Device for wind driven generator main shaft casting with high toughness and low-temperature impact toughness
Through the combination of iron sand-covered casting technology and self-hardened resin sand casting, the lack of toughness and low-temperature impact performance of wind turbine spindle ductile iron is solved, and the high toughness and low-temperature impact performance is improved, and the process flow is simplified. And reduces production costs, suitable for lightweight and low-cost manufacturing of large wind spindles.
Patent Information
- Application Number
- CN202420564540.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2034-03-22
AI Technical Summary
The ductile iron castings of existing wind turbine spindles are inferior to forged steel in terms of toughness and low-temperature impact performance, and the production process of large castings is complex, low efficiency and high cost, which limits their application.
Using iron-type sand-covered casting technology, combined with self-hardened resin sand casting mold, the composite of iron-type sand-covered casting mold with self-hardened resin sand casting mold with multi-level structure is formed. Cast molds to achieve high toughness and low-temperature impact performance.
It realizes high toughness of wind turbine spindle castings and low-temperature impact toughness of -20℃, reduces production costs, simplifies process flow, improves mechanical performance and production efficiency, and is suitable for lightweight and low-cost manufacturing of large wind turbine spindles.
Smart Images

Figure CN222058763U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to a device for a main shaft casting of a wind generator with high toughness and low-temperature impact toughness, and belongs to the technical field of main shaft castings of wind generators. Background Art
[0002] Wind power generation technology is a green and sustainable new energy technology. It has entered a period of rapid development in my country. China has become the world's largest manufacturer and user of wind power generation equipment. Wind power generation technology has developed rapidly, and various new materials, new processes and new technologies have been well applied in the field of wind power. At present, how to enhance the independent design capability and level of wind turbines, improve the structure of wind turbines, reduce the manufacturing cost of wind turbines, and improve the efficiency of wind turbine power generation has become the key for domestic wind power host manufacturing equipment companies to occupy the market and enhance their competitiveness. For large wind turbines above 6 megawatts, improving the material properties of various components of wind turbines and achieving lightweight components of wind turbines is one of the important means to better exert the power generation efficiency of wind turbines and reduce the manufacturing cost of wind turbines.
[0003] In order to reduce the production cost of wind turbine main shaft (hereinafter referred to as wind turbine main shaft), ductile iron casting has gradually replaced the original forged steel production. However, the toughness of cast ductile iron main shaft, especially its low-temperature impact performance, is still far behind that of forged steel main shaft, which greatly limits the application of ductile iron wind turbine main shaft. In addition, the current casting of large wind turbine main shaft castings (generally weighing 15-25 tons per piece) also has some shortcomings in the casting process of ductile iron wind turbine main shaft, such as: the internal structure of the casting is not dense, the comprehensive mechanical properties are low, the production process is relatively complex, the production efficiency is low, the production cost is high, and the production process control requirements are strict; these shortcomings have restricted the further application of ductile iron wind turbine main shaft.
[0004] Iron mold sand-coated casting technology is a new energy-saving, material-saving, high-efficiency, high-quality casting technology. For wind turbine main shaft castings that are hollow and have a certain shape of inner cavity, the use of iron mold sand-coated and self-hardening resin sand (hereinafter referred to as self-hardening sand) composite casting technology can well overcome the above shortcomings. Combined with adjusting the composition of each element in ductile iron, improving the spheroidization and inoculation treatment of ductile iron, the comprehensive mechanical properties of ductile iron are further improved, so that wind turbine main shaft castings have excellent elongation and low-temperature impact properties comparable to forged steel parts. Utility Model Content
[0005] The purpose of the utility model is to overcome the above-mentioned deficiencies in the prior art and to provide a device for a wind turbine main shaft casting with high toughness and low-temperature impact toughness, which has a reasonable structural design, is safe and reliable, energy-saving and environmentally friendly, has good comprehensive performance of the casting, is simple and easy to operate, has low labor intensity for workers, and is easy to realize mechanized production.
[0006] The technical solution adopted by the utility model to solve the above problems is: the device of the high-toughness and low-temperature impact toughness wind turbine main shaft casting comprises a slag collecting ring and several exhaust channels for exhausting the gas of the iron mold covered with sand and covered with sand layers, and is characterized in that: it also comprises an iron mold covered with sand casting mold for the outer side casting mold of the wind turbine main shaft, and the flange bottom surface of the wind turbine main shaft, the inner cavity surface of the wind turbine main shaft, the pouring system of the wind turbine main shaft, and the upper plane of the wind turbine main shaft are all self-hardening resin sand casting molds, and the iron mold covered with sand casting mold is connected with the self-hardening resin sand casting mold. The iron mold sand-covered casting adopts a through-type multi-stage structure. The pouring system includes a straight runner, multiple distributed cross runners, multiple anti-rain-type ingates, a molten iron filtering and slag retaining system, multiple foam ceramic filters and multiple groups of filtering runners. Multiple distributed cross runners are arranged at the bottom of the straight runner. Multiple foam ceramic filters are respectively connected to multiple anti-rain-type ingates. Multiple distributed cross runners are matched with multiple groups of filtering runners. The molten iron filtering and slag retaining system is formed in the self-hardening resin sand casting and the iron mold sand-covered casting, and a slag collecting ring is arranged on the upper part of the inner cavity of the wind turbine main shaft.
[0007] Preferably, the iron mold covered sand casting mold and the self-hardening resin sand casting mold described in the present invention are connected by fastening screws and fastening pins; the fastening screws and fastening pins are conventional components and can also be fixed in other ways.
[0008] Preferably, the iron mold covered with sand casting mold of the utility model can be horizontally divided into several through-type casting molds.
[0009] Preferably, the self-hardening resin sand casting mold of the utility model is divided into sections.
[0010] Preferably, the thickness of the sand coating layer in the iron-coated sand casting mold of the utility model is 5-25 mm, the thickness of the iron mold is 150-250 mm, and the weight of the iron mold: the weight of the wind turbine main shaft casting = 1:4-5.7.
[0011] As a preference, the ratio of each cross-sectional area of the pouring system of the utility model is ∑ 直 :∑ 横 :∑ 内 =1:1.5-1.8:3.8-4.6, pouring time is 210-270 seconds.
[0012] Compared with the prior art, the utility model has the following advantages and effects: 1) The overall structural design is reasonable, safe and reliable, and the casting production of wind turbine main shaft castings with high toughness in the as-cast state of ductile iron and low-temperature impact toughness of more than 11 joules at -20°C is realized; 2) It is of great significance to promote the lightweight and low-cost manufacturing of wind turbines; 3) The production process of the utility model is simple and easy to operate, and the labor intensity of workers is low; 4) For the casting production of large wind turbine main shaft castings, mechanized production is easy to realize; 5) The casting production realizes riser-free casting, the molten iron recovery rate is high, the as-cast production can be realized, and the energy-saving effect of the production process is remarkable; 7) The production process of wind turbine main shaft castings uses less sand and has a good production environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a schematic diagram of the assembly of an iron mold sand-coated and self-hardening resin sand composite casting device according to an embodiment of the utility model.
[0014] Figure 2 This is a schematic diagram of a molten iron filtering device in a casting system of an iron mold covered with sand and a self-hardening resin sand composite casting mold according to an embodiment of the utility model. Figure 1 .
[0015] Figure 3 This is a schematic diagram of a molten iron filtering device in a casting system of an iron mold covered with sand and a self-hardening resin sand composite casting mold according to an embodiment of the utility model. Figure 2 .
[0016] Figure 4 This is a schematic diagram of a molten iron filtering device in a casting system of an iron mold covered with sand and a self-hardening resin sand composite casting mold according to an embodiment of the utility model. Figure 3 .
[0017] Figure 5 This is a schematic diagram of a wind turbine main shaft casting according to an embodiment of the utility model. Figure 1 .
[0018] Figure 6 This is a schematic diagram of a wind turbine main shaft casting according to an embodiment of the utility model. Figure 2 .
[0019] In the figure: an iron mold covered with sand casting mold 1, a self-hardening resin sand casting mold 2, a pouring system 3, a slag collecting ring 4, an exhaust channel 5, a wind turbine main shaft flange F; a straight runner 31, a distributed cross runner 32, a reverse rain-type inner runner 33, a molten iron filtering and slag blocking system 34, a foam ceramic filter 35, a filtering runner 36, a filtering front runner 361, and a filtering rear runner 362. DETAILED DESCRIPTION
[0020] The present invention will be further described in detail below with reference to the accompanying drawings and through examples. The following examples are provided to explain the present invention, but the present invention is not limited to the following examples.
[0021] Example
[0022] See also Figures 1 to 6 The device of the wind turbine main shaft casting with high toughness and low-temperature impact toughness in this embodiment includes an iron mold covered with sand casting mold 1 for casting the outer side of the wind turbine main shaft, a flange bottom surface for the wind turbine main shaft, an inner cavity surface of the wind turbine main shaft, a casting system 3 for the wind turbine main shaft, and an upper plane of the wind turbine main shaft are all self-hardening resin sand casting molds 2, slag collecting rings 4 and several exhaust channels 5 for exhausting gas from the iron mold covered with sand.
[0023] In this embodiment, the pouring system 3 includes a pouring cup, a straight runner 31, a plurality of distributed cross runners 32, a plurality of anti-rain-type ingates 33, a molten iron filtering and slag-blocking system 34, a plurality of foam ceramic filter screens 35 and a plurality of groups of filtering runners 36. A plurality of distributed cross runners 32 are arranged at the bottom of the straight runner 31. The plurality of foam ceramic filter screens 35 are respectively connected to the plurality of anti-rain-type ingates 33. The plurality of distributed cross runners 32 are matched with the plurality of groups of filtering runners 36. The molten iron filtering and slag-blocking system 34 is formed in the self-hardening resin sand casting 2 and the iron mold covered sand casting 1. The slag collecting ring 4 is arranged at the upper part of the inner cavity of the wind turbine main shaft.
[0024] In this embodiment, the molten iron filtering device is matched with the pouring system 3 ; the filtering runner 36 includes a front filtering runner 361 and a rear filtering runner 362 .
[0025] The casting process and technical principle of the as-cast high-toughness, high-low temperature impact performance ductile iron wind turbine main shaft casting of this embodiment are as follows: The wind turbine main shaft casting belongs to a large ductile iron casting ( Figure 5-Figure 6), the weight of the casting is 15-25 tons, and the maximum height of the casting exceeds 3 meters; currently, the casting production mainly adopts two processes: self-hardening sand casting or metal mold casting; these two processes have certain shortcomings and risks in producing ductile iron wind turbine main shaft castings, especially it is difficult to produce ductile iron high toughness and -20℃ low temperature impact toughness of 11 joules or more wind turbine main shaft castings, which greatly limits the further application of ductile iron wind turbine main shaft. The use conditions of wind turbines are relatively harsh, especially in terms of ambient temperature, which often ranges from room temperature to -20℃, or even -40℃; therefore, the mechanical properties of wind turbine main shafts also need to meet the above temperature range requirements, otherwise, there will be a broken shaft phenomenon during use, causing significant losses. In the self-hardening sand casting production of wind turbine main shafts, the solidification and cooling speed of molten iron is slow and the rigidity of the casting mold is poor. Therefore, the metallographic structure of the cast wind turbine main shaft castings is coarse and loose, the graphite ball morphology is relatively poor, and the cast performance is difficult to achieve high elongation and high and low temperature impact performance under medium and high strength. In the metal mold casting of wind turbine main shaft, the molten iron is in direct contact with the metal mold. The quenching effect of the metal mold greatly accelerates the cooling conditions of the molten iron. In order to ensure that the molten iron does not produce carbides under this cooling condition, high silicon solid solution is often used in metal mold casting. The high silicon content in ductile iron is not conducive to the low-temperature impact performance of ductile iron. The higher the silicon content, the lower its low-temperature impact performance. The rigidity of the iron mold sand-coated casting is good. The cooling rate of the molten iron by the iron mold sand-coated casting can be adjusted by the thickness of the sand coating layer and the thickness of the iron mold. In this way, the molten iron can be solidified and cooled at an appropriate cooling rate in the iron mold sand-coated casting. The castings cast by the iron mold sand-coated casting have dense internal structure, fine grains, and good graphite nodule morphology. At the same time, because there is no extreme quenching effect of the cooling rate, the silicon content in the molten iron can be kept at a low level, which is greatly beneficial to improving the low-temperature impact performance of ductile iron. Therefore, the utility model adopts a process method of combining an iron mold covered with sand casting and a self-hardening sand casting to form an integral casting mold of the wind turbine main shaft, and is equipped with a corresponding combination of molten iron elements, molten iron spheroidization, and inoculation treatment methods, and integrated innovation forms a complete set of process technologies and production processes for casting ductile iron wind turbine main shaft castings with high toughness in the cast state and high and low temperature impact performance, and realizes the raw riser casting of the wind turbine main shaft casting. The wind turbine main shaft casting has a dense internal structure, fine grains, and a high spheroidization grade. The cast mechanical properties of the wind turbine main shaft body or the attached casting test block reach: tensile strength: >420MPa, yield strength: >280MPa, elongation: >21%, -20℃ low temperature impact value: >11J.
[0026] The shape of the ductile iron wind turbine main shaft casting produced in this embodiment is shown in Figure 5-Figure 6 As can be seen from the figure, the shape of the wind turbine main shaft is: the lower part is a trumpet-shaped flange structure, which is used to connect the hub of the wind turbine. The shape of the main shaft above the flange is a gradient cylinder, and the interior of the gradient cylinder of the main shaft is a drum-shaped structure - that is: a cylindrical structure with small ends and a large middle.
[0027] In view of the structural characteristics of the wind turbine main shaft, the casting process of this embodiment adopts a multi-level horizontal split mold casting and a vertical bottom pouring reverse rain pouring method, which is similar to ordinary resin sand casting and metal mold casting. The casting device of this embodiment adopts a composite casting device of an iron mold covered sand casting mold 1 and a self-hardening resin sand casting mold 2 according to the requirements of the wind turbine main shaft casting process, the requirements of mold splitting and demolding, and the layout requirements of the pouring system, such as Figure 1 As shown, namely: the outer side casting of the wind turbine main shaft is a multi-stage iron mold covered with sand casting 1, the flange bottom surface, inner cavity surface, wind turbine main shaft casting system and upper plane of the wind turbine main shaft are all self-hardening resin sand casting 2; wherein the iron mold covered with sand casting 1 can be horizontally divided into several through-type castings, and then the box is closed and fastened by closing screws and closing pins to form a complete iron mold covered with sand casting 1 (iron mold covered with sand casting on the outer side of the main shaft); the self-hardening resin sand casting 2 is divided into sections, namely: the lower bell-mouth casting of the wind turbine main shaft casting (the main shaft flange self-hardening sand bottom box casting), including: the bottom plane of the wind turbine main shaft casting, the entire inner cavity of the lower bell-mouth of the wind turbine main shaft; the drum-shaped inner cavity of the wind turbine main shaft is an integral self-hardening sand casting (the main shaft inner cavity self-hardening sand casting); the slag collecting ring 4 on the top of the wind turbine main shaft, the exhaust channel 5 of the iron mold covered with sand and the sand layer, etc. form the main shaft self-hardening sand upper box casting. The iron mold covered with sand casting is combined with the self-hardening sand casting to finally form a composite wind turbine main shaft casting mold.
[0028] In the pouring system 3 of this embodiment, the sprue 31 and the distributed runner 32 are arranged in the self-hardening sand casting mold ( Figure 1 ), the molten iron filtering slag blocking system 34 in the casting system 3 is formed in the self-hardening resin sand casting mold 2 and the iron mold covered sand casting mold 1, the anti-rainfall type inner gate 33 in the casting system 3 is formed in the self-hardening sand, and the slag gathering ring 4 on the upper part of the wind turbine main shaft is formed in the self-hardening resin sand casting mold 2; the molten iron filtering device (such as the attached Figure 2-Figure 4 ), the molten iron rises through the dispersed horizontal runner bottom pouring into the upper structure of the molten iron filtering device, and then descends through the ceramic filter to filter the molten iron. The molten iron ascends through multiple anti-rainfall type inner runners 33 and enters the bottom surface of the wind turbine main shaft flange F, and then continuously fills the mold upward until it fills the entire wind turbine main shaft casting mold; according to the solidification requirements of the wind turbine main shaft casting of the device in this embodiment, the thickness of the sand coating layer in the iron mold sand coating casting is 5-25mm, the thickness of the iron mold is 150-250mm, and the weight of the iron mold: the weight of the wind turbine main shaft casting = 1:4-5.7; the ratio of each cross-sectional area of the pouring system 3 is ∑vertical:∑horizontal:∑inner=1:1.5-1.8:3.8-4.6, and the pouring time is 210-270 seconds.
[0029] In order to obtain wind turbine main shaft castings with high toughness and high and low temperature impact performance, the process conditions of the iron mold covered with sand-self-hardening sand composite casting need to be adjusted and controlled accordingly for the ductile iron molten iron used to cast the wind turbine main shaft casting in this embodiment, so as to obtain the ductile iron structure with a completely ferrite matrix in the cast state, the high-grade stone black ball morphology, and the dense and fine intrinsic grain structure without risers.
[0030] The chemical composition of each element of the ductile iron of this embodiment is controlled at: C: 3.7-3.95%, Si: 1.75-2.00%, S: <0.012%, P: <0.02%, Mn: <0.2%, Ni: 0.3-0.45%; Mg: 0.04-0.055%, RE: 0.008-0.015%. The spheroidization treatment of the molten iron of the utility model adopts the spheroidization ladle flushing method, and adopts heavy rare earth magnesium spheroidizing agent, and the amount of spheroidizing agent added is: 1.0-1.2%; the inoculation treatment adopts three-level inoculation, namely: ladle inoculation, molten iron flow inoculation after spheroidization, and instantaneous flow inoculation during pouring. In view of the large demand for molten iron, long molten iron pouring time, and long molten iron solidification time of wind turbine main shaft castings, the utility model uses a long-term composite inoculant for the inoculation treatment of molten iron. The amount of inoculant added is 0.3-0.5% in the first-level molten iron ladle, 0.45-0.6% in the second-level tapping flow inoculation, and 0.12-0.15% in the third-level instantaneous inoculation. During the melting process of molten iron, the superheated temperature of molten iron is controlled at about 1500℃, the spheroidizing tapping temperature of molten iron is 1430-1450℃, the pouring temperature is controlled at 1330-1360℃, and the pouring time is controlled at 210-270 seconds. ;
[0031] The wind turbine main shaft casting of this embodiment adopts a composite casting of an iron mold covered with sand casting mold 1 and a self-hardening resin sand casting mold 2, and a bottom-pouring molten iron filtration method, combined with high-carbon, low-silicon, large-dose multi-stage inoculation, low-temperature pouring and other molten iron treatment and pouring forms, to achieve the as-cast, riser-free casting of the wind turbine main shaft casting. The casting has a dense structure, a high spheroidization grade and no defects. The mechanical properties of the wind turbine main shaft are as follows: tensile strength: >420MPa, yield strength: >280MPa, elongation: >21%, -20℃ low-temperature impact value: >11J, which meet the mechanical performance requirements for the wind turbine main shaft to work and operate under harsh environmental conditions.
[0032] The production process of the wind turbine main shaft casting with high toughness and high and low temperature impact performance in this embodiment is as follows: the casting mold for the wind turbine main shaft adopts a composite casting mold of an iron mold covered with sand 1 and a self-hardening resin sand casting 2; the reverse rain shower type inner gate 33 of the molten iron pouring system 3 of the casting mold adopts the form of bottom pouring reverse rain showering and floating into the casting mold, and the molten iron filtration adopts a dispersed horizontal runner 32 to float the molten iron through the foam ceramic filter 35 to filter the molten iron. The top of the wind turbine main shaft casting adopts a slag collecting ring 4 to float the slag, and the top pressure edge exhaust channel 5 is used to discharge the organic volatile gas generated by the heating of the iron mold covered with sand; the element composition of the molten iron: C: 3.7-3.95%, Si: 1.75-2.00%, S: <0.012%, P: <0.02%, Mn: <0.2%, Ni: 0.3-0.4%; Mg: 0.04-0.0 55%, RE: 0.008-0.015%; the temperature of molten iron pouring and filling is: 1330-1350℃, and the pouring and filling time is controlled at 210-270 seconds; during the pouring process, the gas generated by the sand layer of the iron mold must be ignited and exhausted between the various faces of the iron mold and the exhaust duct of the upper casting mold; according to the weight of the wind turbine main shaft, the fastening bolts between the iron molds and the iron molds, and between the iron molds and the self-hardening resin sand can be loosened 10-15 hours after the pouring is completed, so that the castings can continue to cool under relatively free conditions, reducing the stress caused by the shrinkage of the castings during the solidification and cooling process; 24-36 hours after the pouring, the iron mold sand and the self-hardening resin sand castings can be loosened and unpacked layer by layer from top to bottom, and the castings can be allowed to continue to cool to room temperature in the air after unpacking, and then the castings can be cleaned and polished, thereby completing the casting process of the wind turbine main shaft. After unpacking, the iron mold is simply cleaned and then sent to the sand-coating molding equipment for sand-coating molding again using the residual heat in the iron mold. It is then combined with the well-shaped self-hardening resin sand casting mold and molten iron is poured. This cycle is repeated to achieve mass production of wind turbine main shaft castings.
[0033] This embodiment adopts iron mold covered with sand, self-hardening sand composite casting mold, bottom pouring open rain balanced water inlet mode, the ratio of various elements of molten iron that conforms to the principle of self-compensation of graphitization expansion in iron mold covered with sand casting, and the spheroidization and inoculation treatment forms adapted thereto, and finally obtains ductile iron high toughness with dense internal structure, excellent matrix and graphite metallographic structure, no inherent adverse casting defects, and -20°C low-temperature impact toughness of more than 11 joules of wind turbine main shaft castings, thereby realizing the mass production of such wind turbine main shaft castings in the cast state.
[0034] Through the above description, those skilled in the art can already implement it.
[0035] In addition, it should be noted that the shapes and names of the parts and components of the specific embodiments described in this specification may be different, and the above content described in this specification is only an example of the structure of the utility model. All equivalent changes or simple changes made based on the structure, features and principles described in the patent concept of the utility model are included in the protection scope of the utility model patent. Technicians in the technical field of the utility model can make various modifications or supplements to the specific embodiments described or replace them in a similar manner, as long as they do not deviate from the structure of the utility model or exceed the scope defined by the claims, they should all fall within the protection scope of the utility model.
Claims
1. A device for casting a main shaft of a wind turbine generator with high toughness and low-temperature impact toughness, comprising a slag collecting ring (4) and a plurality of exhaust passages (5) for exhausting gas from the iron mold sand covering layer, Features: The invention also includes an iron mold coated sand casting mold (1) for casting the outer side of the wind turbine main shaft, and a flange bottom surface, an inner cavity surface of the wind turbine main shaft, a casting system (3) of the wind turbine main shaft, and an upper plane of the wind turbine main shaft, all of which are self-hardening resin sand casting molds (2). The iron mold coated sand casting mold (1) is connected to the self-hardening resin sand casting mold (2) by a box assembly. The iron mold coated sand casting mold (1) adopts a through-type multi-level structure. The casting system (3) includes a straight runner (31), a plurality of dispersed cross runners (32), a plurality of anti-rain-type inner runners (33), and a molten iron A filtering slag retaining system (34), a plurality of foam ceramic filter screens (35) and a plurality of groups of filtering runners (36); a plurality of dispersed cross runners (32) are arranged at the bottom of the straight runner (31); the plurality of foam ceramic filter screens (35) are respectively connected to a plurality of anti-rainfall type inner runners (33); the plurality of dispersed cross runners (32) are matched with the plurality of groups of filtering runners (36); the molten iron filtering slag retaining system (34) is formed in a self-hardening resin sand casting mold (2) and an iron mold covered sand casting mold (1); and a slag collecting ring (4) is arranged at the upper part of the inner cavity of the wind turbine main shaft.
2. The device for the high toughness and low temperature impact toughness wind turbine main shaft casting according to claim 1, Features: The iron mold covered sand casting mold (1) and the self-hardening resin sand casting mold (2) are connected by a closing screw and a closing pin.
3. The device for the high toughness and low temperature impact toughness wind turbine main shaft casting according to claim 1, Features: The iron mold covered with sand casting mold (1) can be horizontally divided into a plurality of through-type casting molds.
4. The device for the high toughness and low temperature impact toughness wind turbine main shaft casting according to claim 1, Features: The self-hardening resin sand casting mold (2) is divided into sections.
5. The device for the high toughness and low temperature impact toughness wind turbine main shaft casting according to claim 1, Features: The thickness of the sand coating layer in the iron-coated sand casting mold (1) is 5-25 mm, the thickness of the iron mold is 150-250 mm, and the weight of the iron mold: the weight of the wind turbine main shaft casting is 1:4-5.7.
Citation Information
Cited By
Device and production method of wind driven generator main shaft casting with high toughness and low-temperature impact toughness
CN118002746A