A method for preparing high-entropy lithium manganese oxide cathode material
By doping with multiple metal ions and coating with silane-triphenylmethane-structured polyimide, the structural instability and manganese leaching problems of lithium manganese oxide cathode materials are solved, improving their cycle performance and thermal stability, making them suitable for high-performance lithium-ion batteries.
Patent Information
- Application Number
- CN202610808054.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-06-05
- Publication Date
- 2026-07-10
AI Technical Summary
Spinel-type LiMn2O4 lithium manganese oxide cathode material is prone to Jahn-Teller distortion during cycling, leading to structural instability and irreversible capacity decay. Mn3+ is easily reduced to Mn2+ and dissolved in the electrolyte, causing loss of active material and seriously affecting its cycle performance and capacity.
A high-entropy structure is formed by synergistic doping of multiple metal ions. The polyimide containing silane triphenylmethane structure is coated by ball milling and low-temperature heat treatment to stabilize the crystal structure, inhibit manganese dissolution and improve electrochemical performance.
It significantly improves the cycle stability, rate performance, and thermal stability of lithium manganese oxide cathode materials, making them suitable for high-performance lithium-ion batteries.
Smart Images

Figure CN122370290A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-entropy lithium manganese oxide cathode materials, and specifically to a method for preparing high-entropy lithium manganese oxide cathode materials. Background Technology
[0002] Lithium-ion batteries (LIBs) are widely used in consumer electronics and electric vehicles, and are a key technology for global decarbonization and greenhouse gas emission reduction. Decarbonization demands are driving the development of LIBs towards greater safety, longer cycle life, higher energy density, and lower cost.
[0003] Current high-energy-density ternary cathode materials heavily rely on cobalt and nickel, both of which have limited reserves and poor thermal stability. Therefore, cobalt-free and nickel-free cathode materials are becoming a research hotspot for next-generation cathode materials. Spinel-type LiMn2O4 has great application potential due to its low cost, high operating potential, and ease of synthesis; however, its short cycle life remains a problem to be solved: firstly, it is prone to Jahn-Teller distortion during cycling, transforming from a cubic phase to a tetragonal phase, leading to structural instability and irreversible capacity decay; secondly, the Mn content within the crystal framework... 3+ Easily reduced to Mn 2+ It dissolves in the electrolyte, causing loss of active material and exacerbating side reactions between the electrode and the electrolyte. These problems lead to a rapid decrease in the capacity of LiMn2O4 and a sharp decline in its cycling performance, severely restricting its further commercialization and application.
[0004] Therefore, developing a preparation method that can synergistically improve the structural stability of lithium manganese oxide, inhibit manganese dissolution, and optimize electrochemical performance has become a key requirement for the research and development of high-performance lithium manganese oxide cathode materials. Summary of the Invention
[0005] In order to overcome the above-mentioned technical problems, the purpose of this invention is to provide a method for preparing high-entropy lithium manganese oxide cathode material.
[0006] The objective of this invention can be achieved through the following technical solutions: This application provides a method for preparing high-entropy lithium manganese oxide cathode material, including the following steps: Step 1: Place the manganese source, lithium salt, and dopant ion M into a ball mill and ball mill for 3-3.2 hours at a speed of 250-300 r / min to obtain a mixture. Step 2: Place the mixture in a muffle furnace and preheat it to 450-550℃ in an air atmosphere at a heating rate of 1-8℃ / min for 4-6 hours. Then, heat it to 750-850℃ at a heating rate of 1-8℃ / min and sinter it for 8-15 hours. Finally, cool it to room temperature at a cooling rate of 1-2℃ / min. After that, take it out and grind it. Then, sieve it through a 250-mesh sieve and take the sieve material to obtain the lithium manganese oxide matrix material. Step 3: Place the lithium manganese oxide matrix material and the silane-containing triphenylmethane structured polyimide into a ball mill and ball mill for 2-2.2 hours at a speed of 200-300 r / min. Then place it in a muffle furnace and keep it at a temperature of 320-380℃ for 3-5 hours. Cool it with the furnace and then sieve it through a 250-mesh sieve. Take the sieve-passing material to obtain the high-entropy lithium manganese oxide cathode material.
[0007] In a preferred embodiment of the present invention, the lithium source in step one is one or more of lithium acetate, lithium oxalate, lithium carbonate, lithium nitrate and lithium hydroxide; the manganese source is one or more of manganese acetate, manganese oxalate, manganese nitrate, manganese carbonate and manganese tetroxide.
[0008] In a preferred embodiment of the present invention, the dopant ion M in step one is Al. 3+ Ce 3+ Ti 4+ With Sb 5+ One or more of them.
[0009] As a preferred embodiment of the present invention, in step one, Al 3+ Derived from at least one of aluminum oxide, aluminum phosphate, aluminum metaphosphate, and aluminum hydroxide; Ce 3+ Derived from at least one of cerium trioxide, cerium carbonate, cerium nitrate, and cerium hydroxide; Ti 4+ Derived from at least one of titanium dioxide, titanium chloride, tetrabutyl titanate, and titanium hydroxide; Sb 5+ It is derived from at least one of antimony pentoxide, antimony pentanitrate, and antimony ammonium fluoride.
[0010] In a preferred embodiment of the present invention, the molar ratio of lithium source, manganese source and doped ion M in step one is (1-1.14):(2-x):x, where x=0.005-0.05.
[0011] In a preferred embodiment of the present invention, the silyltriphenylmethane-containing polyimide in step three is 2-4% of the mass of the lithium manganese oxide matrix material.
[0012] In a preferred embodiment of the present invention, the silyltriphenylmethane-containing polyimide is prepared by the following steps: Step a1: Add 2,6-dimethylaniline to a three-necked flask equipped with a stirrer, thermometer, gas delivery tube, and constant-pressure dropping funnel. Purge with nitrogen for protection. Start stirring at 95-100℃ and a stirring rate of 300-400 r / min. Mix p-hydroxybenzaldehyde, ethylene glycol methyl ether, and p-toluenesulfonic acid, then transfer the mixture to the constant-pressure dropping funnel and add it dropwise to the reaction system, controlling the dropping rate at 1-2 drops / s. After the addition is complete, raise the temperature to 105-110℃. At 0℃, continue stirring for 8-9 hours. After the reaction is complete, cool to room temperature and pour into anhydrous methanol under stirring. Add saturated sodium bicarbonate solution to adjust the pH to 9. Add activated carbon and stir at room temperature for 30-32 minutes. Then, collect the solid by vacuum filtration and wash it 3-4 times with deionized water. Then, recrystallize it by heating with ethyl acetate under reflux. After filtration, place the filter cake in a vacuum drying oven and dry it at 80-85℃ for 12-13 hours to obtain a diamine monomer containing a hydroxyl triphenylmethane structure. Step a2: Add the hydroxytriphenylmethane-containing diamine monomer, hexafluorodianhydride, and anhydrous N-methylpyrrolidone to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Under nitrogen protection, stir at 300-400 r / min for 60-70 min in an ice bath, then stir at room temperature for 6-7 h. Then add acetic anhydride and triethylamine sequentially, continue stirring for 2-2.2 h, raise the temperature to 55-60℃ and hold for 4-4.2 h, then cool to room temperature and pour into anhydrous ethanol under stirring. Collect the solid by vacuum filtration, wash twice with isopropanol, and then place the filter cake in a vacuum drying oven and dry at 95-100℃ for 10-11 h to obtain the hydroxytriphenylmethane-containing polyimide. Step a3: Add the hydroxyl-containing triphenylmethane-structured polyimide, triisopropylchlorosilane, imidazole, and N,N-dimethylformamide to a single-necked flask, purge with nitrogen for protection, and stir for 18-20 h at a temperature of 25-30℃ and a stirring rate of 300-400 r / min. After the reaction is complete, a mixed solution is obtained. The mixed solution is added dropwise to anhydrous ethanol while stirring, then filtered under reduced pressure, washed three times with anhydrous methanol, dissolved in dichloromethane, dried for 30-32 min with anhydrous magnesium sulfate, filtered, and the filtrate is added dropwise to isopropanol to precipitate. The precipitate is then placed in a vacuum drying oven and dried at a temperature of 95-100℃ for 11-12 h to obtain the silyltriphenylmethane-structured polyimide.
[0013] In a preferred embodiment of the present invention, the ratio of 2,6-dimethylaniline, p-hydroxybenzaldehyde, ethylene glycol methyl ether, p-toluenesulfonic acid, anhydrous methanol, and activated carbon in step a1 is 0.2-0.4 mol: 0.1-0.2 mol: 40-80 mL: 0.5-1.0 g: 500-1000 mL: 0.3-0.6 g.
[0014] In a preferred embodiment of the present invention, the ratio of the amount of the hydroxyl triphenylmethane-containing diamine monomer, hexafluorodianhydride, anhydrous N-methylpyrrolidone, acetic anhydride, triethylamine and anhydrous ethanol in step a2 is 4-8 mmol: 4-8 mmol: 20-40 mL: 6-12 mL: 4-8 mL: 200-400 mL.
[0015] In a preferred embodiment of the present invention, the ratio of the amount of hydroxyl triphenylmethane-containing polyimide, triisopropylchlorosilane, imidazole, N,N-dimethylformamide, anhydrous ethanol and dichloromethane in step a3 is 2-4 mmol: 3-6 mmol: 3-6 mmol: 20-40 mL: 200-400 mL: 15-30 mL.
[0016] The beneficial effects of this invention are: This invention discloses a method for preparing a high-entropy lithium manganese oxide cathode material. A manganese source, lithium salt, and dopant ions M are ball-milled to obtain a mixture. This mixture is then sintered in a muffle furnace, cooled, and subsequently ground and sieved to obtain a lithium manganese oxide matrix material. The lithium manganese oxide matrix material and a silyltriphenylmethane-containing polyimide are then ball-milled, coated with a low-temperature heat treatment solution, cooled, and sieved to obtain the high-entropy lithium manganese oxide cathode material. The high-entropy structure is formed by the synergistic doping of multiple metal ions. This increases the system's configuration entropy, stabilizes the crystal lattice, suppresses phase transitions and manganese dissolution, and reduces ion transport impedance, resulting in superior cycle stability and rate performance. Low-temperature coating modification with a silyltriphenylmethane-containing polyimide significantly improves the overall electrochemical performance of the lithium manganese oxide cathode material. Multi-element doping can stabilize the spinel lattice structure by forming stronger MO bonds, reducing the high-spin Mn content. 3+ The content of manganese oxide suppresses Jahn-Teller distortion, thereby reducing manganese dissolution and improving the structural stability and cycle life of the material. The polyimide coating with silane-containing triphenylmethane structure can form a uniform, flexible and high-temperature resistant interfacial protective film on the electrode surface, reducing side reactions between the electrolyte and the active material, lowering interfacial impedance, and improving the thermal stability and rate performance of the material. The preparation process is simple, mild, and easy to industrialize. The resulting high-entropy lithium manganese oxide cathode material has high cycle stability, excellent rate performance and good high-temperature safety, making it suitable for high-performance lithium-ion batteries.
[0017] In the preparation of high-entropy lithium manganese oxide cathode material, a polyimide containing a silyltriphenylmethane structure was first prepared. The initial step involved an acid-catalyzed condensation reaction between an aromatic aldehyde and an aromatic amine. The aldehyde group of p-hydroxybenzaldehyde and the amino group of two molecules of 2,6-dimethylaniline under p-toluenesulfonic acid catalysis underwent dehydration condensation to form a triphenylmethane central skeleton. The phenolic hydroxyl group was retained as the active site for subsequent silanization. After neutralization, decolorization, and recrystallization with ethyl acetate, a diamine monomer containing a hydroxytriphenylmethane structure was obtained. Subsequently, the diamine underwent nucleophilic addition with a dianhydride and... In the imidization process, a diamine monomer containing a hydroxyl triphenylmethane structure first undergoes addition with hexafluorodianhydride at low temperature to form a polyamic acid precursor. Then, under the action of acetic anhydride and triethylamine, it undergoes low-temperature dehydration and cyclization to generate an imide ring. During this process, the phenolic hydroxyl group remains unchanged. The resulting hydroxyl-containing polyimide, due to the large-volume structure of the trifluoromethyl group and triphenylmethane in the hexafluorodianhydride, possesses good solubility, transparency, and heat resistance. Subsequently, under the catalysis of imidazole and the action of a binding acid, the phenolic hydroxyl group is converted into a phenoxy anion and undergoes nucleophilic substitution with triisopropylchlorosilane to form a Si-O-A ring. The r-silyl ether bond transforms the side-chain hydroxyl groups into triisopropylsiloxy groups, and finally, high-purity silyl-containing polyimide is obtained through methanol washing and secondary precipitation with isopropanol. This significantly improves the material's hydrophobicity, resistance to damp heat, and reduces its dielectric constant. The large-volume rigid framework of triphenylmethane can disrupt the molecular chain regularity, significantly improving the solubility of polyimide in organic solvents, while retaining the active phenolic hydroxyl groups. This allows for site-specific and controlled silanization of polyimide without damaging the polymer backbone structure. In terms of silanization modification, silylation can be completed at room temperature. The grafting reaction is carried out under mild conditions and does not lead to polymer degradation. The introduced triisopropylsilane group has a large steric hindrance, which can significantly reduce the polarity and dielectric constant of the polymer, while improving the water resistance, damp heat resistance and insulation properties of the material. Moreover, the modified polymer still maintains good solubility, which is convenient for subsequent film formation, coating and other processing operations. The final prepared silyltriphenylmethane-containing polyimide has excellent properties such as high light transmittance, low dielectric, low water absorption, high heat resistance and high mechanical strength, and has a wide range of applications and can be used in many fields. Attached Figure Description
[0018] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0019] Figure 1 This is an XRD pattern of the lithium manganese oxide cathode material of Example 1 of this application; Figure 2 This is a SEM schematic diagram of the lithium manganese oxide cathode material of Example 1 of this application; Figure 3This is a magnified SEM image of the lithium manganese oxide cathode material of Example 1 of this application; Figure 4 This is a TEM schematic diagram of the lithium manganese oxide cathode material of Example 1 of this application; Figure 5 This is a magnified TEM schematic diagram of the lithium manganese oxide cathode material of Example 1 of this application. Detailed Implementation
[0020] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0021] Example 1: This embodiment describes a method for preparing a high-entropy lithium manganese oxide cathode material, including the following steps: Step s1: Add 0.2 mol 2,6-Dimethylaniline was added to a three-necked flask equipped with a stirrer, thermometer, gas delivery tube, and constant-pressure dropping funnel. Nitrogen gas was introduced for protection, and stirring was started at 95°C and a stirring rate of 300 r / min. 0.1 mol of p-hydroxybenzaldehyde, 40 mL of ethylene glycol methyl ether, and 0.5 g of p-toluenesulfonic acid were mixed and then transferred to a constant-pressure dropping funnel and added dropwise to the reaction system at a dropping rate of 1 drop / s. After the addition was complete, the temperature was raised to 105°C and stirring was continued for 8 h. After the reaction was completed, the mixture was cooled to room temperature and poured into 500 mL of anhydrous methanol under stirring. Saturated sodium bicarbonate solution was added to adjust the pH to 9, and 0.3 g of activated carbon was added. The mixture was stirred at room temperature for 30 min, and then the solid was collected by vacuum filtration. The solid was washed three times with deionized water and then recrystallized by heating with ethyl acetate under reflux. After filtration, the filter cake was placed in a vacuum drying oven and dried at 80°C for 12 h to obtain a diamine monomer containing a hydroxytriphenylmethane structure. Step s2: 4 mmol of hydroxytriphenylmethane-containing diamine monomer, 4 mmol of hexafluorodianhydride, and 20 mL of anhydrous N-methylpyrrolidone were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 60 min at a stirring rate of 300 r / min under ice bath conditions. After stirring at room temperature for 6 h, 6 mL of acetic anhydride and 4 mL of triethylamine were added sequentially, and stirring was continued for 2 h. The temperature was raised to 55 °C and maintained for 4 h. After cooling to room temperature, the mixture was poured into 200 mL of anhydrous ethanol under stirring. The solid was then collected by vacuum filtration, washed twice with isopropanol, and the filter cake was placed in a vacuum drying oven and dried at 95 °C for 10 h to obtain hydroxytriphenylmethane-containing polyimide. Step s3: 2 mmol of hydroxyl triphenylmethane-containing polyimide, 3 mmol of triisopropylchlorosilane, 3 mmol of imidazole and 20 mL of N,N-dimethylformamide were added to a single-necked flask, and nitrogen gas was introduced for protection. The mixture was stirred for 18 h at 25 °C and a stirring rate of 300 r / min. After the reaction was completed, a mixed solution was obtained. The mixed solution was added dropwise to 200 mL of anhydrous ethanol while stirring. The mixture was then filtered under reduced pressure, washed three times with anhydrous methanol, dissolved in 15 mL of dichloromethane, dried for 30 min with anhydrous magnesium sulfate, filtered, and the filtrate was added dropwise to isopropanol to precipitate. The precipitate was then placed in a vacuum drying oven and dried at 95 °C for 11 h to obtain silyltriphenylmethane-containing polyimide. Step s4: Weigh lithium carbonate, manganese tetroxide, aluminum oxide, cerium oxide, titanium dioxide, and antimony pentoxide according to the molar ratio of lithium, manganese, aluminum, cerium, titanium, and antimony of 1:1.98:0.005:0.005:0.005:0.005, and put them into a ball mill. Ball mill at 250 r / min for 3 hours to obtain a mixture. Step s5: Place the mixture in a muffle furnace and pre-fire it for 4 hours at a heating rate of 1℃ / min in an air atmosphere. Then, heat it to 750℃ at a heating rate of 1℃ / min and sinter it for 8 hours. Finally, cool it to room temperature at a cooling rate of 1℃ / min. After that, take it out and grind it. Then, sieve it through a 250-mesh sieve and take the sieve material to obtain the lithium manganese oxide matrix material. Step s6: Place the lithium manganese oxide matrix material and the silane-containing triphenylmethane structured polyimide (the silane-containing triphenylmethane structured polyimide is 2% of the mass of the lithium manganese oxide matrix material) into a ball mill and ball mill for 2 hours at a speed of 200 r / min. Then place it in a muffle furnace and keep it at a temperature of 320℃ for 3 hours. Cool it with the furnace and then sieve it through a 250 mesh sieve. Take the sieve material to obtain the high-entropy lithium manganese oxide cathode material.
[0022] Example 2: This embodiment describes a method for preparing a high-entropy lithium manganese oxide cathode material, including the following steps: Step s1: Add 0.3 mol of 2,6-dimethylaniline to a three-necked flask equipped with a stirrer, thermometer, gas delivery tube, and constant-pressure dropping funnel. Purge with nitrogen for protection and begin stirring at 97°C and a stirring rate of 350 r / min. Mix 0.15 mol of p-hydroxybenzaldehyde, 60 mL of ethylene glycol methyl ether, and 0.75 g of p-toluenesulfonic acid, then transfer the mixture to the constant-pressure dropping funnel and add it dropwise to the reaction system at a rate of 1 drop / s. After the addition is complete, raise the temperature to 107°C. Continue stirring for 8.5 h. After the reaction is complete, cool to room temperature and pour into 750 mL of anhydrous methanol under stirring. Adjust the pH to 9 by adding saturated sodium bicarbonate solution dropwise. Add 0.45 g of activated carbon and stir at room temperature for 31 min. Then, collect the solid by vacuum filtration, wash three times with deionized water, and recrystallize by heating under reflux with ethyl acetate. After filtration, place the filter cake in a vacuum drying oven and dry at 83 °C for 12.5 h to obtain a diamine monomer containing a hydroxyl triphenylmethane structure. Step s2: 6 mmol of hydroxytriphenylmethane-containing diamine monomer, 6 mmol of hexafluorodianhydride, and 30 mL of anhydrous N-methylpyrrolidone were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 65 min at a stirring rate of 350 r / min under ice bath conditions. Then, the mixture was stirred at room temperature for 6.5 h. Subsequently, 9 mL of acetic anhydride and 6 mL of triethylamine were added sequentially, and the mixture was stirred for another 2.1 h. The temperature was raised to 57 °C and maintained for 4.1 h. After cooling to room temperature, the mixture was poured into 300 mL of anhydrous ethanol under stirring. The solid was then collected by vacuum filtration and washed twice with isopropanol. The filter cake was then placed in a vacuum drying oven and dried at 97 °C for 10.5 h to obtain hydroxytriphenylmethane-containing polyimide. Step s3: 3 mmol of hydroxyl triphenylmethane-containing polyimide, 4.5 mmol of triisopropylchlorosilane, 4.5 mmol of imidazole, and 30 mL of N,N-dimethylformamide were added to a single-necked flask. Nitrogen gas was introduced for protection, and the mixture was stirred for 19 h at 27 °C and a stirring rate of 350 r / min. After the reaction was completed, a mixed solution was obtained. The mixed solution was added dropwise to 300 mL of anhydrous ethanol while stirring. The mixture was then filtered under reduced pressure, washed three times with anhydrous methanol, dissolved in 22 mL of dichloromethane, dried for 31 min with anhydrous magnesium sulfate, filtered, and the filtrate was added dropwise to isopropanol to precipitate. The precipitate was then placed in a vacuum drying oven and dried at 97 °C for 11.5 h to obtain silyltriphenylmethane-containing polyimide. Step s4: Weigh lithium carbonate, manganese tetroxide, aluminum oxide, cerium oxide, titanium dioxide, and antimony pentoxide according to the molar ratio of lithium, manganese, aluminum, cerium, titanium, and antimony of 1.05:1.96:0.01:0.01:0.01:0.01, and put them into a ball mill. Ball mill at 270 r / min for 3.1 h to obtain a mixture. Step s5: Place the mixture in a muffle furnace and pre-calcine it for 5 hours at a heating rate of 4℃ / min in an air atmosphere. Then, heat it to 800℃ at a heating rate of 4℃ / min and sinter it for 12 hours. Finally, cool it to room temperature at a cooling rate of 1℃ / min. After that, take it out and grind it. Then, sieve it through a 250-mesh sieve and take the sieve material to obtain the lithium manganese oxide matrix material. Step s6: Place the lithium manganese oxide matrix material and the silyltriphenylmethane-containing polyimide (the silyltriphenylmethane-containing polyimide is 3% of the mass of the lithium manganese oxide matrix material) into a ball mill and ball mill for 2.1 h at a speed of 250 r / min. Then place it in a muffle furnace and keep it at a temperature of 350℃ for 4 h. Cool it with the furnace and then sieve it through a 250 mesh sieve. Take the sieve material to obtain the high-entropy lithium manganese oxide cathode material.
[0023] Example 3: This embodiment describes a method for preparing a high-entropy lithium manganese oxide cathode material, including the following steps: Step s1: Add 0.4 mol of 2,6-dimethylaniline to a three-necked flask equipped with a stirrer, thermometer, gas delivery tube, and constant-pressure dropping funnel. Purge with nitrogen for protection and begin stirring at 100°C and a stirring rate of 400 r / min. Mix 0.2 mol of p-hydroxybenzaldehyde, 80 mL of ethylene glycol methyl ether, and 1.0 g of p-toluenesulfonic acid, then transfer the mixture to the constant-pressure dropping funnel and add it dropwise to the reaction system at a rate of 2 drops / s. After the addition is complete, raise the temperature to 110°C. The mixture was stirred at ℃ for 9 hours. After the reaction was completed, it was cooled to room temperature and poured into 1000 mL of anhydrous methanol under stirring. Saturated sodium bicarbonate solution was added dropwise to adjust the pH to 9. 0.6 g of activated carbon was added and the mixture was stirred at room temperature for 32 minutes. The solid was then collected by vacuum filtration and washed four times with deionized water. The solid was then recrystallized by heating with ethyl acetate under reflux. After filtration, the filter cake was placed in a vacuum drying oven and dried at 85℃ for 13 hours to obtain a diamine monomer containing a hydroxyl triphenylmethane structure. Step s2: 8 mmol of hydroxytriphenylmethane-containing diamine monomer, 8 mmol of hexafluorodianhydride, and 40 mL of anhydrous N-methylpyrrolidone were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 70 min at a stirring rate of 400 r / min under ice bath conditions. Then, the mixture was stirred at room temperature for 7 h. After that, 12 mL of acetic anhydride and 8 mL of triethylamine were added sequentially, and the mixture was stirred for another 2.2 h. The temperature was raised to 60 °C and maintained for 4.2 h. After that, the mixture was cooled to room temperature and poured into 400 mL of anhydrous ethanol under stirring. The solid was then collected by vacuum filtration and washed twice with isopropanol. The filter cake was then placed in a vacuum drying oven and dried at 100 °C for 11 h to obtain hydroxytriphenylmethane-containing polyimide. Step s3: 4 mmol of hydroxyl triphenylmethane-containing polyimide, 6 mmol of triisopropylchlorosilane, 6 mmol of imidazole, and 40 mL of N,N-dimethylformamide were added to a single-necked flask. Nitrogen gas was introduced for protection, and the mixture was stirred for 20 h at 30 °C and a stirring rate of 400 r / min. After the reaction was completed, a mixed solution was obtained. The mixed solution was added dropwise to 400 mL of anhydrous ethanol while stirring. The mixture was then filtered under reduced pressure, washed three times with anhydrous methanol, dissolved in 30 mL of dichloromethane, dried for 32 min with anhydrous magnesium sulfate, filtered, and the filtrate was added dropwise to isopropanol to precipitate. The precipitate was then placed in a vacuum drying oven and dried at 100 °C for 12 h to obtain silyltriphenylmethane-containing polyimide. Step s4: Weigh lithium carbonate, manganese tetroxide, aluminum oxide, cerium oxide, titanium dioxide, and antimony pentoxide according to the molar ratio of lithium, manganese, aluminum, cerium, titanium, and antimony of 1.14:1.8:0.05:0.05:0.05, and put them into a ball mill. Ball mill at 300 r / min for 3.2 h to obtain a mixture. Step s5: Place the mixture in a muffle furnace and pre-fire it for 6 hours at a heating rate of 8℃ / min in an air atmosphere. Then, heat it to 850℃ at a heating rate of 8℃ / min and sinter it for 15 hours. Finally, cool it to room temperature at a cooling rate of 2℃ / min. After that, take it out and grind it. Then, sieve it through a 250-mesh sieve and take the sieve material to obtain the lithium manganese oxide matrix material. Step s6: Place the lithium manganese oxide matrix material and the silyltriphenylmethane-containing polyimide (the silyltriphenylmethane-containing polyimide is 4% of the mass of the lithium manganese oxide matrix material) into a ball mill and ball mill for 2.2 hours at a speed of 300 r / min. Then place it in a muffle furnace and keep it at a temperature of 380℃ for 5 hours. Cool it with the furnace and then sieve it through a 250-mesh sieve. Take the sieve material to obtain the high-entropy lithium manganese oxide cathode material.
[0024] Comparative Example 1: This comparative example illustrates a method for preparing a high-entropy lithium manganese oxide cathode material, comprising the following steps: Step s1: Add 0.2 mol 2,6-Dimethylaniline was added to a three-necked flask equipped with a stirrer, thermometer, gas delivery tube, and constant-pressure dropping funnel. Nitrogen gas was introduced for protection, and stirring was started at 95°C and a stirring rate of 300 r / min. 0.1 mol of p-hydroxybenzaldehyde, 40 mL of ethylene glycol methyl ether, and 0.5 g of p-toluenesulfonic acid were mixed and then transferred to a constant-pressure dropping funnel and added dropwise to the reaction system at a dropping rate of 1 drop / s. After the addition was complete, the temperature was raised to 105°C and stirring was continued for 8 h. After the reaction was completed, the mixture was cooled to room temperature and poured into 500 mL of anhydrous methanol under stirring. Saturated sodium bicarbonate solution was added to adjust the pH to 9, and 0.3 g of activated carbon was added. The mixture was stirred at room temperature for 30 min, and then the solid was collected by vacuum filtration. The solid was washed three times with deionized water and then recrystallized by heating with ethyl acetate under reflux. After filtration, the filter cake was placed in a vacuum drying oven and dried at 80°C for 12 h to obtain a diamine monomer containing a hydroxytriphenylmethane structure. Step s2: 4 mmol of hydroxytriphenylmethane-containing diamine monomer, 4 mmol of hexafluorodianhydride, and 20 mL of anhydrous N-methylpyrrolidone were added to a three-necked flask equipped with a stirrer, thermometer, and gas delivery tube. Nitrogen gas was introduced for protection, and the mixture was stirred for 60 min at a stirring rate of 300 r / min under ice bath conditions. After stirring at room temperature for 6 h, 6 mL of acetic anhydride and 4 mL of triethylamine were added sequentially, and stirring was continued for 2 h. The temperature was raised to 55 °C and maintained for 4 h. After cooling to room temperature, the mixture was poured into 200 mL of anhydrous ethanol under stirring. The solid was then collected by vacuum filtration, washed twice with isopropanol, and the filter cake was placed in a vacuum drying oven and dried at 95 °C for 10 h to obtain hydroxytriphenylmethane-containing polyimide. Step s3: 2 mmol of hydroxyl triphenylmethane-containing polyimide, 3 mmol of triisopropylchlorosilane, 3 mmol of imidazole and 20 mL of N,N-dimethylformamide were added to a single-necked flask, and nitrogen gas was introduced for protection. The mixture was stirred for 18 h at 25 °C and a stirring rate of 300 r / min. After the reaction was completed, a mixed solution was obtained. The mixed solution was added dropwise to 200 mL of anhydrous ethanol while stirring. The mixture was then filtered under reduced pressure, washed three times with anhydrous methanol, dissolved in 15 mL of dichloromethane, dried for 30 min with anhydrous magnesium sulfate, filtered, and the filtrate was added dropwise to isopropanol to precipitate. The precipitate was then placed in a vacuum drying oven and dried at 95 °C for 11 h to obtain silyltriphenylmethane-containing polyimide. Step s4: Weigh lithium carbonate and manganese tetroxide according to the molar ratio of lithium to manganese of 1:2 and put them into a ball mill. Ball mill at 250 r / min for 3 hours to obtain a mixture. Step s5: Place the mixture in a muffle furnace and pre-fire it for 4 hours at a heating rate of 1℃ / min in an air atmosphere. Then, heat it to 750℃ at a heating rate of 1℃ / min and sinter it for 8 hours. Finally, cool it to room temperature at a cooling rate of 1℃ / min. After that, take it out and grind it. Then, sieve it through a 250-mesh sieve and take the sieve material to obtain the lithium manganese oxide matrix material. Step s6: Place the lithium manganese oxide matrix material and the silane-containing triphenylmethane structured polyimide (the silane-containing triphenylmethane structured polyimide is 2% of the mass of the lithium manganese oxide matrix material) into a ball mill and ball mill for 2 hours at a speed of 200 r / min. Then place it in a muffle furnace and keep it at a temperature of 320℃ for 3 hours. Cool it with the furnace and then sieve it through a 250 mesh sieve. Take the sieve material to obtain the high-entropy lithium manganese oxide cathode material.
[0025] Comparative Example 2: This comparative example illustrates a method for preparing a high-entropy lithium manganese oxide cathode material, comprising the following steps: Step s1: Weigh lithium carbonate, manganese tetroxide, aluminum oxide, cerium oxide, titanium dioxide, and antimony pentoxide according to the molar ratio of lithium, manganese, aluminum, cerium, titanium, and antimony of 1:1.98:0.005:0.005:0.005:0.005, and put them into a ball mill. Ball mill at 250 r / min for 3 hours to obtain a mixture. Step s2: Place the mixture in a muffle furnace and pre-calcine it to 450°C at a heating rate of 1°C / min for 4 hours in an air atmosphere. Then, heat it to 750°C at a heating rate of 1°C / min and sinter it for 8 hours. Finally, cool it to room temperature at a cooling rate of 1°C / min. After that, take it out and grind it. Then, sieve it through a 250-mesh sieve and take the sieve material to obtain the high-entropy lithium manganese oxide cathode material.
[0026] Comparative Example 3: This comparative example illustrates a method for preparing a high-entropy lithium manganese oxide cathode material, comprising the following steps: Step s1: Weigh lithium carbonate and manganese tetroxide according to the molar ratio of lithium to manganese of 1:2 and put them into a ball mill. Ball mill at 250 r / min for 3 hours to obtain a mixture. Step s2: Place the mixture in a muffle furnace and pre-calcine it to 450°C at a heating rate of 1°C / min for 4 hours in an air atmosphere. Then, heat it to 750°C at a heating rate of 1°C / min and sinter it for 8 hours. Finally, cool it to room temperature at a cooling rate of 1°C / min. After that, take it out and grind it. Then, sieve it through a 250-mesh sieve and take the sieve material to obtain the high-entropy lithium manganese oxide cathode material.
[0027] Performance testing: The high-entropy lithium manganese oxide cathode materials of Examples 1-3 and Comparative Examples 1-3 were tested according to the following methods; Cyclic stability test: Each sample was mixed with acetylene black and polyvinylidene fluoride at a mass ratio of 8:1:1, and N-methylpyrrolidone was added to form a uniform slurry. The slurry was coated on aluminum foil and dried under vacuum at 120℃ for 12 hours to form a positive electrode. Using lithium metal as the counter electrode, Celgard 2400 as the separator, and 1 mol / L LiPF6 / (EC / DMC / EMC) (volume ratio 1:1:1) as the electrolyte, CR2032 coin cells were assembled. At 25℃ and 0.5C rate (charge and discharge voltage range 3.0-4.3V), the cells were cycled 100 times. The initial discharge specific capacity and the discharge specific capacity after 100 cycles were recorded, and the capacity retention rate was calculated.
[0028] Rate performance test: Using the coin cells assembled above, charge and discharge at 25°C at rates of 0.2C, 0.5C, 1C, 2C, and 5C (voltage range 3.0-4.3V), respectively, for 5 cycles at each rate. Record the discharge specific capacity at each rate. Calculate the capacity retention rate at 5C rate based on the discharge specific capacity at 0.2C rate.
[0029] Manganese leaching test: The button cells made from each sample were cycled 50 times at 25℃ and 0.5C. The cells were then disassembled, the electrolyte was collected, and the concentration of Mn in the electrolyte was detected by inductively coupled plasma atomic emission spectrometry, which is the manganese leaching amount.
[0030] Thermal stability test: Differential scanning calorimeter was used to heat the sample from room temperature to 500℃ in a nitrogen atmosphere at a heating rate of 10℃ / min. The thermal decomposition onset temperature (T0) of the sample was recorded. The higher the T0, the better the thermal stability of the sample.
[0031] The test results are shown in Table 1: Table 1: Test Results Summary Table
[0032] Referring to Table 1, based on the comparison between Examples 1-3 and Comparative Examples 1-3, it can be seen that the high-entropy lithium manganese oxide cathode material has high cycle stability, excellent rate performance and good high-temperature safety, making it suitable for use in high-performance lithium-ion batteries.
[0033] Based on the comparison between Example 1 and Comparative Example 1, it can be seen that, under the premise of coating with silane-containing triphenylmethane-structured polyimide, multi-element doping can significantly improve the overall performance of high-entropy lithium manganese oxide cathode materials. Specifically, the capacity retention rate after 100 cycles and the 5C rate capacity retention rate of Example 1 are much higher than those of Comparative Example 1, the manganese dissolution is significantly lower than that of Comparative Example 1, and the thermal decomposition initiation temperature is higher than that of Comparative Example 1. This indicates that multi-element doping can improve the overall performance of high-entropy lithium manganese oxide cathode materials by forming strong bond energy MO bonds and reducing high-spin Mn bonds. 3+ The content of manganese is reduced to suppress Jahn-Teller distortion, reduce manganese leaching, optimize the crystal structure and ion conduction rate, thereby improving the cycling stability, rate performance and thermal stability of the material.
[0034] Based on the comparison between Example 1 and Comparative Example 2, it can be seen that under the premise of multi-element doping, the polyimide coating with silane-containing triphenylmethane structure can effectively improve the interfacial properties and comprehensive electrochemical performance of the material. The capacity retention rate after 100 cycles, the capacity retention rate at 5C rate, and the thermal decomposition initiation temperature of Example 1 are all higher than those of Comparative Example 2, while the manganese dissolution is lower than that of Comparative Example 2. This indicates that the coating layer can form a uniform interfacial protective film on the electrode surface, physically isolate the electrolyte from the active material, reduce the occurrence of side reactions, reduce interfacial impedance, further inhibit manganese dissolution, and improve the high-temperature resistance and cycle and rate stability of the material.
[0035] Based on the comparison between Example 1 and Comparative Example 3, it can be seen that the synergistic effect of multi-element doping and polyimide coating with silane-containing triphenylmethane structure can maximize the comprehensive performance of high-entropy lithium manganese oxide cathode material. Example 1 is significantly better than Comparative Example 3 in all test indicators, indicating that single missing doping or coating modification will lead to a decrease in material lattice stability, an increase in interface impedance, and an increase in manganese dissolution. The synergistic effect of the two can improve the electrochemical performance and thermal safety of the material from the aspects of lattice stability and interface protection.
[0036] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0037] The above description is merely an example and illustration of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the invention or exceed the scope defined in this application, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a high-entropy lithium manganese oxide cathode material, characterized in that, Includes the following steps: Step 1: Place the manganese source, lithium salt, and dopant ion M into a ball mill and ball mill to obtain a mixture. Step 2: Place the mixture in a muffle furnace for pre-firing, then sinter, cool, grind, and sieve to obtain lithium manganese oxide matrix material; Step 3: The lithium manganese oxide matrix material and the polyimide containing silane triphenylmethane structure are placed in a ball mill for ball milling, then heat-treated in a muffle furnace, cooled, and then sieved to obtain the high-entropy lithium manganese oxide cathode material. In step one, the dopant ion M is Al 3+ Ce 3+ Ti 4+ With Sb 5+ One or more of them.
2. The method for preparing a high-entropy lithium manganese oxide cathode material according to claim 1, characterized in that, The lithium source in step one is one or more of lithium acetate, lithium oxalate, lithium carbonate, lithium nitrate and lithium hydroxide; the manganese source is one or more of manganese acetate, manganese oxalate, manganese nitrate, manganese carbonate and manganese tetroxide.
3. The method for preparing a high-entropy lithium manganese oxide cathode material according to claim 1, characterized in that, Al in step one 3+ Derived from at least one of aluminum oxide, aluminum phosphate, aluminum metaphosphate, and aluminum hydroxide; Ce 3+ Derived from at least one of cerium trioxide, cerium carbonate, cerium nitrate, and cerium hydroxide; Ti 4+ Derived from at least one of titanium dioxide, titanium chloride, tetrabutyl titanate, and titanium hydroxide; Sb 5+ It is derived from at least one of antimony pentoxide, antimony pentanitrate, and antimony ammonium fluoride.
4. The method for preparing a high-entropy lithium manganese oxide cathode material according to claim 1, characterized in that, In step one, the molar ratio of lithium source, manganese source and doped ion M is (1-1.14):(2-x):x, where x=0.005-0.
05.
5. The method for preparing a high-entropy lithium manganese oxide cathode material according to claim 1, characterized in that, In step three, the silyltriphenylmethane-containing polyimide structure accounts for 2-4% of the mass of the lithium manganese oxide matrix material.
6. The method for preparing a high-entropy lithium manganese oxide cathode material according to claim 1, characterized in that, The polyimide containing a silyltriphenylmethane structure is prepared by the following steps: Step a1: Add 2,6-dimethylaniline to a three-necked flask and start stirring. Mix p-hydroxybenzaldehyde, ethylene glycol methyl ether and p-toluenesulfonic acid, then transfer to a constant pressure dropping funnel and add dropwise to the reaction system. Heat and continue stirring. Cool and pour into anhydrous methanol under stirring. Add saturated sodium bicarbonate solution to adjust the pH. Add activated carbon and stir. Then filter under reduced pressure, wash, recrystallize, filter and dry to obtain a diamine monomer containing a hydroxytriphenylmethane structure. Step a2: Add the hydroxytriphenylmethane-containing diamine monomer, hexafluorodianhydride and anhydrous N-methylpyrrolidone to a three-necked flask and stir. Then add acetic anhydride and triethylamine in sequence, continue stirring, cool, pour into anhydrous ethanol under stirring, filter under reduced pressure, wash, and dry to obtain hydroxytriphenylmethane-containing polyimide. Step a3: Add the polyimide containing hydroxyl triphenylmethane, triisopropylchlorosilane, imidazole and N,N-dimethylformamide to a single-necked flask and stir to obtain a mixed solution. While stirring, add the mixed solution dropwise to anhydrous ethanol, then filter under reduced pressure, wash, dissolve in dichloromethane, add anhydrous magnesium sulfate and dry, filter, add the filtrate dropwise to isopropanol to precipitate, and then dry to obtain the polyimide containing silyl triphenylmethane.
7. The method for preparing a high-entropy lithium manganese oxide cathode material according to claim 6, characterized in that, In step a1, the ratio of 2,6-dimethylaniline, p-hydroxybenzaldehyde, ethylene glycol methyl ether, p-toluenesulfonic acid, anhydrous methanol, and activated carbon is 0.2-0.4 mol: 0.1-0.2 mol: 40-80 mL: 0.5-1.0 g: 500-1000 mL: 0.3-0.6 g.
8. The method for preparing a high-entropy lithium manganese oxide cathode material according to claim 6, characterized in that, In step a2, the ratio of the hydroxyl triphenylmethane-containing diamine monomer, hexafluorodianhydride, anhydrous N-methylpyrrolidone, acetic anhydride, triethylamine, and anhydrous ethanol is 4-8 mmol: 4-8 mmol: 20-40 mL: 6-12 mL: 4-8 mL: 200-400 mL.
9. The method for preparing a high-entropy lithium manganese oxide cathode material according to claim 6, characterized in that, In step a3, the ratio of the amount of hydroxyl triphenylmethane-containing polyimide, triisopropylchlorosilane, imidazole, N,N-dimethylformamide, anhydrous ethanol, and dichloromethane is 2-4 mmol: 3-6 mmol: 3-6 mmol: 20-40 mL: 200-400 mL: 15-30 mL.