Room-temperature hydrogen sulfide sensor based on stannic oxide hollow sphere / polypyrrole nanotube and preparation method of room-temperature hydrogen sulfide sensor

By preparing a composite material of SnO2 hollow spheres and PPy nanotubes, the problems of high-temperature operation and slow response of traditional SnO2 sensors were solved, enabling rapid detection of H2S gas at room temperature, with low cost and high performance characteristics.

CN121955099APending Publication Date: 2026-05-01UNIV OF ELECTRONICS SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610360833.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-01-22
Filing Date
2026-03-24
Publication Date
2026-05-01

AI Technical Summary

Technical Problem

Existing SnO2 gas sensors require high temperatures to operate, have high energy consumption and slow response recovery speed, while pure PPy materials have low sensitivity and large baseline drift, making it difficult to achieve low power consumption and high performance detection at room temperature.

Method used

SnO2 hollow spheres and PPy nanotube composite materials were used to prepare SnO2/PPy composite slurry by hydrothermal carbonization and chemical oxidation polymerization. The slurry was then coated on the electrode surface to form a sensitive layer. The process was simplified by combining sacrificial template and soft template methods.

Benefits of technology

It achieves rapid response and recovery of H2S gas at room temperature, improves the sensitivity and stability of the sensor, reduces production costs, and is simple and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN121955099A_ABST
    Figure CN121955099A_ABST
Patent Text Reader

Abstract

The invention discloses a room-temperature hydrogen sulfide (H2S) sensor based on stannic oxide (SnO2) hollow spheres and polypyrrole (PPy) nanotubes and a preparation method of the room-temperature hydrogen sulfide (H2S) sensor, and belongs to the technical field of gas sensors. A green and low-cost chemical synthesis process is adopted, SnO2 hollow spheres and PPy nanotubes are prepared, a gas sensitive material with a multi-stage micro-nano structure and a p-n heterojunction is formed through composite construction, and the surface of an interdigital electrode is coated with the gas sensitive material to prepare a sensing device. The composite material combines abundant active sites brought by high specific surface area of the SnO2 hollow spheres and excellent room temperature conductivity of the PPy nanotubes, and effectively solves the problems of high working temperature and large energy consumption of a traditional metal oxide sensor. Tests show that the sensor has the characteristics of quick response and short recovery time to H2S gas at room temperature. In addition, the preparation process is simple, raw materials are cheap and easy to obtain, and the method is suitable for large-scale production and has wide application prospects in the fields of industrial safety monitoring and environment detection.
Need to check novelty before this filing date? Find Prior Art

Description

A room-temperature hydrogen sulfide sensor based on tin dioxide hollow spheres / polypyrrole nanotubes and its fabrication method Technical Field

[0001] This invention relates to the field of gas sensor technology, specifically to a room-temperature hydrogen sulfide (H2S) sensor based on tin dioxide (SnO2) hollow spheres and polypyrrole (PPy) nanotubes and its preparation method. Background Technology

[0002] H2S is a highly toxic, flammable, and foul-smelling acidic gas widely found in petrochemical, wastewater treatment, and industrial production. Even low concentrations of H2S can pose serious health risks and even be life-threatening. Currently, traditional detection methods such as gas chromatography and iodometric titration, while highly accurate, suffer from drawbacks such as expensive equipment, large size, and difficulty in real-time online monitoring. In contrast, metal oxide semiconductor gas sensors, due to their small size, low cost, fast response, and ease of integration, have become the preferred solution for real-time H2S gas detection.

[0003] In existing technologies, SnO2 is widely used due to its good chemical stability. However, pure SnO2 sensors typically need to operate at high temperatures (200℃-400℃), resulting in high power consumption, poor safety, and slow response recovery. While conductive polymers (such as PPy) have the potential to operate at room temperature, single materials often suffer from low sensitivity, large baseline drift, and insufficient long-term stability. Balancing low power consumption at room temperature with high-performance detection has always been a technical challenge in this field.

[0004] To address the aforementioned issues, combining metal oxides with conductive polymers and leveraging their synergistic effects is an effective approach. In particular, constructing composite materials with unique micro / nano structures (such as hollow spheres and nanotubes) can significantly increase specific surface area and improve gas diffusion and adsorption properties. However, current fabrication processes for such composite materials with specific morphologies are often complex or costly. Therefore, developing a composite sensor that is simple, green, low-cost, and capable of rapid H2S gas response at room temperature has significant application value and market potential. Summary of the Invention

[0005] The purpose of this invention is to provide a room temperature H2S sensor based on SnO2 hollow spheres and PPy nanotubes and its preparation method, so as to solve the technical problems of high operating temperature, high energy consumption and slow response recovery speed of metal oxide gas sensors in the prior art.

[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: a room temperature H2S sensor based on SnO2 hollow spheres and PPy nanotubes, comprising electrodes, characterized in that a sensitive layer formed of SnO2 / PPy composite material is coated on the surface of the electrodes; the SnO2 / PPy composite material is prepared by coating a SnO2 / PPy composite slurry formed by uniformly dispersing SnO2 hollow spheres and PPy nanotubes in deionized water.

[0007] Preferably, in the SnO2 / PPy composite material, the mass ratio of SnO2 hollow spheres to PPy nanotubes is 60:1.

[0008] Preferably, the SnO2 hollow spheres are hollow spherical structures formed by using carbon microspheres formed by hydrothermal carbonization of glucose as sacrificial templates, followed by hydrothermal coating and high-temperature calcination to remove the templates; the PPy nanotubes are tubular structures formed by chemical oxidative polymerization induced by methyl orange as a soft template.

[0009] Preferably, the electrode is a silver cross-finger electrode.

[0010] This invention also discloses a method for preparing a room-temperature H2S sensor based on SnO2 hollow spheres and PPy nanotubes. Utilizing the H2S gas sensor described above, the method comprises the following steps: Step 1: Dissolving methyl orange (MO) in deionized water, adding pyrrole monomer (Py) and oxidant ammonium persulfate (APS) at low temperature to carry out a chemical oxidative polymerization reaction, and obtaining PPy nanotubes after washing and drying after the reaction; Step 2: Performing a hydrothermal carbonization reaction on a glucose solution, and obtaining a carbon microsphere template after washing and drying; Step 3: Dissolving tin source... Then, the carbon microspheres prepared in step 2 are added, the pH value is adjusted, and a hydrothermal reaction is carried out to coat the surface of the carbon microspheres with the precursor. After drying, the carbon template is removed by high-temperature calcination to obtain SnO2 hollow spheres; Step 4, the SnO2 hollow spheres obtained in step 3 and the PPy nanotubes obtained in step 1 are added to deionized water in a preset ratio and mixed by stirring to obtain SnO2 / PPy composite slurry; Step 5, the SnO2 / PPy composite slurry obtained in step 4 is drop-coated onto the surface of the electrode device using a drop-coating method. After vacuum drying and aging treatment, the room temperature H2S sensor is obtained.

[0011] Preferably, in step 1, the low temperature condition is 5°C, and the molar ratio of oxidant to Py is 1:1.

[0012] Preferably, in step 3, the high-temperature calcination temperature is 600°C and the holding time is 3 hours.

[0013] Preferably, in step 5, the aging treatment temperature is 80°C and the treatment time is 12 hours.

[0014] This invention offers the following advantages: 1. Unique micro / nano structure and synergistic effect: This invention combines three-dimensional SnO2 hollow spheres with one-dimensional PPy nanotubes through a composite process. The SnO2 hollow spheres possess a large specific surface area and abundant hollow internal space, providing numerous active sites for gas molecule adsorption and shortening the gas diffusion path. The PPy nanotubes not only construct a good conductive network but also form numerous pn heterojunctions at the two-phase interface. This multi-level micro / nano structure and heterojunction effect work synergistically to significantly improve the sensor's ability to capture H2S gas and its electron transport efficiency. 2. Room temperature detection and rapid response: Benefiting from the excellent room temperature conductivity of PPy and the rapid gas diffusion channels provided by the SnO2 hollow structure, the sensor prepared in this invention overcomes the deficiency of traditional SnO2 sensors that require high-temperature heating (200-400℃) to operate, achieving effective detection at room temperature. Simultaneously, this unique structural design enables the sensor to exhibit rapid response and recovery characteristics to H2S gas. 3. Simple, Green, and Low-Cost Process: The material preparation methods used in this invention (sacrificial template method and soft template method) are mature processes with low equipment requirements and do not require precious metal catalysts. The overall preparation process is simple and controllable, and the raw materials are inexpensive and readily available, conforming to the concept of green chemistry. This greatly reduces the production cost of high-performance gas sensors and facilitates large-scale application. Attached Figure Description

[0015] To make the purpose, technical solution, and advantages of the invention clearer, the invention will be further described in detail below with reference to the accompanying drawings, wherein: Figure 1 is a flow chart of the preparation process of the SnO2 hollow sphere / PPy nanotube composite sensitive material of the present invention. Flow chart of the preparation process of the tin dioxide hollow sphere / polypyrrole nanotube composite sensitive material.

[0016] Figure 2 is a flowchart of the device fabrication and coating process for the H2S sensor based on SnO2 hollow spheres / PPy nanotubes of the present invention. Flowchart of the fabrication process for the tin dioxide hollow sphere / polypyrrole nanotube composite sensing material.

[0017] Figure 3 shows the scanning electron microscope (SEM) morphology of the SnO2 hollow spheres prepared in this invention. Flowchart of the preparation process of the tin dioxide hollow sphere / polypyrrole nanotube composite sensitive material.

[0018] Figure 4 shows the scanning electron microscope (SEM) morphology of the PPy nanotubes prepared in this invention. Flowchart of the preparation process for the tin dioxide hollow sphere / polypyrrole nanotube composite sensitive material.

[0019] Figure 5 shows the scanning electron microscope (SEM) microstructure of the SnO2 hollow sphere / PPy nanotube composite material of the present invention, illustrating the heterojunction contact state between the hollow spheres and nanotubes. A flowchart of the preparation process of the tin dioxide hollow sphere / polypyrrole nanotube composite sensitive material is also included.

[0020] Figure 6 shows the repeatability test curve of the H2S sensor of the present invention to 50 ppm H2S gas at room temperature. Flowchart of the preparation process of the tin dioxide hollow sphere / polypyrrole nanotube composite sensing material.

[0021] Figure 7 shows the single-cycle dynamic response and recovery characteristics of the H2S sensor of the present invention under 50ppm H2S gas, illustrating the response time and recovery time. A flowchart of the fabrication process for the tin dioxide hollow sphere / polypyrrole nanotube composite sensing material is also included.

[0022] Figure 8 shows the dynamic response curves of the H2S sensor of the present invention to different concentrations of H2S gas at room temperature. Flowchart of the preparation process of the tin dioxide hollow sphere / polypyrrole nanotube composite sensing material. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. It should be noted that similar reference numerals and letters in the following drawings indicate similar items; therefore, once an item is defined in one drawing, it does not need to be further defined and explained in subsequent drawings. The embodiments described in this invention are some, but not all, embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0024] This invention aims to address the technical problems of high operating temperature, high energy consumption, and slow response recovery speed in existing metal oxide gas sensors. Based on this, this invention discloses a room-temperature H2S sensor based on SnO2 hollow spheres and PPy nanotubes, and its fabrication method.

[0025] The device used in this embodiment is preferably a silver interdigitated electrode device, with the sensitive layer being a SnO2 hollow sphere / PPy nanotube composite material, and the optimal operating temperature being room temperature (25°C). The SnO2 hollow spheres have a micron-scale hollow structure, and the PPy nanotubes have a one-dimensional tubular structure.

[0026] The specific preparation method is as follows. Step 1: Preparation of PPy nanotubes: Methyl orange (MO) was dissolved in 150 mL of deionized water (DIW) and fully dissolved under magnetic stirring. Pyrrole (Py) monomer was added to the MO solution at 5℃, controlling the molar ratio of MO to Py to be 1:3.5, and stirring was continued for 30 min. An ammonium persulfate (APS) solution (Py to APS molar ratio of 1:1) was prepared and slowly added dropwise to the pre-prepared MO / Py mixed solution, and then the reaction was continuously stirred at 5℃ for 24 h. After the reaction was completed, the resulting black precipitate was washed successively with ethanol and deionized water until the filtrate turned light yellow. After vacuum drying, the PPy nanotube product was finally obtained. Step 2: Preparation of carbon microsphere (CMS) template: Glucose was dissolved in deionized water to prepare a glucose aqueous solution with a concentration of 0.33 mol / L, and it was stirred until it was completely dissolved within 1 h to form a transparent solution. The obtained solution was transferred to an 80 mL stainless steel autoclave lined with polytetrafluoroethylene. The autoclave was heated to 190 °C and maintained at a constant temperature for 9 h. After the reaction was complete, the precipitate was washed three times with deionized water to remove residual impurities. It was dried at 80 °C for 8 h to obtain dark brown carbon microsphere powder. Step 3: Preparation of SnO2 hollow spheres: SnCl4·5H2O was dissolved in ethanol to prepare a 0.5 mol / L precursor solution. After forming a homogeneous solution, the carbon microspheres prepared in step 2 were added as a temporary template. A NaOH aqueous solution was prepared in another container. The two solutions were mixed, and the pH of the mixture was adjusted to 10 using the NaOH aqueous solution. The mixture was reacted for 1 h under magnetic stirring. The mixed solution was transferred to a 50 mL autoclave and reacted at 120 °C for 24 h. It was dried at 60 °C for 12 h to obtain a gray powder. The final product was annealed at 600℃ for 3 hours at a heating rate of 2℃ / min to obtain structurally intact SnO2 hollow spheres. Step 4: Preparation of SnO2 / PPy composite slurry: 120 mg of SnO2 hollow spheres and 2 mg of PPy nanotubes were weighed into a clean beaker (i.e., the mass ratio of SnO2 hollow spheres to PPy nanotubes was 60:1), and 2 mL of deionized water was added to form a suspension. The suspension was stirred in a magnetic stirrer for 12 hours to ensure uniform mixing. After stirring, a SnO2 hollow sphere-PPy nanotube slurry with a doping ratio of 60:1 was obtained. Step 5: Sensor coating and aging: 3 μL of the slurry obtained in Step 4 was accurately pipetted. The slurry was evenly coated onto the surface of the silver interdigitated electrode using a fine brush to ensure the uniformity and integrity of the coating. After coating, the device was placed in a vacuum drying oven and dried at 60℃ for 2 hours to remove excess moisture from the slurry. After drying, the sensor is aged at 80℃ for 12 hours to enhance its stability and performance, ultimately yielding the finished sensor.

[0027] Next, the performance of the prepared materials and sensors will be tested and analyzed.

[0028] Figures 1 and 2 are flowcharts of the sensitive material preparation process and the sensor preparation process, respectively, illustrating the overall steps of the process of this invention.

[0029] The microstructure of the prepared materials is shown in Figures 3 to 5. Figure 3 shows the SEM image of the SnO2 hollow spheres, revealing that the product consists of well-dispersed spherical particles with a relatively rough surface composed of numerous fine nanocrystals. The hollow structure inside the partially broken spheres is clearly visible, providing abundant channels and a large specific surface area for gas diffusion. Figure 4 shows the SEM image of the PPy nanotubes, demonstrating a typical one-dimensional nanotube structure. The nanotubes intertwine to form a loose three-dimensional network structure, which is beneficial for constructing efficient conductive pathways. Figure 5 shows the SEM image of the SnO2 hollow sphere / PPy nanotube composite material, clearly showing that the PPy nanotubes connect multiple SnO2 hollow spheres, inhibiting the aggregation of the hollow spheres and effectively constructing a continuous conductive network. Numerous SnO2 / PPy heterojunctions are formed at the two-phase interface, significantly improving the gas-sensing performance.

[0030] Next, the gas-sensing performance of the prepared sensor was tested. Figure 6 shows the repeatability test curve of the sensor at 50 ppm H2S. As can be observed from Figure 6, the resistance of the H2S gas sensor decreases when the H2S gas concentration is high; when the H2S gas concentration is zero, the resistance of the H2S gas sensor gradually increases until it returns to its maximum value. Furthermore, with the regular occurrence or zeroing of H2S gas concentration, the resistance of the H2S gas sensor shows a highly consistent and regular change following the H2S gas concentration change pattern, exhibiting good response. This consistent response amplitude across multiple cycles of testing fully demonstrates the excellent repeatability of the sensor.

[0031] Figure 7 shows the response and recovery characteristics of the sensor under 50 ppm H2S. Here, we define the response time as the time required for the sensor's resistance to change to reach 90% of its total change after contact with the gas being measured; and the recovery time as the time required for the sensor's resistance to recover to 90% of its baseline resistance change after being removed from the gas environment. As can be observed from Figure 7, when 50 ppm H2S gas is introduced into the test chamber, the sensor's resistance drops sharply within a very short time, and the response curve shows a steep downward trend, indicating that gas molecules can be rapidly captured by the sensitive material. When the gas flow is stopped and the sensor is exposed to clean air, the resistance quickly recovers and approaches its initial state. This rapid response and recovery characteristic (i.e., rapid adsorption and desorption kinetics) is mainly attributed to the unique thin-walled hollow structure of the SnO2 hollow spheres and the loose network structure constructed by PPy nanotubes, which greatly shortens the diffusion path of gas molecules within the material, providing a smooth channel for the rapid transport of gas molecules.

[0032] Figure 8 shows the dynamic response curves of the sensor to different concentrations of H2S gas at room temperature. During the test, the concentration of H2S gas was gradually increased from 5 ppm to 50 ppm. As can be observed from Figure 8, the sensor's response value exhibits a clear and obvious stepwise upward trend with the gradual increase of H2S gas concentration. At each concentration level, the sensor demonstrates a stable response state, and the response amplitude shows a good positive correlation with the gas concentration. Fitting analysis shows that within the test range, the sensor's response value exhibits a good linear relationship with the H2S concentration. This indicates that the SnO2 hollow sphere / PPy nanotube-based sensor possesses excellent gas resolution capabilities and can achieve accurate and quantitative detection of H2S gas.

[0033] In summary, this embodiment demonstrates that the sensor fabrication process disclosed in this invention is simple and low-cost, and the fabricated sensor overcomes the high operating temperature limitation of traditional metal oxide sensors, achieving rapid and sensitive detection of H2S gas at room temperature, and has good application prospects. Example

[0034] The room-temperature H2S sensor based on SnO2 hollow spheres and PPy nanotubes disclosed in this invention is applied to detect the H2S content in the environment. It should be noted that the H2S gas sensor disclosed in this invention can be applied to many occasions and is not limited to this application embodiment.

[0035] H2S, a highly toxic gas with a foul odor, is widely present in industrial production and environmental pollution. Current traditional detection methods are often expensive, complex in operation, and time-consuming, making real-time online monitoring difficult. The H2S gas sensor disclosed in this invention can provide real-time and efficient safety warnings by detecting H2S concentration, exhibiting excellent room temperature operating characteristics and rapid response capabilities.

[0036] The device used in this embodiment is a resistive gas sensor based on silver interdigitated electrodes, which is prepared by the above-mentioned method for preparing an H2S gas sensor. The sensitive layer is a SnO2 hollow sphere / PPy nanotube composite material, and the optimal operating temperature is room temperature (25°C).

[0037] The specific preparation method is as follows: Step 1, Preparation of PPy nanotubes: Methyl orange (MO) was dissolved in 150 mL of deionized water (DIW) and fully dissolved under magnetic stirring. Pyrrole (Py) monomer was added to the MO solution at 5℃, controlling the molar ratio of MO to Py to be 1:3.5, and stirring was continued for 30 min. An ammonium persulfate (APS) solution (Py to APS molar ratio of 1:1) was prepared and slowly added dropwise to the pre-prepared MO / Py mixed solution, and then the reaction was continuously stirred at 5℃ for 24 h. After the reaction was completed, the resulting black precipitate was washed successively with ethanol and deionized water until the filtrate turned light yellow. After vacuum drying, the PPy nanotube product was finally obtained. Step 2, Preparation of carbon microsphere (CMS) template: Glucose was dissolved in deionized water to prepare a glucose aqueous solution with a concentration of 0.33 mol / L, and it was stirred until it was completely dissolved within 1 h to form a transparent solution. The obtained solution was transferred to an 80 mL stainless steel autoclave lined with polytetrafluoroethylene. The autoclave was heated to 190 °C and maintained at a constant temperature for 9 h. After the reaction was complete, the precipitate was washed three times with deionized water to remove residual impurities. It was dried at 80 °C for 8 h to obtain dark brown carbon microsphere powder. Step 3: Preparation of SnO2 hollow spheres: SnCl4·5H2O was dissolved in ethanol to prepare a 0.5 mol / L precursor solution. After forming a homogeneous solution, the carbon microspheres prepared in step 2 were added as a temporary template. In another container, a NaOH aqueous solution was prepared. The two solutions were mixed, and the pH of the mixture was adjusted to 10 using the NaOH aqueous solution. The mixture was reacted for 1 h under magnetic stirring. The mixed solution was transferred to a 50 mL autoclave and reacted at 120 °C for 24 h. It was dried at 60 °C for 12 h to obtain a gray powder. The final product was annealed at 600℃ for 3 hours at a heating rate of 2℃ / min to obtain structurally intact SnO2 hollow spheres. Step 4: Preparation of SnO2 / PPy composite slurry: 120 mg of SnO2 hollow spheres and 2 mg of PPy nanotubes were weighed into a clean beaker (i.e., the mass ratio of SnO2 hollow spheres to PPy nanotubes was 60:1), and 2 mL of deionized water was added to form a suspension. The suspension was stirred in a magnetic stirrer for 12 hours to ensure uniform mixing. After stirring, a SnO2 hollow sphere-PPy nanotube slurry with a doping ratio of 60:1 was obtained. Step 5: Sensor coating and aging: 3 μL of the slurry obtained in Step 4 was accurately pipetted. The slurry was evenly coated onto the surface of the silver interdigitated electrode using a fine brush to ensure the uniformity and integrity of the coating. After coating, the device was placed in a vacuum drying oven and dried at 60℃ for 2 hours to remove excess moisture from the slurry. After drying, the sensor is aged at 80℃ for 12 hours to enhance its stability and performance, ultimately yielding the finished sensor.

[0038] The microstructure of the prepared materials is shown in Figures 3 to 5. Figure 3 shows the SEM image of the SnO2 hollow spheres, revealing that the product consists of well-dispersed spherical particles with a relatively rough surface composed of numerous fine nanocrystals. The hollow structure inside the partially broken spheres is clearly visible, providing abundant channels and a large specific surface area for gas diffusion. Figure 4 shows the SEM image of the PPy nanotubes, demonstrating a typical one-dimensional nanotube structure. The nanotubes intertwine to form a loose three-dimensional network structure, which is beneficial for constructing efficient conductive pathways. Figure 5 shows the SEM image of the SnO2 hollow sphere / PPy nanotube composite material, clearly showing that the PPy nanotubes connect multiple SnO2 hollow spheres, inhibiting the aggregation of the hollow spheres and effectively constructing a continuous conductive network. Numerous SnO2 / PPy heterojunctions are formed at the two-phase interface, significantly improving the gas-sensing performance.

[0039] Next, the performance of the prepared H2S gas sensor based on SnO2 hollow spheres / PPy nanotube composite material was tested, and the test results are shown in Figures 6 to 8.

[0040] Figure 6 shows the repeatability test curve of the sensor at 50 ppm H2S. As can be observed from Figure 6, the resistance of the H2S gas sensor decreases when the H2S gas concentration is high; when the H2S gas concentration is zero, the resistance of the H2S gas sensor gradually increases until it returns to its maximum value. Furthermore, as the H2S gas concentration regularly changes from zero to high, the resistance of the H2S gas sensor shows a highly consistent and regular change, exhibiting good response. This consistent response amplitude across multiple cycles of testing fully demonstrates the excellent repeatability of the sensor.

[0041] Figure 7 shows the response and recovery characteristics of the sensor under 50 ppm H2S. Here, we define the response time as the time required for the sensor's resistance to change to reach 90% of its total change after contact with the gas being measured; and the recovery time as the time required for the sensor's resistance to recover to 90% of its baseline resistance change after being removed from the gas environment. As can be observed from Figure 7, when 50 ppm H2S gas is introduced into the test chamber, the sensor's resistance drops sharply within a very short time, and the response curve shows a steep downward trend, indicating that gas molecules can be rapidly captured by the sensitive material. When the gas flow is stopped and the sensor is exposed to clean air, the resistance quickly recovers and approaches its initial state. This rapid response and recovery characteristic (i.e., rapid adsorption and desorption kinetics) is mainly attributed to the unique thin-walled hollow structure of the SnO2 hollow spheres and the loose network structure constructed by PPy nanotubes, which greatly shortens the diffusion path of gas molecules within the material, providing a smooth channel for the rapid transport of gas molecules.

[0042] Figure 8 shows the dynamic response curves of the sensor to different concentrations of H2S gas at room temperature. During the test, the concentration of H2S gas was gradually increased from 5 ppm to 50 ppm. As can be observed from Figure 8, the sensor's response value exhibits a clear and obvious stepwise upward trend with the gradual increase of H2S gas concentration. At each concentration level, the sensor demonstrates a stable response state, and the response amplitude shows a good positive correlation with the gas concentration. Fitting analysis shows that within the test range, the sensor's response value exhibits a good linear relationship with the H2S concentration. This indicates that the SnO2 hollow sphere / PPy nanotube-based sensor possesses excellent gas resolution capabilities and can achieve accurate and quantitative detection of H2S gas.

[0043] This embodiment demonstrates that the H2S gas sensor disclosed in this invention achieves rapid, room-temperature detection of H2S gas with good linearity and repeatability. At the same time, the device fabrication process is simple, the cost is low, and the operation is easy, overcoming the shortcomings of traditional metal oxide sensors such as high operating temperature and high energy consumption, and has good application prospects.

[0044] It is understood that the present invention has been described through some embodiments, and those skilled in the art will recognize that various changes or equivalent substitutions can be made to these features and embodiments without departing from the spirit and scope of the invention. Under the teachings of the present invention, modifications can be made to these features and embodiments to adapt to specific situations and materials without departing from the spirit and scope of the invention. The embodiments described in this invention are only a part of the embodiments of the invention, not all of them. The components of the embodiments of the invention described and shown in the accompanying drawings can generally be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the invention provided in the accompanying drawings is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention. Therefore, the invention is not limited to the specific embodiments disclosed herein, and all other embodiments obtained by those skilled in the art based on the embodiments of the invention without inventive effort are within the scope of protection of the present invention.

Claims

1. A hydrogen sulfide (H2S) sensor based on tin dioxide (SnO2) hollow spheres and polypyrrole (PPy) nanotubes, comprising electrodes, characterized in that, A sensitive layer formed by SnO2 / PPy composite material is coated on the surface of the electrode; the SnO2 / PPy composite material is prepared by physical mixing and dispersing SnO2 hollow spheres and PPy nanotubes to form a slurry, and the sensitive layer has a multi-level micro-nano structure and pn heterojunction.

2. The H2S sensor based on SnO2 hollow spheres and PPy nanotubes according to claim 1, characterized in that, In the SnO2 / PPy composite material, the mass ratio of SnO2 hollow spheres to PPy nanotubes is 60:

1.

3. The H2S sensor based on SnO2 hollow spheres and PPy nanotubes according to claim 1, characterized in that, The electrode is a silver cross-finger electrode.

4. An H2S sensor based on SnO2 hollow spheres and PPy nanotubes according to claim 1, characterized in that, The SnO2 hollow spheres have a diameter in the micrometer range and are hollow structures formed by removing the template through high-temperature calcination using carbon microspheres as sacrificial templates; the PPy nanotubes are tubular structures formed by chemical oxidation polymerization induced by methyl orange as a soft template.

5. A method for fabricating an H2S sensor based on SnO2 hollow spheres and PPy nanotubes according to any one of claims 1 to 4, characterized in that, The process includes the following steps: Step S1: Preparation of PPy nanotubes: Methyl orange (MO) is dissolved in deionized water as a template agent, pyrrole (Py) monomer is added, and an oxidant solution is added dropwise under low temperature conditions to carry out a chemical oxidative polymerization reaction. After the reaction is completed, PPy nanotubes are obtained by washing and drying. Step S2: Preparation of carbon microsphere template: A glucose solution is subjected to a hydrothermal carbonization reaction, and carbon microspheres are obtained after washing and drying. Step S3: Preparation of SnO2 hollow spheres: A tin source is dissolved and added to the carbon microspheres prepared in step 2 as a template. Step S3: After adjusting the pH value, the SnO2 hollow spheres are coated by hydrothermal reaction, dried, and then calcined at high temperature to remove the carbon template, resulting in SnO2 hollow spheres. Step S4: Preparation of composite slurry: The SnO2 hollow spheres obtained in step 3 and the PPy nanotubes obtained in step 1 are dispersed in deionized water at a preset ratio and stirred for a long time to form a uniform SnO2 / PPy composite suspension. Step S5: Preparation of sensor device: The composite suspension obtained in step 4 is drop-coated onto the electrode surface, and after drying and aging treatment, the H2S sensor is obtained.

6. The preparation method according to claim 5, characterized in that, In step 1, the low temperature condition is 5°C; the oxidant is ammonium persulfate (APS), and the molar ratio of Py to APS is 1:1; the reaction time is 24 hours; the washing process includes washing with ethanol and deionized water in sequence until the filtrate is light yellow.

7. The preparation method according to claim 5, characterized in that, In step 2, the hydrothermal carbonization reaction is carried out at 190°C for 9 hours; the drying is carried out at 80°C for 8 hours.

8. The preparation method according to claim 5, characterized in that, In step 3, the tin source is tin tetrachloride pentahydrate (SnCl4·5H2O); the pH value is adjusted by using NaOH solution to adjust the pH of the mixture to 10; the hydrothermal reaction conditions are 24 hours at 120℃; the high-temperature calcination conditions are 3 hours at 600℃ with a heating rate of 2℃ / min.

9. The preparation method according to claim 5, characterized in that, In step 4, the preset ratio is to weigh 120 mg of SnO2 hollow spheres and 2 mg of PPy nanotubes and add them to 2 mL of deionized water; the stirring time is 12 hours.

10. The preparation method according to claim 5, characterized in that, In step 5, the electrode is a silver interdigitated electrode, and the drop coating amount is 3 μL; the drying conditions are drying at 60°C for 2 hours in a vacuum drying oven; and the aging treatment conditions are treatment at 80°C for 12 hours.