A method for manufacturing an anti-oxidation coating for titanium alloys and the anti-oxidation coating itself.

By setting a diffusion barrier layer and a protective layer on the surface of titanium alloy, the problem of the deterioration of the oxidation performance of titanium alloy at high temperature is solved, and the high temperature stability and bonding strength of the composite anti-oxidation coating are achieved.

CN122081944APending Publication Date: 2026-05-26AECC COMML AIRCRAFT ENGINE CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411714572.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-26
Publication Date
2026-05-26

AI Technical Summary

Technical Problem

The TiO2 oxide film on the surface of titanium alloys is not protective under high temperature conditions. Oxygen atoms diffuse into the titanium alloy matrix, which leads to a deterioration in oxidation resistance. There is a significant diffusion tendency between the existing coating and the substrate, which makes the coating prone to cracking and peeling, thus affecting the oxidation resistance of titanium alloys.

Method used

A diffusion barrier layer and a protective layer are set on the surface of a titanium alloy. The Ni/Re or Ta diffusion barrier layer is prepared by electroplating or spraying, and the MCrAlY or aluminide protective layer is deposited by vapor deposition to form a composite anti-oxidation coating.

Benefits of technology

It improves the interdiffusion of elements between the titanium alloy substrate and the coating, enhances the oxidation resistance and stability of the coating, reduces interfacial embrittlement, and maintains the bonding strength between the coating and the substrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122081944A_ABST
    Figure CN122081944A_ABST
Patent Text Reader

Abstract

A method for manufacturing an anti-oxidation coating for titanium alloys includes the following steps: providing a titanium alloy part and cleaning its surface; depositing a Ni / Re or Ta diffusion barrier layer on the surface of the titanium alloy part; and depositing an MCrAlY protective layer or an aluminide protective layer on the surface of the titanium alloy part using a vapor deposition process, wherein M is Ni or NiCo. The anti-oxidation coating for titanium alloys prepared by this method exhibits excellent high-temperature oxidation resistance and can inhibit interdiffusion between the coating and the titanium alloy substrate, thereby improving the bonding strength of the coating. This invention also provides an anti-oxidation coating for titanium alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-temperature alloys, and specifically relates to a method for manufacturing an anti-oxidation coating for titanium alloys and the anti-oxidation coating itself. Background Technology

[0002] Titanium alloys possess advantages such as high strength, low density, high toughness, and good corrosion resistance, making them an important material choice for aero-engine and gas turbine blades. Furthermore, with the increasing thrust-to-weight ratio of aero-engines, the application of titanium alloys in aero-engines is continuously increasing. However, under high-temperature conditions, the TiO2 oxide film on the surface of titanium alloys lacks protective properties, and the diffusion of oxygen atoms into the titanium alloy matrix leads to a continuous deterioration in the oxidation resistance of titanium alloys. Therefore, severe oxidation and oxygen-induced embrittlement remain unresolved problems for the long-term service of titanium alloys, especially when the temperature exceeds 600°C. To ensure safe application at high temperatures, it is essential to improve the oxidation resistance of titanium alloys.

[0003] Patent CN103305844A discloses a composite coating for high-temperature oxidation resistance on titanium alloy surfaces. This coating consists of a surface alumina layer, an Al deposition layer, and a NiCoCrAlY alloy layer. The coating and the titanium alloy substrate are metallurgically bonded through the NiCoCrAlY diffusion alloy layer. This composite coating exhibits high-temperature oxidation resistance and wear resistance. However, under high-temperature conditions, due to the compositional gradient, a significant diffusion tendency occurs between the coating and the titanium alloy substrate. This leads to the formation of brittle regions in the interdiffusion area, causing the coating to easily crack and peel off, thus affecting the oxidation resistance of the titanium alloy.

[0004] Therefore, providing a method to improve the oxidation resistance of titanium alloys is of great significance for improving the service life of titanium alloy parts under high-temperature oxidation conditions. Summary of the Invention

[0005] The purpose of this invention is to provide a method for manufacturing an anti-oxidation coating for titanium alloys, thereby improving the high-temperature oxidation resistance of titanium alloy parts. This invention also provides an anti-oxidation coating for titanium alloys.

[0006] According to one aspect of the present invention, a method for manufacturing an anti-oxidation coating on a titanium alloy is provided, the method comprising the following steps:

[0007] Step a): Provide a titanium alloy part and clean the surface of the titanium alloy part;

[0008] Step b): A diffusion barrier layer is provided on the surface of the titanium alloy part. The diffusion barrier layer is a Ni / Re diffusion barrier layer provided by electroplating or a Ta diffusion barrier layer provided by spraying.

[0009] Step c): A protective layer is deposited on the surface of the titanium alloy part using a vapor deposition process. The protective layer is an MCrAlY protective layer or an aluminide protective layer, where M is Ni or NiCo.

[0010] The anti-oxidation coating produced by this method has good anti-oxidation properties in the range of 500℃-1000℃, and can effectively improve the interdiffusion of elements between the titanium alloy substrate and the coating.

[0011] Furthermore, in some embodiments, in step a), the cleaning process includes grinding, sandblasting, and ultrasonic cleaning.

[0012] Furthermore, in some embodiments, in step b), the electroplating process is as follows:

[0013] An electroplating solution is provided, wherein the solute components of the electroplating solution include 0.4-0.6 mol / L Ni2SO4, 0.0005-0.0015 mol / L KReO4, and 0.2-0.4 mol / L citric acid, and the solvent is water;

[0014] Set the electroplating tank temperature to 45℃-55℃, adjust the electrolyte pH to 9-11, and the current density to 0.5-1.5A / dm³. 2 Electroplating is performed using the titanium alloy component as the cathode and a pure nickel plate as the anode.

[0015] Furthermore, in some embodiments, in step b), the spraying process includes plasma spraying, supersonic flame spraying, or low-pressure plasma spraying.

[0016] Furthermore, in some embodiments, in step b), the thickness of the Ni / R diffusion barrier layer is 1 μm-20 μm.

[0017] Furthermore, in some embodiments, in step c),

[0018] The MCrAlY protective layer is deposited on the surface of the titanium alloy part.

[0019] The vapor deposition process is configured as an arc ion plating process, and the process parameters of the arc ion plating are as follows:

[0020] Arc voltage 18V-22V, arc current 50A-60A, DC pulse negative bias voltage 230V-250V, duty cycle 50%.

[0021] Furthermore, in some embodiments, in step c),

[0022] The aluminide protective layer is deposited on the surface of the titanium alloy part;

[0023] The vapor deposition process is configured as vapor phase aluminizing or embedded aluminizing.

[0024] Furthermore, in some embodiments, the thickness of the MCrAlY protective layer or the aluminide protective layer is 5μm-40μm.

[0025] According to another aspect of the present invention, a titanium alloy anti-oxidation coating is provided, the titanium alloy anti-oxidation coating being deposited on the surface of a titanium alloy part, and comprising a diffusion barrier layer and a protective layer, wherein the diffusion barrier layer is configured as a Ni / Re barrier layer or a Ta barrier layer, and the protective layer is configured as an MCrAlY protective layer or an aluminide protective layer, wherein M is Ni or NiCo.

[0026] Furthermore, in some embodiments, the thickness of the Ni / Re diffusion barrier layer is 1μm-20μm, and the thickness of the protective layer is 5μm-40μm.

[0027] Furthermore, in some embodiments, the titanium alloy anti-oxidation coating is manufactured using the manufacturing method of the titanium alloy anti-oxidation coating provided in any of the foregoing embodiments. Attached Figure Description

[0028] Figure 1 This is a cross-sectional photograph of the titanium alloy anti-oxidation coating in one embodiment;

[0029] Figure 2 This is a cross-sectional photograph in the thickness direction of an anti-oxidation coating oxidized at 800°C for 500 hours in one embodiment.

[0030] Figure 3 This is a cross-sectional photograph in the thickness direction of a pair of antioxidant coatings oxidized at 800℃ for 500h.

[0031] Figure 4 The oxidation test curves are for comparison between the examples and the comparative examples.

[0032] The purpose of the above figures is to provide a detailed description of the invention so that those skilled in the art can understand the technical concept of the invention, and not to limit the invention. Detailed Implementation

[0033] The present invention will now be described in further detail with reference to specific embodiments and accompanying drawings.

[0034] The term "embodiment" as used herein means that a particular feature, structure, or characteristic described in connection with an embodiment may be included in at least one embodiment herein. The phrase appearing in various places in the specification does not necessarily refer to the same embodiment, nor is it limited to mutually exclusive, independent, or alternative embodiments. Those skilled in the art will understand that the embodiments herein can be combined with other embodiments without causing structural conflicts.

[0035] In this description, terms such as "upper," "lower," "left," "right," "lateral," "longitudinal," "height," "length," and "width," which indicate orientation or positional relationships, are intended to accurately describe the embodiments and simplify the description, rather than limiting the parts or structures involved to have a specific orientation, or to be installed or operated in a specific orientation, and should not be construed as limiting the embodiments in this document.

[0036] In this description, terms such as "first" and "second" are used only to distinguish different objects and should not be construed as indicating relative importance or limiting the number, specific order, or primary / secondary relationship of the described technical features. In this description, "multiple" means at least two.

[0037] Titanium alloys possess advantages such as high strength, low density, high toughness, and good corrosion resistance, making them an important material choice for aero-engine and gas turbine blades. Furthermore, with the increasing thrust-to-weight ratio of aero-engines, the application ratio of titanium alloys in aero-engines is continuously increasing. However, the TiO2 oxide film formed on the surface of titanium alloys lacks protective properties, leading to a continuous deterioration in the oxidation resistance of titanium alloys. Therefore, severe oxidation and oxygen embrittlement remain unresolved problems for the long-term service of titanium alloys, especially at temperatures exceeding 600°C. To ensure safe application at high temperatures, it is essential to improve the oxidation resistance of titanium alloys. In recent years, many technologies have been developed to improve the oxidation resistance of titanium alloys, mainly including bulk alloying and surface modification. Compared with bulk alloying, surface modification can better improve oxidation resistance, especially by adding coatings, which can maintain a good balance between specific mechanical properties and sufficient oxidation resistance. Therefore, depositing anti-oxidation coatings on titanium alloys is considered an effective method to suppress oxidation and oxygen embrittlement.

[0038] Currently, the main technical routes for anti-oxidation coatings on titanium alloy surfaces include the following:

[0039] Preparation of Anti-oxidation Coatings for Titanium Alloys by Spraying: This method mainly uses equipment such as cold spraying and hot spraying to prepare anti-oxidation coating powder on the surface of titanium alloys, thereby providing high-temperature anti-oxidation properties to the titanium alloys. On the one hand, in order to exert the anti-oxidation properties of the coating, the prepared coating needs to be diffused at a high temperature, which affects the mechanical properties of the substrate material; on the other hand, due to the large difference in composition between the substrate and the coating, severe diffusion will occur between the two during service, thus affecting the anti-oxidation properties of the coating and the mechanical properties of the substrate.

[0040] Chemical vapor deposition (CVD) for preparing anti-oxidation coatings on titanium alloys: This method mainly uses slurry deposition or vapor diffusion to prepare protective coatings on the surface of titanium alloys. However, on the one hand, a thick interdiffusion zone is generated between the diffusion coating and the substrate during the preparation process, and this interdiffusion zone will continue to thicken during service, which will seriously affect the performance of the substrate; on the other hand, the preparation temperature of the diffusion coating is high, far exceeding the service temperature of the substrate, which will severely reduce the performance of the substrate.

[0041] Physical vapor deposition method for preparing anti-oxidation coatings for titanium alloys: This method mainly uses magnetron sputtering to prepare TiN or its multilayer coatings, but this type of coating is mainly used in corrosive environments such as the ocean and has insufficient anti-oxidation performance; another method is to use arc ion plating to prepare high-temperature anti-oxidation coatings, but this type of coating has serious interdiffusion with the substrate, which seriously affects the properties of the substrate.

[0042] Among existing antioxidant coatings, NiCrAlY (M = Ni, Co, or a combination thereof) coatings not only possess excellent oxidation and hot corrosion resistance but also exhibit sufficient toughness. In particular, arc ion plating (AIP) has shown many advantages in preparing MCrAlY coatings, as the ion bombardment of the substrate during deposition improves coating adhesion and structure. However, this invention reveals a severe interaction between this coating and the titanium alloy at high temperatures. This chemical incompatibility promotes the growth of brittle phases along the substrate / coating interface, thereby reducing mechanical properties. Therefore, an effective barrier layer is needed between the NiCrAlY coating and the titanium substrate to mitigate interdiffusion and chemical reactions between the coating and substrate.

[0043] One embodiment of the present invention provides a method for manufacturing a titanium alloy anti-oxidation coating, used to prepare a composite anti-oxidation coating with good anti-oxidation properties and the ability to prevent interfacial embrittlement caused by interdiffusion. The method includes the following steps:

[0044] Step a): Provide a titanium alloy part for which an anti-oxidation coating is required, and clean the surface of the titanium alloy part. In a preferred embodiment, the cleaning process specifically includes abrasion treatment, sandblasting, ultrasonic cleaning, and drying.

[0045] Step b): A diffusion barrier layer is formed on the cleaned titanium alloy part surface. In different embodiments, the diffusion barrier layer can be a Ni / Re diffusion barrier layer prepared by electroplating or a Ta diffusion barrier layer formed by spraying. The thickness of the diffusion barrier layer is set to 1 μm.

[0046] 20μm.

[0047] Specifically, the main phase structure of the Ni-Re diffusion barrier layer is r-Ni(Re), which is stable in composition and structure. The Re atomic radius is relatively large, which can effectively hinder the mutual diffusion between Ti elements in the matrix and Ni elements in the coating. The Ta diffusion barrier layer mainly restricts the mutual diffusion between Ti and Ni through the self-binding effect of Ta as a heavy atom, thereby avoiding the large-scale generation of brittle phases formed by diffusion.

[0048] The electroplating process involves preparing an electroplating solution with the following components: 0.4-0.6 mol / L Ni₂SO₄, 0.0005-0.0015 mol / L KReO₄, and 0.2-0.4 mol / L citric acid, using water as the solvent; setting the electroplating tank temperature to 45℃-55℃, adjusting the electrolyte pH to 9-11, and setting the current density to 0.5-1.5 A / dm³. 2 Electroplating is performed using titanium alloy parts as cathodes and pure nickel plates as anodes.

[0049] The spraying process can be ion spraying, supersonic flame spraying or low-pressure plasma spraying.

[0050] Step c): A protective layer is deposited on the surface of the titanium alloy part using a vapor deposition process. In different embodiments, the protective layer can be an MCrAlY protective layer (where M is Ni or NiCo) or an aluminide protective layer. The thickness of the protective layer is set to 5μm-40μm.

[0051] The MCrAlY protective layer can be deposited using an arc ion plating process, while the aluminide protective layer can be prepared using a vapor phase aluminizing or an embedded aluminizing process.

[0052] The anti-oxidation coating manufactured by the above method has good anti-oxidation properties under high temperature conditions, as well as high stability. The coating and the titanium alloy substrate are not prone to interdiffusion, and the coating and the substrate can maintain good bonding strength under long-term service conditions.

[0053] In a preferred embodiment, the process for fabricating the titanium alloy anti-oxidation coating is as follows:

[0054] TC25 welding is used as the base material for titanium alloy parts. The alloy base composition by weight is: Mo 2%, Zr 1%, Al 6.5%, Si 0.2%, Sn 1%, W 1%, with the balance being Ti.

[0055] Before deposition, the alloy substrate was first cleaned. The surface of the titanium alloy part was polished and sandblasted with sandpaper of 200#, 400#, 600#, 800#, 1000# and 2000# in sequence. Then, it was ultrasonically cleaned with acetone for 15 minutes, rinsed with ethanol and dried.

[0056] Next, a Ni / Re diffusion barrier layer is prepared on the surface of the titanium alloy substrate using an electroplating process. The specific steps of the electroplating process are as follows:

[0057] Electroplating solution composition: 0.5 mol / L Ni2SO4, 0.001 mol / L KReO4, 0.3 mol / L citric acid, with water as the solute;

[0058] The electroplating bath temperature is 50℃, the pH is 10, and the current density is 1A / dm³. 2 A Ni / Re diffusion barrier layer with a thickness of 2μm was obtained by electroplating a titanium alloy part as the cathode and a pure nickel plate as the anode.

[0059] A NiCrAlYSi protective layer was prepared using arc ion plating. The specific process is as follows:

[0060] A NiCrAlYSi target material was provided, with the following composition: Cr 18.11%, Al 11.5%, Si 0.9%, Y 0.6%, and the balance being Ni. The deposition process parameters were: arc voltage 20V, arc current 53A, DC pulse negative bias voltage 240V, and duty cycle 50%. The deposition time was set to 5 hours, resulting in a NiCrAlYSi protective layer with a thickness of 40 μm.

[0061] The cross-sectional structure of the finished titanium alloy anti-oxidation coating is as follows: Figure 1 As shown, a Ni / Re diffusion barrier layer 2 and a NiCrAlYSi protective layer 3 are sequentially formed on the titanium alloy substrate 1.

[0062] After the coating and the comparative example without the Ni / Re barrier layer were subjected to oxidation treatment at 800°C for 500 hours, the cross-sectional structure of the coating in the example is as follows. Figure 2 As shown, the cross-sectional structure of the comparative coating is as follows: Figure 3 As shown. It can be seen that, in Figure 2 In the illustrated embodiment, the thickness of region 4, which exhibits relatively mild interdiffusion after high-temperature oxidation treatment, is approximately 5 μm-10 μm; Figure 3 In the comparative example shown, a significant interdiffusion region 5 was formed after high-temperature oxidation treatment, with a thickness exceeding 20 μm.

[0063] Uncoated titanium alloy substrate samples, example samples, and comparative samples were placed in corundum crucibles pre-heated to constant weight for isothermal oxidation experiments. The weight gain curves of the samples were measured using a discontinuous weighing method. During the experiment, the corundum crucibles containing the samples were placed in a high-temperature muffle furnace at the appropriate temperature. The samples were removed at regular intervals, cooled to room temperature, and then measured using a method with an accuracy of 10... -5 The total weight of the crucible containing the sample was weighed using an electronic balance, and then the crucible was placed in a muffle furnace for further oxidation. For example... Figure 4As shown, the antioxidant coating can significantly improve the antioxidant performance, and the antioxidant performance of the high-performance antioxidant coating with Ni / Re diffusion barrier layer is significantly better than that of the comparative coating without diffusion barrier layer.

[0064] The above embodiments demonstrate that the high-performance anti-oxidation coating provided by the present invention has good anti-oxidation performance in the temperature range of 500 to 1000°C; the coating can significantly improve the interdiffusion problem between the titanium alloy substrate and the coating, which is of great significance for the theoretical research and practical application of titanium alloy anti-oxidation coatings.

[0065] The purpose of the above embodiments is to provide a further detailed description of the present invention in conjunction with the accompanying drawings, so that those skilled in the art can understand the technical concept of the present invention. Within the scope of the present invention, optimization or equivalent substitution of the method steps involved, as well as combination of implementation methods in different embodiments without causing structural and principle conflicts, all fall within the protection scope of the present invention.

Claims

1. A method for manufacturing an anti-oxidation coating on a titanium alloy, characterized in that, Includes the following steps: Step a): Provide a titanium alloy part and clean the surface of the titanium alloy part; Step b): A diffusion barrier layer is provided on the surface of the titanium alloy part. The diffusion barrier layer is a Ni / Re diffusion barrier layer provided by electroplating or a Ta diffusion barrier layer provided by spraying. Step c): A protective layer is deposited on the surface of the titanium alloy part using a vapor deposition process. The protective layer is an MCrAlY protective layer or an aluminide protective layer, where M is Ni or NiCo.

2. The method for manufacturing the titanium alloy anti-oxidation coating according to claim 1, characterized in that, In step a), the cleaning process includes grinding, sandblasting, and ultrasonic cleaning.

3. The method for manufacturing the titanium alloy anti-oxidation coating according to claim 1, characterized in that, In step b), the electroplating process is as follows: An electroplating solution is provided, wherein the solute components of the electroplating solution include 0.4-0.6 mol / L Ni2SO4, 0.0005-0.0015 mol / L KReO4, and 0.2-0.4 mol / L citric acid, and the solvent is water; Set the electroplating tank temperature to 45℃-55℃, adjust the electrolyte pH to 9-11, and the current density to 0.5-1.5A / dm³. 2 Electroplating is performed using the titanium alloy component as the cathode and a pure nickel plate as the anode.

4. The method for manufacturing the titanium alloy anti-oxidation coating according to claim 1, characterized in that, In step b), the spraying process includes plasma spraying, supersonic flame spraying, or low-pressure plasma spraying.

5. The method for manufacturing the titanium alloy anti-oxidation coating according to claim 1, 3, or 4, characterized in that, In step b), the thickness of the diffusion barrier layer is 1μm-20μm.

6. The method for manufacturing the titanium alloy anti-oxidation coating according to claim 1, characterized in that, In step c), The MCrAlY protective layer is deposited on the surface of the titanium alloy part. The vapor deposition process is configured as an arc ion plating process, and the process parameters of the arc ion plating are as follows: Arc voltage 18V-22V, arc current 50A-60A, DC pulse negative bias voltage 230V-250V, duty cycle 50%.

7. The method for manufacturing the titanium alloy anti-oxidation coating according to claim 1, characterized in that, In step c), The aluminide protective layer is deposited on the surface of the titanium alloy part; The vapor deposition process is configured as vapor phase aluminizing or embedded aluminizing.

8. The method for manufacturing the titanium alloy anti-oxidation coating according to claim 1, 6, or 7, characterized in that, The thickness of the MCrAlY protective layer or aluminide protective layer is 5μm-40μm.

9. A titanium alloy anti-oxidation coating, characterized in that, The titanium alloy anti-oxidation coating is deposited on the surface of the titanium alloy part and includes a diffusion barrier layer and a protective layer. The diffusion barrier layer is configured as a Ni / Re barrier layer or a Ta barrier layer, and the protective layer is configured as an MCrAlY protective layer or an aluminide protective layer, wherein M is Ni or NiCo.

10. The titanium alloy anti-oxidation coating according to claim 9, characterized in that, The thickness of the Ni / Re diffusion barrier layer is 1μm-20μm, and the thickness of the protective layer is 5μm-40μm.

11. The titanium alloy anti-oxidation coating according to claim 9 or 10, characterized in that, The titanium alloy anti-oxidation coating is manufactured using the manufacturing method of titanium alloy anti-oxidation coating as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Composite coating with high-temperature oxidation resistance and abrasion resistance on surface of titanium alloy and preparation method of composite coating

    CN103305844A