A method for preparing Bi2O2CO3 modified materials and its application
By controlling the morphology of Bi2O2CO3 material to a hierarchical three-dimensional microsphere structure using sodium citrate, the problem of insufficient visible light utilization in photo-assisted electro-controlled ion exchange technology of Bi2O2CO3 material was solved, achieving efficient, low-consumption and selective extraction of iodine ions, and the material maintained good stability after multiple cycles.
Patent Information
- Application Number
- CN202610609876.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2026-05-06
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2046-05-06
AI Technical Summary
Bi2O2CO3 materials have insufficient visible light utilization in photo-assisted electro-controlled ion exchange technology, which limits the efficient extraction of iodide ions. Furthermore, traditional methods are energy-intensive, have poor selectivity, and are prone to causing secondary pollution.
Sodium citrate was used as a morphology modifier and CO32- source to prepare CO32-induced amorphous Bi2O2CO3 material via a one-step hydrothermal method. This method altered the morphology of the material to a hierarchical three-dimensional microsphere structure, increasing the specific surface area and active sites, and broadening the visible light absorption range.
It significantly improved the adsorption capacity and photo-assisted efficiency of iodide ions, achieved highly selective extraction of iodide ions, reduced energy consumption and environmental pollution, and the material still maintained 95% of its adsorption capacity after 10 cycles.
Smart Images

Figure CN122187205B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of iodine ion extraction technology, and in particular to a method for preparing Bi2O2CO3 modified materials and their applications. Background Technology
[0002] Iodine is a vital non-metallic element that plays an irreplaceable role in many fields, including medicine and chemicals. The rapid pace of industrialization has generated large amounts of iodine-containing wastewater. Direct discharge of this wastewater not only wastes iodine resources but also harms the environment and human health. However, traditional technologies for iodine utilization are inefficient and lack selectivity, easily leading to secondary pollution.
[0003] Electrochemically controlled ion exchange (ESIX) technology is a novel selective ion separation technology that integrates electrochemistry and ion exchange principles. By alternately applying oxidation and reduction potentials, it achieves membrane material regeneration and target ion adsorption / desorption without the need for additional chemical reagents, thus avoiding secondary pollution. However, the entire system relies entirely on electricity for energy, resulting in high energy consumption.
[0004] Photo-assisted electro-controlled ion exchange technology (P-ESIX) couples photocatalysis and ESIX technology. Using photoelectro-active ion exchange materials as working electrodes, it achieves efficient adsorption and desorption of target ions through the synergistic effect of light and electric fields, reducing power consumption while improving ion adsorption capacity and exchange rate.
[0005] Bi₂O₂CO₃, as a photoelectric dual-active material, has been applied to the extraction of I₂ in the P-ESIX system. - However, Bi2O2CO3 only absorbs ultraviolet light and some visible light, which limits its utilization of visible light and results in insufficient light-assisted efficiency.
[0006] Therefore, developing a Bi2O2CO3 modified material that can broaden the visible light absorption range and significantly increase the specific surface area and active sites, and applying it to P-ESIX technology to achieve efficient, low-consumption, and highly selective extraction of iodide ions, is an urgent problem to be solved. Summary of the Invention
[0007] The purpose of this invention is to provide a method for preparing Bi2O2CO3 modified materials and their applications, in order to solve the above-mentioned problems.
[0008] This invention provides a method for preparing Bi2O2CO3 modified materials, comprising the following steps: Bismuth salt and urea are dissolved in a solvent and mixed to obtain a mixed solution. Sodium citrate is then added to the mixed solution and stirred. After mixing, a hydrothermal reaction is carried out. The product obtained by hydrothermal treatment was washed and dried successively with deionized water and anhydrous ethanol to obtain CO3.2- Induced amorphous Bi2O2CO3 materials.
[0009] Preferably, the bismuth salt is 1 mmol, the urea is 50 mmol, and the molar ratio of the bismuth salt to sodium citrate is 0.05-0.2:1.
[0010] Preferably, the bismuth salt is bismuth nitrate, and the solvent is ethanol.
[0011] Preferably, the hydrothermal reaction temperature is 160°C and the reaction time is 4 hours; the drying treatment temperature is 60°C and the drying time is 12 hours.
[0012] Provides an application of Bi2O2CO3 modified materials, CO3 2- Iodide ion extraction was induced in amorphous Bi2O2CO3 materials using photo-assisted electro-controlled ion exchange technology.
[0013] Preferred, CO3 2- A method for inducing the extraction of iodide ions from amorphous Bi2O2CO3 materials using photo-assisted electro-controlled ion exchange technology includes the following steps: 1) Utilizing the CO3 2- Induced amorphous Bi2O2CO3 material to prepare working electrodes; 2) A photo-assisted electro-controlled ion exchange system was built using the working electrode, and iodine ions were extracted from iodine-containing solutions using the photo-assisted electro-controlled ion exchange system.
[0014] Preferably, the method for preparing the working electrode in step 1) includes: preparing CO3 2- Amorphous Bi2O2CO3 material is induced to mix with a conductive agent, a binder, and an organic solvent to obtain a slurry; the slurry is then coated onto conductive glass to obtain a working electrode.
[0015] Preferably, the CO3 2- The mass ratio of the induced amorphous Bi2O2CO3 material to the conductive agent and binder is 8:1:1.
[0016] Preferably, the adsorption potential for iodine ion extraction in step 2) is 0.2~0.6V based on the silver / silver chloride electrode, and the adsorption time is 10~90 min.
[0017] Preferably, the iodine ion concentration in the iodine-containing solution in step 2) is ≥1 ppm.
[0018] Therefore, the present invention, employing the above-mentioned method for preparing Bi2O2CO3 modified materials and its application, has the following beneficial effects: (1) A one-step hydrothermal method was used, with sodium citrate as a morphology modifier and CO3 as a catalyst. 2- Source, successfully prepared CO32- Induced amorphous Bi₂O₂CO₃ materials. The addition of sodium citrate caused Bi₂O₂CO₃ to evolve from a two-dimensional nanosheet morphology to a hierarchical three-dimensional microsphere structure. Accompanied by particle size refinement and lattice expansion, the specific surface area and pore volume were significantly increased, providing more active sites. At the same time, the visible light absorption range was extended from 381 nm to 410 nm, accelerating the separation and migration of photogenerated carriers.
[0019] (2) The CO3 2- When induced amorphous Bi₂O₂CO₃ materials are used for iodine extraction via P-ESIX, the iodine ion adsorption capacity reaches 632 mg·g⁻¹ under 0.6 V and visible light irradiation. -1 The light-assisted efficiency is as high as 29.77%, which is far superior to pure phase Bi2O2CO3 materials.
[0020] (3) The material of the present invention is effective against I - It exhibits excellent selectivity, in comparison with F - Cl - ,Br - SO4 2- NO3 - When competing anions coexist, I - / F - I - / Cl - I - / Br - I - SO4 2- and I - / NO3 - The separation factors were 4.59, 3.01, 10.63, 4.19 and 3.32, respectively, which enabled the selective extraction of iodide ions in complex systems.
[0021] (4) The material has good cycle stability. After 10 adsorption-desorption cycles, the iodine ion adsorption capacity still maintains more than 95% of the initial value. After 24 hours of cycle adsorption-desorption, the current remains basically unchanged. It can be reused to reduce the cost of use. Moreover, the whole extraction process is environmentally friendly and has no secondary pollution.
[0022] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0023] Figure 1 This invention relates to a method for preparing Bi2O2CO3 modified materials and its application. Example 2 shows a pure-phase Bi2O2CO3 material and CO3. 2-SEM images of induced amorphous Bi2O2CO3 materials, where (a) is an SEM image of pure-phase Bi2O2CO3 material composed of a single nanosheet, and (b) is an SEM image of CO3 material with a three-dimensional microsphere structure. 2- SEM images of induced amorphous Bi2O2CO3 materials: (c) is the Bi element mapping image of BOC, (d) is the O element mapping image of BOC, (e) is the C element mapping image of BOC, (f) is the Bi element mapping image of C-BOC, (g) is the O element mapping image of C-BOC, and (h) is the C element mapping image of C-BOC. Figure 2 The images shown are TEM and HRTEM images of BOC and C-BOC in Example 2 of the preparation method and application of Bi2O2CO3 modified material of the present invention. (a) is the TEM image of BOC, (b) is the HRTEM image of BOC, (c) is the TEM image of C-BOC, and (d) is the HRTEM image of C-BOC. Figure 3 The XRD patterns of BOC and C-BOC in Example 2 of the preparation method and application of Bi2O2CO3 modified material of the present invention are shown. Figure 4 XPS spectra of BOC and C-BOC in Example 2 of the preparation method and application of Bi2O2CO3 modified material of the present invention, wherein (ab) is the Bi 4f peak spectrum of BOC and C-BOC; (c) is the O 1s peak spectrum of BOC and C-BOC; and (d) is the C 1s peak spectrum of BOC and C-BOC. Figure 5 This invention provides a method for preparing Bi2O2CO3 modified materials and its application. Example 2 shows the adsorption isotherm, pore size distribution, and specific surface area of BOC and C-BOC. Among them, (a) is the adsorption isotherm, (b) is the pore size distribution, and (c) is the specific surface area. Figure 6 The present invention discloses a method for preparing Bi2O2CO3 modified material and its application. In Example 3, the CV curves of BOC and C-BOC under different conditions are shown. Among them, (a) is the CV curve of conductive substrate, BOC and C-BOC under light and dark conditions with a scan rate of 200mV / s, (b) is the CV curve of BOC film electrode with different scan rates under the non-Radal interval, (c) is the CV curve of C-BOC film electrode with different scan rates under the non-Radal interval, and (d) is the curve of the change of scan rate of BOC and C-BOC with the difference of current density. Figure 7EIS spectra and FTacV curves of BOC membrane electrode and C-BOC membrane electrode in Example 3 of the preparation method and application of Bi2O2CO3 modified material of the present invention, wherein (a) is the EIS spectra and (b) is the FTacV curve; Figure 8 The transient photocurrent response curves of the BOC film electrode and the C-BO film electrode C in Example 3 of the preparation method and application of Bi2O2CO3 modified material of the present invention are shown. Figure 9 This invention provides a method for preparing Bi2O2CO3 modified materials and its application. Example 4 describes the use of C-BOC membrane electrodes with different proportions of sodium citrate in ESIX and P-ESIX for the treatment of I... - Adsorption capacity diagram; Figure 10 This invention relates to a method for preparing Bi2O2CO3 modified materials and its application. Example 4 shows the BOC and C-BOC film electrodes used in the ESIX and P-ESIX processes to modify I... - The adsorption capacity and light-assisted efficiency of the light are shown in Figure 1, where (a) represents the adsorption capacity and (b) represents the light-assisted efficiency. Figure 11 The selective test diagrams of BOC membrane electrode and C-BOC membrane electrode in Example 5 of the preparation method and application of Bi2O2CO3 modified material of the present invention are shown. Figure 12 The following are stability test diagrams of BOC membrane electrode and C-BOC membrane electrode in Example 5 of the preparation method and application of Bi2O2CO3 modified material of the present invention. Among them, (a) is the stability of BOC and C-BOC membrane electrodes, (b) is the timing step potential setting diagram, (c) is the current change diagram of BOC membrane electrode over 24 h, and (d) is the current change diagram of C-BOC membrane electrode over 24 h. Figure 13 The optical analysis diagrams of BOC and C-BOC in Example 6 of the preparation method and application of Bi2O2CO3 modified material of the present invention are shown. (a) is the UV-Vis diffuse reflectance spectrum of BOC and C-BOC, (b) is the relationship between (αhν)1 / 2 and photon energy (hν), (c) is the XPS-VB spectrum of BOC and C-BOC, and (d) is the energy level structure diagram. Detailed Implementation
[0024] To better understand the above technical solutions, a detailed description of the solutions will be provided below in conjunction with the accompanying drawings and specific embodiments. Obviously, the described embodiments are merely some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0025] The terminology used in the embodiments of this invention is for the purpose of describing particular embodiments only and is not intended to limit the invention. The singular forms “a,” “the,” and “the” as used in the embodiments of this invention and the appended claims are also intended to include the plural forms, and “multiple” generally includes at least two unless the context clearly indicates otherwise.
[0026] It should also be noted that the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that an article or device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such an article or device. Without further limitation, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the article or device that includes said element.
[0027] Example 1 This embodiment prepares pure-phase Bi2O2CO3 materials and CO3. 2- Induced amorphous Bi₂O₂CO₃ materials and the use of pure-phase Bi₂O₂CO₃ materials and CO₃²⁻ 2- Induced amorphous Bi2O2CO3 material to prepare membrane electrodes.
[0028] Step 1: Preparation of pure-phase Bi2O2CO3 (BOC) material; Weigh 1 mmol Bi(NO3)3·5H2O and 50 mmol urea, and dissolve them separately in 20 mL of ethanol. Stir the solutions magnetically to form a mixed solution. Transfer the mixture to a Teflon-lined reactor and heat to 160 °C for 4 h, then cool to room temperature. Collect the powder by centrifugation, wash three times each with deionized water and anhydrous ethanol, and dry at 60 °C for 12 h to obtain pure-phase Bi2O2CO3 material, denoted as BOC.
[0029] Step 2: CO3 2- Preparation of induced amorphous Bi2O2CO3 (C-BOC) materials; Weigh 1 mmol Bi(NO3)3·5H2O and 50 mmol urea, and dissolve them separately in 20 mL of ethanol. Stir magnetically to form a mixed solution. Add 0.15 mmol sodium citrate (molar ratio of sodium citrate to Bi(NO3)3·5H2O is 0.15), and continue stirring for 30 min. Transfer the mixture to a Teflon-lined reactor, heat to 160 °C for 4 h, and then cool to room temperature. Collect the powder by centrifugation, wash three times each with deionized water and anhydrous ethanol, and dry at 60 °C for 12 h to obtain CO3. 2-Induced amorphous Bi2O2CO3 material, denoted as C-BOC.
[0030] Step 3: Fabrication of the membrane electrode; The pure-phase Bi₂O₂CO₃ material prepared in step 1, polyvinylidene fluoride (PVDF), and conductive carbon black were mixed at a mass ratio of 8:1:1 and ground for 10 minutes. Then, an appropriate amount of 1-methyl-2-pyrrolidone (NMP) was added and stirred for 6 hours to obtain a uniform slurry. The slurry was uniformly coated onto pretreated fluorine-doped tin oxide (FTO) conductive glass to a thickness of 15 μm, and then dried in a vacuum drying oven at 60 °C for 12 h to obtain a BOC film electrode.
[0031] The CO3 prepared in step 2 2- Amorphous Bi₂O₂CO₃ material, polyvinylidene fluoride (PVDF), and conductive carbon black were mixed at a mass ratio of 8:1:1 and ground for 10 minutes. Then, an appropriate amount of 1-methyl-2-pyrrolidone (NMP) was added and the mixture was stirred for 6 hours to obtain a homogeneous slurry. The slurry was uniformly coated onto pretreated fluorine-doped tin oxide (FTO) conductive glass to a thickness of 15 μm, and then dried in a vacuum drying oven at 60 °C for 12 h to obtain a C-BOC film electrode.
[0032] Example 2 In this embodiment, the BOC and C-BOC materials prepared in Example 1 were characterized using scanning electron microscopy (SEM), transmission electron microscopy (TEM), high-resolution transmission electron microscopy (HRTEM), X-ray diffraction (XRD), and X-ray photoelectron spectroscopy (XPS). The microstructure, crystal structure, surface chemical state, and pore structure characteristics of the materials were systematically analyzed, as detailed below: SEM characterization results are as follows: Figure 1 As shown, unlike pure-phase BOC which is composed of a large number of single nanosheets, the morphology of BOC changes from two-dimensional nanosheets to a hierarchical three-dimensional microsphere structure with the addition of sodium citrate. This morphology can generate multiple light scattering and reflection, which is beneficial to improving the light-harvesting ability. Figure 1 (c)-(e) and (f)-(h) are elemental mapping images of BOC and C-BOC, respectively, clearly showing the uniform distribution of Bi, O and C elements.
[0033] TEM and HRTEM characterization results are as follows Figure 2 As shown, BOC exhibits a two-dimensional sheet-like stacked morphological feature, such as... Figure 2 As shown in (a), the clear lattice fringe spacing is 0.273 nm, corresponding to the (110) crystal plane of the BOC crystal, as... Figure 2As shown in (b) in the figure. TEM images of the C-BOC sample show that its morphology has changed from two-dimensional sheet-like to finer nanoparticles with a significant reduction in particle size. The lattice fringe spacing in the HRTEM image is 0.282 nm, which also corresponds to the (110) crystal plane. Compared with BOC, there is obvious lattice expansion and the lattice fringes are also more blurred, indicating that C-BOC has more lattice defects and distortions, which is beneficial to improving light-harvesting ability.
[0034] XRD characterization results are as follows Figure 3 As shown, all diffraction peaks can be attributed to the tetragonal phase of Bi₂O₂CO₃ (JCPDS card number 41-1488), indicating that the sample is a pure phase. With the addition of sodium citrate, the XRD characteristic peaks of C-BOC gradually broaden, attributed to grain refinement and lattice expansion, indicating the presence of excess CO₃²⁻. 2- Some of them enter the interstitial spaces of the crystal lattice, forming an amorphous structure.
[0035] XPS characterization results are as follows Figure 4 As shown, the Bi 4f peak of C-BOC shifts towards lower binding energies compared to BOC, indicating an increase in electron cloud density around the Bi sites; in the O 1s spectrum, both the CO peak and the Bi-O peak of C-BOC shift towards higher binding energies, indicating an excess of CO32-. 2- It altered the chemical environment of the O atom; CO3 in C-BOC in the C 1s spectrum 2- The characteristic peaks shift to lower binding energies, while the C and D peaks shift to higher binding energies, indicating the introduction of additional CO3. 2- The work of embedding into the lattice alters the chemical state of surface carbon species.
[0036] Based on the above characterization, it was preliminarily confirmed that the specific surface area of C-BOC was effectively increased. To obtain more conclusive evidence, nitrogen adsorption-desorption tests were conducted on both materials. Firstly, the isotherms of both BOC and C-BOC exhibited Type IV characteristics, such as... Figure 5 As shown in (a), an H3-type hysteresis ring appears in the high relative pressure region, indicating the presence of a mesoporous structure in the material. Figure 5 The pore size distribution diagram shown in (b) confirms this. Furthermore, compared to BOC, C-BOC exhibits a wider pore size distribution, larger pore volume, and a more diverse pore structure. In addition, its specific surface area increases from 12.73 m² / g. 2 ·g -1 Increased to 29.83 m 2 ·g -1 The increase exceeded 2 times, such as Figure 5 As shown in (c), the increase in specific surface area and pore volume increases the surface roughness of the material and the exposed active sites, while providing more channels for mass transfer processes, which is consistent with the broadened peak results in XRD.
[0037] Example 3 This embodiment performs CV testing on the C-BOC membrane electrode and BOC membrane electrode prepared in Example 1.
[0038] The photoelectrochemical performance was tested using a two-electrode system. The working electrodes were the C-BOC membrane electrode and the BOC membrane electrode prepared in Example 1, the counter electrode was FTO conductive glass, the electrolyte was 0.1 M KI solution, and the scan rate was 200 mV·s. -1 Simultaneously applying simulated sunlight irradiation (λ>380 nm) to simulate light-assisted conditions, the CV test results are as follows: Figure 6 As shown in (a), C-BOC exhibits a larger electrochemical active area and a higher peak current under dark conditions, indicating that the addition of sodium citrate significantly improves the electrochemical response capability. Under light conditions, the peak current and electrochemical active area of both membrane electrodes increase significantly, and the peak current and electrochemical active area of C-BOC are greater than those of BOC, indicating that C-BOC has more free electrons entering the electrochemical process under light conditions.
[0039] The results of calculating the electric double-layer capacitance using CV curves at different scan rates within the non-Radida interval are as follows: Figure 6 As shown in (b)-(c), Figure 6 The linear fitting results in (d) show that the C-BOC's C dl The value is 3.92 mF·cm -2 It is significantly higher than BOC's 2.52 mF·cm⁻¹ -2 From the formula The calculated electrochemically active surface area (ECSA) of C-BOC is 98 cm². 2 BOC is 63 cm 2 C-BOC exhibits a larger electrochemically active surface area; where Cs represents the specific capacitance per unit area of an ideal smooth planar electrode surface.
[0040] EIS test results are as follows Figure 7 As shown in (a), the semicircular diameter of C-BOC in the high-frequency region is smaller than that of BOC under both dark and light conditions, indicating that the charge transfer resistance of the C-BOC film electrode is lower and the electron transfer rate is faster; the slope of C-BOC in the low-frequency region of the P-ESIX system is the largest, indicating that under light conditions, I - The diffusion rate is faster. For example... Figure 7As shown in (b), the peak currents of both materials were enhanced after illumination, indicating that the introduction of the external light field excited more electrons from the material surface into the electrochemical system. C-BOC exhibited the largest peak current near 0.27 V, suggesting that the introduction of sodium citrate enhanced charge transfer in BOC. Furthermore, C-BOC reached its peak current at a lower potential, indicating that charge transfer was more readily achieved than in BOC, consistent with the EIS analysis results above.
[0041] Transient photocurrent response test results are as follows Figure 8 As shown, under simulated sunlight irradiation (λ>380 nm), the peak current of the photocurrent of both membrane electrodes increases. The increase in peak current of the C-BOC membrane electrode is more significant and has good repeatability, indicating that C-BOC has higher charge separation efficiency and stronger photocurrent response capability.
[0042] Example 4 This embodiment performs adsorption tests on the C-BOC membrane electrode and BOC membrane electrode prepared in Example 1.
[0043] A three-electrode system was employed, using the C-BOC membrane electrode and the BOC membrane electrode prepared in Example 1 as the working electrodes, Ag / AgCl as the reference electrode, and FTO conductive glass as the counter electrode. The entire electrolytic cell was constructed of quartz glass to facilitate illumination of the entire apparatus by a light source throughout the experiment, which was conducted entirely in a dark box. Visible light with a wavelength greater than 380 nm (intensity 100 mW / cm²) was applied for illumination. 2 The specific details are as follows: The adsorption experiment was conducted in a 0.4 mM KI solution for 90 min. An adsorption voltage of 0.6 V was set, and a desorption experiment was performed before the adsorption experiment to remove some CO32-. 2- , for I - The adsorption creates ion channels. Desorption experiments were conducted in 0.1 M Na₂SO₄ solution at a desorption voltage of -0.6 V.
[0044] The effect of different sodium citrate concentrations on adsorption capacity is as follows: Figure 9 As shown, the adsorption capacity of both the ESIX and P-ESIX systems reached its maximum when the molar ratio of sodium citrate to Bi(NO3)3·5H2O was 0.15. When the ratio was less than 0.15, the adsorption capacity showed a significant increasing trend with increasing concentration, while when the ratio was greater than 0.15, the adsorption capacity dropped sharply. This trend may be attributed to the gradual increase in the light absorption range and specific surface area. However, excessive sodium citrate can lead to problems such as the covering of active sites and the blockage of ion channels, which in turn reduces its photo-assisted efficiency and adsorption capacity. Therefore, the optimal concentration of sodium citrate is a molar ratio of 0.15.
[0045] The adsorption properties of C-BOC membrane electrodes and BOC membrane electrodes, for example... Figure 10 As shown, after introducing an external light field, the adsorption capacity of the BOC film electrode increased from 415 mg·g⁻¹. -1 Increased to 512 mg / g -1 The light-assisted efficiency was 23.37%; the adsorption capacity of the C-BOC membrane electrode increased from 487 mg·g⁻¹. -1 Increased to 632 mg·g -1 The light-assisted efficiency reached 29.77%, indicating that C-BOC not only improved the efficiency of I... - It not only improves adsorption performance but also enhances the utilization rate of visible light.
[0046] Example 5 This embodiment performs selectivity and stability tests on the C-BOC membrane electrode and BOC membrane electrode prepared in Example 1.
[0047] Selectivity test: in each anion (F - Cl - ,Br - SO4 2- NO3 - ) and I - When the molar concentrations are the same, a competitive adsorption experiment is conducted. The results are as follows: Figure 11 As shown, the C-BOC film electrode is used for I - / F - I - / Cl - I - / Br - I - SO4 2- and I - / NO3 - The separation factors were 4.59, 3.01, 10.63, 4.19, and 3.32, respectively, all higher than those of the BOC membrane electrode, indicating that C-BOC has a better effect on I. - The selectivity has been significantly improved.
[0048] Stability testing: Multiple cyclic adsorption-desorption experiments were conducted in 0.1 M KI solution and Na2SO4 solution. The results are as follows: Figure 12 As shown in (a), after 10 adsorption and desorption cycles, the adsorption rates of both materials remained above 95%. The membrane electrode was subjected to a 24-hour cycle test using the time-lapse step potential method, as shown in (a). Figure 12As shown in (b)-(d), after applying a positive potential of 0.6 V and a negative potential of -0.6 V for one minute each, the currents of the BOC membrane electrode and the C-BOC membrane electrode remained essentially unchanged, further demonstrating the stability of the materials. The current value of the C-BOC membrane electrode was significantly higher than that of the BOC membrane electrode, further proving the superior electrochemical activity of C-BOC.
[0049] Example 6 This embodiment performs optical analysis on the C-BOC and BOC prepared in Example 1 to explore the performance improvement mechanism.
[0050] Optical analysis results as follows Figure 13 As shown in (a), C-BOC has a higher absorption intensity in the ultraviolet region than BOC and exhibits absorption characteristics in the visible light region. The addition of sodium citrate extends the light absorption range of BOC from 381 nm to 410 nm. Band gap calculation results show that, as Figure 13 As shown in (b), the band gaps of BOC and C-BOC are 3.13 eV and 2.99 eV, respectively, for excess CO3. 2- Entering the crystal lattice effectively reduces the band gap value of BOC. For example... Figure 13 As shown in (c), XPS valence band spectroscopy calculations show that the valence band position for both BOC and C-BOC is 1.82 eV, while the conduction band positions are -1.31 eV and -1.17 eV, respectively. This indicates that the valence band position remains unchanged, but the conduction band position decreases, thus reducing the band gap. Figure 13 As can be seen from the energy level structure diagram (d) in the diagram, the decrease in band gap makes it easier for electrons to transition into photogenerated electrons and enter the electrochemical process, accelerating the electron migration rate and the number of free electrons, thereby realizing the C-BOC effect on I. - Improved adsorption performance.
[0051] Therefore, this invention employs the above-mentioned method for preparing Bi2O2CO3 modified materials and its application, using a one-step hydrothermal method with sodium citrate as a morphology modifier and CO3. 2- Source, successfully prepared CO3 2- Induced amorphous Bi₂O₂CO₃ materials. The addition of sodium citrate caused Bi₂O₂CO₃ to evolve from a two-dimensional nanosheet morphology to a hierarchical three-dimensional microsphere structure. Accompanied by particle size refinement and lattice expansion, the specific surface area and pore volume were significantly increased, providing more active sites. At the same time, the visible light absorption range was extended from 381 nm to 410 nm, accelerating the separation and migration of photogenerated carriers.
[0052] The CO3 2- When induced amorphous Bi₂O₂CO₃ materials are used for iodine extraction via P-ESIX, the iodine ion adsorption capacity reaches 632 mg·g⁻¹ under 0.6 V and visible light irradiation. -1The light-assisted efficiency reached 29.77%, far superior to that of pure-phase Bi₂O₂CO₃ materials, while the adsorption capacity of Bi₂O₂CO₃ materials was 512 mg·g⁻¹. -1 The light-assisted efficiency is 23.37%.
[0053] The material of the present invention is related to I - It exhibits excellent selectivity, in comparison with F - Cl - ,Br - SO4 2- NO3 - When competing anions coexist, I - / F - I - / Cl - I - / Br - I - SO4 2- and I - / NO3 - The separation factors were 4.59, 3.01, 10.63, 4.19 and 3.32, respectively, which enabled the selective extraction of iodide ions in complex systems.
[0054] The material exhibits excellent cycle stability. After 10 adsorption-desorption cycles, the iodine ion adsorption capacity remains above 95% of the initial value. After 24 hours of cycle adsorption-desorption, the current remains essentially unchanged, making it reusable and reducing usage costs. Furthermore, the entire extraction process is environmentally friendly and produces no secondary pollution.
[0055] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit them. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can still be made to the technical solutions of the present invention, and these modifications or equivalent substitutions cannot cause the modified technical solutions to deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. An application of a Bi2O2CO3 modified material, characterized in that, CO3 2- The extraction of iodide ions from amorphous Bi₂O₂CO₃ materials using photo-assisted electro-controlled ion exchange technology includes the following steps: 1) Utilizing the CO3 2- Induced amorphous Bi2O2CO3 material to prepare working electrodes; 2) A photo-assisted electro-controlled ion exchange system was built using the working electrode, and iodide ions were extracted from iodine-containing solutions using the photo-assisted electro-controlled ion exchange system; CO3 2- The preparation method of induced amorphous Bi2O2CO3 materials includes the following steps: Bismuth salt and urea are dissolved in a solvent and mixed to obtain a mixed solution. Sodium citrate is then added to the mixed solution and stirred. After mixing, a hydrothermal reaction is carried out. The product obtained by hydrothermal treatment was washed and dried successively with deionized water and anhydrous ethanol to obtain CO3. 2- Induced amorphous Bi2O2CO3 materials.
2. The application of the Bi2O2CO3 modified material according to claim 1, characterized in that, The method for preparing the working electrode in step 1) includes: preparing CO3 2- Amorphous Bi2O2CO3 material is induced to mix with a conductive agent, a binder, and an organic solvent to obtain a slurry; the slurry is then coated onto conductive glass to obtain a working electrode.
3. The application of the Bi2O2CO3 modified material according to claim 2, characterized in that, The CO3 2- The mass ratio of the induced amorphous Bi2O2CO3 material to the conductive agent and binder is 8:1:
1.
4. The application of the Bi2O2CO3 modified material according to claim 1, characterized in that, The adsorption potential for iodine ion extraction in step 2) is 0.2~0.6 V, and the adsorption time is 10~90 min.
5. The application of the Bi2O2CO3 modified material according to claim 1, characterized in that, The iodine ion concentration in the iodine-containing solution described in step 2) is ≥1 ppm.
6. The application of the Bi2O2CO3 modified material according to claim 1, characterized in that, The bismuth salt is 1 mmol, the urea is 50 mmol, and the molar ratio of the bismuth salt to sodium citrate is 0.05-0.2:
1.
7. The application of the Bi2O2CO3 modified material according to claim 1, characterized in that, The bismuth salt is bismuth nitrate, and the solvent is ethanol.
8. The application of the Bi2O2CO3 modified material according to claim 1, characterized in that, The hydrothermal reaction was carried out at a temperature of 160°C for 4 hours; the drying process was carried out at a temperature of 60°C for 12 hours.
Citation Information
Patent Citations
Method for extracting iodide ions through photo-assisted electric control ion exchange based on oxygen vacancy type BiOI material