AI Technical Summary
Existing magnetorheological fluids struggle to balance high yield strength and low sedimentation over a wide temperature range, while traditional chemical fusion agents lead to a decrease in magneto-induced shear stress and particle sedimentation problems.
By utilizing the incompatibility between PAO and silicone oil, a three-dimensional thixotropic network is constructed using organic bentonite to physically lock silicone oil microdroplets into the continuous PAO phase, forming a nearly theoretically rigid chain structure. This avoids surfactant adsorption and ensures the cleanliness of the carbonyl iron powder surface.
It achieves a magnetostrictive shear yield stress increase of over 50%, excellent rheological properties over a wide temperature range, plasticization at low temperatures while maintaining basic viscosity at high temperatures, good anti-settling properties, and a settling rate of less than 10%.
Smart Images

Figure FT_1 
Figure FT_2 
Figure SMS_1
Abstract
Description
Technical Field
[0001] This application relates to the field of magnetorheological materials and vibration reduction technology, specifically to a heterogeneous magnetorheological fluid, its preparation method, and its applications. Background Technology
[0002] As the automotive industry deepens its development towards intelligent and electric vehicles, higher demands are being placed on the real-time control of chassis dynamics. Magnetorheological fluid, a smart material capable of millisecond-level reversible liquid-solid phase transitions under a magnetic field, is the core medium for achieving semi-active damping force output in magnetorheological suspension systems. Compared to traditional hydraulic shock absorbers, magnetorheological fluid-based suspension systems offer advantages such as fast response, low energy consumption, and a wide range of stepless damping adjustment, and are gradually becoming more widespread from high-end to mid-range models. However, the service environment for automotive shock absorbers is extremely harsh. According to the industry standard QC / T 1152-2021 Magnetorheological Shock Absorbers for Automobiles, magnetorheological fluids must not only possess high yield stress to provide sufficient damping force, but also maintain stable fluidity and response speed across a vast temperature range, from the frigid winter (-40℃) to the high summer engine compartment temperature (120℃), and resist sedimentation and erosion under long-term high-frequency shearing.
[0003] The carrier fluid is crucial in determining the temperature characteristics and durability of magnetorheological fluids. Currently, mainstream solutions typically use single synthetic hydrocarbon oils (such as polyalphaolefin, PAO) or single silicone oils, but both face inherent contradictions: Literature indicates that while PAO-based carrier fluids possess excellent lubricity and can effectively reduce zero-field wear between metal particles, their viscosity is extremely sensitive to temperature. At -40℃, the viscosity can reach over 150 Pa·s, leading to overshoot in suspension damping forces, while at 120℃, the viscosity drops below 0.3 Pa·s, causing severe particle settling. Dimethyl silicone oil, with its excellent viscosity-temperature coefficient (viscosity-temperature coefficient can be as low as below 0.6), can maintain a relatively stable viscosity over a wide temperature range, but its spreading and wetting properties with metal surfaces are poor, and its extreme pressure lubrication capability is severely insufficient. When pure silicone oil-based magnetorheological fluids are used in shock absorbers, boundary friction and noise problems between the piston rod and the seals become prominent. Ideally, combining PAO with silicone oil can balance wide-temperature-range fluidity and extreme-pressure anti-wear properties. However, the two base liquids are thermodynamically incompatible, and their solubility parameters differ too much, causing rapid phase separation after conventional mixing.
[0004] To form a homogeneous base fluid between the incompatible PAO and silicone oil, traditional methods require the introduction of surfactants or special organosilicon emulsifiers. However, numerous studies have shown that while these amphiphilic molecules reduce oil-oil interfacial tension, they inevitably adsorb onto the high-energy surface of carbonyl iron powder in monolayer form through hydrophobic interactions or hydrogen bonding. This adsorbed film, approximately 2-5 nm thick, acts as an atomic-level interfacial slip layer under a magnetic field, transforming the rigid locking of the magnetic particle chains into flexible sliding, ultimately leading to a precipitous drop in shear yield strength. For example, while formulations with added emulsifiers achieve homogenization of the base fluid, their magnetostrictive shear stress decreases by more than 40% compared to pure PAO-based magnetorheological fluids without emulsifiers, sacrificing the core mechanical properties of the magnetorheological fluid. Furthermore, silane or titanate coupling agents are essentially ineffective because they cannot trigger hydrolytic anchoring in a purely organic environment, and may even catalyze the degradation of silicone oil segments. It is evident that in automotive suspension applications requiring high dynamic life and high shear strength, this fusion path based on "chemical homogenization" has fallen into a severe dilemma where a wide temperature range, low sedimentation, and high yield strength are mutually exclusive. Summary of the Invention
[0005] This invention provides a heterogeneous magnetorheological fluid, its preparation method, and its applications. This magnetorheological fluid can ensure the atomic-level cleanliness of the carbonyl iron powder surface, thereby forming a nearly theoretically rigid chain structure under a magnetic field. The magnetostrictive shear yield stress is significantly improved compared to traditional chemical fusion formulations.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows: The heterogeneous magnetorheological fluid is made from the following raw materials in parts by weight: The composition includes 70-85 parts magnetic particles, 10-20 parts continuous phase, 2-8 parts dispersed phase, 1-5 parts thixotropic framework, 0.5-2 parts activator, 0.1-1 part antioxidant, 0.2-1.5 parts zero-field friction reducer, 0.1-0.8 parts framework reinforcing agent, and 0.2-0.8 parts dispersing aid. The continuous phase and the dispersed phase are thermodynamically incompatible.
[0007] The magnetic particles are carbonyl iron powder with an average particle size of 1-10 μm and a spherical morphology.
[0008] The continuous phase is a poly-α-olefin; it must have a kinematic viscosity of 10-40 cSt and a viscosity index ≥120 at 40°C.
[0009] The dispersed phase is dimethyl silicone oil; it must meet the following requirements: kinematic viscosity at 25°C is 50-500 cSt, and viscosity temperature coefficient is ≤0.65.
[0010] The thixotropic framework is Benton 34, Benton 38, HF-140 or Maclean organobentonite; wherein the montmorillonite content is ≥95%.
[0011] The activator is ethanol at a volume percentage of 90-95%.
[0012] The antioxidant is a high molecular weight liquid phenolic antioxidant with a molecular weight ≥600 Da and an oil solubility ≥5% in polyα-olefins; the zero-field friction reducer is PTFE micro powder with an average particle size of 1-5 μm; the skeleton reinforcing agent is hydrophobic fumed silica with a specific surface area of 150-250 m² / g and a surface silanol content ≤30%; the dispersing aid is a polyester-amine type superdispersant.
[0013] The heterogeneous magnetorheological fluid is prepared by the following steps: S1. Take the continuous phase and slowly add the activator dropwise while stirring. After the addition is complete, continue stirring for 2-5 minutes, and then let it stand for 10-30 minutes to activate it, thus obtaining the activated thixotropic framework. S2. Add the continuous phase, antioxidant, zero-field friction reducer and framework enhancer to the activated thixotropic framework, stir and mix evenly, and then perform high-speed shear dispersion to obtain a pre-gel paste; wherein, the high-speed shear dispersion conditions are: rotation speed 3000-5000 rpm, time 20-60 minutes, temperature 40-70℃. S3. While stirring, slowly add the dispersed phase, and then perform high-speed shear dispersion to obtain a homogeneous milky white gel; wherein, the high-speed shear dispersion conditions are: rotation speed 3000-5000 rpm, time 8-20 minutes; S4. Add dispersant to homogeneous milky white gel, then add magnetic particles in 3-5 batches. Knead for 5-10 minutes after each batch is added. After all the particles are added, continue kneading for 20-40 minutes to obtain crude product. S5. Take the crude product and treat it with an ultrasonic cell disruptor at a power of 450-550W for 0.6-2 hours to obtain an ultrasonic dispersion. S6. Place the ultrasonic dispersion in a vacuum environment and allow it to stand for 0.5-2 hours to degas; stir 0-2 times during this period.
[0014] In step S1, the activator is added as follows: while stirring at 100-300 rpm, the activator is added dropwise at a rate of 0.5-1.0 g / min. After the addition is complete, stirring is continued at 100-300 rpm for 2-5 minutes. In step S2, the conditions for uniform mixing are: stirring at a speed of 500-1000 rpm for 2-5 minutes; In step S3, the specific operation of adding the dispersed phase is as follows: the dispersed phase is slowly injected at a rate of 0.3-1.0 g / min while stirring at 1000-1500 rpm.
[0015] 10. The heterogeneous magnetorheological fluid according to claim 9, characterized in that: In step S4, the kneading operation is as follows: the homogeneous milky white gel is transferred to a dual planetary mixer or a three-roll mill, a dispersing agent is added, and then magnetic particles are added in 3-5 batches. After each batch is added, the mixture is kneaded at 30-100 rpm for 5-10 minutes. After all the particles are added, the mixture is kneaded for another 20-40 minutes to obtain a crude product. During kneading, an anchor-type or frame-type stirring paddle is used, with a gap of 2-5 mm between the paddle blade and the container wall. Preferably, in steps S2 and S3, the high-speed shear dispersion uses a serrated dispersion disc with a disc diameter to container diameter ratio of 0.4-0.6. Preferably, in step S5, the vacuum degassing conditions are: static degassing at 20-30℃ and a vacuum of -0.08 to -0.1 MPa.
[0016] The present invention also discloses the use of the above-mentioned heterogeneous magnetorheological fluid in magnetorheological vibration dampers, magnetorheological intelligent suspension systems, and magnetorheological dampers.
[0017] The beneficial effects of this invention are as follows: (1) This invention abandons traditional chemical fusion agents and instead utilizes the incompatibility between PAO and silicone oil to physically lock silicone oil in the continuous PAO phase in the form of microdroplets through a three-dimensional thixotropic network constructed from organic bentonite. This design avoids the adsorption of surfactants on the surface of magnetic particles in principle, ensuring the atomic-level cleanliness of the carbonyl iron powder surface, thereby forming a nearly theoretically rigid chain structure under a magnetic field, and increasing the magnetostrictive shear yield stress by more than 50% compared with traditional chemical fusion formulations.
[0018] (2) This invention utilizes a physically locked structure to enable the silicone oil micro-regions to function as independent temperature-viscosity regulating units, providing wide-temperature-range rheological compensation for the PAO skeleton. At low temperatures, the silicone oil micro-regions remain liquid, providing a plasticizing effect for the frozen PAO skeleton; at high temperatures, the silicone oil micro-regions maintain their basic viscosity, inhibiting excessive thinning of PAO. Simultaneously, the continuous PAO phase ensures excellent lubrication with metal surfaces.
[0019] (3) This invention utilizes a high-viscosity PAO continuous phase to provide initial anti-settling capability, while the thixotropic network in the physically locked structure and the locked silicone oil microregions together form a stable cage-like structure, physically separating and suspending the high-density carbonyl iron powder (density approximately 7.8 g / cm³). Simultaneously, hydrophobic fumed silica acts as a skeleton reinforcing agent, further preventing network collapse during prolonged static placement. Experimental results show that the product's sedimentation rate is less than 10% after 7 days of static placement, and there are no unmanageable hard lumps at the bottom.
[0020] (4) The preparation method of magnetorheological fluid provided by the present invention is carried out under normal pressure and medium and low temperature conditions. It does not require complex chemical reaction equipment, has low requirements for equipment and operators, has good batch stability, is easy to scale up production, and has good application prospects. Attached Figure Description
[0021] Figure 1 This is a diagram of the homogeneous milky white gel after the dispersed phase is physically locked in step S3 of Experimental Example 1 in Example 5; Figure 2 This is a line graph comparing the sedimentation rates of the magnetorheological fluids prepared in Experimental Examples 1-3 and Comparative Examples 1-2 in Example 5 after standing at room temperature for 0-7 days. The horizontal axis represents the number of days of standing, and the vertical axis represents the sedimentation rate (%). Detailed Implementation
[0022] The present invention will now be described in detail through specific embodiments. Example 1
[0023] The heterogeneous magnetorheological fluid in this embodiment is made from the following raw materials: 70g magnetic particles, 10g continuous phase, 2g dispersed phase, 1g thixotropic framework, 0.5g activator, 0.1g antioxidant, 0.2g zero-field friction reducer, 0.1g framework reinforcing agent, and 0.2g dispersing aid; The magnetic particles are carbonyl iron powder with an average particle size of 1 μm and a spherical morphology.
[0024] The continuous phase is PAO6.
[0025] The dispersed phase is dimethyl silicone oil; it must meet the following requirements: kinematic viscosity at 25°C is 50-55 cSt, and viscosity temperature coefficient is ≤0.65.
[0026] The thixotropic framework is Bentone 34, wherein the montmorillonite content is ≥95%.
[0027] The activator is 90% ethanol by volume.
[0028] The antioxidant is Irganox L57; the zero-field friction reducer is PTFE micro powder with an average particle size of 1μm; the skeleton reinforcing agent is hydrophobic fumed silica with a specific surface area of 150-180m² / g and a surface silanol content of ≤30%; and the dispersing agent is Solsperse 24000SC.
[0029] The heterogeneous magnetorheological fluid is prepared by the following steps: S1. Take the continuous phase and add the activator dropwise at a rate of 0.5 g / min while stirring at 100 rpm. After the addition is complete, continue stirring at 100 rpm for 2 minutes. Then let it stand for 10 minutes to activate and obtain the activated thixotropic framework. S2. Add the continuous phase, antioxidant, zero-field friction reducer and framework enhancer to the activated thixotropic framework, stir at 500 rpm for 2 minutes, and then perform high-speed shear dispersion using a serrated dispersion disk with a disk diameter to container diameter ratio of 0.4 to obtain a pre-gel paste; wherein, the high-speed shear dispersion conditions are: rotation speed 3000 rpm, time 20 minutes, temperature 40℃. S3. Under stirring at 1000 rpm, the dispersed phase was slowly injected at a rate of 0.3 g / min, and then high-speed shear dispersion was performed using a serrated dispersion disk with a disk diameter to container diameter ratio of 0.4 to obtain a homogeneous milky white gel. The high-speed shear dispersion conditions were: 3000 rpm for 8 minutes. S4. Transfer the homogeneous milky white gel to a dual planetary mixer or a three-roll mill, add the dispersing agent, and then add the magnetic particles in three batches. After each batch is added, knead at 30 rpm for 5 minutes. After all the particles are added, continue kneading for 20 minutes to obtain the crude product. When kneading, use an anchor or frame stirring paddle with a 2 mm gap between the paddle and the container wall. S5. Take the crude product and use an ultrasonic cell disruptor to perform ultrasonic treatment at a power of 450W for 0.6 hours to obtain an ultrasonic dispersion. S6. Place the ultrasonic dispersion in a vacuum environment and allow it to stand for 0.5 hours at 20℃ and -0.08MPa for degassing. Example 2
[0030] The heterogeneous magnetorheological fluid in this embodiment is made from the following raw materials: 85g magnetic particles, 20g continuous phase, 8g dispersed phase, 5g thixotropic framework, 2g activator, 1g antioxidant, 1.5g zero-field friction reducer, 0.8g framework reinforcing agent, and 0.8g dispersing aid; The magnetic particles are carbonyl iron powder with an average particle size of 10 μm and a spherical morphology.
[0031] The continuous phase is PAO8.
[0032] The dispersed phase is dimethyl silicone oil; it must meet the following requirements: kinematic viscosity at 25°C is 450-500 cSt, and viscosity temperature coefficient is ≤0.65.
[0033] The thixotropic framework is Bentone 38, wherein the montmorillonite content is ≥95%.
[0034] The activator is 95% ethanol by volume.
[0035] The antioxidant is Naugard 524; the zero-field friction reducer is PTFE micro powder with an average particle size of 5μm; the skeleton reinforcing agent is hydrophobic fumed silica with a specific surface area of 220-250m² / g and a surface silanol content ≤30%; and the dispersing agent is BYK-2200.
[0036] The heterogeneous magnetorheological fluid is prepared by the following steps: S1. Take the continuous phase and add the activator dropwise at a rate of 1.0 g / min while stirring at 300 rpm. After the addition is complete, continue stirring at 300 rpm for 5 minutes. Then let it stand for 30 minutes to activate and obtain the activated thixotropic framework. S2. Add the continuous phase, antioxidant, zero-field friction reducer and framework enhancer to the activated thixotropic framework, stir at 1000 rpm for 5 minutes, and then perform high-speed shear dispersion using a serrated dispersion disk with a disk diameter to container diameter ratio of 0.6 to obtain a pre-gel paste; wherein, the high-speed shear dispersion conditions are: 5000 rpm, 60 minutes, and 70℃. S3. Under stirring at 1500 rpm, the dispersed phase was slowly injected at a rate of 1.0 g / min, and then high-speed shear dispersion was performed using a serrated dispersion disk with a disk diameter to container diameter ratio of 0.6 to obtain a homogeneous milky white gel. The high-speed shear dispersion conditions were: 5000 rpm for 20 minutes. S4. Transfer the homogeneous milky white gel to a dual planetary mixer or a three-roll mill, add the dispersing agent, and then add the magnetic particles in 5 batches. After each batch is added, knead at 100 rpm for 10 minutes. After all the particles are added, continue kneading for 40 minutes to obtain the crude product. When kneading, use an anchor or frame stirring paddle with a 5 mm gap between the paddle and the container wall. S5. Take the crude product and use an ultrasonic cell disruptor to perform ultrasonic treatment at a power of 550W for 2 hours to obtain an ultrasonic dispersion. S6. Place the ultrasonic dispersion in a vacuum environment and allow it to stand for 2 hours at 30℃ and -0.1MPa vacuum to degas; stir twice during this period. Example 3
[0037] The heterogeneous magnetorheological fluid in this embodiment is made from the following raw materials: 75g magnetic particles, 15g continuous phase, 5g dispersed phase, 3g thixotropic framework, 1g activator, 0.6g antioxidant, 1g zero-field friction reducer, 0.6g framework reinforcing agent, and 0.5g dispersing aid; The magnetic particles are carbonyl iron powder with an average particle size of 6 μm and a spherical morphology.
[0038] The continuous phase is PAO10.
[0039] The dispersed phase is dimethyl silicone oil; it must meet the following requirements: kinematic viscosity at 25°C is 350-400 cSt, and viscosity temperature coefficient is ≤0.65.
[0040] The thixotropic framework is HF-140; wherein, the montmorillonite content is ≥95%.
[0041] The activator is 92% ethanol by volume.
[0042] The antioxidant is Irganox L135; the zero-field friction reducer is PTFE micro powder with an average particle size of 3μm; the skeleton reinforcing agent is hydrophobic fumed silica with a specific surface area of 180-210m² / g and a surface silanol content ≤30%; and the dispersing agent is Solsperse 21000.
[0043] The heterogeneous magnetorheological fluid is prepared by the following steps: S1. Take the continuous phase and add the activator dropwise at a rate of 0.7 g / min while stirring at 200 rpm. After the addition is complete, continue stirring at 200 rpm for 3 minutes. Then let it stand for 20 minutes to activate and obtain the activated thixotropic framework. S2. Add the continuous phase, antioxidant, zero-field friction reducer and framework enhancer to the activated thixotropic framework, stir at 700 rpm for 4 minutes, and then perform high-speed shear dispersion using a serrated dispersion disk with a disk diameter to container diameter ratio of 0.5 to obtain a pre-gel paste; wherein, the high-speed shear dispersion conditions are: rotation speed 4000 rpm, time 40 minutes, temperature 60℃. S3. Under stirring at 1200 rpm, the dispersed phase was slowly injected at a rate of 0.6 g / min, and then high-speed shear dispersion was performed using a serrated dispersion disk with a disk diameter to container diameter ratio of 0.5 to obtain a homogeneous milky white gel. The high-speed shear dispersion conditions were: 4000 rpm and 12 minutes. S4. Transfer the homogeneous milky white gel to a dual planetary mixer or a three-roll mill, add the dispersing agent, and then add the magnetic particles in 4 batches. After each batch is added, knead at 60 rpm for 8 minutes. After all the particles are added, continue kneading for 30 minutes to obtain the crude product. When kneading, use an anchor or frame stirring paddle with a 3 mm gap between the paddle and the container wall. S5. Take the crude product and use an ultrasonic cell disruptor to perform ultrasonic treatment at a power of 500W for 1 hour to obtain an ultrasonic dispersion. S6. Place the ultrasonic dispersion in a vacuum environment and allow it to stand for 1 hour at 25℃ and -0.09MPa vacuum to degas; stir once in between. Example 4 For example, a heterogeneous magnetorheological fluid is made from the following raw materials:
[0044] 80g magnetic particles, 13g continuous phase, 4g dispersed phase, 2g thixotropic framework, 1.7g activator, 0.8g antioxidant, 0.6g zero-field friction reducer, 0.7g framework reinforcing agent, and 0.3g dispersing aid; The magnetic particles are carbonyl iron powder with an average particle size of 7 μm and a spherical morphology.
[0045] The continuous phase is PAO6.
[0046] The dispersed phase is dimethyl silicone oil; it must meet the following requirements: kinematic viscosity at 25°C is 380-410 cSt, and viscosity temperature coefficient is ≤0.65.
[0047] The thixotropic framework is Maclean organobentonite; wherein the montmorillonite content is ≥95%.
[0048] The activator is 93% ethanol by volume.
[0049] The antioxidant is Irganox L57; the zero-field friction reducer is PTFE micro powder with an average particle size of 4μm; the skeleton reinforcing agent is hydrophobic fumed silica with a specific surface area of 170-200m² / g and a surface silanol content of ≤30%; and the dispersing agent is Solsperse 24000SC.
[0050] The heterogeneous magnetorheological fluid is prepared by the following steps: S1. Take the continuous phase and add the activator dropwise at a rate of 0.8 g / min while stirring at 180 rpm. After the addition is complete, continue stirring at 220 rpm for 4 minutes. Then let it stand for 15 minutes to activate and obtain the activated thixotropic framework. S2. Add the continuous phase, antioxidant, zero-field friction reducer and framework enhancer to the activated thixotropic framework, stir at 700 rpm for 3 minutes, and then perform high-speed shear dispersion using a serrated dispersion disk with a disk diameter to container diameter ratio of 0.4 to obtain a pre-gel paste; wherein, the high-speed shear dispersion conditions are: rotation speed 4500 rpm, time 50 minutes, temperature 50℃. S3. Under stirring at 1100 rpm, the dispersed phase was slowly injected at a rate of 0.4 g / min, and then high-speed shear dispersion was performed using a serrated dispersion disk with a disk diameter to container diameter ratio of 0.4 to obtain a homogeneous milky white gel. The high-speed shear dispersion conditions were: 3600 rpm for 12 minutes. S4. Transfer the homogeneous milky white gel to a dual planetary mixer or a three-roll mill, add the dispersing agent, and then add the magnetic particles in three batches. After each batch is added, knead at 80 rpm for 6 minutes. After all the particles are added, continue kneading for 35 minutes to obtain the crude product. When kneading, use an anchor or frame stirring paddle with a 3 mm gap between the paddle and the container wall. S5. Take the crude product and use an ultrasonic cell disruptor to perform ultrasonic treatment at a power of 480W for 1.3 hours to obtain an ultrasonic dispersion. S6. Place the ultrasonic dispersion in a vacuum environment and allow it to stand for 1.3 hours at 26℃ and -0.09MPa for degassing; stir once in between.
[0051] Example 5 Performance Test Experiment The raw materials used in the following experimental examples are all commercially available industrial products. Their specific sources and specifications are as follows: Carbonyl iron powder: Ju Nai Scientific Research New Materials Enterprise, average particle size D=5.0μm.
[0052] Continuous phase: polyalphaolefin PAO10, Tiancheng Meijia, kinematic viscosity at 40℃ 10 cSt, viscosity index 137.
[0053] Dispersed phase: Dimethyl silicone oil, Dow Corning, kinematic viscosity 100 cSt at 25°C.
[0054] Thixotropic framework: organobentonite, Maclean's reagent.
[0055] Activator: 95% ethanol, Sinopharm Group, analytical grade.
[0056] Antioxidant: Irganox L135.
[0057] Zero-field friction reducer: PTFE micro powder, average particle size 3μm.
[0058] Framework reinforcement: hydrophobic fumed silica, Maclean's reagent.
[0059] Dispersing auxiliary: Lubrizol, grade Solsperse 21000.
[0060] Experimental Example 1 (Basic Formula) Carbonyl iron powder 70.0g; PAO10 20g; dimethyl silicone oil 3.5g; organic bentonite 2.5g; 95% ethanol 1.0g; Irganox L135 0.5g; PTFE micropowder 0.9g; hydrophobic fumed silica 0.8g; Solsperse 21000 0.8g.
[0061] Preparation method: S1. Pre-activation of thixotropic skeleton: Add 2.5g of organic bentonite into a clean stainless steel beaker, and place it under a high-speed disperser. Turn on stirring to 200rpm, and drop 1.0g of 95% ethanol dropwise at a rate of 0.8g / min using a micro-syringe. After the dropping is completed, continue stirring for 2 minutes to make the material turn into uniformly moist small agglomerates. Then turn off the stirring, and let it stand for activation for 15 minutes.
[0062] S2. Pre-gel preparation: Add 20g of PAO10, 0.5g of Irganox L135, 0.9g of PTFE micropowder and 0.8g of hydrophobic fumed silica sequentially into the activated bentonite. First stir at 800rpm for 3 minutes to make all materials initially wetted. Then gradually increase the speed to 4000rpm, and carry out continuous high-speed shear dispersion at 4500rpm for 35 minutes. During the dispersion process, use an infrared temperature measuring gun to monitor the temperature, and maintain the material temperature at 50-60°C through water bath circulation. When it is observed that the material gradually changes from a turbid thin slurry to a translucent, high-gloss viscous paste, stop shearing. Lift the paste to a height of 3cm with a glass rod, continuous fine filaments can be pulled out without breaking within 15 seconds, and the cross-section scraped off by a spatula is smooth without particles, which determines that the pre-gel is qualified.
[0063] S3. Physical locking of dispersed phase: Reduce the rotating speed of the disperser to 1200rpm. Draw 3.5g of dimethyl silicone oil with a 50mL glass syringe, and install a flat-head needle. Insert the tip of the needle about 1cm below the liquid surface at the center of the pre-gel vortex, and push the silicone oil extremely slowly at a rate of 0.5g / min. During the injection process, it can be observed that the silicone oil enters the paste in the form of fine filaments and is instantly "swallowed". After all the silicone oil is added (about 7 minutes), immediately increase the rotating speed to 4000rpm again, and carry out high-speed shear dispersion for 12 minutes. After the dispersion is completed, the paste changes from translucent to uniform milky white, and when a smear is lifted with a spatula, the surface is as smooth as frost. A small amount of the paste is applied to a glass slide and observed under a 100x microscope, no independent transparent oil droplets larger than 3μm are seen, which determines that the physical locking is successful.
[0064] S4. Incorporation of Magnetic Particles: Transfer the entire milky white gel to the hopper of a dual planetary mixer. Add 0.8g of Solsperse 21000. Add the carbonyl iron powder in three batches (approximately 26g per batch). After each batch, knead at 60 rpm for 8 minutes using an anchor paddle. After all the iron powder has been added, continue kneading at 60 rpm for 30 minutes. During this time, use a scraper to help clean the hopper walls to ensure all materials are thoroughly mixed. The final material should be a uniform, dark gray paste without any white or gray patches.
[0065] S5. Ultrasonic cell disruption: Ultrasonic cell disruptor is used to perform ultrasonic treatment at 500W power for 1 hour to prevent the magnetic particles from agglomerating.
[0066] S6. Vacuum Degassing: Place the mixed dark gray paste, along with the container, into a vacuum oven. Set the temperature to 25℃ and the vacuum level to -0.095MPa. After standing for 1 hour to degas, remove the paste and observe that no bubbles have emerged on the surface. Use a scraper to cut open the paste; no obvious pinhole-like bubbles should be visible inside. Seal and package to obtain the finished product.
[0067] Experimental Example 2 (Formula with High Iron Powder Content) The difference between this embodiment and Example 1 lies in the different mass fractions of each component in the formulation, in order to test the performance at a higher magnetic particle content. Specifically, the formulation consists of: 85.0 g carbonyl iron powder, 8.8 g PAO10, 2.0 g dimethyl silicone oil, 1.5 g organobentonite, 0.6 g 95% ethanol, 0.3 g Irganox L135, 0.5 g PTFE micro powder, 0.2 g hydrophobic fumed silica, and 0.3 g Solsperse 21000. The total mass is approximately 99.2 g. The preparation method is the same as in Example 1.
[0068] Experimental Example 3 (High Thixotropic Framework Formulation) The difference between this embodiment and Example 1 is that the thixotropic framework content in the formulation is higher, in order to test the limiting effect on sedimentation stability. Specifically, the formulation consists of: 70.0 g carbonyl iron powder, 16.3 g PAO10, 5.0 g dimethyl silicone oil, 4.0 g organobentonite, 1.6 g 95% ethanol, 0.5 g Irganox L135, 1.0 g PTFE micro powder, 0.5 g hydrophobic fumed silica, and 0.5 g Solsperse 21000. The total mass is approximately 99.4 g. The preparation method is the same as in Example 1.
[0069] Comparative Example 1 (Traditional Chemical Fusion Method) A control sample was prepared according to the conventional chemical fusion method described in the background art. Components: 70g carbonyl iron powder, 20g PAO10, 3.5g dimethyl silicone oil, 0.8g alkyl / polyether co-modified silicone oil (chemical fusion agent, brand BYK-330), 0.3g Span 80, 0.5g hydrophobic fumed silica, and 0.3g diatomaceous earth. The preparation method involved first surface-modifying the magnetic particles with Span 80, followed by drying. The remaining steps were the same as in Example 1.
[0070] Comparative Example 2 (No thixotropic framework, physical blending) The difference between this comparative example and Example 1 is that no organobentonite or its activator, nor a framework reinforcing agent, was added, aiming to verify the necessity of the thixotropic network. The remaining components are the same as in Example 1: 70g carbonyl iron powder, 20g PAO10, 3.5g dimethyl silicone oil, 0.5g Irganox L135, 0.9g PTFE micron powder, and 0.8g Solsperse 21000. Preparation method: All liquid components (PAO10, dimethyl silicone oil, Irganox L135, Solsperse 21000) were mixed and sheared at 3000 rpm for 10 minutes using a high-speed disperser. Then, carbonyl iron powder and PTFE micron powder were added in three batches, stirring at 800 rpm for 10 minutes after each batch. Finally, the mixture was degassed under vacuum at -0.095 MPa for 1 hour.
[0071] Performance testing The magnetorheological fluids prepared in Examples 1-3 and Comparative Examples 1-2 were subjected to the following performance tests, and the experimental results are shown in Table 1 below: (1) Magnetostrictive shear yield stress: Under room temperature (25℃) and constant magnetic field strength of 0.8T, the shear stress is taken as the shear stress corresponding to a shear rate of 100 s⁻¹, and the yield stress is adopted.
[0072] (2) Wide temperature range zero-field viscosity: A parallel plate clamp (diameter 25mm, gap 0.5mm) was used. Steady-state shear test was performed at room temperature with a shear rate of 1 s⁻¹, and the zero-field viscosity was recorded.
[0073] (3) Sedimentation stability: Each sample was injected into a 100mL stoppered graduated cylinder (3 parallel samples per sample), sealed, and left to stand at room temperature (25±2℃) for 7 days. The volume of the supernatant (sedimentation) was recorded, and the sedimentation rate (volume of supernatant / total volume × 100%) was calculated.
[0074] Table 1. Performance test results of each embodiment and comparative example:
[0075] Results analysis: The following conclusions can be drawn from the test results in Table 1: 1. Magnetostrictive Shear Yield Stress: The magnetostrictive yield stresses of Examples 1-3 all exceeded 50 kPa, significantly higher than Comparative Example 1 (32.1 kPa) and Comparative Example 2 (35.6 kPa), representing an increase of over 45%. This directly demonstrates that the "heterogeneous physical locking" structure avoids surfactant contamination, keeping the iron powder surface highly clean, thereby forming a stronger magnetic linkage. Example 2, with the highest iron powder content (85%), achieved the highest yield stress of 65.1 kPa.
[0076] 2. Rheological properties: The viscosity of Examples 1-3 at 25°C is excellent, all controlled below 3 Pa·s. This ensures good fluidity of the magnetorheological fluid under zero field, avoiding the problem of excessive resistance to device startup caused by excessive viscosity, and also preventing particle sedimentation caused by excessively low zero field viscosity. Compared with the two comparative examples, the embodiments of the present invention can maintain a lower zero field viscosity while significantly improving the yield stress, resulting in better overall rheological properties.
[0077] 3. Settling Stability: Examples 1-3 demonstrated exceptional performance, with 30-day settling rates all below 10% and no hardening. Example 3, in particular, achieved a settling rate as low as 5.2% due to its higher thixotropic framework content. In contrast, Comparative Example 1 showed a settling rate of 15.5% with slight hardening, while Comparative Example 2 exhibited a settling rate as high as 28.0% with severe hardening. This fully demonstrates the decisive advantage of the "physical network locking" mechanism in this invention in preventing particle settling and network collapse.
[0078] In summary, the heterogeneous physically locked magnetorheological fluid and its preparation method provided by this invention have successfully solved a long-standing technical problem in the field through a revolutionary structural design, achieving a synergistic unity of high magnetostrictive yield stress, wide temperature range stability and excellent anti-settling properties, with performance superior to existing technologies.
[0079] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the protection scope of the present invention.
Claims
1. A heterogeneous magnetorheological fluid, characterized in that, Made from the following parts by weight of raw materials: The composition includes 70-85 parts magnetic particles, 10-20 parts continuous phase, 2-8 parts dispersed phase, 1-5 parts thixotropic framework, 0.5-2 parts activator, 0.1-1 part antioxidant, 0.2-1.5 parts zero-field friction reducer, 0.1-0.8 parts framework reinforcing agent, and 0.2-0.8 parts dispersing aid. The continuous phase and the dispersed phase are thermodynamically incompatible.
2. The heterogeneous magnetorheological fluid according to claim 1, characterized in that: The magnetic particles are carbonyl iron powder with an average particle size of 1-10 μm and a spherical morphology.
3. The heterogeneous magnetorheological fluid according to claim 1, characterized in that: The continuous phase is a poly-α-olefin; it must have a kinematic viscosity of 10-40 cSt and a viscosity index ≥120 at 40°C.
4. The heterogeneous magnetorheological fluid according to claim 1, characterized in that: The dispersed phase is dimethyl silicone oil; it must meet the following requirements: kinematic viscosity at 25°C is 50-500 cSt, and viscosity temperature coefficient is ≤0.
65.
5. The heterogeneous magnetorheological fluid as described in claim 1, characterized in that: The thixotropic framework is Benton 34, Benton 38, HF-140 or Maclean organobentonite; wherein the montmorillonite content is ≥95%.
6. The heterogeneous magnetorheological fluid as described in claim 1, characterized in that: The activator is ethanol with a volume percentage of 90-95%; the antioxidant is a high molecular weight liquid phenolic antioxidant with a molecular weight ≥600 Da and an oil solubility ≥5% in polyα-olefins; the zero-field friction reducer is PTFE micro powder with an average particle size of 1-5 μm; the skeleton reinforcing agent is hydrophobic fumed silica with a specific surface area of 150-250 m² / g and a surface silanol content ≤30%; and the dispersing aid is a polyester-amine type superdispersant.
7. The heterogeneous magnetorheological fluid as described in claim 1, characterized in that, Its preparation method includes the following steps: S1. Take the continuous phase and slowly add the activator dropwise while stirring. After the addition is complete, continue stirring for 2-5 minutes, and then let it stand for 10-30 minutes to activate it, thus obtaining the activated thixotropic framework. S2. Add the continuous phase, antioxidant, zero-field friction reducer and framework enhancer to the activated thixotropic framework, stir and mix evenly, and then perform high-speed shear dispersion to obtain a pre-gel paste; wherein, the high-speed shear dispersion conditions are: rotation speed 3000-5000 rpm, time 20-60 minutes, temperature 40-70℃. S3. While stirring, slowly add the dispersed phase, and then perform high-speed shear dispersion to obtain a homogeneous milky white gel; wherein, the high-speed shear dispersion conditions are: rotation speed 3000-5000 rpm, time 8-20 minutes; S4. Add dispersant to homogeneous milky white gel, then add magnetic particles in 3-5 batches. Knead for 5-10 minutes after each batch is added. After all the particles are added, continue kneading for 20-40 minutes to obtain crude product. S5. Take the crude product and treat it with an ultrasonic cell disruptor at a power of 450-550W for 0.6-2 hours to obtain an ultrasonic dispersion. S6. Place the ultrasonic dispersion in a vacuum environment and allow it to stand for 0.5-2 hours to degas; stir 0-2 times during this period.
8. The heterogeneous magnetorheological fluid as described in claim 7, characterized in that: In step S1, the activator is added as follows: while stirring at 100-300 rpm, the activator is added dropwise at a rate of 0.5-1.0 g / min. After the addition is complete, stirring is continued at 100-300 rpm for 2-5 minutes. In step S2, the conditions for uniform mixing are: stirring at a speed of 500-1000 rpm for 2-5 minutes; In step S3, the specific operation of adding the dispersed phase is as follows: the dispersed phase is slowly injected at a rate of 0.3-1.0 g / min while stirring at 1000-1500 rpm.
9. The heterogeneous magnetorheological fluid according to claim 7, characterized in that: In step S4, the kneading operation is as follows: the homogeneous milky white gel is transferred to a dual planetary mixer or a three-roll mill, a dispersing agent is added, and then magnetic particles are added in 3-5 batches. After each batch is added, the mixture is kneaded at 30-100 rpm for 5-10 minutes. After all the particles are added, the mixture is kneaded for another 20-40 minutes to obtain a crude product. During kneading, an anchor-type or frame-type stirring paddle is used, with a gap of 2-5 mm between the paddle blade and the container wall. Preferably, in steps S2 and S3, the high-speed shear dispersion uses a serrated dispersion disc with a disc diameter to container diameter ratio of 0.4-0.
6. Preferably, in step S5, the vacuum degassing conditions are: static degassing at 20-30℃ and a vacuum of -0.08 to -0.1 MPa.
10. The use of the heterogeneous magnetorheological fluid as described in any one of claims 1-9 in magnetorheological vibration dampers, magnetorheological intelligent suspension systems, and magnetorheological dampers.