Phosphotungstic acid supported Zr-SBA-12 molecular sieve as well as preparation method and application thereof

By introducing zirconium and loading phosphotungstic acid into SBA-12 molecular sieve, a phosphotungstic acid-supported Zr-SBA-12 molecular sieve is formed, which solves the problem of insufficient acidity of SBA-12 molecular sieve, realizes the efficient nitration reaction of acetanilide, avoids the environmental pollution of the traditional mixed acid nitration method, and the catalyst can be recycled.

CN121467086APending Publication Date: 2026-02-06LIAONING UNIVERSITY OF PETROLEUM AND CHEMICAL TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202511686962.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-11-18
Publication Date
2026-02-06

AI Technical Summary

Technical Problem

The existing SBA-12 molecular sieve has relatively weak acidity, which limits its catalytic application prospects in the nitration reaction of acetanilide. In addition, the traditional mixed acid nitration method has problems such as equipment corrosion, difficulty in waste acid treatment and environmental pollution.

Method used

By introducing zirconium (Zr) into SBA-12 molecular sieve and loading phosphotungstic acid, a phosphotungstic acid-supported Zr-SBA-12 molecular sieve is formed. The synergistic effect of Zr doping enhancing acidity and phosphotungstic acid is utilized to form a composite catalyst with high acidity, site density and good structural stability.

Benefits of technology

It increases the number of acidic sites and catalytic activity of the catalyst, solves the problems of difficult and costly recovery of phosphotungstic acid, realizes a green nitration process, avoids the generation of waste acid and equipment corrosion, and has high catalytic efficiency and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121467086A_ABST
    Figure CN121467086A_ABST
Patent Text Reader

Abstract

The invention provides a phosphotungstic acid supported Zr-SBA-12 molecular sieve as well as a preparation method and application thereof, and belongs to the technical field of molecular sieve catalysts. According to the preparation method, an SBA-12 molecular sieve is taken as a carrier, Zr is introduced into an SBA-12 molecular sieve framework through a hydrothermal synthesis method, then phosphotungstic acid is loaded on the Zr-SBA-12 molecular sieve through a direct hydrothermal method, and the composite catalyst with high acidity, site density and good structural stability is obtained. Through the synergistic effect of the metal Zr and the phosphotungstic acid, the number of acid sites and the catalytic activity of the catalyst are remarkably improved, the surface acidity of the molecular sieve is improved, and the problems of difficult recovery and high cost are solved. And the phosphotungstic acid supported Zr-SBA-12 molecular sieve as a catalyst has important research value and application prospect in the field of acetanilide nitration reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of molecular sieve catalyst technology, and in particular to a phosphotungstic acid supported Zr-SBA-12 molecular sieve, its preparation method, and its application. Background Technology

[0002] Aromatic nitro compounds are important intermediates in the production of fine chemicals such as dyes, pharmaceuticals, and pesticides. p-Nitroacetanilide, as an important organic intermediate, is widely used in these fields. Currently, the industrial production of p-nitroacetanilide mainly employs the mixed acid (H2SO4 / HNO3) nitration method. However, this method suffers from problems such as severe equipment corrosion, difficulty in waste acid treatment, significant environmental pollution, and low selectivity.

[0003] Molecular sieve catalysts have become a research hotspot in green nitration technology due to their regular pore structure, tunable acidic sites, and good thermal stability. SBA-12 molecular sieves possess a three-dimensional hexagonal structure (space group P63 / mmc) and a high specific surface area (typically greater than 1000 m²). 2 With its good thermal stability (g / g), SBA-12 molecular sieve is an ideal catalyst support. However, the weak acidity of existing SBA-12 molecular sieves limits its catalytic application prospects. Summary of the Invention

[0004] The purpose of this invention is to provide a phosphotungstic acid-supported Zr-SBA-12 molecular sieve, its preparation method, and its application. It features high acidity, high site density, and good structural stability, and has the advantage of high catalytic efficiency in the nitration reaction of acetanilide.

[0005] To achieve the above-mentioned objectives, the present invention provides the following technical solution: This invention provides a method for preparing phosphotungstic acid-supported Zr-SBA-12 molecular sieves, comprising the following steps: A mixture is obtained by mixing silicon source, zirconium source, template agent, acid and water; The mixture was mixed with phosphotungstic acid and subjected to a hydrothermal reaction to obtain a hydrothermal product; The hydrothermal product was calcined to obtain phosphotungstic acid-supported Zr-SBA-12 molecular sieve.

[0006] Preferably, the silicon source includes tetraethyl silicate, methyl orthosilicate, silica sol, diatomaceous earth, or photovoltaic silicon waste; the zirconium source includes ZrOCl2·8H2O, Zr(NO3)4·5H2O, Zr(CH3COO)4·4H2O, or Zr(OH)4.

[0007] Preferably, the molar ratio of Zr in the zirconium source to Si in the silicon source is 0.025 to 0.1:1.

[0008] Preferably, the template agent includes Brij76, Brij58, Brij78, P123, or F127; the acid includes hydrochloric acid or nitric acid; the mass concentration of the hydrochloric acid is 36%~38%, and the mass concentration of the nitric acid is 65%. The mass ratio of the template agent, acid, and water is 1:(5.7~6.1):(18.5~19.9); The mass ratio of the template agent to the silicon source is 1:2.78~3.0.

[0009] Preferably, the mass of the phosphotungstic acid is 5 to 55% of the total mass of the phosphotungstic acid-supported Zr-SBA-12 molecular sieve.

[0010] Preferably, the hydrothermal reaction is carried out at a temperature of 90-110°C for 20-28 hours.

[0011] Preferably, the calcination temperature is 500~600℃ and the time is 6~8h.

[0012] The present invention provides a phosphotungstic acid supported Zr-SBA-12 molecular sieve prepared by the preparation method described in the above technical solution.

[0013] This invention provides the application of the phosphotungstic acid-supported Zr-SBA-12 molecular sieve described above in the nitration reaction of acetanilide.

[0014] Preferably, the method of application includes: mixing the catalyst, acetanilide and HNO3 to carry out a nitration reaction, wherein the catalyst is the phosphotungstic acid supported Zr-SBA-12 molecular sieve described in the above technical solution; The nitration reaction takes 6-10 hours and is carried out at a temperature of 70-90°C. The mass ratio of the catalyst to acetanilide is 1:(2.25-4.5). The molar ratio of HNO3 to acetanilide is 1.5-3:1.

[0015] This invention provides a method for preparing a phosphotungstic acid-supported Zr-SBA-12 molecular sieve. Using SBA-12 molecular sieve as a support, Zr is first introduced into the SBA-12 molecular sieve framework via a hydrothermal synthesis method, and then phosphotungstic acid is supported on the Zr-SBA-12 molecular sieve using a direct hydrothermal method, resulting in a composite catalyst with high acidity, high site density, and good structural stability. The introduction of zirconium (Zr) enhances the acidity of the molecular sieve, increases the number of surface active sites, and improves the thermal stability of the molecular sieve. Phosphotungstic acid, as a strong acidic heteropolyacid, exhibits good catalytic performance in nitration reactions, but its specific surface area is low (<30 m² / g) and it is easily soluble in polar solvents, making it difficult to recover. This invention supports phosphotungstic acid on a molecular sieve support to form a heterogeneous catalyst, using Zr… 4+Ionic substitution of Si in the SBA-12 molecular sieve framework 4+ The Zr-doped Zr-SBA-12 molecular sieve is formed. The synergistic effect between the Zr-doped molecular sieve and phosphotungstic acid significantly increases the number of acidic sites and catalytic activity of the catalyst, which not only increases the surface acidity of the molecular sieve, but also solves the problems of difficult recovery and high cost.

[0016] The synergistic effect of Zr-doped molecular sieves and phosphotungstic acid in this invention is manifested in: 1) Structural level: Zr doping provides stable loading sites for phosphotungstic acid, inhibiting agglomeration and pore blockage; Acidity level: Synergistically constructs a "L-acid-B-acid multi-component system", improving acid quantity and acid strength; Stability level: Zr doping enhances the interaction between phosphotungstic acid and the support, reducing the loss of active components. Therefore, this invention can improve catalytic activity through the synergistic effect of Zr doping and phosphotungstic acid; 2) Solves the pain points of "difficult recovery and high cost" of phosphotungstic acid; 3) Maintains the ordered structure of molecular sieves and extends the service life of catalysts; 4) Adapts to green nitration processes and replaces traditional mixed acid systems.

[0017] This invention can effectively control the acidity and pore structure of the catalyst by adjusting the Zr loading and phosphotungstic acid loading, thereby regulating the catalytic performance.

[0018] The preparation method of this invention is simple, the raw materials are readily available, the catalytic efficiency is high, and it can be recycled, thus having broad prospects for industrial application.

[0019] The phosphotungstic acid-supported Zr-SBA-12 molecular sieve catalyst prepared in this invention is applied to the nitration of acetanilide. This method eliminates the use of sulfuric acid, avoiding waste acid generation and equipment corrosion, and provides an environmentally friendly new method for acetanilide nitration, possessing significant research value and application prospects. This invention avoids the environmental pollution problems of traditional mixed acid nitration processes, allows for catalyst recycling, and offers advantages such as high catalytic efficiency, environmental friendliness, and process simplicity.

[0020] The prepared phosphotungstic acid-supported Zr-SBA-12 molecular sieve was used as a catalyst in the nitration reaction of acetanilide. Under the conditions of 8 h reaction time, 80 °C reaction temperature, HNO3 / acetanilide molar ratio of 2, and catalyst dosage of 0.02 g, the conversion rate of acetanilide reached the highest of 81.4% under the catalysis of Z(35%)-Zr(0.05)-SBA-12, and the selectivity of p-nitroacetanilide was 84.8%. Under the same reaction conditions, the conversion rate could still reach 80.8% after the catalyst was recycled 4 times, and the selectivity of p-nitroacetanilide was 84.1%. Attached Figure Description

[0021] Figure 1The XRD small-angle (a1~a2) and wide-angle (b1~b2) comparison images of Zr-SBA-12 with different phosphotungstic acid loading prepared in Examples 1~6, as well as the small-angle XRD pattern (c1) of Zr(0.05)-SBA-12 prepared in Comparative Example 2 and the standard XRD information (c2) of phosphotungstic acid; Figure 2 Infrared comparison images of Zr-SBA-12 with different phosphotungstic acid loadings prepared in Examples 3-5; Figure 3 The N2 adsorption-desorption isotherm of Z(15%)-Zr(0.05)-SBA-12 phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 2; Figure 4 SEM images of Z(35%)-Zr(0.05)-SBA-12 phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 4, where ① is 5.00 μm and ② is 1.00 μm; Figure 5 Mapping and EDS diagrams of Z(35%)-Zr(0.05)-SBA-12 phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 4; Figure 6 The TEM image shows the Z(35%)-Zr(0.05)-SBA-12 phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 4, where ① is 200 nm and ② is 100 nm. Figure 7 NH3-TPD spectra of the SBA-12 molecular sieve prepared in Comparative Example 1 and the phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 4. Figure 8 The conversion rate of acetanilide and the selectivity of p-nitroacetanilide were determined by different catalysts. Figure 9 The effect of Z(35%)-Zr(0.05)-SBA-12 on the nitration of acetanilide with different cycle numbers. Detailed Implementation

[0022] In this invention, unless otherwise specified, the raw materials or reagents required for preparation are all commercially available products well known to those skilled in the art.

[0023] This invention provides a method for preparing phosphotungstic acid-supported Zr-SBA-12 molecular sieves, comprising the following steps: A mixture is obtained by mixing silicon source, zirconium source, template agent, acid and water; The mixture was mixed with phosphotungstic acid and subjected to a hydrothermal reaction to obtain a hydrothermal product; The hydrothermal product was calcined to obtain phosphotungstic acid-supported Zr-SBA-12 molecular sieve.

[0024] In this invention, the silicon source preferably includes tetraethyl orthosilicate (TEOS), methyl orthosilicate, silica sol, diatomaceous earth, or photovoltaic silicon waste; this invention does not have any special limitations on the source and specifications of the photovoltaic silicon waste, and photovoltaic silicon waste obtained by methods known in the art is acceptable.

[0025] In this invention, the zirconium source preferably includes ZrOCl2·8H2O, Zr(NO3)4·5H2O, Zr(CH3COO)4·4H2O or Zr(OH)4.

[0026] In this invention, the molar ratio of Zr in the zirconium source to Si in the silicon source is preferably 0.025~0.1:1, more preferably 0.01~0.10:1, and even more preferably 0.05:1.

[0027] In this invention, the template agent preferably includes Brij76, Brij58, Brij78, P123 or F127; the acid preferably includes hydrochloric acid or nitric acid; the mass concentration of the hydrochloric acid is preferably 36% to 38%, and the mass concentration of the nitric acid is preferably 65%.

[0028] In this invention, the mass ratio of the template agent, acid and water is preferably 1:(5.7~6.1):(18.5~19.9), more preferably 1:5.9:19.1.

[0029] In this invention, the mass ratio of the template agent to the silicon source is preferably 1:2.78~3.0, more preferably 1:2.88~2.92.

[0030] In this invention, the template agent, acid and water are mixed and stirred until completely dissolved. Then, a zirconium source is added and stirred for 20 minutes. Next, a silicon source is added dropwise and stirred for another 30 minutes to obtain a mixture.

[0031] The present invention does not have any special limitation on the source of the phosphotungstic acid, and any commercially available product well known in the art is acceptable.

[0032] In this invention, the phosphotungstic acid is preferably used in the form of an aqueous solution, which can be prepared in a conventional manner to achieve the required concentration. This invention does not impose a specific limitation on the concentration of the aqueous phosphotungstic acid solution; it can be adjusted according to requirements. In the embodiments of this invention, a phosphotungstic acid aqueous solution with a concentration of 1 g / mL is specifically used.

[0033] In this invention, an aqueous solution of phosphotungstic acid is added dropwise to the mixture, and stirring is continued at room temperature for 20 hours. The resulting mixture is then placed in a polytetrafluoroethylene reactor for hydrothermal reaction.

[0034] In this invention, the mass of the phosphotungstic acid (based on the actual mass of phosphotungstic acid in the aqueous solution) is preferably 5-55% of the total mass of the phosphotungstic acid-supported Zr-SBA-12 molecular sieve, more preferably 10-35%, and even more preferably 20-25%. While loading with phosphotungstic acid enhances the surface acidity of the molecular sieve, it also alters the original surface morphology and pore structure, leading to a decrease in the stability of the molecular sieve. Excessive loading can damage the mesoporous structure of the molecular sieve. This invention controls the phosphotungstic acid loading to improve catalytic performance while maintaining the integrity of the molecular sieve's crystal structure.

[0035] In this invention, the temperature of the hydrothermal reaction is preferably 90~110℃, more preferably 95~100℃, and the time is preferably 20~28h, more preferably 24~26h.

[0036] After the hydrothermal reaction is completed, the present invention preferably recovers the solid product by filtration, and dries the solid product in air at room temperature for 12 hours, and then calcines it in a muffle furnace.

[0037] In this invention, the calcination temperature is preferably 500-600℃, more preferably 550-580℃, the calcination time is preferably 6-8 hours, more preferably 7-8 hours, and the heating rate to the calcination temperature is preferably 2℃ / min. This invention removes the template agent through calcination.

[0038] The present invention provides a phosphotungstic acid supported Zr-SBA-12 molecular sieve prepared by the preparation method described in the above technical solution.

[0039] This invention provides the application of the phosphotungstic acid-supported Zr-SBA-12 molecular sieve described above in the nitration reaction of acetanilide.

[0040] In this invention, the preferred method of application includes: mixing a catalyst, acetanilide and HNO3 to carry out a nitration reaction, wherein the catalyst is the phosphotungstic acid supported Zr-SBA-12 molecular sieve described in the above technical solution; In this invention, the nitration reaction time is preferably 6-10 h, more preferably 8-9 h, and the reaction temperature is preferably 70-90 °C, more preferably 80-85 °C; the mass ratio of the catalyst to acetanilide is preferably 1:(2.25-4.5), more preferably 1:3.375, and the molar ratio of HNO3 to acetanilide is preferably 1.5-3:1, more preferably 2:1.

[0041] The specific embodiments of the present invention are described in detail below, but it should be understood that the scope of protection of the present invention is not limited to the specific embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0042] Unless otherwise specified, the experimental methods described in the various embodiments of this invention are conventional methods; unless otherwise specified, the reagents and raw materials described below are all commercially available.

[0043] The reagents used in the following examples were sourced from: Hydrochloric acid (HCl) 36%~38%, produced by Sinopharm Chemical Reagent Co., Ltd. Phosphotungstic acid (HPWA) H3PW 12 O 40 Analytical grade reagents from Shanghai Aladdin Reagent Co., Ltd. Tetraethyl silicate (TEOS) C8H 20 O4Si analytical grade, produced by Sinopharm Chemical Reagent Co., Ltd. S10 polyoxyethylene stearate (Brij76) C 58 H 118 O 21 Analytical grade reagents from Shanghai Aladdin Reagent Co., Ltd. Nitric acid (HNO3) 65% - Sinopharm Chemical Reagent Co., Ltd. Acetonitrile (C2H3N) - Analytical grade - Sinopharm Chemical Reagent Co., Ltd. Zirconium oxychloride (ZrOCl2·8H2O) analytical grade, Shanghai Aladdin Reagent Co., Ltd.

[0044] Example 1

[0045] Mix 3g Brij76, 17.7g 36wt% hydrochloric acid, and 57.4g deionized water, and stir until completely dissolved. Then add 0.67g ZrOCl2·8H2O (Zr / Si = 0.05, molar ratio), and stir for 20 minutes. Next, add 8.65g TEOS dropwise, and continue stirring for 30 minutes. Finally, add a 1 g / mL phosphotungstic acid aqueous solution (H3PW) containing 0.25g phosphotungstic acid to the resulting mixture. 12 O 40 (equivalent to 5% mass load), continue stirring for 20 hours; The resulting mixed solution was transferred into a polytetrafluoroethylene reactor and hydrothermally reacted at 100°C for 24 hours. After cooling, the mixture was filtered, and the resulting solid product was dried in air at room temperature for 12 hours. The product was then calcined in a muffle furnace at 2°C / min to 550°C for 8 hours to obtain 5g of Z(5%)-Zr(0.05)-SBA-12 molecular sieve.

[0046] Example 2

[0047] The only difference from Example 1 is that an aqueous solution of phosphotungstic acid (H3PW) with a concentration of 1 g / mL containing 0.75 g of phosphotungstic acid is added. 12 O 40 (equivalent to 15% mass loading), resulting in Z(15%)-Zr(0.05)-SBA-12 molecular sieve.

[0048] Example 3

[0049] The only difference from Example 1 is that an aqueous solution of phosphotungstic acid (H3PW) with a concentration of 1 g / mL containing 1.25 g of phosphotungstic acid is added. 12 O 40 (equivalent to 25% mass loading), resulting in Z(25%)-Zr(0.05)-SBA-12 molecular sieve.

[0050] Example 4

[0051] The only difference from Example 1 is that an aqueous solution of phosphotungstic acid (H3PW) with a concentration of 1 g / mL containing 1.75 g of phosphotungstic acid is added. 12 O 40 (equivalent to 35% mass loading), resulting in Z(35%)-Zr(0.05)-SBA-12 molecular sieve.

[0052] Example 5

[0053] The only difference from Example 1 is that an aqueous solution of phosphotungstic acid (H3PW) with a concentration of 1 g / mL containing 2.25 g of phosphotungstic acid was added. 12 O 40 (equivalent to 45% mass loading), resulting in Z(45%)-Zr(0.05)-SBA-12 molecular sieve.

[0054] Example 6

[0055] The only difference from Example 1 is that an aqueous solution of phosphotungstic acid (H3PW) with a concentration of 1 g / mL containing 2.75 g of phosphotungstic acid was added. 12 O 40 (equivalent to 55% mass loading), resulting in Z(55%)-Zr(0.05)-SBA-12 molecular sieve.

[0056] Comparative Example 1

[0057] Place 57.4g of deionized water, 17.7g of 36wt% hydrochloric acid and 3g of Brij76 into a beaker, place a magnetic stir bar at room temperature and stir until completely dissolved, then add 8.65g of TEOS dropwise and continue stirring the mixture at room temperature for 20 hours to obtain a solution; The solution was placed in a polytetrafluoroethylene reactor and hydrothermally reacted at 100°C for 24 hours. After the reactor cooled, the solid product was recovered by filtration. The obtained solid product was dried in air at room temperature for 12 hours and then calcined in a muffle furnace at a temperature of at least 550°C at a rate of 2°C / rise for 8 hours to obtain SBA-12 molecular sieve.

[0058] Comparative Example 2

[0059] Place 3g of template agent Brij76, 17.7g of 36wt% hydrochloric acid, and 57.4g of deionized water into a beaker and stir at room temperature until completely dissolved. Then add 0.67g of ZrOCl2·8H2O (Zr / Si=0.05, molar ratio) and stir for 20min. Then add 8.65g of TEOS dropwise and stir at room temperature for 20h to obtain a mixed solution. The obtained mixed solution was loaded into a polytetrafluoroethylene reactor and hydrothermally reacted at 100°C for 24 hours. After the reactor cooled, the solid product was recovered by filtration. The obtained product was dried in air at room temperature for 12 hours, and then calcined in a muffle furnace at 2°C / min to 550°C for 8 hours to obtain Zr-SBA-12 molecular sieve, namely Zr(0.05)-SBA-12.

[0060] Comparative Example 3

[0061] The only difference from Comparative Example 2 is that the Zr / Si molar ratio was changed sequentially to 0.025, 0.06, 0.075, and 0.1 to obtain Zr(X)-SBA-12, where X is the Zr / Si molar ratio, thus obtaining Zr-SBA-12 molecular sieve.

[0062] Conclusions: Zr(0.025): has fewer acidic sites, and the conversion rate of acetanilide is only 40.6% (lower than 59.6% of Zr(0.05)); Zr(0.05): has a complete crystal structure, uniform Zr dispersion, sufficient acidic sites, and the best conversion rate (59.6%) and selectivity (83.3%), and its performance is stable after 4 cycles; For Zr(0.06) / Zr(0.075) / Zr(0.1): excessive Zr loading leads to blockage of molecular sieve channels and a decrease in orderliness, among which the conversion rate of Zr(0.1) drops to 55.1% (lower than Zr(0.05)).

[0063] Characterization and performance testing

[0064] Figure 1 The XRD small-angle (a1~a2) and wide-angle comparison images (b1~b2) of Zr-SBA-12 with different phosphotungstic acid loadings prepared in Examples 1~6, and the small-angle XRD pattern (c1) and standard XRD information (c2) of Zr(0.05)-SBA-12 prepared in Comparative Example 2 are shown. Figure 1 Analysis of small angles (a1~a2, c1) shows that, compared to Zr-SBA-12, the characteristic peaks between 1° and 2° of SBA-12 are still clearly observable after loading with phosphotungstic acid, indicating that the loading of metallic Zr did not change the ordered three-dimensional hexagonal mesoporous structure of the SBA-12 molecular sieve. However, as the loading of phosphotungstic acid increases, the diffraction peaks almost disappear, indicating that the ordered three-dimensional hexagonal mesoporous structure of the p63 / mmc space group of the sample is destroyed. It is speculated that excessive acid corrosion of the mesoporous material may have led to pore collapse. The optimal loading rate is reached at 35%. Even at higher phosphotungstic acid loading rates, no clear diffraction peaks were observed at other positions, meaning that phosphotungstic acid was uniformly loaded into the internal channels of the SBA-12 molecular sieve.

[0065] Wide-angle (b1~b2) analysis revealed typical amorphous silica characteristic diffraction peaks between 20° and 30°. These peaks did not change significantly, only broadening slightly. This indicates that the Zr-SBA-12 molecular sieve supported on phosphotungstic acid still maintains an amorphous crystal structure, although the regularity of the catalyst is reduced. Furthermore, this is consistent with the standard XRD pattern of phosphotungstic acid. Figure 1 Compared with the characteristic peak of (c2), the loaded sample did not show obvious diffraction peaks of the characteristic crystals of the loaded phosphotungstic acid, indicating that the phosphotungstic acid was uniformly loaded on the molecular sieve. This result is consistent with the small angle test results.

[0066] Figure 2 The images show the infrared comparison of Zr-SBA-12 with different phosphotungstic acid loadings prepared in Examples 3-5; phosphotungstic acid with a Keggin structure has characteristic infrared spectral peaks in the range of 700-1100 cm⁻¹. -1 It exhibits four main absorption peaks, located at 1080.21, 948.33, 897.16, and 806.42 cm⁻¹, respectively. -1 At this location, 1080.21cm -1 PO4 3- Absorption peaks of the symmetric stretching vibration of the PO bond in the tetrahedron, 948.33, 897.16, and 806.42 cm⁻¹. -1 This is the absorption peak of the antisymmetric stretching vibration of the WOW bond. For example... Figure 2 As shown, 1080.21 and 806.42 cm -1 Absorption peaks appeared on both sides, but at 948.33 and 897.16 cm⁻¹ -1 The absorption peak at the given location was covered by SBA-12, indicating that the catalyst contains phosphotungstic acid and that the Keggin structure of phosphotungstic acid has not been destroyed.

[0067] Figure 3The N2 adsorption-desorption isotherm of Z(15%)-Zr(0.05)-SBA-12 phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 2 was observed. It was observed that the molecular sieve supported by phosphotungstic acid still has a type IV isotherm similar to that of mesoporous molecular sieves like SBA-12, and shows a type H1 hysteresis loop.

[0068] Figure 4 SEM images of Z(35%)-Zr(0.05)-SBA-12 phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 4, where ① is 5.00 μm and ② is 1.00 μm; Figure 4 As shown, after the addition of phosphotungstic acid, the particle morphology did not change, still exhibiting certain peak crystal morphology and planar plate morphology, but the pore structure lost a certain regularity. This may be because the introduction of metal or acid changed the original structure of the sample surface, leading to the collapse of some pores.

[0069] Figure 5 Mapping and EDS plots of the Z(35%)-Zr(0.05)-SBA-12 phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 4. From... Figure 5 The results show that phosphotungstic acid is uniformly dispersed in the sample, and P and W elements are uniformly distributed on the surface of the molecular sieve without agglomeration. Combined with XRD and infrared results, it indicates that phosphotungstic acid has been successfully loaded into the SBA-12 framework.

[0070] Figure 6 The image shows a TEM image of the Z(35%)-Zr(0.05)-SBA-12 phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 4; where ① represents 200 nm and ② represents 100 nm. It can be observed that the mesoporous arrangement is clearly regular, which may be due to the phosphotungstic acid eroding the mesoporous structure, thus affecting the overall regularity, consistent with the XRD results. Uniformly distributed metallic Zr can also be observed.

[0071] Figure 7 The NH3-TPD spectra of the SBA-12 molecular sieve prepared in Comparative Example 1 and the phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared in Example 4 are shown. It can be seen that the pure SBA-12 molecular sieve exhibits an NH3 desorption peak above 400℃, while no obvious desorption peaks are observed at other positions, indicating that the surface material does not have many obvious acidic sites. However, Z(35%)-Zr(0.05)-SBA-12 shows obvious peaks at both medium-strong acid (200~400℃) and strong acid (>400℃) positions, with the area gradually increasing, indicating the simultaneous presence of numerous weak acid and medium / strong acid sites.

[0072] Application examples

[0073] 1. Weigh 0.02 g of SBA-12, Zr(0.05)-SBA-12, Z(5%)-Zr(0.05)-SBA-12, Z(35%)-Zr(0.05)-SBA-12, and Z(55%)-Zr(0.05)-SBA-12 molecular sieve catalysts respectively, and apply them to a nitration reaction containing 0.0675 g of acetanilide. Simultaneously, control the reaction time to 8 h, reaction temperature to 80 °C, and the molar ratio of HNO3 / acetanilide to 2:1. After the reaction, centrifuge the resulting sample, and use high-performance liquid chromatography (HPLC) to determine the concentrations of p-nitroacetanilide and acetanilide in the sample. Calculate the conversion rate of acetanilide and the selectivity of p-nitroacetanilide. The results are shown in [Figure number missing]. Figure 8 See Table 1.

[0074] Table 1. Conversion rate of acetanilide and selectivity of p-nitroacetanilide with different catalysts

[0075] Compared to catalysts supported only by metallic Zr, the acetanilide conversion rate of the catalyst supported by phosphotungstic acid was significantly improved. Furthermore, with increasing phosphotungstic acid loading, the conversion rate increased from 61.8% and 60.9% at 5% to 81.4% and 80.3% at 35%. However, if the phosphotungstic acid loading was further increased, the acetanilide conversion rate decreased instead of increasing. This may be because excessive acid loading disrupts the mesoporous structure of the molecular sieve, thus affecting catalytic activity, which is consistent with the characterization results. The Z(35%)-Zr(0.05)-SBA-12 molecular sieve catalyst exhibited the best catalytic activity.

[0076] 2. Effect of catalyst cycle number on catalytic performance

[0077] To verify the effect of recycling on the catalytic performance of the Z(35%)-Zr(0.05)-SBA-12 molecular sieve prepared in Example 4, the catalyst obtained by centrifugation after the reaction was further processed by repeatedly washing with anhydrous ethanol and deionized water, and then drying in an oven at 100°C for 6 hours to obtain the recovered Z(35%)-Zr(0.05)-SBA-12 molecular sieve. The recovered molecular sieve was then used to re-initiate the nitration reaction of acetanilide, cyclically four times. The results are shown in Table 2 and [Table data would be inserted here]. Figure 9 As shown.

[0078] Table 2. Effect of Z(35%)-Zr(0.05)-SBA-12 on the nitration of acetanilide with different cycle numbers.

[0079] From Table 2 and Figure 9It can be seen that the conversion rate of acetanilide decreased slightly with the increase of the number of cycles, from 81.4% before the first cycle to 81.3% in the first cycle and then to 80.8% in the fourth cycle, a decrease of 0.6%. This may be because some of the active material loaded on the catalyst surface was lost during the cycle, or it may be that the reactants or products that were not washed clean blocked the pores of the molecular sieve. However, the overall decrease was very small, and the selectivity did not change significantly with the increase of the number of cycles. This indicates that the catalytic performance of Z(35%)-Zr(0.05)-SBA-12 molecular sieve still maintains high activity after cycling, and it is a recyclable catalyst.

[0080] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a phosphotungstic acid-supported Zr-SBA-12 molecular sieve, characterized in that, Includes the following steps: A mixture is obtained by mixing silicon source, zirconium source, template agent, acid and water; The mixture was mixed with phosphotungstic acid and subjected to a hydrothermal reaction to obtain a hydrothermal product; The hydrothermal product was calcined to obtain phosphotungstic acid-supported Zr-SBA-12 molecular sieve.

2. The preparation method according to claim 1, characterized in that, The silicon source includes tetraethyl silicate, methyl orthosilicate, silica sol, diatomaceous earth, or photovoltaic silicon waste; the zirconium source includes ZrOCl2·8H2O, Zr(NO3)4·5H2O, Zr(CH3COO)4·4H2O, or Zr(OH)4.

3. The preparation method according to claim 2, characterized in that, The molar ratio of Zr in the zirconium source to Si in the silicon source is 0.025~0.1:

1.

4. The preparation method according to claim 1, characterized in that, The template agent includes Brij76, Brij58, Brij78, P123, or F127; the acid includes hydrochloric acid or nitric acid; the mass concentration of the hydrochloric acid is 36%~38%, and the mass concentration of the nitric acid is 65%. The mass ratio of the template agent, acid, and water is 1:(5.7~6.1):(18.5~19.9); The mass ratio of the template agent to the silicon source is 1:2.78~3.

0.

5. The preparation method according to claim 1, characterized in that, The mass of the phosphotungstic acid is 5 to 55% of the total mass of the phosphotungstic acid-supported Zr-SBA-12 molecular sieve.

6. The preparation method according to claim 1, characterized in that, The hydrothermal reaction is carried out at a temperature of 90~110℃ for a duration of 20~28h.

7. The preparation method according to claim 1, characterized in that, The roasting temperature is 500~600℃ and the time is 6~8h.

8. The phosphotungstic acid-supported Zr-SBA-12 molecular sieve prepared by the preparation method according to any one of claims 1 to 7.

9. The application of the phosphotungstic acid-supported Zr-SBA-12 molecular sieve of claim 8 in the nitration reaction of acetanilide.

10. The application according to claim 9, characterized in that, The method of application includes: mixing the catalyst, acetanilide and HNO3 to carry out a nitration reaction, wherein the catalyst is the phosphotungstic acid supported Zr-SBA-12 molecular sieve as described in claim 8; The nitration reaction takes 6-10 hours and is carried out at a temperature of 70-90°C. The mass ratio of the catalyst to acetanilide is 1:(2.25-4.5), and the molar ratio of HNO3 to acetanilide is 1.5-3:1.