Hardened body, manufacturing method of hardened body, and building material
By using amorphous volcanic glass fine powder as a silica source, the production of Al-substituted tobermorite is increased, resulting in a stronger and thermally stable building material with improved tobermorite content.
Patent Information
- Application Number
- JP2023089386
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-12
AI Technical Summary
Existing building materials using low density additives with volcanic ash may produce insufficient amounts of tobermorite due to the presence of crystalline silica, limiting their strength and thermal properties.
Incorporating amorphous volcanic glass fine powder as a silica source material, along with a calcium source, to enhance the production of Al-substituted tobermorite through hydrothermal reactions, thereby increasing the tobermorite content in the cured product.
The method results in a cured product with a higher tobermorite content, enhancing the strength and thermal stability of the building material.
Smart Images

Figure 2024171988000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a hardened body, a method for producing the hardened body, and a building material. [Background technology]
[0002] Patent Document 1 describes a fiber cement building material containing a low-density additive. This building material is composed of a building material mixture, which contains Portland cement, aggregate, only cellulose fibers, and a low-density additive. The Portland cement accounts for 5 to 80% by weight of the building material mixture, the aggregate accounts for less than 80% by weight of the building material mixture, and only cellulose fibers accounts for more than 4% by weight of the building material mixture. The low-density additive also reduces the density of the building material to 1.2 g / cm. 3 The building material contains volcanic ash, microspheres, or a mixture thereof in an amount sufficient to replace the aggregate on a weight basis so as to reduce the moisture expansion rate of the building material to 0.17% or less and maintain the moisture expansion rate of the building material at a level of 0.17% or less. Patent Document 1 discloses a building material obtained by autoclaving a mixture containing the above-mentioned building material mixture (paragraph
[0016] ). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5025872 Summary of the Invention [Problem to be solved by the invention]
[0004] Patent Document 1 discloses a low-density additive containing volcanic ash, which contains 30% by weight of crystalline silica and 70% by weight of amorphous volcanic ash glass. Therefore, the building material obtained by autoclaving a building material mixture containing this volcanic ash may produce insufficient tobermorite due to the crystalline silica.
[0005] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a method for producing a hardened body which produces a large amount of tobermorite.
[0006] Another object of the present invention is to provide a hardened body and a building material having a high tobermorite content. [Means for solving the problem]
[0007] A method for producing a hardened body according to one aspect of the present invention is a method for producing a hardened body by hardening a raw material containing a calcium source material and a silica source material. The silica source material contains a fine volcanic glass powder. The fine volcanic glass powder is amorphous.
[0008] A hardened body according to one embodiment of the present invention contains Al-substituted tobermorite, which is a reaction product of a calcium source material and fine powder of amorphous volcanic glass.
[0009] A construction material according to one aspect of the present invention comprises the hardened body and a functional part. Effect of the Invention
[0010] According to the present invention, there is an advantage that a hardened body having a high content of tobermorite can be obtained. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a graph showing the relationship between the Al2O3 / SiO2 ratio of the silica source and the tobermorite strength. [Diagram 2] FIG. 2 is a graph showing the relationship between the SiO2 content of the silica source and the tobermorite strength. [Diagram 3] FIG. 3 is a graph showing the relationship between the average particle size of the fine volcanic glass powder and the tobermorite strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following describes the hardened body, the manufacturing method of the hardened body, and the building material according to the embodiment of the present invention. The configuration described in the following embodiment is merely one example of the present invention. The present invention is not limited to the following embodiment, and various modifications are possible depending on the design, etc., as long as the effects of the present invention can be achieved.
[0013] (Embodiment) <Method of manufacturing the hardened body> The method for producing a hardened body according to the present embodiment involves hardening a raw material containing a calcium source material and a silica source material.
[0014] The calcium source material is not particularly limited as long as it contains a calcium component, and for example, either one or both of cement and slaked lime can be used. Examples of cement that can be used include Portland cement, fly ash cement, and blast furnace cement.
[0015] The silica source material contains volcanic glass powder (VGP). Volcanic glass powder is a fine powder made by grinding amorphous glassy powder of volcanic origin contained in volcanic ejecta deposit minerals such as Shirasu. Volcanic glass powder is made by isolating amorphous glassy powder (average particle size 80-100μm) from volcanic ejecta deposit minerals using a dry specific gravity separator, and then grinding the amorphous glassy powder into a fine powder using a grinder such as a roller mill.
[0016] The average particle size of the volcanic glass fine powder is preferably 1 μm or more and 50 μm or less. If the average particle size of the volcanic glass fine powder is within this range, the production of the volcanic glass fine powder is easy, the amount of tobermorite produced is large, and the powder is easily mixed uniformly with other materials during kneading when preparing the raw materials, and is less likely to settle. If the average particle size of the volcanic glass fine powder is less than 1 μm, it may be difficult to produce the volcanic glass fine powder (a jet mill is required) and the amount of tobermorite produced may be small. If the average particle size of the volcanic glass fine powder exceeds 50 μm, the volcanic glass fine powder is difficult to mix uniformly during kneading of the raw materials, and the volcanic glass fine powder may settle, especially in the case of a papermaking method. It is more preferable that the average particle size of the volcanic glass fine powder is 6 μm or more and 40 μm or less. The average particle size can be the median diameter (D50) of the particle size distribution obtained by the laser diffraction / scattering method.
[0017] Volcanic glass powder has a specific surface area of 5000 cm as measured by the BET method. 2 / g or more 40000cm 2 If the specific surface area of the volcanic glass fine powder is within this range, the production of the volcanic glass fine powder is easy, the amount of tobermorite produced is large, it is easy to mix uniformly with other materials during kneading when preparing the raw materials, and it is less likely to settle. 2 If the specific surface area of the volcanic glass powder is less than 40,000 cm / g, the volcanic glass powder will be coarse and will not be uniformly mixed with the raw materials when kneading. In particular, in the case of papermaking, the volcanic glass powder may settle. 2 If it exceeds 1 / g, the amount of tobermorite produced will be small, and it may take time to refine the volcanic glass fine powder. The BET method can conform to JIS R 1626 "Method of measuring specific surface area of fine ceramic powder by gas adsorption BET method."
[0018] The volcanic glass fine powder may contain 62.0 to 76.0% by weight of SiO2 and 11.5 to 18.6% by weight of Al2O3 as the constituent components. The volcanic glass fine powder may contain ion elution of Si4+ 13.5-18.0 ppm, Al 3+ A concentration of 3.5 to 5.0 ppm can be used.
[0019] In this embodiment, only volcanic glass fine powder can be used as the silica source material. In addition, in this embodiment, volcanic glass fine powder and other silica-containing components can be used in combination as the silica source material. Examples of other silica-containing components include silica powder and fly ash. When volcanic glass fine powder and silica powder are used in combination as the silica source material, the amount of tobermorite produced can be increased compared to when only silica powder is used as the silica source material.
[0020] When silica powder and fine volcanic glass powder are used in combination as the silica source material, the weight ratio of the silica powder and fine volcanic glass powder contained in the silica source material is preferably silica powder: volcanic glass fine powder = 1: 3 to 3: 1. In this case, the amount of tobermorite produced can be increased compared to when only silica powder is used as the silica source material.
[0021] When silica powder and fine volcanic glass powder are used in combination as the silica source material, the ratio (weight ratio) of alumina to silica contained in the silica source material is preferably Al2O3 / SiO2=more than 0.03 and not more than 0.16. In this case, the amount of tobermorite produced can be increased compared to when only silica powder is used as the silica source material.
[0022] In this embodiment, a raw material containing a calcium source material and a silica source material is prepared, water is added to the raw material, the raw material is molded into a desired shape, and then the raw material is hardened to form a hardened body. The raw material may contain aggregates, reinforcing fibers, admixtures, etc. in addition to the calcium source material and the silica source material.
[0023] In the present embodiment, a papermaking method, an extrusion method, a dry method, or the like can be used to produce the cured body.
[0024] In the papermaking method, water is mixed with the raw materials to prepare a slurry, and this slurry is papered onto a dehydrating sheet such as felt to create a green sheet (uncured sheet material). This green sheet is then cured in an autoclave (high-temperature, high-pressure steam curing) to harden it and form a hardened body.
[0025] In the extrusion method, a molding material is prepared by mixing the raw materials with water, and this molding material is extruded using a mold or the like to produce a green sheet. This green sheet is then cured in an autoclave to form a hardened body.
[0026] In the dry method, the dry-mixed raw materials are supplied in layers on a forming belt, water is sprayed onto the layered raw materials, and then the raw materials are compressed and molded using a roll or the like to produce a green sheet. This green sheet is then cured in an autoclave to form a hardened body.
[0027] In addition, autoclave curing may be used as secondary curing, and before the secondary curing, the green sheet may be subjected to moist heat curing or natural curing as primary curing.
[0028] <Cured body> The hardened body produced as described above is a product of the calcium source material and the silica source material being hardened by a hydrothermal reaction during curing such as autoclave curing. The hardened body contains tobermorite. Tobermorite is calcium silicate, and when only silica powder is used as the silica source material, it has a composition formula of 5CaO·6SiO2·5H2O (normal type). On the other hand, in this embodiment, since the silica source material contains volcanic glass fine powder, Al-substituted (aluminum-substituted) tobermorite is generated. That is, the hardened body of this embodiment contains tobermorite represented by the composition formula (Al-substituted type) of 9K2O·91CaO·9Al2O3·102SiO2·100H2O. Since the hardened body contains such Al-substituted tobermorite, the stable region of the hardened body can be expanded (or the thermal properties can be improved) compared to the case where only normal tobermorite is contained. The aluminum (Al) that constitutes Al-substituted tobermorite comes from volcanic glass fine powder and cement contained in the calcium source material. Cement contains about 5% by weight of Al2O3.
[0029] Furthermore, when the silica source material contains silica powder and volcanic glass fine powder, the hardened body of this embodiment contains both normal tobermorite and Al-substituted tobermorite. When the silica source material is only silica powder, a large amount of normal tobermorite is produced, and the peak of tobermorite (002 plane) by X-ray diffraction method appears at around 2θ=7.8°, but as the content of volcanic glass fine powder in the silica source material increases, 2θ shifts to the lower angle side. This suggests that as the content of volcanic glass fine powder increases, tobermorite transitions from normal to Al-substituted tobermorite.
[0030] <Construction materials> The building material according to the present embodiment is, for example, an exterior wall material, an interior wall material, a roofing material, etc., and is formed with the above-mentioned hardened body and a functional part. The functional part is a part that imparts the function of the hardened body as a building material to the hardened body. An example of the functional part is a coating film formed on the surface of the hardened body. In this case, the hardened body can be imparted with weather resistance, waterproofness, designability, etc. Another example of the functional part is an uneven shape formed on the surface of the hardened body. In this case, the hardened body can be imparted with designability, etc. Another example of the functional part is a solid part formed at the end of the hardened body. In this case, the hardened body can be imparted with the function of connecting to other hardened bodies.
[0031] (summary) As described above, the method for producing a hardened body according to the first aspect is a method for producing a hardened body by hardening a raw material containing a calcium source material and a silica source material. The silica source material contains a fine volcanic glass powder. The fine volcanic glass powder is amorphous.
[0032] According to this embodiment, the use of amorphous volcanic glass powder increases the amount of ion elution and the amount of tobermorite produced, so that a hardened body with high strength can be obtained.
[0033] The second aspect is a method for producing a hardened body according to the first aspect, wherein the volcanic glass fine powder has a specific surface area of 5000 cm as measured by the BET method. 2 / g or more 40000cm 2 / g or less.
[0034] According to this embodiment, the amount of tobermorite produced is increased, so that a hardened body with high strength can be obtained, and further, the volcanic glass powder can be easily dispersed in the raw material, so that a homogeneous raw material can be obtained.
[0035] A third aspect is a method for producing a hardened body according to the first or second aspect, wherein the fine volcanic glass powder has an average particle size of 1 μm or more and 50 μm or less.
[0036] According to this embodiment, the production of fine volcanic glass powder can be easily carried out, the amount of tobermorite produced can be increased, and the volcanic glass powder can be easily dispersed in the raw materials, making it possible to obtain homogeneous raw materials.
[0037] A fourth aspect is the method for producing a hardened body according to any one of the first to third aspects, wherein the silica source material further contains silica stone powder.
[0038] According to this embodiment, the combined use of volcanic glass powder and silica powder increases the amount of tobermorite produced, making it possible to obtain a hardened body with high strength.
[0039] A fifth aspect is a method for producing a hardened body according to the fourth aspect, wherein a weight ratio of the silica powder to the volcanic glass fine powder contained in the silica source material is silica powder:volcanic glass fine powder=1:3 to 3:1.
[0040] According to this embodiment, the combined use of volcanic glass powder and silica powder increases the amount of tobermorite produced, making it possible to obtain a hardened body with high strength.
[0041] A sixth aspect is the method for producing a cured body according to the fourth or fifth aspect, wherein a ratio of alumina to silica contained in the silica source material is Al2O3 / SiO2=more than 0.03 and not more than 0.16.
[0042] According to this embodiment, the combined use of volcanic glass powder and silica powder increases the amount of tobermorite produced, making it possible to obtain a hardened body with high strength.
[0043] The hardened body according to the seventh embodiment contains Al-substituted tobermorite, which is a reaction product of a calcium source material and an amorphous volcanic glass fine powder.
[0044] According to this embodiment, by using amorphous volcanic glass powder, the amount of ion elution is high, and the content of tobermorite is large, so that a hardened body with high strength is obtained.
[0045] An eighth aspect is the hardened body according to the seventh aspect, further comprising normal tobermorite which is a reaction product of the calcium source material and silica powder.
[0046] According to this embodiment, the combined use of volcanic glass powder and silica powder results in a high tobermorite content, resulting in a hardened body with high strength.
[0047] A construction material according to a ninth aspect includes the hardened body according to the seventh or eighth aspect and a functional part.
[0048] According to this embodiment, the content of tobermorite is high, resulting in a building material with high strength. EXAMPLES
[0049] Example 1 A raw material was prepared by mixing 5 parts by weight of cement, which is a calcium source material, and 5 parts by weight of a silica source material. The total amount (100% by weight) of the silica source material was amorphous volcanic glass fine powder (average particle size 38.9 μm). Next, 10 parts by weight of water was mixed with the raw material, and the mixture was cured in an autoclave at 165°C for 8 hours under hydrothermal conditions of a saturated vapor pressure of 5 to 6 atm to form a plate-shaped hardened body.
[0050] Example 2 A mixture of 75% by weight of fine volcanic glass powder and 25% by weight of silica powder (average particle size 23.5 μm) was used as the silica source material. A hardened body was formed in the same manner as in Example 1 except for this.
[0051] Example 3 A mixture of 50% by weight of fine volcanic glass powder and 50% by weight of silica stone powder was used as the silica source material. A hardened body was formed in the same manner as in Example 1 except for this.
[0052] Example 4 A mixture of 25% by weight of fine volcanic glass powder and 75% by weight of silica powder was used as the silica source material. A hardened body was formed in the same manner as in Example 1 except for this.
[0053] Comparative Example 1 As the silica source material, 100% by weight of silica powder was used. A hardened body was formed in the same manner as in Example 1 except for this.
[0054] For Examples 1 to 4 and Comparative Example, the XRD intensity derived from the tobermorite (002 plane) of the hardened body was measured by X-ray diffraction. The results are shown in Figures 1 and 2. In Figure 1, the horizontal axis shows the Al2O3 / SiO2 ratio of the silica source material, and the vertical axis shows the XRD intensity as the tobermorite intensity. In Figure 2, the horizontal axis shows the SiO2 content of the silica source material, and the vertical axis shows the XRD intensity as the tobermorite intensity.
[0055] As is clear from FIG. 1, Examples 1 to 4 have higher tobermorite strength than Comparative Example 1. Therefore, the amount of tobermorite produced is greater when volcanic glass fine powder is used as the silica source material than when only silica powder is used. Examples 2 to 4 also have higher tobermorite strength than Example 1. Therefore, the amount of tobermorite produced is greater when volcanic glass fine powder and silica powder are used in combination as the silica source material than when only volcanic glass fine powder is used. Example 3 also has the highest tobermorite strength compared to the other Examples. Therefore, the silica source material with an Al2O3 / SiO2 ratio of 0.09 produces the greatest amount of tobermorite, and the amount of tobermorite produced is preferably within the range of an Al2O3 / SiO2 ratio of 0.06 to 0.14.
[0056] As is clear from FIG. 2, Examples 1 to 4 have higher tobermorite strength than Comparative Example 1. Therefore, when the SiO2 content of the silica source material is 75% by weight or more, the amount of tobermorite produced is large. Moreover, Example 3 has the highest tobermorite strength compared to the other Examples. Therefore, when the SiO2 content of the silica source material is about 84%, the amount of tobermorite produced is the largest, and when the SiO2 content is in the range of 80 to 90% by weight, the amount of tobermorite produced is preferably in the range.
[0057] Example 5 As the silica source material, 100% by weight of fine volcanic glass powder having an average particle size of 6.8 μm was used. A hardened body was formed in the same manner as in Example 1, except for this.
[0058] Example 6 As the silica source material, 100% by weight of fine volcanic glass powder having an average particle size of 21.1 μm was used. A hardened body was formed in the same manner as in Example 1 except for this.
[0059] Example 7 As the silica source material, 100% by weight of fine volcanic glass powder having an average particle size of 38.9 μm was used. A hardened body was formed in the same manner as in Example 1 except for this.
[0060] Comparative Example 2 As the silica source material, 100% by weight of silica powder having an average particle size of 23.5 μm was used. A hardened body was formed in the same manner as in Example 1 except for this.
[0061] Comparative Example 3 As the silica source material, 100% by weight of fly ash having an average particle size of 17.3 μm was used. A hardened body was formed in the same manner as in Example 1 except for this.
[0062] For Examples 5 to 7 and Comparative Examples 2 and 3, the XRD intensities derived from the tobermorite (002 plane) of the hardened bodies were measured by X-ray diffraction. The results are shown in Figure 3. In Figure 3, the horizontal axis shows the average particle size of the silica source material, and the vertical axis shows the XRD intensity as the tobermorite intensity.
[0063] 3, Examples 5 to 7 have higher tobermorite strength than Comparative Examples 2 and 3. Therefore, when a fine volcanic glass powder having an average particle size of 6.8 to 38.9 μm is used as the silica source material, the amount of tobermorite produced is equal to or greater than that of fly ash, and is greater than that of silica stone powder.
Claims
1. A method for producing a hardened body by hardening a raw material containing a calcium source material and a silica source material, comprising: The silica source material contains fine volcanic glass powder, and the fine volcanic glass powder is amorphous. A method for producing a hardened body.
2. The volcanic glass fine powder has a specific surface area of 5000 cm as measured by the BET method. 2 / g or more 40000cm 2 / g or less, A method for producing the cured product according to claim 1.
3. The volcanic glass fine powder has an average particle size of 1 μm or more and 50 μm or less. A method for producing the cured product according to claim 1.
4. The silica source material further contains silica powder. A method for producing the cured product according to claim 1.
5. the weight ratio of the silica powder to the fine volcanic glass powder contained in the silica source material is silica powder: volcanic glass fine powder=1:3 to 3:1; A method for producing the cured product according to claim 4.
6. The ratio of alumina to silica contained in the silica source material is Al 2 O 3 / SiO 2 = greater than 0.03 and equal to or less than 0.16; A method for producing the cured product according to claim 4.
7. Contains Al-substituted tobermorite, which is a reaction product of a calcium source material and amorphous volcanic glass fine powder. Hardened body.
8. The composition further contains tobermorite, which is a reaction product of the calcium source material and silica powder. The hardened body according to claim 7.
9. The cured body according to claim 7 or 8 and a functional part are provided. Building materials.