film slowly and fully escapes, making the photoresist film dry.

[0052] Exposure and development: A micro-nano processing technology mainly involving ultraviolet lithography, which involves coating photoresist on the surface of a substrate sample, then shining ultraviolet light through a mask onto the substrate surface, using photochemical reactions to change the properties of the photoresist exposed to light, then dissolving the light-reacted area into a specific solution to achieve the purpose of creating a specific pattern on the substrate.

[0053] Etching: A microfabrication process that uses dry (other) and wet (liquid) methods to etch metal or other materials to form the desired structure.

[0054] In situ oxidation refers to the process of directly oxidizing the surface of a superconducting metal layer in the same vacuum environment or process chamber without breaking the vacuum or exposing it to the atmosphere.

[0055] Lift-off: After the substrate is coated with photoresist, exposed, and developed, the photoresist layer with a certain pattern is used as a mask, and the desired material such as metal is deposited by evaporation or other methods. Then, while removing the photoresist layer, the non-required material on the photoresist layer is also removed, leaving only the original patterned material structure on the substrate.

[0056] Peripheral electrode region: The area near the edge of the junction region of a Josephson junction, which still belongs to the junction region of the Josephson junction.

[0057] The inventors of the present application found that in the current superconducting quantum chip manufacturing process, the two-step patch process can effectively avoid the generation of parasitic junctions, and to some extent, reduce the damage of IBE near the junction area to the substrate, but it increases the steps of defining the patch in the photolithography pattern, patch metal growth and lift-off in the process of electrical connection patch, at least one mask and one photolithography etching cycle are needed, which makes the process flow complex, and may also introduce damage factors to the Josephson junction during the process. Because the Josephson junction (usually Al-AlO x -Al) needs to be etched by IBE to remove the upper electrode layer except the junction area after the formation of the Josephson junction, IBE has high energy and high penetration, although the dielectric patch layer protects the substrate below from the interface defects caused by direct bombardment of IBE, but IBE etching will still be carried out in a large area around the junction area (in order to define the junction area circuit), and its high-energy ion scattering and secondary effects (such as X-ray, ultraviolet radiation) may still cause large-area damage to the surrounding substrate material (especially the easily damaged substrate such as Si, sensitive interface or adjacent structure on sapphire). These defects will limit the performance of the prepared superconducting quantum chip.

[0058] In order to solve the above problems existing in the superconducting quantum chip manufacturing process in the prior art, the embodiments of the present application provide a superconducting quantum chip preparation method, as shown in Figure 1 The method comprises the following steps: S101: preparing a bottom layer circuit on a substrate; S101: preparing a Josephson junction on the substrate on which the bottom layer circuit has been prepared; S103: spin-coating a first photoresist on the substrate on which the bottom layer circuit and the Josephson junction have been prepared and baking; S104: spin-coating a second photoresist on the substrate on which the first photoresist has been coated and baking; S105: aligning a first mask plate to the Josephson junction, exposing and developing the first photoresist and the second photoresist to form a hollow pattern of a bridge pier in the first photoresist and the second photoresist; S106: evaporating bridge pier metal on the hollow pattern of the bridge pier by electron beam evaporation to connect the bottom layer circuit and the Josephson junction; S107: spin-coating a sacrificial layer photoresist on the substrate on which the bridge pier metal has been evaporated and baking; S108: aligning a second mask plate to the Josephson junction, exposing and developing the sacrificial layer to remove the non-air bridge area in the sacrificial layer; S109: globally etching the oxide layer by ion beam etching, and etching the deposited metal material in the non-air bridge area by inductively coupled plasma to form an air bridge patch; S110: The glue is stripped off to obtain the superconducting quantum chip.

[0059] The preparation method of the superconducting quantum chip provided in the embodiment of the application directly replaces the electrical connection patch with the air bridge patch, uses the air bridge structure for interconnection isolation as the connection structure of the Josephson junction below or nearby, retains the advantages of the patch process, avoids the parasitic junction and reduces the IBE damage to the substrate, and does not reduce the low-temperature performance of the chip. Before or at the same time as the key step of air bridge production (usually, the bridge metal is electroplated / deposited, and the sacrificial layer is released), the metallized area (i.e., the future "pier") below can be defined as the patch area. After the air bridge patch is produced, the area below the bridge body, from which the sacrificial layer is etched and released, naturally forms a low-loss air gap (air) "isolation layer", which protects the underlying material from the subsequent IBE damage of the Josephson junction layer and provides electrical isolation integrated with the air bridge structure.

[0060] The preparation method of the superconducting quantum chip provided in the embodiment of the application directly replaces the electrical connection patch with the air bridge patch, uses the air bridge structure for interconnection isolation as the connection structure of the Josephson junction below or nearby, retains the advantages of the patch process, avoids the parasitic junction and reduces the IBE damage to the substrate, and does not reduce the low-temperature performance of the chip. Before or at the same time as the key step of air bridge production (usually, the bridge metal is electroplated / deposited, and the sacrificial layer is released), the metallized area (i.e., the future "pier") below can be defined as the patch area. After the air bridge patch is produced, the area below the bridge body, from which the sacrificial layer is etched and released, naturally forms a low-loss air gap (air) "isolation layer", which protects the underlying material from the subsequent IBE damage of the Josephson junction layer and provides electrical isolation integrated with the air bridge structure.

[0061] The preparation method of the superconducting quantum chip provided in the embodiment of the application directly replaces the electrical connection patch with the air bridge patch, uses the air bridge structure for interconnection isolation as the connection structure of the Josephson junction below or nearby, retains the advantages of the patch process, avoids the parasitic junction and reduces the IBE damage to the substrate, and does not reduce the low-temperature performance of the chip. Before or at the same time as the key step of air bridge production (usually, the bridge metal is electroplated / deposited, and the sacrificial layer is released), the metallized area (i.e., the future "pier") below can be defined as the patch area. After the air bridge patch is produced, the area below the bridge body, from which the sacrificial layer is etched and released, naturally forms a low-loss air gap (air) "isolation layer", which protects the underlying material from the subsequent IBE damage of the Josephson junction layer and provides electrical isolation integrated with the air bridge structure.

[0062] Compared with a two-step patch process, the preparation method of the superconducting quantum chip provided in the embodiments of the present application saves the additional steps required for special deposition, lithography and etching of a dielectric patch layer, at least reduces one mask and one lithography and etching cycle, simplifies the process procedure, significantly reduces the manufacturing cost and period, improves the process efficiency, and improves the yield and fault tolerance of the wafer.

[0063] In one embodiment, the substrate used in the step S101 can be high resistivity silicon (HR-Si) or sapphire (Sapphire), and more specifically, for example, can be double-polished sapphire (Al2O3) or high-resistance silicon (HR-Si) with a resistivity of >10 kΩ·cm. The size of the substrate can be selected according to actual needs, for example, a typical size of 4-inch or 6-inch wafer is used. The thickness of the substrate can be 500±25 In order to grow a purer Josephson junction on the substrate, the roughness (Root Mean Square Roughness, RMS) of the substrate can be selected as RMS<0.3 nm.

[0064] In the embodiments of the present application, the substrate can be cleaned before the step S101 is performed. The specific cleaning process can include the following steps: First, the substrate is placed in Piranha solution at 120°C or higher for 10 minutes to clean the surface of the substrate and remove organic residues.

[0065] Then, the substrate is rinsed with deionized water (DI) to remove the residual Piranha solution on the surface of the substrate; Next, the substrate is blown dry with dry nitrogen; Finally, the substrate is baked in a clean oven at 150-180°C for 15-30 minutes to remove adsorbed water vapor.

[0066] The ratio of the Piranha solution used to clean the substrate in the embodiments of the present application can be H2SO4:H2O2=3:1.

[0067] In one embodiment, the step S101 of preparing a bottom layer circuit on the substrate includes the following steps: S10111: applying a negative photoresist on the substrate and baking; S10112: aligning a third mask with the substrate to expose the negative photoresist; S10113: performing flood exposure and development on the exposed negative photoresist to form a bottom layer circuit pattern on the negative photoresist; S10114: Evaporating superconducting metal on the bottom layer circuit pattern by electron beam evaporation; S10115: Immersing the substrate with the evaporated superconducting metal into a stripping solution to strip the negative photoresist, obtaining the bottom layer circuit.

[0068] In one embodiment, the step S10111 of coating the substrate with negative photoresist and baking, specifically includes the following steps: Spinning the negative photoresist on the substrate at a first rotation speed; Spinning the negative photoresist thin at a second rotation speed to reach a target thickness; Baking the negative photoresist in a hot plate.

[0069] For example, the step S10111 of coating the substrate with negative photoresist and baking, can first spin the negative photoresist on the substrate with Josephson junction prepared at a rotation speed of 500-1000 rpm for 5-10 seconds (coating); then spin the negative photoresist thin at a rotation speed of 3000-3500 rpm for 40-60 seconds to reach a target thickness, for example, less than 1.5 μm; finally, bake the negative photoresist in a hot plate for 60-90 seconds.

[0070] In the embodiment of the present application, the negative photoresist is spun and then thinned, which optimizes the uniformity and adhesion of the negative photoresist by two-step method. When spinning thin, it is necessary to ensure sufficient thickness to prevent sidewall climbing caused by metal deposition. After spinning thin to the target thickness, the purpose of pre-baking the negative photoresist is to ensure complete evaporation of the solvent, making the photoresist more dense and stable.

[0071] In the embodiment of the present application, the negative photoresist used in the step S10111 can be, for example, AZ 5214E or AZ nLOF 2000 series photoresist.

[0072] In the step S10112, the third mask plate sets the bottom layer circuit pattern, and the alignment accuracy of the third mask plate should be <±1 , preferably, the target alignment accuracy is <±0.5 .

[0073] In a specific embodiment, the step S10112 of exposing the negative photoresist can use ultraviolet exposure, which can be achieved by the following steps: Precisely aligning the third mask plate with the substrate, and using ultraviolet light to irradiate the substrate surface through the mask plate to expose the negative photoresist. The ultraviolet light source can use I-line (wavelength 365 nm), and the exposure dose can be selected as 180-280 mJ / cm².

[0074] In one embodiment, if the negative photoresist is AZ 5214E photoresist, after the negative photoresist is exposed, the method can further include: post-exposure baking the exposed negative photoresist to promote the chemical cross-linking reaction of the negative photoresist in the exposed area, and to improve the performance of the pattern after subsequent development. Specifically, the negative photoresist can be baked in a hot plate at a preset temperature range, for example, 110-130°C, for a preset time, for example, 45-120 seconds.

[0075] In one embodiment, in step S10113, the exposed negative photoresist is subjected to flood exposure and development to form a bottom layer circuit pattern on the negative photoresist, specifically including the following steps: First, without using a mask, ultraviolet light is irradiated onto the surface of the substrate to perform full exposure on the entire wafer (substrate), so that all photoresists in the area that is not exposed in step S10112 (the area that is originally to be reserved) undergo cross-linking reaction and change to insoluble negative photoresist, while the photoresist in the exposed area of step S10112 becomes soluble in the developing solution.

[0076] Then, using a developing solution, for example, AZ 726 MIF or AZ 351B (usually diluted 1:4), the wafer is subjected to shaking development or spraying development for a set time, for example, 60-120 seconds, to form a bottom layer circuit pattern on the negative photoresist.

[0077] In one embodiment, after the negative photoresist is developed in step S10113, the method can further include: hardening the negative photoresist to enhance the chemical and mechanical stability of the negative photoresist, withstand the stress of subsequent metal evaporation, and achieve complete peeling of the negative photoresist. Specifically, the negative photoresist can be baked in a hot plate at a preset temperature range, for example, 110-130°C, for a preset time, for example, 60-120 seconds.

[0078] In one embodiment, in step S10114, the bottom layer circuit is evaporated on the bottom layer circuit pattern using electron beam evaporation, specifically including the following steps: The substrate is placed in an electron beam evaporation device, and a superconducting metal, for example, aluminum or tantalum, is evaporated on the bottom layer circuit pattern in the electron beam evaporation device to form a bottom layer circuit. For example, the device parameters of the electron beam evaporation device can be set, including the vacuum base pressure and the substrate temperature, for example, the vacuum base pressure is set to 1 x 10-6 Torr, and the substrate temperature is set to <50°C. In the embodiments of the present application, a liquid nitrogen cold trap or a circulating water-cooled electron beam evaporation device base plate can be used to keep the substrate at a low temperature to prevent the negative photoresist from melting and deforming.

[0079] In an embodiment, the step S10115 of stripping the negative photoresist by immersing the substrate with the bottom layer circuit into the stripping solution can include the following steps: The stripping solution is heated to a preset temperature range, and the substrate with the bottom layer circuit is immersed in the heated stripping solution for a preset time, for example, more than 30 minutes, to strip the negative photoresist. As shown in FIG. 6, a bottom layer circuit on the substrate surface is obtained. Figure 2 The stripping solution is heated to a preset temperature range, and the substrate with the bottom layer circuit is immersed in the heated stripping solution for a preset time, for example, more than 30 minutes, to strip the negative photoresist. As shown in FIG. 6, a bottom layer circuit on the substrate surface is obtained.

[0080] In the embodiment, the negative photoresist is used to form a barrier in the exposed area, and the negative photoresist is stripped to form all the bottom layer circuits (i.e., the bottom layer superconducting metal circuit) except the Josephson junction connection point. The third mask can ensure that the bottom layer circuit avoids the Josephson junction structure area or the subsequent connection window (Pad) area. Compared with the metal etching method in the prior art, the superconducting metal is not damaged by etching.

[0081] In the embodiment, the stripping solution can use a high-strength special stripping solution, such as Microposit 1165, AZ400T, or similar high-temperature and high-efficiency stripping solution, and the corresponding heating temperature range can be 70-85°C.

[0082] In a specific embodiment, after the substrate with the bottom layer circuit is immersed in the heated stripping solution in the step S10115, a very mild ultrasonic wave (<50W, 40kHz) or megasonic wave stripping solution can be used to improve the stripping efficiency.

[0083] In an embodiment, after the substrate with the bottom layer circuit is immersed in the stripping solution to strip the negative photoresist in the step S10115, the method can further include: The substrate with the stripped negative photoresist is immersed in fresh stripping solution for a preset time. The substrate with the stripped negative photoresist is sequentially rinsed with pure acetone solution, isopropyl alcohol solution, and deionized water to obtain the bottom layer circuit. Nitrogen is used for drying.

[0084] In a specific embodiment, after the substrate with the stripped negative photoresist is immersed in the fresh stripping solution, a very mild ultrasonic wave (<50W, 40kHz) or megasonic wave stripping solution can be used for short-time oscillation to improve the cleaning efficiency.

[0085] In another embodiment, the step S101 of preparing the bottom layer circuit on the substrate can include the following steps: S10121: depositing a superconducting metal on the substrate; S10122: spin-coating a positive photoresist on the substrate on which the superconducting metal has been deposited; S10123: exposing and developing the positive photoresist on the substrate by using a fourth mask; S10124: etching the superconducting metal on the substrate after development to obtain a bottom layer circuit; S10125: stripping the remaining positive photoresist.

[0086] In an embodiment, the step S10121 of depositing a superconducting metal on the substrate can be performed by using an electron beam evaporation or a magnetron sputtering deposition.

[0087] In an embodiment, the superconducting metal used in the step S10121 can be aluminum or tantalum, or other superconducting metals.

[0088] For example, when Al is used as the bottom layer metal, such as 5N pure Al, the substrate is placed in an electron beam evaporation device, the superconducting metal is evaporated in the electron beam evaporation device, and the superconducting metal is deposited to a preset thickness, such as 150 nm. Before deposition, the device parameters of the electron beam evaporation device can be set, including the base pressure and the substrate temperature, for example, the base pressure is set to 5x10-6Torr, and the substrate temperature is set to <50°C. In an embodiment, a liquid nitrogen cold trap or a circulating water-cooled electron beam evaporation device base plate can be used to keep the substrate at a low temperature to prevent the negative photoresist from melting and deforming.

[0089] For example, when Ta is used as the bottom layer metal, such as 3N5 Ta, the substrate is placed in a magnetron sputtering device, the superconducting metal is first pre-sputtered for a preset time, such as 5 min, to remove the oxide layer, and then the superconducting metal is magnetron sputtered on the substrate to a preset thickness, such as 100 nm. Before deposition, the device parameters of the magnetron sputtering device can be set, including the power, Ar pressure, and deposition rate, for example, the power is set to 500 W, the Ar pressure is set to 5 mTorr, and the deposition rate is set to 10 nm / min, to obtain a Ta metal layer with a resistivity of 1.0x10-5

[0090] ​​In step S10122, the positive photoresist is spin-coated on the substrate and baked. The spin-coating of the photoresist can be performed by a spin coater, a spin coater, etc. During the spin-coating process, the photoresist is uniformly spread on the surface of the substrate under the action of centrifugal force. As the rotation speed increases, the thickness of the photoresist gradually thins and the distribution becomes more uniform. The rotation speed and spin-coating time of the spin coater can be set according to the amount of photoresist to be spin-coated and the final desired thickness of the photoresist.

[0091] For example, in step S10122, the spin-coating speed of the positive photoresist AZ1500 is 3000 rpm, and the thickness of the photoresist layer is 1.2 .

[0092] In the embodiment of the present application, in step S10123, the fourth mask is provided with a bottom layer circuit pattern, and the alignment accuracy of the fourth mask should be <±1 , and preferably, the target alignment accuracy is <±0.5 .

[0093] In a specific embodiment, in step S10123, the positive photoresist is exposed, and ultraviolet exposure can be used, which can be implemented by the following steps: The fourth mask is accurately aligned with the substrate, and the mask alignment accuracy can be ±0.5 UV light is used to irradiate the surface of the substrate through the mask, and the positive photoresist is exposed. The UV light source can use I-line (wavelength 365 nm), and the exposure dose can be selected as 120 mJ / cm².

[0094] In an embodiment, in step S10123, the exposed positive photoresist is developed, which includes the following steps: Using a developing solution, shake developing or spray developing is performed according to the set time, for example, 60-120 seconds, to form a bottom layer circuit pattern on the photoresist.

[0095] In an embodiment, the developing solution used in step S10123 can be AZ 300 MIF or AZ326 MIF (usually diluted by 1:4).

[0096] In a specific embodiment, in step S10123, the substrate after development is etched to obtain a bottom layer circuit, which includes: The substrate after development is etched by inductively coupled plasma (ICP) etching or reactive ion etching (RIE) to obtain a bottom layer circuit.

[0097] For example, if the deposited bottom metal is Al, the process of etching the superconducting metal using ICP on the developed substrate can include: putting the developed substrate into an ICP chamber and fixing it; after vacuumizing, precisely introducing Cl2 / BCl3 / Ar mixed gas into the chamber, adjusting the gas pressure, for example, 20 mTorr; setting and applying radio frequency power, for example, 300 W, to generate plasma, and at the same time, setting a bias voltage, for example, 50 V, to etch the metal oxide layer of the bottom circuit pattern at a preset etching rate, for example, 200 nm / min, to obtain the bottom circuit.

[0098] For example, if the deposited bottom metal is Ta, the process of etching the superconducting metal using RIE on the developed substrate can include: putting the substrate into the chamber of a reactive ion etching machine and fixing it; after vacuumizing, precisely introducing CF4 / O2 mixed gas into the chamber; adjusting the gas pressure, for example, 20 mTorr; setting and applying radio frequency power, for example, 200 W, to generate plasma, and at the same time, setting a bias voltage, for example, 50 V, to etch the metal oxide layer of the bottom circuit pattern at a preset etching rate, for example, 40 nm / min, to obtain the bottom circuit.

[0099] In an embodiment, the step S10125 of removing the remaining positive photoresist by peeling off can include the following steps: using a plasma (O2) cleaning device to ash the substrate with the prepared bottom circuit, for example, ashing for 300 s, to remove the remaining positive photoresist; putting the substrate with the removed positive photoresist into an acetone solution and using ultrasonic oscillation of the acetone solution to remove the residual positive photoresist, to obtain the bottom circuit on the surface of the substrate, as shown in Figure 2 .

[0100] In an embodiment, the step S102 of preparing a Josephson junction on the substrate with the prepared bottom circuit can include the following steps: S1021: spin-coating a third photoresist on the substrate with the prepared bottom circuit and baking; S1022: spin-coating a fourth photoresist on the substrate with the prepared bottom circuit and baking; S1023: exposing, developing and fixing the third photoresist and the fourth photoresist to form a hollow pattern of a cross-shape gap in the third photoresist and the fourth photoresist; the cross-shape gap includes a first gap and a second gap intersecting with each other; S1024: depositing a bottom superconducting metal layer in the first gap with electron beam evaporation at a first angle θ1; S1025: performing in-situ oxidation treatment on the surface of the bottom superconducting metal layer to generate an in-situ oxidation layer; S1026: depositing a top superconducting metal layer in the second gap with electron beam evaporation at a second angle θ2; the top superconducting metal layer intersects with the bottom superconducting metal layer having prepared the in-situ oxidation layer; S1027: peeling off the remaining third photoresist and fourth photoresist to obtain a Josephson junction.

[0101] In the embodiment of the present application, the third photoresist can be methyl methacrylate (MMA) for example. The fourth photoresist can be polymethyl methacrylate (PMMA) for example.

[0102] In the above step S1021, the third photoresist is spin-coated on the substrate and baked to form a lower photoresist layer. The third photoresist can be spin-coated by a spin coater, a spin coater, etc. During the spin coating process, the photoresist is uniformly spread on the surface of the substrate under the action of centrifugal force. With the increase of the speed, the thickness of the photoresist will gradually become thinner, and the distribution will be more uniform. The speed and spin time of the spin coater can be set according to the amount of photoresist to be spin-coated and the final desired thickness of the photoresist. In the above step S1022, the fourth photoresist is spin-coated and baked to form an upper photoresist layer. The principle and steps of the third photoresist are similar, and will not be repeated here.

[0103] For example, in the embodiment of the present application, the third photoresist and the fourth photoresist use two different types of PMMA, and the thickness of the two photoresists is set to 300 nm. More specifically, the third photoresist uses PMMA A4, 950K, and the thickness of the photoresist is 150 nm, while the fourth photoresist uses PMMA A4, 495K, and the thickness of the photoresist is 150 nm.

[0104] In the embodiment of the present application, the lower photoresist (third photoresist) is spin-coated to facilitate the exposure, development and fixation in the subsequent step S1023 to form a controllable undercut, and the upper photoresist (fourth photoresist) is spin-coated to provide a high-resolution pattern carrier for the exposure, development and fixation in the subsequent step S1023.

[0105] In the embodiment of the present application, after spin coating, the purpose of pre-baking the third photoresist is to remove the solvent in the photoresist, and the purpose of pre-baking the fourth photoresist is to enhance the adhesion of the photoresist, making the photoresist more dense and stable. Baking can be done in a hot plate or an oven.

[0106] For example, the temperature for baking the third photoresist in the hot plate is set to 110°C, and the baking time is 90s. The temperature for baking the fourth photoresist in the hot plate is set to 180°C, and the baking time is 300s.

[0107] In an embodiment, the exposure of the third photoresist and the fourth photoresist in S1023 can be performed by using an electron beam. Specifically, the exposure can be performed by the following steps: exposing the third photoresist and the fourth photoresist in the Josephson junction core junction region by using a first preset dose of exposure amount in an electron beam lithography device with a preset voltage and beam current; and exposing the third photoresist and the fourth photoresist in the peripheral electrode region outside the Josephson junction core junction region by using a second preset dose of exposure amount.

[0108] In an embodiment, the device parameters of the electron beam lithography device, including the preset voltage and beam current, can be set according to actual conditions. For example, the dose is set to 550 C / cm², the voltage is set to 100 kV, and the beam current is set to 1nA.

[0109] The principle of electron beam exposure is to directly hit the focused electron beam spot on the photoresist surface, so that the chemical properties of the photoresist change. The electron beam can scan the photoresist surface according to the required pattern in advance. When the electron beam irradiates the photoresist surface, the molecules in the photoresist will absorb the energy of the electrons and undergo a chemical reaction, thereby changing the solubility of the photoresist. In the development process, the exposed area will be dissolved by the developer, and the unexposed area will remain, forming the desired hollow pattern of the Josephson junction.

[0110] In an embodiment, the development of the third photoresist and the fourth photoresist in S1013 can be performed by using a developer mixed by methyl isobutyl ketone (MIBK) and isopropyl alcohol (IPA) in a ratio of 1:3. The exposed part of the third photoresist and the fourth photoresist is developed at room temperature, for example, 22°C, for a set time, for example, 60±5s.

[0111] In an embodiment, after the development of the third photoresist and the fourth photoresist in S1013, the following method can be used for stopping development: the developed substrate is soaked in an isopropyl alcohol solution for a preset time, for example, 30s, to remove the developer; and then dried by using dry nitrogen.

[0112] In one embodiment, the third photoresist and the fourth photoresist are fixed in S1013, and a light etching is performed on the developed substrate using plasma to remove the residual developer, so as to achieve the fixing and form the hollow pattern of the cross-shaped gap in the third photoresist and the fourth photoresist. The active particles in the plasma can quickly react with the organic matter remaining on the surface or physically impact the organic matter to separate the organic matter from the surface of the object, so as to remove the residual organic matter on the sidewall of the cross-shaped gap and the surface of the substrate.

[0113] The power used by the plasma cleaning equipment directly determines the degree of gas ionization and the density and energy state of the active particles (such as ions, electrons, radicals, etc.) in the generated plasma. For example, the light etching of the developed substrate using plasma can use a plasma cleaning equipment with a cleaning power of 50 W and a light etching time of 10 s.

[0114] In the embodiment of the present application, the superconducting metal layer in S10124 and S1026 can be an aluminum layer or other superconducting metal layer. The evaporation of the superconducting metal layer can be achieved by electron beam evaporation. For example, the first angle in S1024 can be 0°, and the second angle in S1026 can be ±30°.

[0115] For example, when the superconducting metal layer is an aluminum layer, the substrate can be placed in an electron beam evaporation equipment, and S1024 to S1026 can be performed in the electron beam evaporation equipment to form a Josephson junction. For example, the device parameters of the electron beam evaporation equipment can be set, including the vacuum base pressure and the substrate temperature. For example, the vacuum base pressure can be set to 1e-6 Torr, and the substrate temperature can be set to 80 K. For example, when the thickness of the third photoresist is 40 nm, the rate is 1 nm / s, the O2 pressure for in-situ oxidation is 500 mTorr, and the exposure time is 90 s, and the thickness of the third photoresist is 60 nm, the rate is 1.5 nm / s, a Josephson junction is formed. For example, the size of the Josephson junction can be a typical size of 0.2x0.2 m², and the critical current density Jc≈50 A / m².

[0116] In one embodiment, the remaining third photoresist and fourth photoresist are removed in S1027 to obtain a Josephson junction. For example, the substrate with the bottom superconducting metal layer and the top superconducting metal layer evaporated and intersected can be immersed in an N-methyl pyrrolidone (NMP) solution at a preset temperature, for example, 80°C, for a preset time, for example, 120 min, to remove the remaining third photoresist and fourth photoresist, and obtain a Josephson junction, as shown in FIG. 8B. Figure 3 ​​​as shown.

[0117] NMP has strong solubility, which can quickly and effectively dissolve photoresist. This helps to completely remove residual photoresist after the photoetch process, improves cleaning efficiency, reduces the impact of photoresist residues on subsequent processes, in addition, NMP has less solubility to the underlying substrate material or other adjacent materials. This selective dissolution property can maximize the protection of the bottom layer material and the integrity of the device structure during the removal of photoresist, which is beneficial to realize high-precision, complex structure micro-nano processing.

[0118] In a specific embodiment, during the removal of the remaining third photoresist and fourth photoresist, the NMP solution can also be ultrasonically or megasonic oscillated.

[0119] In another embodiment, the remaining third photoresist and fourth photoresist are removed in step S1027 to obtain the Josephson junction. The substrate on which the bottom superconducting metal layer and the top superconducting metal layer are deposited can be immersed in an acetone solution for a predetermined time, for example, 30 min, to remove the remaining third photoresist and fourth photoresist and obtain the Josephson junction.

[0120] In a specific embodiment, during the removal of the remaining third photoresist and fourth photoresist, the acetone solution can also be ultrasonically or megasonic oscillated.

[0121] In one embodiment, after the remaining third photoresist and fourth photoresist are removed to obtain the Josephson junction, the following steps can also be performed: The substrate from which the third photoresist and fourth photoresist are removed is immersed in an isopropyl alcohol (IPA) solution for a predetermined time to remove organic matter. Blow-dried with nitrogen.

[0122] The isopropyl alcohol solution can further remove the organic matter generated or remaining in the previous steps, so as to ensure the cleanliness of the prepared Josephson junction, improve the quality and performance of the Josephson junction, and improve the yield.

[0123] In the embodiments of the present application, the first photoresist can be LOR 3A, and the second photoresist can be AZ1500. The thickness of the two photoresist layers is 2.5 m.

[0124] In an embodiment, the first photoresist is spin-coated and baked on the substrate with the prepared bottom circuit and Josephson junction in step S103. The spin-coating of the photoresist can be performed by a spin coater, a spinner, or the like. During the spin-coating process, the photoresist is spread uniformly on the surface of the substrate under the action of centrifugal force. As the rotation speed increases, the thickness of the photoresist gradually thins, and the distribution becomes more uniform. The rotation speed and the spin-coating time of the spin coater or the spinner can be set according to the amount of the photoresist to be spin-coated and the final desired thickness of the photoresist. In step S104, the second photoresist is spin-coated and baked to form the upper photoresist layer. The steps and principles of forming the upper photoresist layer are similar to those of the first photoresist, which are not described here again.

[0125] In an embodiment of the present application, the purpose of pre-baking the first photoresist and the second photoresist after spin-coating is to remove the solvent in the photoresist, making the photoresist more dense and stable. The baking can be performed in a hot plate or an oven. For example, the temperature of the hot plate for baking the photoresist is set to 90-100°C, and the baking time is 60-90s.

[0126] In step S105, the first mask is provided with all the bridge patterns needed to be connected to the Josephson junction. Before exposure, the first mask needs to be accurately aligned with the prepared Josephson junction. The overlay accuracy should be <±1 m, and preferably, the target overlay accuracy is <±0.5 m, so as to ensure the alignment of the exposed area with the bridge pattern reserved in advance.

[0127] In a specific embodiment, the first photoresist and the second photoresist are exposed in step S105. Ultraviolet exposure can be used, which can be achieved by the following steps: The first mask is accurately aligned with the prepared Josephson junction, and ultraviolet light is used to irradiate the surface of the substrate through the mask to expose the first photoresist and the second photoresist. The ultraviolet light source can use I-line (wavelength 365nm). Assuming that the size of the bridge is , the exposure dose can be set to 200mJ / cm².

[0128] In an embodiment, the first photoresist and the second photoresist after exposure are developed in step S105 to form the hollow pattern of the bridge in the first photoresist and the second photoresist, which includes the following steps: A developing solution, such as AZ 300MIF, is used for shaking development or spray development according to the set time, such as 45-60 seconds, to form the hollow pattern of the bridge in the first photoresist and the second photoresist, as shown in Figure 4 .

[0129] In an embodiment, after the third photoresist is developed in step S105, the method further comprises: The first photoresist and the second photoresist are baked to enhance the chemical and mechanical stability of the first photoresist and the second photoresist. Specifically, the first photoresist and the second photoresist can be baked in a hot plate at a preset temperature range, for example, 110-120°C, for a preset time, for example, 60-90 seconds.

[0130] In a specific embodiment, after the first photoresist and the second photoresist are developed in step S105, the method further comprises: The developed substrate is cleaned by using plasma to remove the first photoresist and the second photoresist remaining in the hollow pattern of the bridge.

[0131] For example, the developed substrate is cleaned by using a plasma cleaning device, so that more oxygen molecules are ionized to form oxygen radicals with strong oxidizing properties, thereby more efficiently decomposing and removing organic contaminants and ensuring clean interface cleaning. For example, the cleaning power of the plasma cleaning device can be set to <50W, the rotation speed is set to 100-200 mTorr, and the cleaning time is 30-60s.

[0132] In an embodiment, in step S106, the bridge metal is deposited on the hollow pattern of the bridge by electron beam evaporation to connect the bottom layer circuit and the Josephson junction, which can specifically include the following steps: The substrate is placed in an electron beam evaporation device, and a superconducting metal, for example, aluminum or tantalum, is deposited on the hollow pattern of the bridge in the electron beam evaporation device to form an air bridge structure. For example, the device parameters of the electron beam evaporation device can be set, including the vacuum base pressure and the substrate temperature, for example, the vacuum base pressure is set to <5x10⁻ 7 Torr, and the substrate temperature is set to <50°C. In the embodiment of the present application, a liquid nitrogen cold trap or a circulating water-cooled electron beam evaporation device base can be used to keep the substrate at a low temperature to prevent the photoresist from melting and deforming.

[0133] In the embodiment of the present application, the superconducting metal deposited in the hollow pattern of the bridge can be 5N grade Al, and the thickness of the superconducting metal film can be 4nm to ensure the mechanical strength and superconducting current carrying capacity of the connection, and the film covers the window sidewall (needs to cover the JJ junction area edge to expand 1 m), to ensure that the Josephson junction patch forms good ohmic contact and superconducting connection with the Josephson junction and the bottom layer circuit.

[0134] In an embodiment, in the step S107, the sacrificial layer photoresist is spin-coated on the substrate and baked. The spin-coating of the photoresist can be performed by a spin coater, a spin coater, etc. During the spin-coating process, the photoresist is uniformly spread on the surface of the substrate under the action of centrifugal force. As the rotation speed increases, the thickness of the photoresist gradually thins, and the distribution becomes more uniform. The rotation speed and spin-coating time of the spin coater can be set according to the amount of photoresist to be spin-coated and the final desired thickness of the photoresist.

[0135] For example, the sacrificial layer photoresist can be AZ 4903 (high thickness photoresist). After spin-coating at a speed of 1000 rpm for 5 s and maintaining the speed at 800 rpm for 60 s, the thickness of the photoresist is 10 m.

[0136] In an embodiment of the present application, after spin-coating is completed, the sacrificial layer photoresist is pre-baked to remove the solvent in the photoresist, making the photoresist more dense and stable. The baking can be performed in a hot plate or an oven.

[0137] For example, the temperature of the hot plate for baking the sacrificial layer photoresist is set to 90-110°C, and the baking time is 5-10 min.

[0138] In an embodiment, before performing the step S107, the method can further include the following steps: The substrate with the deposited bridge metal is placed in a hexamethyldisilazane (HMDS) pretreatment device for adhesion treatment with HMDS vapor to improve the adhesion of the photoresist to the substrate. The pretreatment time can be set according to actual conditions, for example, 60 s.

[0139] In an embodiment of the present application, in the step S108, the second mask plate is provided with an air bridge pattern, for example, the width of the suspended bridge body in the air bridge pattern is 5-15 m, and the length is 20-100 m.

[0140] In a specific embodiment, in the step S108, the exposure of the sacrificial layer can be performed by ultraviolet exposure, which can be achieved by the following steps: The second mask plate is precisely aligned with the substrate, and ultraviolet light is used to irradiate the surface of the substrate through the mask plate to expose the sacrificial layer photoresist. The ultraviolet light source can be I-line (wavelength 365 nm), and the exposure dose can be selected as 500 mJ / cm².

[0141] In an embodiment, in the step S108, the exposed sacrificial layer photoresist is developed to remove the non-air bridge region in the sacrificial layer, which includes the following steps: Spray development is performed using a developer, such as AZ 400K (typically diluted 1:4), for a set time, such as 60-120 seconds, to remove the non-air-bridge regions in the sacrificial layer.

[0142] In an embodiment, the globally etching the oxide layer in S109 is performed by ion beam etching (IBE), and includes the following steps: The substrate is placed into a chamber of an Ar+ ion beam etching machine and fixed; After vacuumizing, Ar gas is precisely introduced into the chamber; The etching parameters of the Ar+ ion beam etching machine are set, and the oxide layer is globally etched, wherein the etching parameters include: acceleration voltage, typically 400V, beam current density, typically 0.8 mA / cm2, incident angle: 0° vertical etching, etching time, such as 120s, to achieve 200nm etching.

[0143] In an embodiment, the deposited metal material in the non-air-bridge region is etched in S109 by inductively coupled plasma to form an air-bridge patch, and includes the following steps: The substrate is placed into a chamber of an ICP device and fixed; After vacuumizing, Cl2 / BCl3 / Ar mixed gas is precisely introduced into the chamber, and the gas pressure is adjusted, such as 20mTorr; Power, such as 300W, is set and applied to generate plasma, and at the same time, bias voltage, such as 50V, is set, and the deposited metal material in the non-air-bridge region is etched at a preset etching rate, such as 200nm / min, to form an air-bridge patch.

[0144] In the embodiments, when etching, accurate etching parameters are selected to ensure that the Josephson junction is not damaged.

[0145] In an embodiment, the photoresist is removed in S110 to obtain a superconducting quantum chip, and the method can include the following steps: The substrate is immersed in a N-methyl pyrrolidone (NMP) solution at a preset temperature, such as 80℃, for a preset time, such as 60min, to remove the remaining photoresist, and obtain a superconducting quantum chip, as shown in Figure 5 .

[0146] Based on the same inventive concept, the embodiments of the present application also provide a superconducting quantum chip, which is prepared according to the method for preparing a superconducting quantum chip as described above.

[0147] Obviously, many modifications and variations of the present application are possible in light of the above teachings. It is, therefore, to be understood that within the scope of the appended claims and their equivalents, the application can be practiced otherwise than as specifically described.

Claims

1. A method of fabricating a superconducting quantum chip, characterized by, The method comprises the following steps: preparing a bottom layer circuit on a substrate; preparing a Josephson junction on the substrate on which the bottom layer circuit has been prepared; spinning a first photoresist on the substrate on which the bottom layer circuit and the Josephson junction have been prepared and baking; spinning a second photoresist on the substrate on which the first photoresist has been coated and baking; aligning a first mask plate with the Josephson junction, exposing and developing the first photoresist and the second photoresist to form a hollow pattern of a bridge pier in the first photoresist and the second photoresist; evaporating a bridge pier metal on the hollow pattern of the bridge pier by using electron beam evaporation to connect the bottom layer circuit and the Josephson junction; spinning a sacrificial layer photoresist on the substrate on which the bridge pier metal has been evaporated and baking; aligning a second mask plate with the Josephson junction, exposing and developing the sacrificial layer photoresist to remove the non-air-bridge area in the sacrificial layer photoresist; globally etching the oxide layer by using ion beam etching and etching the deposited metal material in the non-air-bridge area by using inductively coupled plasma to form an air-bridge patch; stripping to obtain a superconducting quantum chip.

2. The method of claim 1, wherein, Before the step of spinning the sacrificial layer photoresist on the substrate on which the bridge pier metal has been evaporated and baking, the method further comprises the following step: putting the substrate on which the bridge pier metal has been evaporated into a hexamethyldisilazane pretreatment device to perform tackiness treatment by using hexamethyldisilazane vapor.

3. The method of claim 1, wherein, The step of stripping to obtain a superconducting quantum chip comprises the following step: immersing the etched substrate into an N-methylpyrrolidone solution to remove all remaining photoresists and obtain a superconducting quantum chip.

4. The method of claim 1, wherein, The step of preparing a bottom layer circuit on a substrate comprises the following steps: coating a negative photoresist on the substrate and baking; aligning a third mask plate with the substrate, exposing the negative photoresist; performing flood exposure and development on the exposed negative photoresist to form a bottom layer circuit pattern on the negative photoresist; evaporating a superconducting metal on the bottom layer circuit pattern by using electron beam evaporation; immersing the substrate on which the superconducting metal has been evaporated into a stripping solution to strip the negative photoresist and obtain a bottom layer circuit.

5. The method of claim 4, wherein, The step of coating a negative photoresist on a substrate and baking comprises the following steps: spinning a negative photoresist on the substrate at a first rotation speed; spinning the negative photoresist at a second rotation speed to achieve a target thickness of the negative photoresist; baking the negative photoresist in a hot plate.

6. The method of claim 4, wherein, The negative photoresist is AZ 5214E photoresist. After the step of exposing the negative photoresist, the method further comprises the following step:

7. The method of claim 4, wherein, post-baking the exposed negative photoresist.

8. The method of claim 4, wherein, After the step of developing the negative photoresist, the method further comprises the following step: hardening the negative photoresist.

9. The method of claim 4, wherein, The step of immersing the substrate on which the superconducting metal has been evaporated into a stripping solution to strip the negative photoresist comprises the following steps: heating the stripping solution to a preset temperature range, immersing the substrate on which the superconducting metal has been evaporated into the heated stripping solution for a preset time length, and stripping the negative photoresist. After the step of immersing the substrate on which the superconducting metal has been evaporated into a stripping solution to strip the negative photoresist and obtain a bottom layer circuit, the method further comprises the following steps: replacing fresh stripping solution, immersing the substrate on which the negative photoresist has been stripped into the fresh stripping solution for a preset time length; sequentially flushing the substrate on which the negative photoresist has been stripped with pure acetone solution, isopropyl alcohol solution and deionized water; blowing dry with nitrogen.

10. The method of claim 1, wherein, The method for preparing the bottom layer circuit on the substrate comprises: depositing a superconducting metal on the substrate; spin-coating a positive photoresist on the substrate on which the superconducting metal has been deposited; exposing and developing the positive photoresist on the substrate by aligning a fourth mask to the substrate; etching the superconducting metal on the developed substrate to obtain the bottom layer circuit; stripping the remaining positive photoresist.

11. The method of any one of claims 1-10, wherein, The method for preparing the Josephson junction on the substrate on which the bottom layer circuit has been prepared comprises: spin-coating a third photoresist on the substrate on which the bottom layer circuit has been prepared and baking; spin-coating a fourth photoresist on the substrate on which the first photoresist has been coated and baking; exposing, developing and fixing the third photoresist and the fourth photoresist to form a hollow pattern of cross-shaped gaps in the third photoresist and the fourth photoresist; the cross-shaped gaps comprise first gaps and second gaps intersecting with each other; depositing a bottom layer superconducting metal layer in the first gaps at a first angle by electron beam evaporation; performing in-situ oxidation treatment on the surface of the bottom layer superconducting metal layer to generate an in-situ oxidation layer; depositing a top layer superconducting metal layer in the second gaps at a second angle by electron beam evaporation; the top layer superconducting metal layer intersects with the bottom layer superconducting metal layer on which the in-situ oxidation layer has been prepared; stripping the remaining third photoresist and fourth photoresist to obtain the Josephson junction.

12. A superconducting quantum chip, characterized by The superconducting quantum chip is prepared according to the method for preparing the superconducting quantum chip according to any one of claims 1-11. The method for preparing the bottom layer circuit on the substrate comprises: depositing a superconducting metal on the substrate; spin-coating a positive photoresist on the substrate on which the superconducting metal has been deposited; exposing and developing the positive photoresist on the substrate by aligning a fourth mask to the substrate; etching the superconducting metal on the developed substrate to obtain the bottom layer circuit; stripping the remaining positive photoresist. The method for preparing the Josephson junction on the substrate on which the bottom layer circuit has been prepared comprises: spin-coating a third photoresist on the substrate on which the bottom layer circuit has been prepared and baking; spin-coating a fourth photoresist on the substrate on which the first photoresist has been coated and baking; exposing, developing and fixing the third photoresist and the fourth photoresist to form a hollow pattern of cross-shaped gaps in the third photoresist and the fourth photoresist; the cross-shaped gaps comprise first gaps and second gaps intersecting with each other; depositing a bottom layer superconducting metal layer in the first gaps at a first angle by electron beam evaporation; performing in-situ oxidation treatment on the surface of the bottom layer superconducting metal layer to generate an in-situ oxidation layer; depositing a top layer superconducting metal layer in the second gaps at a second angle by electron beam evaporation; the top layer superconducting metal layer intersects with the bottom layer superconducting metal layer on which the in-situ oxidation layer has been prepared; stripping the remaining third photoresist and fourth photoresist to obtain the Josephson junction. The superconducting quantum chip is prepared according to the method for preparing the superconducting quantum chip according to any one of claims 1-11.