A wear-resistant and corrosion-resistant nickel-based alloy material and a preparation method thereof

By constructing a dense nickel-molybdenum protective layer and a nanoscale tantalum carbide reinforcing phase layer in nickel-based alloy materials, the interfacial bonding problem of nickel-based alloy materials in severe wear and corrosion environments was solved, and the high wear resistance and corrosion resistance were improved.

CN122629345APending Publication Date: 2026-08-25ZHUZHOU RUILI TOOLS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611017828.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-09
Publication Date
2026-08-25

AI Technical Summary

Technical Problem

Existing nickel-based alloy materials suffer from insufficient hardness and short wear life when facing severe mechanical wear. Furthermore, they exhibit poor wettability, easy spalling, and intergranular corrosion caused by the malignant diffusion of carbon elements at heterogeneous interfaces.

Method used

A core-shell structure heterogeneous reinforced microsphere with a dense nickel-molybdenum protective layer is used, combined with multi-element single-metal micropowders to carry out in-situ chemical reactions in micro-regions during spark plasma sintering, to construct a three-dimensional synergistic reinforcement and interface defense network with high bonding strength. The sintering efficiency is improved by sponge titanium powder, and tantalum powder captures free carbon atoms to form a nanoscale tantalum carbide reinforced phase layer.

Benefits of technology

This study achieved high density, excellent pitting resistance, and long-life self-lubricating properties in nickel-based alloy materials, significantly improving the wear resistance and corrosion resistance of the materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN122629345A_ABST
    Figure CN122629345A_ABST
Patent Text Reader

Abstract

The application belongs to the technical field of nickel alloy manufacturing, and particularly relates to a kind of wear-resistant and corrosion-resistant nickel-based alloy material and a preparation method thereof, the nickel-based alloy material is sintered from Ni-Cr-Mo pre-alloy powder, Co powder, Ta powder, rare earth oxide powder, titanium sponge powder and core-shell structure reinforcing phase, the reinforcing phase adopts the core-shell structure of Ni-Mo coated silicon carbide-graphite, which is used to eliminate heterogeneous interface pores and in-situ anchor effectively to prevent particle peeling, and effectively block the malignant outward diffusion of carbon atoms to protect the intergranular corrosion resistance of alloy matrix, the nickel-based alloy material is purified by in-situ deoxidization, carbide interface is anchored effectively, and the corrosion-resistant hardening of core-shell reinforcing phase, a high-bonding composite reinforcement network is built inside, the problem of intergranular corrosion caused by heterogeneous phase peeling and carbon diffusion is solved, and efficient combination of high metallurgical density, lubrication and corrosion resistance is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nickel alloy manufacturing technology, specifically relating to a wear-resistant and corrosion-resistant nickel-based alloy material and its preparation method. Background Technology

[0002] Nickel-based alloys are widely used in extremely harsh service environments such as chemical, petroleum, and aerospace industries due to their excellent high-temperature resistance, oxidation resistance, and corrosion resistance. However, a single nickel-based alloy matrix often suffers from insufficient hardness and short wear life when facing severe mechanical or abrasive wear. To overcome this limitation, current research often employs powder metallurgy to introduce high-hardness ceramic particles or solid lubricating phases into the nickel matrix for composite modification. Theoretically, the introduction of such heterogeneous particles can balance the strength and toughness of the matrix, the hardness support of ceramics, and the friction reduction properties of carbon-based materials, making it an important direction in the research of high-performance composite materials.

[0003] However, in actual preparation and production processes, these conventional composite materials often exhibit extremely poor wettability between the non-metallic reinforcing phase and the metallic matrix. Direct mechanical mixing and sintering easily generates micropores and gaps at the heterogeneous interface. These defects not only become breeding grounds for pitting and crevice corrosion but also cause hard particles to easily peel off under frictional shear forces, thus accelerating material wear through abrasive action. Simultaneously, lubricating phases such as graphite readily undergo uncontrolled malignant diffusion to the matrix grain boundaries during high-temperature sintering, reacting with elements such as chromium in the matrix to precipitate brittle carbides, leading to severe chromium depletion in the matrix and triggering severe intergranular corrosion. Current solutions typically focus on pre-treating the surface of non-metallic particles with a single metallization coating or suppressing element diffusion by optimizing sintering temperature and pressure parameters. However, effective solutions are still lacking in simultaneously achieving a fully metallurgically dense interface, blocking the cross-interface migration of harmful elements, and balancing wear resistance and corrosion resistance. Summary of the Invention

[0004] To address the above issues, this invention provides a wear-resistant and corrosion-resistant nickel-based alloy material and its preparation method. By constructing a core-shell structure heterogeneous reinforced microsphere with a dense nickel-molybdenum protective layer, and combining it with the in-situ chemical reaction of multi-element single-metal micropowders during spark plasma sintering, a three-dimensional synergistic reinforcement and interface defense network with high bonding strength is built in the nickel matrix. This aims to solve the common problems in traditional nickel-based composite materials, such as poor wettability between non-metallic phases and the metal matrix, easy peeling and cracking of heterogeneous interfaces, and intergranular corrosion caused by the malignant diffusion of carbon elements.

[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows: This invention provides a wear-resistant and corrosion-resistant nickel-based alloy material, which comprises the following raw materials in parts by weight: 80-90 parts of Ni-Cr-Mo (nickel-chromium-molybdenum) pre-alloy powder, 1-3 parts of Co (cobalt) powder, 0.5-2 parts of Ta (tantalum) powder, 0.5 parts of rare earth oxide powder, 0.5 parts of sponge titanium powder, and 5-10 parts of reinforcing phase.

[0006] Furthermore, the Ni-Cr-Mo pre-alloyed powder is atomized spherical particles with the following composition: Ni 82.7%, Cr 9.8%, Mo 4.3%, W (tungsten) 2.5%, Al (aluminum) 0.6% and impurities 0.1%.

[0007] Furthermore, the rare earth oxide powder is selected from Y2O3 (yttrium oxide) or CeO2 (cerium oxide).

[0008] Furthermore, the reinforcing phase comprises the following raw materials: silicon carbide, flake graphite, nickel acetate, ammonium molybdate, and polyvinyl alcohol, wherein the mass ratio of silicon carbide, flake graphite, nickel acetate, ammonium molybdate, and polyvinyl alcohol is 5.5:2:9.5:0.5:0.3.

[0009] Furthermore, the nickel acetate and ammonium molybdate are in tetrahydrate form.

[0010] Furthermore, the preparation method of the reinforcing phase is as follows: S1: After dissolving nickel acetate and ammonium molybdate together, polyvinyl alcohol is added to dissolve. Polyvinyl alcohol is used as a binder for the dispersion, bonding and stabilization of suspended particles in the subsequent dispersion liquid to obtain the initial solution. Silicon carbide and flake graphite are added to the initial solution, and the mixture is stirred for 1 h using a high shear mixer and ultrasonically dispersed for 30 min to obtain the precursor slurry. S2: Spray dry the precursor slurry to granulate it. Set the inlet air temperature to 190℃ and the outlet air temperature to 95℃. Control the internal material temperature to maintain 57-63℃ to obtain precursor microspheres. S3: The precursor microspheres were placed in a tubular atmosphere furnace, and a hydrogen-argon mixed gas was introduced. The temperature was increased in stages, reaching 550℃ at a rate of 3℃ / min and held for 2 h. Then, the temperature was increased to 800℃ at a rate of 5℃ / min and held for 1.5 h. The gaseous substances generated during the heating process were collected. Nickel acetate gradually decomposed under the action of hydrogen during the heating process, successively generating nickel oxide and metallic nickel. Ammonium molybdate was dehydrated and transformed into molybdenum trioxide, molybdenum dioxide, and metallic molybdenum. These formed a nickel-molybdenum protective layer on the surface of the microspheres in situ with metallic nickel. Polyvinyl alcohol acted as a binder at room temperature and low temperature, adhering nickel acetate and ammonium molybdate to the surface of silicon carbide and flake graphite. At high temperature, pyrolysis and carbonization occurred, and the gas generated during the degradation process acted as a pore-forming agent to form a porous carbon channel structure, preventing the microspheres from cracking and obtaining the reinforcing phase.

[0011] This invention also provides a method for preparing a wear-resistant and corrosion-resistant nickel-based alloy material, the specific steps of which are as follows: Step 1: Weigh Ni-Cr-Mo pre-alloyed powder, Co powder, Ta powder, rare earth oxide powder, sponge titanium powder and reinforcing phase and mix them in a three-dimensional mixer for 30 min to obtain mixed powder; Step 2: Place the mixed powder in a mold and pre-press it on a press. Transfer it to a spark plasma sintering furnace, sinter it under vacuum, apply an axial stacking pressure of 50 MPa, turn on the pulse current, control the heating rate to 35℃ / min to heat to 1050℃, and hold for 15 min. In the early stage of sintering, the sponge titanium powder, due to its high surface activity, reacts with the residual oxygen adsorbed on the surface of each powder and inside the microspheres to improve the sintering efficiency and the bonding ability of each component. Ta powder can capture the trace amount of free carbon atoms escaping across the interface in the reinforcing phase to form a protective layer of TaC (tantalum carbide) to obtain the sintered phase. Step 3: Cool the sintered phase. When the temperature drops to 200℃, release the axial pressure and break the vacuum. Open the furnace, remove the mold, and demold to obtain a wear-resistant and corrosion-resistant nickel-based alloy material.

[0012] The beneficial effects achieved by this invention are as follows: The wear-resistant and corrosion-resistant nickel-based alloy material provided by this invention features an in-situ generated nickel-molybdenum protective layer that perfectly encapsulates the silicon carbide and graphite core. This shell acts as a "metallurgical bridge," significantly reducing the non-wetting barrier between the ceramic / carbon phase and the nickel matrix, achieving solid-phase fusion at the heterogeneous interface. Simultaneously, its dense structure locks the graphite inside the microspheres to retain complete solid lubrication activity and prevents the malignant outward diffusion of carbon atoms into the matrix. Furthermore, during sintering, sponge titanium powder, with its extremely high oxygen affinity, captures and eliminates residual oxygen adsorbed at the powder interface in situ, significantly improving the sintering density of the entire alloy. Tantalum powder, enriched around the reinforcing phase microspheres, captures trace amounts of free carbon atoms escaping across the interface, forming a nanoscale tantalum carbide reinforcing phase layer in situ. This creates a high-hardness shell structure around the microspheres, firmly fixing the reinforcing phase within the matrix and preventing particle detachment during sintering and pressing. Cobalt powder effectively improves the work hardening rate of the alloy. Finally, a highly dense, wear-resistant and corrosion-resistant nickel-based alloy material with excellent pitting corrosion resistance and long-life self-lubricating properties was prepared. Attached Figure Description

[0013] Figure 1 The stress-strain curves of the nickel-based alloy materials prepared in Examples 1-4 and Comparative Examples 1-2 are shown. Figure 2 The microstructure characterization results are for the nickel-based alloy materials prepared in Example 2 and Comparative Example 1. Figure 3The results show the wear resistance of the nickel-based alloy materials prepared in Example 2 and Comparative Example 1. Detailed Implementation

[0014] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0015] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to this invention. The preferred embodiments and materials described herein are for illustrative purposes only and do not limit the scope of this application.

[0016] Unless otherwise specified, all methods used in the following embodiments are conventional. Unless otherwise specified, all materials used in the following embodiments are new materials purchased from the market, and all quantities are by weight. Specifically, the nickel acetate used is nickel acetate tetrahydrate; the ammonium molybdate used is ammonium molybdate tetrahydrate; the silicon carbide used is micron-sized silicon carbide, model BESC-T10, with a D50 of 10.3 μm and a silicon carbide content >99%; the average particle size of the flake graphite used is 64.2 μm, with a carbon content of 98.8%; and the titanium content in the sponge titanium powder used is ≥99.4%.

[0017] In the following examples and comparative examples, the reinforcing phase comprises the following raw materials: 55 parts silicon carbide, 20 parts flake graphite, 95 parts nickel acetate, 5 parts ammonium molybdate, and 3 parts polyvinyl alcohol. The preparation method of the reinforcing phase is as follows: S1: Dissolve 95 parts of nickel acetate and 5 parts of ammonium molybdate in 300 parts of deionized water, then add 3 parts of polyvinyl alcohol and heat to dissolve to obtain a preliminary solution. Add 55 parts of silicon carbide and 20 parts of flake graphite to the preliminary solution, stir with a high shear mixer for 1 h at 2000 rpm, and ultrasonically disperse at 400 W power for 30 min to obtain the precursor slurry. S2: Spray dry and granulate the precursor slurry, set the inlet air temperature to 190℃, the outlet air temperature to 95℃, the feed rate to 20 mL / min, the centrifugal physicochemical disc speed to 15000 rpm, and control the internal material temperature to maintain at about 60℃ to obtain precursor microspheres. S3: Place the precursor microspheres in a tubular atmosphere furnace, evacuate the furnace to remove air, and then introduce high-purity argon gas containing 15% high-purity hydrogen by volume at a flow rate of 200 mL / min. Heat to 550℃ at a heating rate of 3℃ / min and hold for 2 h, then heat to 800℃ at a rate of 5℃ / min and hold for 1.5 h. Collect the gaseous substances generated during the heating process. After sintering, cool to room temperature with the furnace to obtain the reinforcing phase.

[0018] Example 1: This example provides a wear-resistant and corrosion-resistant nickel-based alloy material, which includes the following raw materials by weight: 80 parts Ni-Cr-Mo pre-alloy powder, 3 parts Co powder, 2 parts Ta powder, 0.5 parts Y2O3, 0.5 parts sponge titanium powder, and 10 parts reinforcing phase.

[0019] This invention also provides a method for preparing a wear-resistant and corrosion-resistant nickel-based alloy material, the specific steps of which are as follows: Step 1: Weigh 80 parts of Ni-Cr-Mo pre-alloyed powder, 3 parts of Co powder, 2 parts of Ta powder, 0.5 parts of Y2O3, 0.5 parts of sponge titanium powder and 10 parts of reinforcing phase and mix them in a three-dimensional mixer for 30 min at a speed of 30 rpm. After mixing, pass the mixture through a 200-mesh sieve to obtain mixed powder. Step 2: Place the mixed powder in a high-strength graphite mold with graphite carbon paper lining the inner wall and upper and lower punches, and pre-press and shape it at 10 MPa for 2 min on a press to remove the pore gas between the powder particles. Transfer it to a spark plasma sintering furnace, sinter it under vacuum, apply an axial stacking pressure of 50 MPa, turn on the pulse current, control the heating rate to 35℃ / min to heat to 1050℃, hold for 15 min, and obtain the sintered phase. Step 3: Cool the sintered phase and maintain an axial pressure of 50 MPa. Turn on the equipment's circulating water cooling system to prevent thermal stress microcracks or elastic rebound cracks in the material. Reduce the temperature to 200℃, release the axial pressure and break the vacuum. Open the furnace, remove the mold, and mechanically demold it. Use mechanical grinding to remove the graphite carbon paper adhering to the surface to obtain a wear-resistant and corrosion-resistant nickel-based alloy material.

[0020] Example 2: This example provides a wear-resistant and corrosion-resistant nickel-based alloy material, which includes the following raw materials in parts by weight: 88 parts of Ni-Cr-Mo pre-alloy powder, 2 parts of Co powder, 1 part of Ta powder, 0.5 parts of Y2O3, 0.5 parts of sponge titanium powder, and 7 parts of reinforcing phase.

[0021] This invention also provides a method for preparing a wear-resistant and corrosion-resistant nickel-based alloy material, the specific steps of which are as follows: Step 1: Weigh 88 parts of Ni-Cr-Mo pre-alloyed powder, 2 parts of Co powder, 1 part of Ta powder, 0.5 parts of Y2O3, 0.5 parts of sponge titanium powder and 7 parts of reinforcing phase and mix them in a three-dimensional mixer for 30 min at a speed of 30 rpm. After mixing, pass the mixture through a 200-mesh sieve to obtain mixed powder. Step 2: Place the mixed powder in a high-strength graphite mold with graphite carbon paper lining the inner wall and upper and lower punches, and pre-press and shape it at 10 MPa for 2 min on a press to remove the pore gas between the powder particles. Transfer it to a spark plasma sintering furnace, sinter it under vacuum, apply an axial stacking pressure of 50 MPa, turn on the pulse current, control the heating rate to 35℃ / min to heat to 1050℃, hold for 15 min, and obtain the sintered phase. Step 3: Cool the sintered phase and maintain an axial pressure of 50 MPa. Turn on the equipment's circulating water cooling system to prevent thermal stress microcracks or elastic rebound cracks in the material. Reduce the temperature to 200℃, release the axial pressure and break the vacuum. Open the furnace, remove the mold, and mechanically demold it. Use mechanical grinding to remove the graphite carbon paper adhering to the surface to obtain a wear-resistant and corrosion-resistant nickel-based alloy material.

[0022] Example 3: This example provides a wear-resistant and corrosion-resistant nickel-based alloy material, which includes the following raw materials in parts by weight: 90 parts Ni-Cr-Mo pre-alloy powder, 1 part Co powder, 0.5 parts Ta powder, 0.5 parts CeO2, 0.5 parts sponge titanium powder, and 5 parts reinforcing phase.

[0023] This invention also provides a method for preparing a wear-resistant and corrosion-resistant nickel-based alloy material, the specific steps of which are as follows: Step 1: Weigh 90 parts of Ni-Cr-Mo pre-alloyed powder, 1 part of Co powder, 0.5 parts of Ta powder, 0.5 parts of CeO2, 0.5 parts of sponge titanium powder and 5 parts of reinforcing phase and mix them in a three-dimensional mixer for 30 min at a speed of 30 rpm. After mixing, pass the mixture through a 200-mesh sieve to obtain mixed powder. Step 2: Place the mixed powder in a high-strength graphite mold with graphite carbon paper lining the inner wall and upper and lower punches, and pre-press and shape it at 10 MPa for 2 min on a press to remove the pore gas between the powder particles. Transfer it to a spark plasma sintering furnace, sinter it under vacuum, apply an axial stacking pressure of 50 MPa, turn on the pulse current, control the heating rate to 35℃ / min to heat to 1050℃, hold for 15 min, and obtain the sintered phase. Step 3: Cool the sintered phase and maintain an axial pressure of 50 MPa. Turn on the equipment's circulating water cooling system to prevent thermal stress microcracks or elastic rebound cracks in the material. Reduce the temperature to 200℃, release the axial pressure and break the vacuum. Open the furnace, remove the mold, and mechanically demold it. Use mechanical grinding to remove the graphite carbon paper adhering to the surface to obtain a wear-resistant and corrosion-resistant nickel-based alloy material.

[0024] Example 4: This example provides a wear-resistant and corrosion-resistant nickel-based alloy material, which includes the following raw materials by weight: 82 parts Ni-Cr-Mo pre-alloy powder, 2 parts Co powder, 1.5 parts Ta powder, 0.5 parts CeO2, 0.5 parts sponge titanium powder, and 8 parts reinforcing phase.

[0025] This invention also provides a method for preparing a wear-resistant and corrosion-resistant nickel-based alloy material, the specific steps of which are as follows: Step 1: Weigh 82 parts of Ni-Cr-Mo pre-alloyed powder, 2 parts of Co powder, 1.5 parts of Ta powder, 0.5 parts of CeO2, 0.5 parts of sponge titanium powder and 8 parts of reinforcing phase and mix them in a three-dimensional mixer for 30 min at a speed of 30 rpm. After mixing, pass the mixture through a 200-mesh sieve to obtain mixed powder. Step 2: Place the mixed powder in a high-strength graphite mold with graphite carbon paper lining the inner wall and upper and lower punches, and pre-press and shape it at 10 MPa for 2 min on a press to remove the pore gas between the powder particles. Transfer it to a spark plasma sintering furnace, sinter it under vacuum, apply an axial stacking pressure of 50 MPa, turn on the pulse current, control the heating rate to 35℃ / min to heat to 1050℃, hold for 15 min, and obtain the sintered phase. Step 3: Cool the sintered phase and maintain an axial pressure of 50 MPa. Turn on the equipment's circulating water cooling system to prevent thermal stress microcracks or elastic rebound cracks in the material. Reduce the temperature to 200℃, release the axial pressure and break the vacuum. Open the furnace, remove the mold, and mechanically demold it. Use mechanical grinding to remove the graphite carbon paper adhering to the surface to obtain a wear-resistant and corrosion-resistant nickel-based alloy material.

[0026] Comparative Example 1: The difference from Example 2 is that a reinforcing phase is added; the rest is the same as Example 2. Comparative Example 2: Alloy materials were prepared using only Ni-Cr-Mo pre-alloyed powder according to the method described in Example 2.

[0027] Tensile property testing: Nickel-based alloy materials prepared in Examples 1-4 and Comparative Examples 1-2 were pressed into standard dumbbell-shaped specimens (57 mm long, 18 mm long at both ends, 10 mm wide at both ends, 15 mm long in the middle, and 3 mm radius of the corner). An MTS tensile testing machine (model DBSL-XS-20tN) was used with a strain rate of 1 mm / min and a preload of 0.01 kN to obtain stress-strain curves. The results are shown in [Figure number missing]. Figure 1 The tensile strength and elongation of the alloy material were calculated, and the results are shown in Table 1.

[0028] Microstructure characterization: The microstructure of the nickel-based alloy materials prepared in Example 2 and Comparative Example 1 was examined using scanning electron microscopy. The results are shown in the figure. Figure 2 .

[0029] Wear resistance test: Nickel-based alloy materials prepared in Example 2 and Comparative Example 1 were subjected to symmetrical loading using a friction and wear testing machine. All wear surfaces underwent standard metallographic pretreatment. A constant normal load of 10 N was applied using G5 precision steel balls with a diameter of 6.5 mm and a hardness of HRC60. The sliding distance was 3 mm, the frequency was 1 Hz, and the total test time was 30 min. The results are shown in [Figure number missing]. Figure 3 .

[0030] Corrosion resistance test: The corrosion resistance of the nickel-based alloy materials prepared in Examples 1-4 and Comparative Examples 1-2 was investigated according to the national standard GB / T 17897-2016 "Corrosion of Metals and Alloys - Test Method for Pitting Corrosion of Stainless Steel with Ferric Chloride". The initial weight of the sample was 25 g, denoted as W0. The corrosive solution was a 6% (w / v) ferric chloride solution. The test was conducted at a constant temperature of 50℃ for 72 h. After the test, the surface corrosion products were removed, and the samples were washed, dried, and weighed, denoted as W1. The weight loss rate was calculated as (W0 - W1) / (S × t), where S is 0.0012 m. 2 The time interval (t) was 72 h, and the results are shown in Table 2.

[0031] Table 1. Tensile strength and elongation of nickel-based alloy materials prepared in Examples 1-4 and Comparative Examples 1-2

[0032] Table 2. Corrosion resistance of nickel-based alloy materials prepared in Examples 1-4 and Comparative Examples 1-2

[0033] Figure 1As shown in Table 1, the nickel-based alloy materials of Examples 1-4 prepared using the raw materials and methods described in this application all exhibit good tensile strength and excellent elongation at break. Among them, the nickel-based alloy material prepared in Example 2 has a fracture strain exceeding 20% ​​and can maintain higher strength. In contrast, the comparative examples clearly have defects such as lower strength (Comparative Example 2) or poor plasticity due to embrittlement (Comparative Example 1).

[0034] Figure 2 The results showed that a distinct granular structure was observed in the nickel-based alloy material prepared in Example 2, while the structure in Comparative Example 1 was smoother. This indicates that the added reinforcing phase can achieve good dispersion in the alloy material and has a positive effect on improving the material uniformity and mechanical strength.

[0035] Figure 3 The results showed that the nickel-based alloy prepared in Example 2 had stronger wear resistance than that in Comparative Example 1. Under the same pressure and frequency, its wear depth was less than 60 μm, while that in Comparative Example 1 was nearly 130 μm, indicating that the added reinforcing phase could significantly improve the wear resistance of the alloy material.

[0036] Table 2 shows that the nickel-based alloy materials prepared in Examples 1-4 can maintain a good weight loss rate and strong corrosion resistance in ferric chloride corrosive solution, while the alloy materials prepared in Comparative Examples 1-2 have relatively weak corrosion resistance.

[0037] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

[0038] The present invention and its embodiments have been described above. This description is not restrictive, and the accompanying drawings are only one embodiment of the present invention. The actual application is not limited to this. In conclusion, if those skilled in the art are inspired by this description and design similar methods and embodiments without departing from the spirit of the present invention, they should all fall within the protection scope of the present invention.

Claims

1. A wear-resistant and corrosion-resistant nickel-based alloy material, characterized in that, The nickel-based alloy material comprises the following raw materials in parts by weight: 80-90 parts Ni-Cr-Mo pre-alloy powder, 1-3 parts Co powder, 0.5-2 parts Ta powder, 0.5 parts rare earth oxide powder, 0.5 parts sponge titanium powder, and 5-10 parts reinforcing phase; The reinforcing phase comprises the following raw materials: silicon carbide, flake graphite, nickel acetate, ammonium molybdate, and polyvinyl alcohol. The preparation method of the reinforcing phase is as follows: S1: After dissolving nickel acetate and ammonium molybdate together, add polyvinyl alcohol to dissolve and obtain a preliminary solution. Add silicon carbide and flake graphite to the preliminary solution, stir under high shear and sonicate to obtain a precursor slurry. S2: Spray dry the precursor slurry to obtain precursor microspheres; S3: The precursor microspheres are heated at high temperature to obtain the reinforcing phase.

2. The wear-resistant and corrosion-resistant nickel-based alloy material according to claim 1, characterized in that, The mass ratio of silicon carbide, flake graphite, nickel acetate, ammonium molybdate, and polyvinyl alcohol is 5.5:2:9.5:0.5:0.

3.

3. The wear-resistant and corrosion-resistant nickel-based alloy material according to claim 2, characterized in that, The rare earth oxide powder is selected from Y2O3 or CeO2.

4. The wear-resistant and corrosion-resistant nickel-based alloy material according to claim 2, characterized in that, The Ni-Cr-Mo pre-alloyed powder is atomized spherical particles with the following composition: Ni 82.7%, Cr 9.8%, Mo 4.3%, W 2.5%, Al 0.6% and impurities 0.1%.

5. The wear-resistant and corrosion-resistant nickel-based alloy material according to claim 2, characterized in that, In step S3, the high-temperature heating process is carried out in stages in a tubular atmosphere furnace, and a hydrogen-argon mixed gas is introduced.

6. A method for preparing a wear-resistant and corrosion-resistant nickel-based alloy material according to any one of claims 1-5, characterized in that, The specific steps are as follows: Step 1: Weigh out Ni-Cr-Mo pre-alloyed powder, Co powder, Ta powder, rare earth oxide powder, sponge titanium powder and reinforcing phase and mix them together to obtain a mixed powder; Step 2: The mixed powder is subjected to spark plasma sintering to obtain a sintered phase; Step 3: Cool and demold the sintered phase to obtain a wear-resistant and corrosion-resistant nickel-based alloy material.