A controlled oxidative degradation method of oxygen-functionalized rubber
By using a variable-valence metal-supported molecular sieve catalyst to activate oxygen in an oxygen-containing atmosphere, the active sites of oxygen-functionalized rubber molecular chains are selectively attacked, thus achieving controllable oxidative degradation of oxygen-functionalized rubber. This solves the problems of low degradation efficiency and uncontrollability in existing technologies and meets the needs of resource utilization.
Patent Information
- Application Number
- CN202611346594.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-13
AI Technical Summary
Existing technologies fail to effectively utilize the structural characteristics of oxygen-functionalized rubber, resulting in a slow degradation rate in the natural environment. Furthermore, existing degradation methods are energy-intensive, inefficient, have limited applicability, and lack controllability.
A variable-valence metal-supported molecular sieve catalyst is used to activate oxygen in an oxygen-containing atmosphere, selectively attacking the active sites of oxygen-functionalized rubber molecular chains. Controllable oxidative degradation under mild conditions is achieved by adjusting the reaction conditions, including the regulation of temperature, time, and catalyst type.
It achieves controllable cleavage of rubber molecular chains under normal pressure, the molecular weight of degradation products is adjustable, it has a wide range of applications, is environmentally friendly, the degradation process is controllable, it is applicable to a variety of matrix rubbers, and meets the needs of resource utilization.
Smart Images

Figure CN123083160A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of waste polymer material resource utilization and polymer degradation technology, specifically to a method for controlled oxidative degradation of oxygen-functionalized rubber. Background Technology
[0002] Styrene-butadiene rubber (SBR), butadiene rubber (BR), and other diene rubbers are widely used in aerospace, automotive manufacturing, electronic packaging, and building materials, leading to a year-on-year increase in their waste volume. After curing, these rubber products form a dense, cross-linked three-dimensional polymer network, significantly restricting molecular chain movement and making them extremely difficult to degrade in the natural environment. Improper disposal will result in long-term environmental burden and resource waste. Among various methods for recycling waste polymers, chemical recycling, by selectively breaking down the polymer backbone, transforms cross-linked rubber into reusable oligomers or small molecule products, representing an important pathway that balances environmental protection and resource recycling. However, current chemical recycling processes are mostly developed for general-purpose rubbers and plastics, and controllable degradation technologies adapted to oxygen-functionalized modified rubber adhesives remain very limited.
[0003] Our team previously developed a method for preparing oxygen-functionalized polymers from waste butadiene rubber via catalytic oxidation (Chinese Invention Patent CN121736187A). This method utilizes selective catalytic oxidation to functionalize waste butadiene rubber, introducing oxygen-containing polar functional groups such as hydroxyl and carboxyl groups into the rubber molecular chain under mild conditions. This upgrades waste rubber from low-value solid waste to high-value adhesive raw materials, effectively solving the technical challenges of waste rubber recycling, modification, and functionalization. However, existing research mainly focuses on the front-end preparation and performance optimization of modified waste rubber, with insufficient attention paid to the end-of-life disposal of modified rubber products. Although rubber materials prepared through a single oxidation functionalization process show significant improvements in polarity, hydrophilicity, and adhesion due to the introduction of oxygen-containing functional groups, their degradation rate in the natural environment remains extremely slow.
[0004] From a chemical structural perspective, after modification using the aforementioned catalytic oxidation method, the bond dissociation energies of the oxygen-containing polar functional groups such as hydroxyl and carboxyl groups introduced into the rubber molecular chain, as well as their adjacent C=C bonds, are significantly lower than those of conventional C=C bonds in the rubber backbone. This structural feature means that under appropriate oxidative conditions, these sites will become preferential targets for free radical reactions, thus serving as active sites for deep oxidative degradation and providing a structural basis for subsequent controlled chain scission. However, existing recycling and degradation technologies have failed to identify and utilize this structural advantage inherent in rubber itself.
[0005] For the degradation and recycling of rubber and its products, various solutions have been proposed in existing technologies. While thermal pyrolysis technologies (such as CN106367098A and CN207227348U) can decompose rubber, they typically require temperatures above 400℃, resulting in high energy consumption and complex products, making selective chain scission difficult. Photocatalytic degradation technologies (such as CN119751974B) are limited by low degradation efficiency and long processing cycles, making them unsuitable for industrial applications. Alkaline hydrolysis (CN107418492B) and solvent dissolution recovery (CN112480829A) are mainly applicable to specific systems, have limited scope, and are prone to secondary pollution. Existing adhesive recycling technologies for adhesive products made from oxygen-functionalized rubber also suffer from similar problems. The common drawback of these methods is that they fail to consider the structural characteristics of oxygen-functionalized rubber itself, and also fail to achieve controllable oxidative degradation under mild conditions through systematic regulation of multiple conditions such as catalysts, oxidizing atmospheres, temperature, and time.
[0006] In summary, existing oxygen-functionalized rubbers suffer from prominent problems such as low degradation efficiency, lack of dedicated degradation processes, and uncontrollable degradation processes. Therefore, it is necessary to provide a controllable oxidative degradation method suitable for oxygen-functionalized rubbers, enabling effective breakage of rubber molecular chains under relatively mild conditions. Furthermore, by adjusting reaction conditions, the degree of degradation and the molecular weight of degradation products can be gradient-controlled, providing a technological foundation for the resource utilization of waste rubber and its products. Summary of the Invention
[0007] To address the technical problems of existing oxygen-functionalized rubbers (such as the products described in our previous patent CN121736187A) lacking dedicated degradation methods, having low degradation efficiency, and exhibiting uncontrollable degradation processes after use and disposal, this invention provides a controllable oxidative degradation method for oxygen-functionalized rubbers. This method enables the rubber molecular chains to break effectively under relatively mild conditions, and allows for gradient control of the degree of degradation and the molecular weight of degradation products by adjusting the reaction conditions.
[0008] To achieve the above objectives, the present invention adopts the following technical solution: A method for controlled oxidative degradation of oxygen-functionalized rubber, comprising the following steps: S1. Contact oxygen-functionalized rubber with an organic solvent to perform swelling or dissolution treatment; S2. Disperse the variable-valence metal supported molecular sieve catalyst in an organic solvent; S3. Mix the mixture obtained in step S1 with the mixture obtained in step S2, and carry out an oxidative degradation reaction at 60-200°C in an oxygen or air atmosphere; S4. Separate the reaction products, remove the solvent, and obtain the degradation products; The temperature and time of the oxidative degradation reaction are adjustable to achieve gradient control of the molecular weight of the degradation products. Preferably, the matrix polymer of the oxygen-functionalized rubber adhesive is selected from at least one of styrene-butadiene rubber, polybutadiene rubber, isoprene rubber, or natural rubber.
[0009] Preferably, the oxidative degradation reaction temperature is 80-200℃, and the reaction time is 8-48 h.
[0010] Preferably, the variable valence metal in the variable valence metal supported molecular sieve catalyst is selected from at least one of iron, cobalt, manganese, and copper; and the molecular sieve is a titanium-silicon molecular sieve. More preferably, the variable valence metal is iron, and the titanium-silicon molecular sieve is a TS-1 type titanium-silicon molecular sieve.
[0011] Preferably, the mass loading of the variable valence metal is 1-10%; based on the total reactants in the system, the amount of the catalyst is 0.2-2 mol.
[0012] Preferably, the organic solvent is a chloroalkane, and more preferably o-dichlorobenzene.
[0013] Preferably, the separation is performed by centrifugation at a speed of 4000-8000 r / min.
[0014] Preferably, the degradation products comprise oxygen-containing small molecule compounds and / or oligomers, wherein the oxygen-containing small molecule compounds are selected from at least one of carboxylic acids, ketones, aldehydes or esters.
[0015] Preferably, the molecular weight of the degradation products is characterized by gel permeation chromatography, and the product structure is characterized by Fourier transform infrared spectroscopy or nuclear magnetic resonance hydrogen spectroscopy.
[0016] The core of this invention lies in utilizing the oxygen-containing polar functional groups such as hydroxyl and carboxyl groups, along with their adjacent C / C bonds, already introduced into the oxygen-functionalized rubber molecular chain as preferential attack sites for oxidative chain scission. A variable-valence metal-supported molecular sieve catalyst is used to activate oxygen in an oxygen-containing atmosphere to generate reactive oxygen species, selectively attacking these active sites, thus causing the rubber molecular chain to break under mild conditions. The variable-valence metal (such as Fe, Co, Mn, Cu, etc.) undergoes a valence cycle (e.g., Fe...) 2+ / Fe 3+ Co 2+ / Co 3+ It continuously activates oxygen, thereby achieving controllable breakage of the main chain.
[0017] The controllability of the controlled oxidative degradation method is reflected in the following aspects: (1) the rate and depth of the oxidation reaction can be controlled by adjusting the reaction temperature; (2) the molecular weight of the degradation products can be controlled by adjusting the reaction time; and (3) the selectivity and efficiency of chain scission can be controlled by adjusting the type and amount of catalyst. The molecular weight of the degradation products can be characterized and verified by gel permeation chromatography (GPC).
[0018] Compared with the prior art, the present invention has the following beneficial effects: 1. Mild reaction conditions and highly controllable degradation degree. This invention can achieve the oxidative degradation of oxygen-functionalized rubber under normal pressure and 60-200℃ conditions (Example 5: molecular weight decrease can be detected at 60℃), without the need for high temperature and high pressure, resulting in low energy consumption and high safety. Furthermore, by adjusting the reaction temperature and reaction time, the molecular weight of the degradation products can be gradient-controlled (Examples 5-16: when the temperature increases from 60℃ to 200℃, Mn decreases from 180 kDa to 827 Da; when the time is extended from 2 h to 48 h, Mn decreases from 45.5 kDa to 856 Da), making it suitable for different resource recovery needs.
[0019] 2. Wide applicability and flexible, adjustable catalyst system. This invention is applicable to oxygen-functionalized rubbers with various matrices, such as styrene-butadiene rubber, cis-butadiene rubber, polybutadiene rubber, isoprene rubber, and natural rubber (Examples 1-4), demonstrating strong substrate versatility. Furthermore, the catalyst system can utilize various variable-valence metals such as iron, cobalt, manganese, and copper supported on titanium-silicon molecular sieves. Different variable-valence metals can activate oxygen through valence state cycling to achieve oxidative chain scission (Examples use Fe / TS-1 as an example). This allows for flexible selection based on cost and performance requirements, resulting in excellent industrial adaptability.
[0020] 3. Environmentally friendly, achieving full-chain resource utilization of waste rubber. This invention uses oxygen or air as a green oxidant, eliminating the need for highly polluting additives; the supported molecular sieve catalyst can be filtered, recovered, and recycled multiple times, resulting in minimal waste generation. This invention, together with previous patent CN121736187A and the adhesive material patent filed on the same day, constitutes a complete closed-loop technology encompassing preparation, application, degradation, and regeneration, realizing the full life-cycle resource utilization of waste rubber from low-value recycling to functional utilization and then to controlled degradation. Attached Figure Description
[0021] Figure 1 GPC spectra of four rubber raw materials: styrene-butadiene rubber (SBR), butadiene rubber (PBR), isoprene rubber (IR), and natural rubber (NR).
[0022] Figure 2 GPC spectra of various oxygen-functionalized modified rubbers (OSBR, OPBR, OIR, and ONR).
[0023] Figure 3 GPC spectra of oxidative degradation products of various oxygen-functionalized modified rubbers (OSBR, OPBR, OIR, and ONR).
[0024] Figure 4 This is a comparison of the Fourier transform infrared (FTIR) spectra of oxygen-functionalized rubber before and after degradation.
[0025] Figure 5 The 1H NMR spectra of oxygen-functionalized rubber before and after degradation ( 1 H NMR comparison image.
[0026] Figure 6 These are photos comparing the physical state of oxygen-functionalized rubber adhesive products before and after degradation. Detailed Implementation
[0027] The present invention will be further described below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the following embodiments. Unless otherwise specified, the raw materials used in the embodiments can be purchased commercially. The room temperature mentioned in the embodiments refers to 25±3℃.
[0028] The oxygen-functionalized rubber raw material used in this invention embodiment was prepared according to the method described in our team's previous patent CN121736187A. This method introduces oxygen-containing polar functional groups such as hydroxyl and carboxyl groups onto the diene rubber molecular chain under mild conditions using a variable-valence metal-supported molecular sieve catalyst. This invention uses this type of oxygen-functionalized rubber as a degradation substrate, utilizing the oxygen-containing functional groups introduced into its molecular chain as active sites for oxidative chain scission, thereby achieving controlled degradation.
[0029] Catalyst Preparation: Unless otherwise specified, the variable-valence metal-supported molecular sieve catalysts used in the embodiments of this invention were prepared by an equal-volume impregnation method. The variable-valence metal is selected from at least one of iron, cobalt, manganese, and copper, preferably iron; the molecular sieve is a titanium-silicon molecular sieve, preferably a TS-1 type titanium-silicon molecular sieve. The specific preparation process is as follows: Weigh the titanium-silicon molecular sieve support (preferably TS-1) according to the designed loading (preferably 1-10 wt.%), calculate the corresponding metal salt (such as ferrous acetate, ferric nitrate, cobalt acetate, manganese nitrate, copper acetate, etc.) according to the target metal loading ratio, and prepare an impregnation aqueous solution; add the metal salt solution dropwise to the molecular sieve support, and let it stand at room temperature for 12-24 h for impregnation; after impregnation, place it in an oven at 110-140℃ for 6-12 h to remove free moisture, and finally calcine it at 400-650℃ in air for 2-8 h, and obtain the target supported catalyst material after cooling.
[0030] In the following examples, Fe / TS-1 is used as a representative scheme for variable valence metal supported molecular sieve catalysts. Those skilled in the art will understand that the catalyst systems of variable valence metals (including but not limited to cobalt, manganese, and copper) supported on titanium silicate molecular sieves (including but not limited to TS-1) described in this invention can all achieve similar oxidative degradation effects based on the same mechanism of variable valence metal cyclic activation of oxygen.
[0031] Testing and Characterization: The degree of molecular chain breakage of the degradation products was quantitatively determined by gel permeation chromatography (GPC). The dried degradation products were fully dissolved in tetrahydrofuran (THF) mobile phase and tested using a Waters 1515 gel permeation chromatograph. The number-average molecular weight, weight-average molecular weight, and molecular weight distribution index of the polymer before and after degradation were obtained from the chromatograms. The change in molecular weight was used to evaluate the depth of chain breakage of the rubber macromolecular backbone, thereby measuring the controllable degradation effect under different process conditions.
[0032] The sample structure and properties were characterized by the following tests: Fourier transform infrared spectroscopy (FTIR, Nicoleti S10) was used to compare the evolution of functional group structures before and after degradation of the modified rubber to verify the oxidative chain scission reaction; and nuclear magnetic resonance spectroscopy (NMR) was used to characterize the samples. 1 The functional groups in the degradation products were qualitatively analyzed by 1H NMR (AVANCE 400) to clarify the structural changes of various functional groups during the degradation process.
[0033] Examples 1-4: Oxidative Degradation of Different Types of Rubber Adhesives This set of examples aims to illustrate the applicability of the method of the present invention to the degradation of different rubber adhesives. The specific operation is as follows: Take 100 mg of different types of oxygen-functionalized rubber and add it to 2 mL of o-dichlorobenzene solvent. Stir and dissolve at 60 °C and atmospheric pressure, then cool to room temperature. This solution is denoted as solution A. Separately, take 10 mg of catalyst (Fe / TS-1, metal loading 10 wt.%) and add it to 2 mL of o-dichlorobenzene. Stir until homogeneous. This solution is denoted as solution B. Mix solutions A and B and place them in a 20 mL flask equipped with a reflux condenser. Stir and react for 12 hours at 160 °C under an oxygen atmosphere and atmospheric pressure. After the reaction is complete, centrifuge the mixture for 3 min to achieve solid-liquid separation, and then remove the solvent by rotary evaporation to obtain the product.
[0034] The number-average molecular weight, weight-average molecular weight, and molecular weight distribution index (measured by GPC) of the degradation products of various rubber adhesives in each embodiment are listed in Table 1 below. To verify the necessity of oxygen-containing functional groups for degradation, comparative data of corresponding rubber raw materials without oxidative functionalization treatment under the same conditions are also listed (Comparative Examples 1-4).
[0035] Table 1. Oxidative degradation results of different types of rubber adhesives
[0036] As shown in Table 1, after treatment with the method of this invention, the molecular weight of various oxygen-functionalized rubbers was significantly reduced, with the number-average molecular weight decreasing from over 100,000 Da to 100,000 Da. 2 ~10 3 Da indicates that the method of the present invention has a good degradation effect on oxygen-functionalized rubbers of different matrices.
[0037] In contrast, the molecular weight of the corresponding rubber raw materials (Comparative Examples 1-4) that were not treated with oxidative functionalization remained essentially unchanged under the same conditions, confirming that the oxygen-containing functional groups introduced by the previous oxidation are the structural basis for the efficient oxidative chain scission achieved in this invention. Without these oxygen-containing functional groups as active sites, the rubber molecular chains would be difficult to break effectively under the same conditions.
[0038] Examples 5-11: Effect of Reaction Temperature This set of examples used oxygen-functionalized styrene-butadiene rubber adhesive as the degradation raw material and Fe / TS-1 supported molecular sieve as the catalyst. The specific operating steps were the same as in Example 1, except that the reaction temperature (60-200℃) was varied to systematically investigate the effect of reaction temperature on the oxidative degradation of rubber. The corresponding experimental results are summarized in Table 2.
[0039] Table 2. Effect of reaction temperature on oxidative degradation performance (fixed time: 12 h)
[0040] As shown in Table 2, temperature significantly affects the degree of degradation. When the reaction temperature increases from 60℃ to 100℃, Mn drops sharply from 180784 Da to 105798 Da, indicating that the degradation reaction exhibits a clear temperature response characteristic, with the reaction initiation temperature being approximately 80-100℃. When the temperature further increases to 160℃, Mn decreases to 922 Da, achieving deep degradation. When the temperature rises to 200℃, Mn further decreases to 827 Da. The above temperature gradient data directly support the technical effect of this invention in achieving gradient control of the degree of degradation by adjusting the reaction temperature. Notably, PDI increases significantly above 120℃ (from 1.2 to 21.6), indicating that non-uniform chain breakage occurs during degradation, consistent with the characteristics of free radical chain scission.
[0041] Examples 12-16: Effect of Reaction Temperature In this series of examples, oxygen-functionalized styrene-butadiene rubber (SBR) was used as the degradation raw material, Fe / TS-1 was used as the catalyst, the reaction temperature was kept constant at 160℃, and only the reaction time (2-48 h) was varied to systematically investigate the effect of reaction time on the oxidative degradation of rubber. The corresponding experimental results are summarized in Table 3.
[0042] Table 3. Effect of reaction time on oxidative degradation performance (at a fixed temperature of 160 °C)
[0043] As shown in Table 3, the molecular weight decreases most significantly in the early stage of the reaction (2-12 h), with Mn decreasing from 45500 Da to 922 Da; after 12 h, the degradation tends to slow down. This pattern indicates that the present invention can achieve precise control of the degree of degradation by controlling the reaction time, and can obtain a wide range of controllable products from oligomers to deeply small molecules within 2-12 hours, meeting different resource utilization needs.
[0044] The experimental data above show that the present invention can achieve effective oxidative degradation of modified rubber adhesives within a wide process range of 60-200℃ and 2-48 h; and as the reaction temperature increases or the reaction time prolongs, the degree of chain scission of rubber macromolecules gradually deepens, and the degradation effect gradually increases. The results confirm that the process of the present invention has a wide applicable window and excellent adjustability of process parameters, enabling the controllable degradation of waste rubber adhesives.
[0045] Example 17: Effect of Oxidizing Atmosphere Example 17: The procedure was the same as in Example 1, but the oxidant was changed from oxygen to air. The experimental results are listed in Table 4.
[0046] Comparative Example 5: The procedure was the same as in Example 1, but nitrogen gas was introduced into the system to remove oxygen. After the reaction, GPC analysis of the product showed no significant decrease in molecular weight, confirming that the reaction cannot occur under anaerobic conditions.
[0047] Table 4. Effect of reaction atmosphere
[0048] As shown in Table 4, when air is used instead of oxygen, the degradation effect decreases slightly but still achieves effective degradation (Mn increases from 922 Da to 1256 Da), proving that air can also be used as an oxidant in the method of this invention. Under anaerobic conditions (Comparative Example 5), the molecular weight remains essentially unchanged, confirming that oxygen is a necessary condition for the oxidative chain scission reaction to occur.
[0049] The method of this invention enables the controlled oxidative degradation of oxygen-functionalized rubber. The principle lies in the fact that the polar groups such as hydroxyl and carboxyl groups introduced into the molecular chain of oxygen-functionalized rubber, and their adjacent carbon-carbon bonds, have low bond dissociation energies. Under oxygen-containing atmosphere and the action of a variable-valence metal catalyst, preferential oxidative chain scission can occur under relatively mild conditions. By adjusting the reaction temperature and reaction time, the degree of chain scission can be controlled, achieving gradient regulation of the molecular weight of the degradation products.
[0050] Those skilled in the art should understand that the above embodiments using Fe / TS-1 as a catalyst are representative schemes, but the present invention is not limited thereto. Based on the same mechanism of oxygen activation through the cycling of variable valence metals, catalyst systems using other variable valence metals such as cobalt (Co), manganese (Mn), and copper (Cu) supported on TS-1 or other titanium-silicon molecular sieves can also achieve the technical effects of the present invention. The salts corresponding to each metal include, but are not limited to: cobalt acetate, cobalt nitrate, manganese nitrate, manganese acetate, copper acetate, and copper nitrate. The mass loading of the variable valence metal can be adjusted within the range of 1-10%, and the catalyst dosage can be adjusted within the range of 0.2-2 mol% (based on the total reactants in the system), both of which can achieve effective oxidative degradation effects.
[0051] Figure 1 The figure shows the GPC (Gross Polymerization) spectra of four rubber raw materials: styrene-butadiene rubber (SBR), butadiene rubber (PBR), isoprene rubber (IR), and natural rubber (NR). As can be seen from the figure, all four rubbers exhibit high molecular weight distribution characteristics, with their number-average molecular weights (Mn) ranging from 10 to 10. 5 ~10 6 Da.
[0052] Figure 2 GPC spectra of four rubbers—styrene-butadiene rubber (SBR), butadiene rubber (PBR), isoprene rubber (IR), and natural rubber (NR)—oxidized to oxygen-functionalized modified rubbers (OSBR, OPBR, OIR, and ONR). Compared with the raw materials, the oxidation products of all four rubbers exhibit a high molecular weight distribution range (Mn distributed in the range of 10). 5 ~10 6 The molecular weight distribution curve is smooth and complete, indicating that the main chain of the raw material did not break significantly during the oxidative degradation process, and the molecular chain structure remained intact (Comparative Examples 1-4).
[0053] Figure 3 The GPC curves of various oxygen-functionalized modified rubbers (OSBR, OPBR, OIR, and ONR) after degradation by the method of this invention (Fe / TS-1 catalyst, 160℃, 12 h, oxygen atmosphere) are shown. Figure 2 The comparison shows that the GPC curves of the four oxygen-functionalized rubber degradation products all shifted significantly towards the lower molecular weight region, with the number-average molecular weight (Mn) decreasing from 10. 5 ~10 6 Da dropped to 10 2 ~10 3 Da indicates that the rubber molecular chains undergo efficient breakage. The degree of degradation varies among different rubbers (Examples 1-4), but all achieve efficient conversion from high molecular weight polymers to oligomers / small molecules.
[0054] Figure 4This is a comparison of the Fourier transform infrared (FTIR) spectra of oxygen-functionalized styrene-butadiene rubber (OSBR) before degradation and after degradation using the method of this invention. Before degradation, OSBR exhibits a wavelength of ~3400 cm⁻¹. -1 The characteristic absorption peak of hydroxyl groups is observed at ~1700 cm⁻¹. -1 The presence of a carbonyl characteristic absorption peak indicates that oxygen-containing functional groups were successfully introduced during the initial oxidative functionalization. After degradation, the characteristic absorption intensities corresponding to hydrocarbon and olefin groups significantly decreased, indicating that the carbon chains and unsaturated double bonds of the rubber macromolecules broke; the intensity of the aforementioned oxygen-containing functional group characteristic absorption peaks changed, and the 1000-1300 cm⁻¹ range also showed a decrease. -1 The enhanced absorption signal of CO bonds in the interval indicates that the rubber macromolecular chain undergoes oxidative breakage, generating oxygen-containing small molecule compounds such as ketones, esters, hydroxyl groups, and ethers.
[0055] Figure 5 This is a comparison of the ¹H NMR spectra of oxygen-functionalized styrene-butadiene rubber (OSBR) before degradation and after degradation using the method of this invention. The aromatic hydrogen signals of the benzene ring remained essentially unchanged before and after degradation, indicating that the styrene structural units were not destroyed during the degradation process. However, the olefin hydrogen signals (~5.0-5.5 ppm) were significantly weakened, and a characteristic peak for aldehyde hydrogens appeared at ~9.0-10.0 ppm, proving that the C=C bonds in the rubber backbone underwent oxidative breakage, generating small molecule products with oxygen-functionalized end caps.
[0056] Figure 6 These are comparative photographs showing the physical states of oxygen-functionalized rubber adhesive products before (left) and after (right) degradation. Before degradation, the rubber adhesive products exist in the form of solid sheets; after degradation by the method of this invention, the solids completely dissolve in the organic solvent, forming a homogeneous and transparent solution (Examples 1-4). The changes in physical state directly demonstrate the breakdown of the rubber cross-linking network and the effective cleavage of the molecular chains, verifying the degradation effect of the method of this invention.
Claims
1. A method for controlled oxidative degradation of oxygen-functionalized rubber, characterized in that, Includes the following steps: S1. Contact oxygen-functionalized rubber with an organic solvent to perform swelling or dissolution treatment; S2. Disperse the variable-valence metal supported molecular sieve catalyst in an organic solvent; S3. Mix the mixture obtained in step S1 with the mixture obtained in step S2, and carry out an oxidative degradation reaction at 60-200°C in an oxygen or air atmosphere; S4. Separate the reaction products, remove the solvent, and obtain the degradation products.
2. The method according to claim 1, characterized in that, The matrix polymer of the oxygen-functionalized rubber adhesive is selected from at least one of styrene-butadiene rubber, polybutadiene rubber, isoprene rubber, or natural rubber.
3. The method according to claim 1, characterized in that, The reaction temperature in step S3 is 80-200℃, and the reaction time is 8-48 h.
4. The method according to claim 1, characterized in that, The variable valence metal in the variable valence metal supported molecular sieve catalyst is selected from at least one of iron, cobalt, manganese, and copper; the molecular sieve is a titanium-silicon molecular sieve.
5. The method according to claim 4, characterized in that, The variable valence gold is iron, and the titanium-silicon molecular sieve is TS-1 type titanium-silicon molecular sieve; the mass loading of the variable valence metal is 1-10%; based on the total reactants of the system, the amount of the catalyst is 0.2-2 mol.
6. The method according to claim 1, characterized in that, The organic solvent is a chlorinated alkane, preferably o-dichlorobenzene.
7. The method according to claim 1, characterized in that, The separation is performed by centrifugation at a speed of 4000-8000 r / min.
8. The method according to claim 1, characterized in that, The degradation products comprise oxygen-containing small molecule compounds and / or oligomers, wherein the oxygen-containing small molecule compounds are selected from at least one of carboxylic acids, ketones, aldehydes, or esters.
9. The method according to any one of claims 1-7, characterized in that, The molecular weight of the degradation products was characterized by gel permeation chromatography, and the product structure was characterized by Fourier transform infrared spectroscopy or nuclear magnetic resonance hydrogen spectroscopy.
Citation Information
Patent Citations
Continuous waste rubber cracking reactor
CN106367098A
A biodegradable adhesive, its preparation method and uses
CN107418492B
Method for recycling cyanoacrylate solid gum
CN112480829A
Method for photo-induced deconstruction of waste rubber
CN119751974B
Method for preparing oxygen-containing functionalized polymer through catalytic oxidation of waste butadiene rubber