A method for additive manufacturing of multi-material, multi-functional structures with integrated embedded fiber optic sensing
Patent Information
- Application Number
- CN202610170153.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-02-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-02-06
AI Technical Summary
Traditional FDM technology is limited by a single material supply system, resulting in printed parts exhibiting singular characteristics in terms of mechanical, thermal, and electrical functions. This makes it difficult to meet the diverse requirements of complex service environments for component strength, heat transfer, and conductivity. Furthermore, the installation method of fiber optic sensors suffers from poor contact and reduced measurement accuracy.
By employing a multi-material, multi-functional additive manufacturing method, a spatial coupling structure of microchannels, wires, and optical fibers is constructed inside the substrate. Multi-degree-of-freedom robotic arms work collaboratively to simultaneously implant wires and optical fibers in the molten state of the substrate, forming an in-situ metallurgical-grade bond of heterogeneous materials. This enables integrated manufacturing of electrical and thermal conductivity functions as well as temperature and strain sensing.
It achieves deep coupling between structure and function, improves the bonding strength of heterogeneous material interfaces, endows the structure with full life cycle sensing capabilities, significantly improves manufacturing efficiency and integration, and solves the problems of matrix softening failure and poor fiber contact caused by thermal accumulation in traditional methods.
Smart Images

Figure CN121829672B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of multi-material, multi-functional additive manufacturing, and more specifically to a method for additive manufacturing of multi-material, multi-functional structures with integrated embedded fiber optic sensing. Background Technology
[0002] Fused deposition modeling (FDM) is one of the most widely used 3D printing technologies. Its principle involves heating thermoplastic filaments to a molten state, then extruding them through a nozzle and building up layer by layer to ultimately form a three-dimensional solid. This technology has rapidly gained popularity in fields such as industrial design, education, healthcare, and consumer electronics due to its advantages including low equipment cost, ease of operation, and diverse material selection.
[0003] However, traditional FDM processes are limited by a single material supply system, allowing only one homogeneous material to be deposited per layer. This results in printed parts exhibiting singular characteristics in terms of mechanical, thermal, and electrical properties, making it difficult to meet the diverse requirements of complex service environments for component strength, heat transfer, and electrical conductivity. Furthermore, it cannot achieve multi-functional integration such as embedded circuitry and flow channels, or real-time monitoring of structural status. With the urgent need for integrated structural and functional components in high-end equipment applications such as aerospace, robotics, and personalized medicine, developing additive manufacturing technologies that enable on-demand, point-to-point printing of multiple materials and parallel multi-functional integration within the same printing process has become an inevitable trend.
[0004] On the other hand, fiber optic sensing detects external physical quantities based on changes in the transmission characteristics of light within optical fibers. When external factors such as temperature and stress act on the fiber, they cause changes in optical parameters such as the intensity, phase, wavelength, or polarization state of the light wave. By demodulating these changes, accurate monitoring of the measured quantity can be achieved, offering advantages over sensors based on electrical principles, such as resistance to electromagnetic interference and high sensitivity. While there are existing engineering applications using fiber optics to monitor parameters such as structural temperature and strain, fiber optic installation methods primarily involve surface bonding and pre-embedding, which can lead to poor contact between the fiber and the substrate and decreased measurement accuracy. Summary of the Invention
[0005] This invention provides an additive manufacturing method for a multi-material, multi-functional structure integrating embedded fiber optic sensing. The aim is to construct a coupled spatial structure integrating fiber optic sensing, metal wire conductivity, and microfluidic heat exchange within a substrate, thereby achieving integrated manufacturing of electrical conductivity, thermal conductivity, and temperature and strain sensing functions.
[0006] The above objectives are achieved through the following technical solutions:
[0007] A multi-material, multi-functional structure for integrated embedded fiber optic sensing includes a substrate, a microchannel disposed on the substrate, a conductor located within the substrate and accompanying the microchannel, and an optical fiber located at the interface between the heterogeneous materials of the substrate and the conductor.
[0008] Optionally, the substrate is made of polylactic acid or polyetheretherketone, the conductor is made of metal, carbon nanotube fiber or conductive polymer, and the optical fiber is made of polyimide coated optical fiber.
[0009] Optionally, the wires and microchannels are distributed in parallel, that is, the direction of wire extension is parallel to the axis of microchannel and the spacing is kept constant; or, the wires and microchannels are distributed in a spiral winding pattern.
[0010] Optionally, the wire diameter is 50-150μm; the microchannel inner diameter is 1-3mm; the distance between the wire and the microchannel is 0.5-2mm; the optical fiber outer diameter is 125-150μm, and it is embedded in the interface of heterogeneous materials along an S-shaped, spiral, or three-dimensional mesh path with a radius of curvature of not less than 10mm.
[0011] Optionally, when the conductors cross longitudinally, through holes are provided on the substrate to connect the conductors of adjacent layers or across layers, and the through holes are filled with a conductive medium.
[0012] Optionally, the conductive medium is silver paste.
[0013] Optionally, the substrate is provided with a fluid inlet, a fluid outlet, and a standard interface that communicates with the microchannel, such as an electrical interface for connecting to a wire or an optical fiber interface for connecting to an optical fiber.
[0014] The above-mentioned additive manufacturing method for multi-material, multi-functional structures integrating embedded fiber optic sensors includes the following steps:
[0015] Step 1: Design the spatial coupling structure and use the suspension support optimization algorithm for structural design;
[0016] Step 2: Divide the forming area into multiple collaborative subdomains, generate motion trajectories based on time-space dual constraints, and execute collaborative operations of multiple printing devices based on slice data;
[0017] The first printing device is responsible for printing the polymer matrix and the flow channel walls; the second printing device follows the trajectory of the first printing device and presses the wires and optical fibers into the matrix when the matrix temperature is above the glass transition temperature to form a multi-material, multi-functional structure with integrated embedded optical fiber sensing.
[0018] Optionally, step three: conformally manufacture the fiber optic interface flange, the electrical spring-pin hybrid connector, and the fluid quick-connect base on the component surface; the interface area uses polyetheretherketone (PEEK) / carbon fiber (CF) composite material to improve mechanical strength and achieve anti-mating and unmolding; after printing, ensure flatness ≤0.02mm;
[0019] Optionally, step four: Anneal the component to eliminate residual stress.
[0020] Optionally, step five involves: performing OTDR testing on the fiber optic network to locate the loss point and record the initial wavelength-temperature / strain coefficient; performing four-wire resistance testing on the conductive lines to establish a resistance-temperature calibration curve; and performing a water pressure sealing test on the flow channel to ensure that the leakage rate meets the requirements, confirming that the linear response of the fiber optic sensing network to temperature and strain R²>0.99, and the leak-free performance of the microchannel under 0.5MPa water pressure, ultimately obtaining a qualified multi-material, multi-functional structure for integrated embedded fiber optic sensing.
[0021] The beneficial effects of the multi-material, multi-functional structure for integrated embedded fiber optic sensing of the present invention are as follows:
[0022] Within the formed polymer matrix, a spatial coupling structure of "microchannel-metal wire-optical fiber" is created. For the microchannel overhang structure, a self-supporting profile design combined with multi-arm variable angle printing is used to prevent top collapse. The metal wire and millimeter-level microchannel are arranged in an accompanying manner, and active thermal management is achieved by using the fluid medium embedded circuit within the microchannel. The optical fiber is embedded at the interface between the polymer matrix and the metal wire, forming a full life cycle sensing network for monitoring interlayer stress and interface temperature. The optical fiber interface, electrical interface, and fluid inlet / outlet are integrated and printed on the component surface to achieve the integration of four functions: load bearing, sensing, conductivity, and heat exchange.
[0023] The beneficial effects of the additive manufacturing method for a multi-material, multi-functional structure integrating embedded fiber optic sensing of the present invention are as follows:
[0024] 1. Achieved deep coupling of "structure-function": This invention does not simply embed wires and channels into the substrate, but instead pioneers a topology of "microchannels accompanied by metal wires", using microchannels directly as heat sinks for embedded high-power circuits, effectively solving the problem of substrate softening and failure caused by heat accumulation inside the sealed composite material structure.
[0025] 2. Solves the "fragmentation" problem at heterogeneous material interfaces: Through a multi-robotic arm spatiotemporal collaborative process, optical fibers and metal wires are simultaneously implanted when the substrate is in its optimal molten viscous flow state, achieving "in-situ metallurgical bonding" or "microscopic physical interlocking" of heterogeneous materials. Unlike traditional single-nozzle printing, this method controls the timing of each robotic arm's operation to ensure that the embedding of materials other than the substrate, such as metal wires and / or optical fibers, occurs within a specific "thermal window" (melting point ±5℃) after the substrate material is printed. In-situ thermal fusion encapsulation is achieved using the residual heat of the substrate, eliminating the need for additional adhesives. Compared to traditional cold-state embedding, this process significantly improves interlayer bonding strength.
[0026] 3. Imparting the structure's full life cycle sensing capability: The embedded optical fiber is located at the interface of the most vulnerable heterogeneous materials, which not only monitors the residual stress during the manufacturing process, but also provides in-situ data on temperature (-50℃~200℃), strain (±5000με) and vibration during the service life of the component, acting as the "nervous system" of the structure.
[0027] 4. Significantly improves manufacturing efficiency and integration: truly realizes "design as manufacturing", simplifying the assembly of discrete components that traditionally requires more than ten processes into a one-time additive manufacturing process, greatly reducing the size and weight of complex electromechanical systems such as aerospace and satellite brackets. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the multi-material, multi-functional structure of the integrated embedded fiber optic sensing of the present invention;
[0029] Figure 2 This is a schematic diagram of an in-situ embedded fiber optic sensor network.
[0030] Figure 3 This is a schematic diagram of the structure of an in-situ embedded wire;
[0031] Figure 4 A schematic diagram of a microchannel for heat dissipation;
[0032] Figure 5 This is a schematic diagram of standard interfaces on the surface of the components of the present invention, such as optical fiber, electrical, and fluid interfaces;
[0033] Figure 6 A schematic diagram of the multi-degree-of-freedom robotic arm, FDM nozzle, and wire conveying mechanism included in a multi-degree-of-freedom collaborative additive manufacturing system;
[0034] Figure 7 This is a schematic diagram of the structure of the FDM nozzle of the present invention;
[0035] Figure 8 This is a schematic diagram of the heat treatment and calibration experiment of the printed component of the present invention;
[0036] Figure 9 This is a schematic diagram of the system integration and functional verification of the present invention.
[0037] Figure Descriptions: 1. Multi-material, multi-functional structure integrating embedded fiber optic sensing; 101. Substrate; 102. Microchannel; 103. Conductor; 104. Through-hole; 105. Optical fiber; 106. Standard interface; 2. FDM nozzle; 201. Housing; 202. Heating block; 203. Screw; 204. Throat; 205. Melting chamber; 206. Nozzle; 3. Multi-degree-of-freedom robotic arm; 4. Wire conveying mechanism. Detailed Implementation
[0038] A multi-material, multi-functional structure for integrated embedded fiber optic sensing 1, reference Figures 1 to 4 It includes a substrate 101, in which microchannels 102, wires 103 and optical fibers 105 are disposed, and the microchannels 102, wires 103 and optical fibers 105 form a spatial coupling structure.
[0039] Specifically, the substrate 101 is made of polylactic acid (PLA) or polyether ether ketone (PEEK); the conductor 103 can be made of annealed copper wire, silver-clad aluminum wire, carbon nanotube fiber or conductive polymer wire, etc., which have electrical and thermal conductivity properties.
[0040] The conductor 103 is located next to the microchannel 102, forming an embedded circuit and an accompanying heat dissipation structure. That is, in the plane (XY plane) perpendicular to the printing stacking direction (Z-axis), the center of the conductor 103 maintains a set horizontal distance from the outer edge of the wall of the microchannel 102; or in three-dimensional space, the conductor 103 is designed to be equidistantly enveloped by closely following the outer wall contour of the microchannel 102. This allows for in-situ thermal management of the energized conductor 103 using the fluid medium inside the microchannel 102, and also enables signal transmission.
[0041] The diameter of the conductor 103 is 50-150μm; the inner diameter of the microchannel 102 is 1-3mm; the spacing between the conductor 103 and the side of the microchannel 102 is 0.5-2mm.
[0042] Example 1 of accompanying heat dissipation: The wires 103 and the microchannels 102 are distributed in parallel, that is, the extension direction of the wires 103 is parallel to the axis of the microchannels 102, and the spacing is kept constant.
[0043] Example 2 of accompanying heat dissipation: The conductive wires 103 and microchannels 102 are spirally wound together. That is, the conductive wires 103 are spirally wound around the outer wall of the microchannels 102 with the microchannels 102 as the central axis. At the intersections of conductive wires 103 at different heights, a layered jumper structure needs to be designed. That is, the conductive wires 103 arranged at different printing layer heights are connected through through holes 104 in the Z-axis direction. The through holes 104 are reserved vertical holes used to connect the conductive wires 103 in adjacent layers or across layers, realizing the three-dimensional interconnection of the conductive wires 103.
[0044] The through-hole 104 is filled with conductive silver paste to prevent short circuits caused by crossover of the conductors 103 in the same layer. The silver paste has extremely low resistivity and good fluidity, which can fully fill the interlayer micropores left by 3D printing. After curing, it can significantly reduce interlayer contact resistance, ensuring the stability of signal transmission and heat dissipation efficiency.
[0045] An optical fiber 105 is embedded at the interface between the substrate 101 and the conductor 103, forming a life-cycle sensing network for monitoring interlayer stress and interface temperature. The optical fiber 105 has a polyimide coating and an outer diameter of 125-150 μm. As a reinforcing phase and sensing unit, it is embedded in the heterogeneous material interface along an S-shaped, spiral, or three-dimensional mesh path with a radius of curvature of not less than 10 mm.
[0046] The substrate 101 can be equipped with standard interfaces 106, such as a fluid inlet and a fluid outlet connected to the microchannel 102, an electrical interface connected to the wire 103, and an optical fiber interface connected to the optical fiber 105, to realize the integration of four functions: load carrying, sensing, conduction, and heat exchange.
[0047] The manufacturing method of the above-mentioned multi-material, multi-functional structure 1 with integrated embedded fiber optic sensing includes the following steps:
[0048] Step 1: Design a spatial coupling structure. Use a suspension support optimization algorithm for structural design. Utilize the rapid cooling characteristics of the polymer matrix 101 to prevent the top of the flow channel from collapsing and ensure the flow channel's sealing performance.
[0049] The conductor 103 is an annealed copper wire with a diameter of 100μm; the microchannel 102 has an inner diameter of 2mm; the path of the conductor 103 is planned on the side of the microchannel 102, with a distance of 1.5mm between them, forming an embedded circuit.
[0050] After the conductor 103 is embedded in the substrate 101, the wetting and bonding area formed by the contact between the surface of the conductor 103 and the substrate 101 is the interface between the two. The optical fiber 105 is arranged along the tangential direction or the main stress direction of this bonding area / interface to capture the interface stress caused by the mismatch of thermal expansion coefficients to the greatest extent.
[0051] Step 2: A multi-degree-of-freedom collaborative additive manufacturing system can be used, which includes two sets of multi-degree-of-freedom robotic arms 3 carrying FDM printing nozzles 2. The forming area is divided into multiple collaborative sub-domains. The central controller generates the motion trajectories of the two multi-degree-of-freedom robotic arms 3 based on "time-space dual constraints". Based on the slice data, the two multi-degree-of-freedom robotic arms 3 perform collaborative printing, so that the trajectories of the two FDM printing nozzles 2 are the same.
[0052] One FDM printing nozzle 2 is responsible for ejecting molten substrate 101 raw material to construct the substrate 101 and microchannels 102; the second robotic arm's FDM nozzle 2 is responsible for ejecting wires 103 and optical fibers 105 coated with molten substrate material. When the substrate 101 temperature is above its glass transition temperature (within a window of ±5°C of the melting point), the wires 103 and optical fibers 105 are pressed into the substrate 101 to form components. In this way, the time difference between the two multi-degree-of-freedom robotic arms 3 is strictly calculated by the central controller to ensure that the subsequent embedding action occurs when the substrate 101 still has sufficient wettability and viscosity, thereby achieving a tight wrapping of the metal wires 103, optical fibers 105, and substrate 101 and avoiding cold seams.
[0053] To further explain, the multi-degree-of-freedom robotic arm 3 can be a six-axis industrial robotic arm, preferably the UR5 series CB3 model robotic arm from Universal Robots. A wire feeding mechanism 4 is fixed at the third joint (upper arm segment) of each multi-degree-of-freedom robotic arm 3. The wire 103 and optical fiber 105 need to be wound onto two material trays with dampers, respectively. The material trays are mounted on the robotic arm base via a 3D-printed bracket. The wire passes through a polytetrafluoroethylene conduit, and the optical fiber 105 and wire 103 are synchronously fed into the throat 204 at a speed of 0.1-1 mm / s with constant tension to reach the molten pool. The tension of 0.05-0.2 N ensures the positional accuracy of the optical fiber in the complex three-dimensional path and prevents micro-bending losses.
[0054] The FDM nozzle 2 includes a housing 201, inside which a heating block 202 is installed. The heating block 202 can be an electric heating element or a medium that introduces heat from a heat source into the housing 201. The housing 201 has a first flow channel and a second flow channel. A first screw 203 is installed in the first flow channel, and a second screw 203 is installed in the second flow channel. The tops of the two screws 203 are driven by a set of synchronous gears and rotated by a miniature high-torque stepper motor fixed above the housing 201, thereby achieving quantitative extrusion of the matrix raw material. A throat 204 for guiding optical fibers and metal wires is provided between the first and second flow channels. Thus, the first and second flow channels form a Y-shaped three-way flow channel, which also serves as a molten pool, i.e., a molten cavity 205. The bottom of the throat 204 communicates with a converging flow channel, guiding the guide wire 103 and the optical fiber 105 into the converging flow channel. When the first and second screws rotate, they can transport molten matrix 101 raw material to the converging channel to coat the conductor 103 and optical fiber 105 to form a composite wire. The bottom of the heat sink housing 201 is fixedly connected to and connected to a nozzle 206. A wire channel with a wider top and a narrower bottom is formed inside the nozzle 206. The wire channel coincides with the axis of the throat 204 to guide the composite wire to be extruded from the bottom of the nozzle 206.
[0055] Step 3: Conformally manufacture fiber optic interface flanges, electrical spring-pin hybrid connectors, and fluid quick-connect bases on the component surface; the interface area uses high-filled polyether ether ketone (PEEK) / carbon fiber (CF) composite material to improve mechanical strength and achieve anti-mating and unmolding; after printing, the mating surface is CNC micro-milled to ensure flatness ≤0.02mm, ensuring the reliability of optical, electrical, and hydraulic connections and improving the sealing connection with external equipment.
[0056] Step 4: The entire component is placed in a nitrogen furnace at 120℃ for annealing for 2 hours to eliminate residual stress.
[0057] Step 5: Perform OTDR testing on the fiber optic network to locate the loss point and record the initial wavelength-temperature / strain coefficient; perform four-wire resistance testing on the conductive lines to establish a resistance-temperature calibration curve; perform a water pressure sealing test on the flow channels to ensure the leakage rate meets requirements. Connect the testing equipment (e.g., ...). Figure 8 , Figure 9 The linear response of the fiber optic sensing network to temperature and strain (R²>0.99) and the leak-free performance of the microchannel under 0.5MPa water pressure were confirmed, and finally a qualified multi-material, multi-functional printed component was obtained, namely the multi-material, multi-functional structure with integrated embedded fiber optic sensing 1.
[0058] Step 5: Connect the printed component to an external laser source, photodetector, data acquisition card, programmable power supply and coolant circulation pump through standard interface 106 to build an integrated experimental platform for load-bearing, sensing, conductivity and heat exchange; verify its comprehensive performance of simultaneously achieving structural load-bearing, temperature monitoring, strain monitoring, conductivity and electrical signal transmission, and microchannel heat exchange under static load, cyclic thermal shock and vibration combined conditions.
[0059] To verify the effectiveness of the "coupling structure" and "cooperative process" proposed in this invention, the following comparative experiments were conducted:
[0060] Example 1: Using the above manufacturing method, the multi-material, multi-functional structure 1 of the integrated embedded fiber optic sensing obtained in steps three and five is removed, and a copper wire with a diameter of 100 μm and a microchannel with an inner diameter of 2 mm are arranged in a spiral pattern with a spacing of 0.5 mm. A current of 5 A is applied and a coolant at 20 °C is introduced.
[0061] Comparative Example 1: The same wires were directly embedded in the polymer matrix without any accompanying flow channels.
[0062] Results: In the example, the surface equilibrium temperature of the conductor was maintained at 45°C, and the resistance value was stable; while in the comparative example, the conductor temperature rose to 120°C within 2 minutes, leading to local softening of the substrate and circuit melting. This demonstrates the necessity of the "microchannel-conductor" coupling structure proposed in this invention in the manufacture of high-density electronic devices.
[0063] Further verification of interface bonding strength:
[0064] Comparative Example 2: Traditional single-nozzle step-by-step printing (print one layer -> pause -> lay out lines -> cover).
[0065] Results: The interlayer shear strength at the heterogeneous material interface of the prototype sample reached 42 MPa, exceeding 90% of the strength of the pure PEEK matrix, and exhibited low optical fiber signal transmission loss (<0.02 dB / m). In contrast, the comparative sample, due to the "cold waiting" process, showed significant cold seams, with a shear strength of only 25 MPa, and the optical fiber was prone to micro-bending loss. This demonstrates that the co-manufacturing process of this invention can effectively solve the interfacial tearing problem in multi-material structures.
Claims
1. A multi-material, multi-functional structure integrating embedded fiber optic sensing, characterized in that, It includes a substrate, microchannels disposed on the substrate, a conductor located within the substrate and accompanying the microchannels, and an optical fiber located at the interface between the heterogeneous materials of the substrate and the conductor. The conductors and microchannels are distributed in parallel, that is, the direction of the conductors is parallel to the axis of the microchannels and the spacing is kept constant; or, the conductors and microchannels are distributed in a spiral winding pattern. The wire diameter is 50-150μm; the microchannel inner diameter is 1-3mm; the distance between the wire and the microchannel is 0.5-2mm; the optical fiber outer diameter is 125-150μm, and it is embedded in the interface of heterogeneous materials along an S-shaped, spiral, or three-dimensional mesh path with a radius of curvature of not less than 10mm. The substrate is provided with a fluid inlet and a fluid outlet that are connected to the microchannel, an electrical interface that connects to the wire, and an optical fiber interface that connects to the optical fiber.
2. The multi-material, multi-functional structure for integrated embedded fiber optic sensing according to claim 1, characterized in that, The substrate is made of polylactic acid or polyetheretherketone, the conductor is made of metal, carbon nanotube fiber or conductive polymer, and the optical fiber is made of polyimide coated optical fiber.
3. The multi-material, multi-functional structure for integrated embedded fiber optic sensing according to claim 1, characterized in that, When conductors cross longitudinally, through holes are provided on the substrate to connect conductors in adjacent layers or across layers, and the through holes are filled with conductive medium.
4. The multi-material, multi-functional structure for integrated embedded fiber optic sensing according to claim 3, characterized in that, The conductive medium is silver paste.
5. The additive manufacturing method for the multi-material, multi-functional structure with integrated embedded fiber optic sensing as described in any one of claims 1 to 4, characterized in that, Includes the following steps: Step 1: Design the spatial coupling structure and use the suspension support optimization algorithm for structural design; Step 2: Divide the forming area into multiple collaborative subdomains, generate motion trajectories based on time-space dual constraints, and execute collaborative operations of multiple printing devices based on slice data; The first printing device is responsible for printing the polymer matrix and the flow channel walls; the second printing device follows the trajectory of the first printing device and presses the wires and optical fibers into the matrix when the matrix temperature is above the glass transition temperature to form a multi-material, multi-functional structure with integrated embedded optical fiber sensing. When the substrate temperature is above the glass transition temperature and within a window of ±5°C of the melting point, wires and optical fibers are pressed into the substrate to form a component. One FDM printing nozzle is only responsible for ejecting molten substrate material to build the substrate and microchannels, while the FDM nozzle of the second robotic arm is responsible for ejecting wires and optical fibers coated with molten substrate material. The time difference between the two multi-degree-of-freedom robotic arms is strictly calculated by the central controller to ensure that the subsequent embedding action occurs when the substrate still has sufficient wettability and viscosity.
6. The additive manufacturing method according to claim 5, characterized in that, it further... include: Step 3: Conformally manufacture the fiber optic interface flange, electrical spring-pin hybrid connector, and fluid quick-connect base on the component surface; the interface area uses polyetheretherketone (PEEK) / carbon fiber (CF) composite material to improve mechanical strength and achieve anti-mating and unmating; after printing, ensure flatness ≤0.02 mm; Step 4: Anneal the multi-material, multi-functional structure with integrated embedded fiber optic sensing to eliminate residual stress.
7. The additive manufacturing method according to claim 6, characterized in that, it further... include: Step 5: Perform OTDR testing on the fiber optic network, locate the loss point, and record the initial wavelength-temperature / strain coefficient; Four-wire resistance testing was performed on the conductive circuit to establish a resistance-temperature calibration curve; a water pressure sealing test was performed on the flow channel to ensure that the leakage rate meets the requirements, confirming that the linear response of the fiber optic sensing network to temperature and strain R²>0.99, and the leak-free performance of the microchannel under 0.5MPa water pressure, finally obtaining a qualified multi-material, multi-functional structure for integrated embedded fiber optic sensing.