Adhesive and adhesive sheet

The adhesive sheet with microcapsules and polyurea shell in an acrylic resin ensures stable initial adhesion and easy peeling, addressing the challenges of maintaining adhesive strength and residue-free removal.

JP2024172744AInactive Publication Date: 2024-12-12TOPPAN EDGE INC +2

Patent Information

Application Number
JP2023090671
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing adhesive sheets struggle with maintaining high adhesive strength initially but are difficult to peel off without leaving residue, and require special operations or vibrations for easy removal.

Method used

An adhesive sheet with microcapsules containing a plasticizer and a polyurea shell, dispersed in an acrylic resin with specific glass transition temperature, allowing for stable adhesion and easy peeling by pressure without special operations.

Benefits of technology

The adhesive sheet maintains high adhesive strength initially and can be easily peeled off at any desired time without leaving residue, enhancing usability and ease of application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024172744000007
    Figure 2024172744000007
  • Figure 2024172744000001
    Figure 2024172744000001
  • Figure 2024172744000002
    Figure 2024172744000002
Patent Text Reader

Abstract

To provide an adhesive sheet having an adhesive layer which can maintain high adhesive force in an initial stage after being bonded to an object, and can be easily peeled without leaving an adhesive layer on the object, without requiring special operation, in a stage of being peeled from the object, and an adhesive for forming the adhesive layer.SOLUTION: There is provided an adhesive in which microcapsules are dispersed, wherein the adhesive contains an acrylic resin (A) which has a structural unit (a1) that has Tg of -60 to -40°C and is derived from an alkyl (meth)acrylate ester and a structural unit (a2) derived from (meth)acrylic acid, in which an alkyl group has 4 or more carbon atoms, in the acrylic resin (A), a ratio of the amount of the structural unit (a1) with respect to the total amount of the structural units is 50 to 99.5 mass%, a ratio of the amount of the structural unit (a2) is 0.5 to 5 mass%, and the microcapsules have outer shells composed of polyurea, and include a plasticizer (Z) which is liquid at normal temperature.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive and a pressure-sensitive adhesive sheet. [Background technology]

[0002] Adhesive sheets having an adhesive layer are widely used as adhesive labels, adhesive tapes, etc. In some adhesive sheets, in the initial stage after application to an object to which the sheet is applied, it is desired that the sheet can be stably attached with high adhesive strength, but when the sheet is peeled off from the object, the adhesive layer does not remain on the object and the sheet can be easily peeled off.

[0003] As an adhesive sheet that can be easily peeled off from an object, one has been disclosed in which microcapsules are dispersed in an acrylic adhesive, the microcapsules encapsulate a crosslinking agent and a softener for the acrylic adhesive, and the adhesive layer is formed using an adhesive composition that is broken by pressure (see Patent Document 1). When this adhesive sheet is used and is applied to an object, the microcapsules are broken by pressure applied to the adhesive layer, and the crosslinking agent released from the microcapsules spreads into the adhesive layer together with the softener, crosslinking the acrylic adhesive, and it is presumed that the adhesiveness of the adhesive layer gradually disappears and the cohesiveness improves, making it easier to peel off the adhesive sheet from the object.

[0004] As an adhesive that can be easily peeled off from an object, there has been disclosed an adhesive in which microcapsules are dispersed, the microcapsules encapsulate a softener for the adhesive, and the microcapsules are destroyed by application of frequency vibration (see Patent Document 2). When this adhesive is used, it is presumed that the microcapsules are destroyed by application of frequency vibration to the adhesive, and the softener released from the microcapsules permeates the adhesive, reducing the adhesive strength of the adhesive and making it easier to peel off the adhesive from the object. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-34051 [Patent Document 2] JP 2001-214148 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the adhesive sheet disclosed in Patent Document 1 has a problem in that it takes a long time for the adhesive layer to lose its adhesiveness, and therefore the adhesive sheet cannot be easily peeled off at a desired timing. Furthermore, since the adhesive is crosslinked by the crosslinking agent, and the adhesive strength of the adhesive sheet increases after the adhesive sheet is applied to an object, there is a problem in that when the adhesive sheet is peeled off from the object, cohesive failure occurs in the adhesive layer, and part of the adhesive layer is likely to remain on the object.

[0007] On the other hand, the adhesive disclosed in Patent Document 2 has the problem that it is necessary to apply a frequency vibration to it in order to facilitate peeling it off from an object, and therefore a special operation is required.

[0008] The present invention aims to provide an adhesive sheet having an adhesive layer, which can maintain a stable attached state with high adhesive strength in the initial stage after application to an object, and which, when peeled off from the object at any desired time, can be easily peeled off without requiring any special operation and without leaving the adhesive layer on the object, and an adhesive for forming the adhesive layer. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention employs the following configuration. [1] An adhesive having microcapsules dispersed therein, the adhesive comprising an acrylic resin (A) having a glass transition temperature of -60 to -40°C, the acrylic resin (A) having a structural unit (a1) derived from an alkyl (meth)acrylate ester and a structural unit (a2) derived from (meth)acrylic acid, the alkyl group constituting the alkyl ester in the alkyl (meth)acrylate ester having 4 or more carbon atoms, the proportion of the amount of the structural unit (a1) relative to the total amount of the structural units in the acrylic resin (A) being 50 to 99.5% by mass, the proportion of the amount of the structural unit (a2) relative to the total amount of the structural units in the acrylic resin (A) being 0.5 to 5% by mass, the outer shell of the microcapsules being made of polyurea, and the microcapsules encapsulating a plasticizer (Z) that is liquid at room temperature.

[0010] [2] The pressure-sensitive adhesive according to [1], wherein the ratio of the content of the plasticizer (Z) to the content of the acrylic resin (A) in the pressure-sensitive adhesive is 0.5 to 30 mass %. [3] An adhesive sheet having an adhesive layer, the adhesive sheet comprising a substrate and the adhesive layer provided on the substrate, the adhesive layer being formed using the adhesive described in [1] or [2] and containing the microcapsules. [4] The pressure-sensitive adhesive sheet according to [3], wherein the ratio of the median diameter of the microcapsules to the thickness of the pressure-sensitive adhesive layer is 65 to 105%. Effect of the Invention

[0011] According to the present invention, there is provided an adhesive sheet having an adhesive layer, which can maintain a stable attached state with high adhesive strength in the initial stage after application to an object, and which, when peeled off from the object at any desired time, can be easily peeled off without requiring special operations and without leaving the adhesive layer on the object, and an adhesive for forming the adhesive layer. [Brief description of the drawings]

[0012] [Figure 1] 1 is a cross-sectional view illustrating an example of a pressure-sensitive adhesive sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] ◇Adhesive An adhesive according to one embodiment of the present invention is an adhesive having microcapsules dispersed therein, the adhesive comprising an acrylic resin (A) having a glass transition temperature of −60 to −40° C., the acrylic resin (A) having a structural unit (a1) derived from an alkyl (meth)acrylate ester and a structural unit (a2) derived from (meth)acrylic acid, the alkyl group constituting the alkyl ester in the alkyl (meth)acrylate ester having 4 or more carbon atoms, the proportion of the amount of the structural unit (a1) relative to the total amount of the structural units in the acrylic resin (A) being 50 to 99.5% by mass, the proportion of the amount of the structural unit (a2) relative to the total amount of the structural units in the acrylic resin (A) being 0.5 to 5% by mass, the shells of the microcapsules being made of polyurea, and the microcapsules encapsulating a plasticizer (Z) that is liquid at room temperature.

[0014] The adhesive of the present embodiment contains dispersed microcapsules and acrylic resin (A) as described above, and the microcapsules contain a plasticizer (Z) that is liquid at room temperature by an outer shell made of polyurea, and the acrylic resin (A) has a glass transition temperature in a specific range and has a specific range of types of structural units in a specific range of amounts. The adhesive layer formed using such an adhesive can maintain a stable attached state with high adhesive strength at the initial stage after application to the object. On the other hand, at the stage of peeling from the object at any desired timing, it can be easily peeled off without remaining on the object without requiring special operations. The adhesive sheet having such an adhesive layer can also maintain a stable attached state with high adhesive strength at the initial stage after application when applied to an object by the adhesive layer therein, and can be easily peeled off without remaining on the object without requiring special operations at the stage of peeling from the object at any desired timing.

[0015] <<Microcapsules>> The adhesive contains microcapsules in a dispersed state. The outer shell of the microcapsule is made of polyurea. The outer shell is also called a wall material, and in this embodiment, it can be said that a constituent component of the wall material is polyurea.

[0016] The polyurea is not particularly limited as long as it is a polycondensation product of a polyisocyanate compound having two or more isocyanate groups in one molecule and a polyamine compound having two or more amino groups in one molecule.

[0017] The microcapsules are pressure sensitive and are broken by the application of pressure. When the adhesive sheet is applied to an object, in the initial stage after application, unless the adhesive sheet (microcapsules) are excessively pressurized, the adhesive sheet can maintain a more stable attached state with high adhesive strength. On the other hand, in the stage of peeling the adhesive sheet from the object, the microcapsules are quickly broken by pressure application, and the released plasticizer (Z) reduces the adhesive strength of the adhesive layer as described below, so that the adhesive sheet can be peeled off more easily without the adhesive layer remaining on the object. That is, peeling at this time typically occurs at the interface between the object and the adhesive layer.

[0018] <Polyisocyanate compounds> The number of isocyanate groups that the polyisocyanate compound has in one molecule is not particularly limited as long as it is two or more, but it is preferable that the number is two or three.

[0019] The polyisocyanate compound is preferably a trimethylolpropane adduct of a polyisocyanate compound (sometimes referred to as a "polyisocyanate compound-TMP adduct" in this specification) and a polymethylene polyphenyl polyisocyanate (sometimes referred to as a "polymeric MDI" in this specification). That is, the polyurea preferably contains both a polycondensate of a polyisocyanate compound-TMP adduct and a polyamine compound, and a polycondensate of a polymeric MDI and a polyamine compound. When the microcapsule has an outer shell made of such polyurea, the adhesive sheet can maintain a more stable attached state with high adhesive strength at the initial stage after attachment when the adhesive sheet is attached to the object. On the other hand, at the stage of peeling the adhesive sheet from the object, the adhesive sheet can be peeled off more easily without leaving any adhesive layer on the object.

[0020] [Polyisocyanate compound-TMP adduct] Among the polyisocyanate compound-TMP adducts, examples of the aliphatic polyisocyanate compound-TMP adducts (trimethylolpropane adducts of an aliphatic polyisocyanate compound) include aliphatic diisocyanate-TMP adducts such as a trimethylolpropane adduct of pentamethylene diisocyanate, a trimethylolpropane adduct of hexamethylene diisocyanate, a trimethylolpropane adduct of 2,4,4-trimethylhexamethylene diisocyanate, a trimethylolpropane adduct of isophorone diisocyanate, a trimethylolpropane adduct of dicyclohexylmethane-4,4'-diisocyanate, and a trimethylolpropane adduct of dicyclohexylmethane-2,4'-diisocyanate.

[0021] Among the polyisocyanate compound-TMP adducts, examples of aromatic polyisocyanate compound-TMP adducts (trimethylolpropane adducts of aromatic polyisocyanate compounds) include aromatic diisocyanate-TMP adducts such as a trimethylolpropane adduct of tolylene-2,4-diisocyanate, a trimethylolpropane adduct of tolylene-2,6-diisocyanate (in this specification, a trimethylolpropane adduct of tolylene diisocyanate may be referred to as a "TDI-TMP adduct"), a trimethylolpropane adduct of xylylene-1,3-diisocyanate, and a trimethylolpropane adduct of xylylene-1,4-diisocyanate.

[0022] The polyisocyanate compound-TMP adduct used when forming the polyurea (in other words, a structural unit derived from the polyisocyanate compound-TMP adduct that the polyurea has) may be only one type or two or more types, and when two or more types are used, the combination and ratio thereof can be selected arbitrarily.

[0023] [Polymeric MDI] The polymeric MDI is represented by the following general formula (P1).

[0024] [ka] (In the formula, n is an integer of 0 or more.)

[0025] In the general formula (P1), n ​​may be an integer of 0 or more, for example, 0-300.

[0026] The NCO content of the polymeric MDI can be appropriately adjusted and may be, for example, 30 to 33% by mass.

[0027] Polymeric MDI is liquid at room temperature, and its viscosity at 25° C. is not particularly limited, but is preferably 150 to 250 mPa·s. In this specification, "room temperature" means a temperature that is neither particularly cooled nor heated, that is, an ordinary temperature, and examples thereof include temperatures of 15 to 25°C.

[0028] The polymeric MDI used in forming the polyurea (in other words, the structural units of the polyurea derived from the polymeric MDI) may be one type or two or more types, and when two or more types are used, the combination and ratio thereof can be selected arbitrarily.

[0029] The polyurea may have, as the structural unit derived from the polyisocyanate compound, only one type of structural unit derived from a polyisocyanate compound-TMP adduct and two or more types of structural units derived from polymeric MDI, or may have two or more types of structural units derived from a polyisocyanate compound-TMP adduct and only one type of structural unit derived from polymeric MDI, or may have only one type of structural unit derived from a polyisocyanate compound-TMP adduct and only one type of structural unit derived from polymeric MDI, or may have two or more types of structural units derived from a polyisocyanate compound-TMP adduct and only one type of structural unit derived from polymeric MDI.

[0030] In terms of high reactivity in a polycondensation reaction with the polyamine compound and ability to form a more robust polyurea, the polyisocyanate compound-TMP adduct is preferably an aromatic polyisocyanate compound-TMP adduct, more preferably an aromatic diisocyanate-TMP adduct, and even more preferably a TDI-TMP adduct.

[0031] In the polyurea, the amount of the structural unit derived from the polyisocyanate compound-TMP adduct relative to the amount of the structural unit derived from the polymeric MDI is preferably 0.6 to 12 times by mass, more preferably 0.8 to 10 times by mass, and even more preferably 1 to 8.5 times by mass. By using such a polyurea, the effect of the present invention is further enhanced. That is, when the pressure-sensitive adhesive sheet is applied to an object, in the initial stage after application, the applied state can be maintained more stably with high adhesive strength, and in the stage of peeling the pressure-sensitive adhesive sheet from the object, the pressure-sensitive adhesive sheet can be peeled off more easily without requiring special operations and without leaving any pressure-sensitive adhesive layer on the object.

[0032] <Polyamine compounds> The number of amino groups in one molecule of the polyamine compound is not particularly limited as long as it is 2 or more, but is preferably 2 to 6, more preferably 2 to 5, even more preferably 2 to 4, and particularly preferably 2 or 3.

[0033] The polyamine compound is preferably an organic polyamine compound. Preferred examples of the organic polyamine compounds include aliphatic polyamine compounds having a structure in which two or more hydrogen atoms (-H) of an aliphatic hydrocarbon are substituted with amino groups (-NH2); and NH-substituted aliphatic polyamine compounds having a structure in which one or more methylene groups (-CH2-) of the aliphatic polyamine compounds are substituted with a group represented by the formula "-NH-".

[0034] The polyamine compound is preferably an aliphatic polyamine compound having a cyclic aliphatic hydrocarbon group, more preferably an aliphatic polyamine compound having both a cyclic aliphatic hydrocarbon group and a chain aliphatic hydrocarbon group, and further preferably an organic polyamine compound having a structure in which hydrogen atoms bonded to two or more different carbon atoms constituting the ring skeleton of a cycloalkane are substituted with aminoalkyl groups. An example of such an organic polyamine compound is 1,3-bisaminomethylcyclohexane.

[0035] The amine compound used when forming the polyurea (in other words, the structural unit of the polyurea derived from the amine compound) may be only one type, or may be two or more types, and when two or more types are used, the combination and ratio thereof can be selected arbitrarily.

[0036] It is particularly preferable that the polyurea contains both a polycondensate of a polyisocyanate compound-TMP adduct and an aliphatic polyamine compound having both a cyclic aliphatic hydrocarbon group and a chain aliphatic hydrocarbon group, and a polycondensate of polymeric MDI and an aliphatic polyamine compound having both a cyclic aliphatic hydrocarbon group and a chain aliphatic hydrocarbon group. In such polyurea, the ratio of the total amount of the constituent units derived from the polyisocyanate compound-TMP adduct, the constituent units derived from the polymeric MDI, and the constituent units derived from the aliphatic polyamine compound having both a cyclic aliphatic hydrocarbon group and a chain aliphatic hydrocarbon group to the total amount of the constituent units (([amount of constituent units derived from the polyisocyanate compound-TMP adduct in the polyurea (parts by mass)] + [amount of constituent units derived from the polymeric MDI in the polyurea (parts by mass)] + [amount of constituent units derived from the aliphatic polyamine compound having both a cyclic aliphatic hydrocarbon group and a chain aliphatic hydrocarbon group in the polyurea (parts by mass)]) / [total amount of constituent units in the polyurea (parts by mass)] × 100) is preferably 80 mass% or more, more preferably 90 mass% or more, and may be, for example, any one of 95 mass% or more, 97 mass% or more, and 99 mass% or more. When the ratio is equal to or greater than the lower limit, when the adhesive sheet is applied to an object, the adhesive state can be maintained more stably with high adhesive strength in the initial stage after application, and when the adhesive sheet is peeled off from the object, the adhesive sheet can be peeled off more easily without the need for special operations and without leaving any adhesive layer on the object. On the other hand, the proportion is 100% by mass or less.

[0037] <Plasticizer (Z)> The microcapsules encapsulate a plasticizer (Z). That is, the plasticizer (Z) is the core material of the microcapsules. The plasticizer (Z) encapsulated in the microcapsules is not particularly limited as long as it is liquid at room temperature.

[0038] The plasticizer (Z) is encapsulated in microcapsules in the adhesive and in the adhesive layer under normal conditions, and does not act on the adhesive and the adhesive layer. On the other hand, when the microcapsules are broken and the plasticizer (Z) is released into the adhesive layer by a simple pressure application to the adhesive layer, such as rubbing or pressing with a finger or rubbing or pressing with any tool, the adhesive strength of the adhesive layer is reduced by the action of the plasticizer (Z). It is presumed that the plasticizer (Z) released into the adhesive layer penetrates into the structure of the acrylic resin (A) in the adhesive layer and reduces the adhesive strength of the adhesive layer.

[0039] Examples of the plasticizer (Z) include esters such as monoesters, diesters, and triesters of monobasic acids having 1 to 18 carbon atoms or polybasic acids having 1 to 18 carbon atoms and polyalkylene glycols or monohydric alcohols having 20 or less carbon atoms other than polyalkylene glycols; esters of saturated fatty acids having 12 to 18 carbon atoms or unsaturated fatty acids having 12 to 18 carbon atoms and polyalkylene glycols or dihydric to tetrahydric alcohols other than polyalkylene glycols; esters such as diesters, triesters, and tetraesters of hydroxy acids and monobasic acids or alcohols; fatty acid esters in which the unsaturated site is epoxidized with a peroxide or the like; and phosphate esters.

[0040] Examples of esters of monobasic acids having 1 to 18 carbon atoms or polybasic acids having 1 to 18 carbon atoms and monohydric alcohols having 20 or less carbon atoms other than polyalkylene glycols include isostearyl laurate, isopropyl myristate, cetyl myristate, octyldodecyl myristate, isostearyl palmitate, isocetyl stearate, octyldodecyl oleate, diisostearyl adipate, diisocetyl sebacate, trioleyl trimellitate, and triisocetyl trimellitate.

[0041] Examples of esters of monobasic acids having 1 to 18 carbon atoms or polybasic acids having 1 to 18 carbon atoms and polyalkylene glycols include polyethylene glycol dihexylate, polyethylene glycol di-2-ethylhexylate, polyethylene glycol dilaurate, polyethylene glycol dioleate, and dipolyethylene glycol methyl ether adipate.

[0042] Examples of the saturated fatty acid having 12 to 18 carbon atoms or the unsaturated fatty acid having 12 to 18 carbon atoms constituting the ester of a saturated fatty acid having 12 to 18 carbon atoms or an unsaturated fatty acid having 12 to 18 carbon atoms and a polyalkylene glycol or a dihydric, dihydric, or tetrahydric alcohol other than a polyalkylene glycol include lauric acid, myristic acid, palmitic acid, stearic acid, isopalmitic acid, isostearic acid, myristoleic acid, oleic acid, linoleic acid, and linolenic acid. The polyalkylene glycol constituting the ester may be a known one, and specific examples thereof include polyethylene glycol, polypropylene glycol, polybutylene glycol, polyoxyethylene polyoxypropylene glycol, and the like. Examples of the dihydric to tetrahydric alcohol other than the polyalkylene glycol that constitutes the ester include ethylene glycol, propylene glycol, glycerin, trimethylolpropane, pentaerythritol, and sorbitan.

[0043] Examples of esters of hydroxy acids and monobasic acids or alcohols include octyldodecyl lactate, diisostearyl malate, methyl 2-hydroxymyristate, 2-ethylhexyl 12-hydroxystearate, ethyl ricinoleate, methyl o-acetylricinoleate, butyl o-acetylricinoleate, triethyl citrate, tributyl o-acetylcitrate, and tri(2-ethylhexyl) o-acetylcitrate.

[0044] Examples of fatty acid esters in which the unsaturated site is epoxidized with a peroxide or the like include epoxidized fats and oils such as epoxidized soybean oil, epoxidized linseed oil, and epoxidized cottonseed oil; and esters of compounds in which unsaturated fatty acids having 8 to 18 carbon atoms are epoxidized and linear or branched alcohols having 1 to 6 carbon atoms.

[0045] Examples of phosphate esters include esters of phosphorous acid or phosphoric acid and linear or branched alcohols having a carbon number of 2 to 18. More specific examples of such esters include tributyl phosphate, 2-ethylhexyl acid phosphate, oleyl acid phosphate, and ethylene glycol acid phosphate.

[0046] Among the above, preferred examples of the plasticizer (Z) include ether ester plasticizers (plasticizers having both an ether bond and an ester bond); ester plasticizers such as fatty acid esters (plasticizers having an ester bond but no ether bond); and the like.

[0047] The molecular weight of the plasticizer (Z) is preferably 100-700.

[0048] The plasticizer (Z) encapsulated in the microcapsules may be of only one type, or may be of two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0049] In the pressure-sensitive adhesive, the ratio of the content of the plasticizer (Z) to the content of the acrylic resin (A) ([content of the plasticizer (Z) in the pressure-sensitive adhesive (parts by mass)] / [content of the acrylic resin (A) in the pressure-sensitive adhesive (parts by mass)]×100) is preferably 0.5 to 30% by mass, more preferably 1.5 to 20% by mass, and even more preferably 3 to 10% by mass. When the ratio is equal to or greater than the lower limit, the pressure-sensitive adhesive sheet can be more easily peeled off from the object after being attached to the object without requiring any special operation and without leaving any pressure-sensitive adhesive layer on the object. When the ratio is equal to or less than the upper limit, the pressure-sensitive adhesive sheet can be more stably maintained in an attached state with high adhesive strength in the initial stage after attachment when attached to the object.

[0050] In the adhesive in which the ratio of the plasticizer (Z) content to the acrylic resin (A) content satisfies the above-mentioned condition, it is preferable that the plasticizer (Z) encapsulated in the microcapsules satisfies the above-mentioned ratio (the ratio of the plasticizer (Z) content to the acrylic resin (A) content in the adhesive).

[0051] In the pressure-sensitive adhesive, the ratio of the microcapsule content to the acrylic resin (A) content ([microcapsule content in pressure-sensitive adhesive (parts by mass)] / [acrylic resin (A) content in pressure-sensitive adhesive (parts by mass)]×100) is preferably 1.5 to 40 mass%, more preferably 2.5 to 30 mass%, and even more preferably 5 to 20 mass%. When the ratio is equal to or greater than the lower limit, the pressure-sensitive adhesive sheet can be more easily peeled off from the object after being attached to the object without requiring any special operation and without leaving any pressure-sensitive adhesive layer on the object. When the ratio is equal to or less than the upper limit, the pressure-sensitive adhesive sheet can be more stably maintained in an attached state with high adhesive strength in the initial stage after attachment when attached to the object. Here, the "microcapsule content" may be equivalent to the total content of components other than water in an aqueous dispersion of microcapsules, for example, when the aqueous dispersion of microcapsules described below is used in the production of an adhesive.

[0052] The median diameter of the microcapsules is preferably from 6.5 to 19 μm, more preferably from 9 to 16 μm, and may be, for example, any one of from 9 to 14 μm and from 11 to 16 μm. By having the median diameter of the microcapsules be equal to or greater than the lower limit, it becomes easy to make the size of the microcapsules close to the thickness of the adhesive layer described below within an appropriate range. In this case, after the adhesive sheet is attached to an object, when it is peeled off from the object, the adhesive force of the adhesive layer to the object can be more easily reduced without the need for special operations, and the adhesive sheet can be more easily peeled off from the object without any adhesive layer remaining on the object. By setting the median diameter of the microcapsules to the upper limit or less, it becomes easy to make the size of the microcapsules equal to or smaller than the thickness of the adhesive layer described below. In that case, when the adhesive sheet is applied to an object, the adhesive state can be maintained more stably with higher adhesive strength in the initial stage after application.

[0053] In this specification, unless otherwise specified, the "median diameter" refers to the median diameter of the volume particle size distribution of particles measured using a particle size distribution analyzer.

[0054] In the microcapsules, the ratio of the thickness of the outer shell to the particle diameter of the microcapsule ([thickness of the outer shell of the microcapsule (μm)] / [particle diameter of the microcapsule (μm)]×100) is preferably 3 to 20%, more preferably 4 to 18%, and even more preferably 5 to 15%. When the ratio is equal to or greater than the lower limit, when the adhesive sheet is applied to an object, the seepage of the plasticizer (Z) encapsulated in the microcapsules from the microcapsules can be more highly suppressed in the initial stage after application, and the applied state can be maintained more stably with higher adhesive strength. When the ratio is equal to or less than the upper limit, when the adhesive sheet is applied to an object and then peeled off from the object, a larger amount of the microcapsules can be destroyed by applying pressure to the adhesive sheet, and a larger amount of the encapsulated plasticizer (Z) can be released from the microcapsules, and the adhesive sheet can be more easily peeled off.

[0055] The thickness of the outer shell of the microcapsule and the particle size of the microcapsule can be measured by preparing a cross section of the microcapsule, which is cooled (frozen) to an extremely low temperature using a refrigerant such as liquid nitrogen, and measuring the cross section using a scanning electron microscope, etc. When preparing the cross section of the microcapsule, for example, a coating of the water dispersion of the microcapsule described later may be dried, the obtained dried product is cooled, and the cooled product is cut to prepare the cross section of the microcapsule.

[0056] When calculating the ratio of the thickness of the outer shell of a microcapsule to the particle diameter of the microcapsule using the above method, as described later in the Examples, it is preferable to calculate the ratio for multiple microcapsules in the cross section and use the average of the multiple calculated values ​​as the ratio. In this case, as described later in the examples, it is preferable to use an average value obtained by excluding the upper calculated values ​​(the calculated values ​​from the maximum calculated value to a specific size in ascending order) and the lower calculated values ​​(the calculated values ​​from the minimum calculated value to a specific size in ascending order) among the calculated values ​​of the ratio for a plurality of microcapsules. By doing so, the ratio (average value) can be calculated with higher accuracy. In this case, as described later in the examples, it is preferable to exclude more upper calculated values ​​than lower calculated values. In this way, the ratio (average value) can be calculated with higher accuracy. The reason is that in microcapsules cut near an end far away from the center of the microcapsule, the ratio becomes unduly large without reflecting the actual situation, and such a cross section is easy to create when creating a cross section of the microcapsule. By eliminating more calculated values ​​based on the cross section of such a microcapsule, a highly accurate average value can be calculated.

[0057] The microcapsules can be produced by a known method. For example, when the interfacial polycondensation method is applied, the microcapsules can be produced by a production method including a step of adding a second solution containing a plasticizer (Z) and the polyisocyanate compound to a first solution containing water and an emulsifier to obtain an emulsion (sometimes abbreviated as "emulsification step" in this specification), and a step of adding the polyamine compound to the emulsion to carry out a polycondensation reaction (sometimes abbreviated as "polycondensation step" in this specification). In this case, the microcapsules are obtained as a water dispersion by carrying out the polycondensation step. However, the interfacial polycondensation method is not limited to this.

[0058] The obtained microcapsules can be used for the production of a pressure-sensitive adhesive, for example, in the state of a dispersion dispersed in a reaction liquid obtained by carrying out a reaction for producing the microcapsules, or in the state of a post-treated dispersion obtained by carrying out a known post-treatment on the dispersion. Examples of such dispersions include the aqueous dispersion of microcapsules obtained in the polycondensation step in the above-mentioned interfacial polycondensation method. The obtained microcapsules can be used, for example, in the form of a dried product obtained by removing them from the reaction solution, washing them by a known method if necessary, and then drying them, for producing an adhesive.

[0059] <<Acrylic resin (A)>> The acrylic resin (A) contained in the pressure-sensitive adhesive has a structural unit (a1) derived from an alkyl (meth)acrylate ester and a structural unit (a2) derived from (meth)acrylic acid. The acrylic resin (A) acts as an adhesive resin.

[0060] In this specification, the term "(meth)acrylic acid" is a concept that encompasses both "acrylic acid" and "methacrylic acid".

[0061] The alkyl group constituting the alkyl ester in the (meth)acrylic acid alkyl ester that forms the acrylic resin (A) (in other words, the alkyl ester in the structural unit (a1); the same applies below) has 4 or more carbon atoms, and preferably 4 to 12 carbon atoms. The alkyl group having 4 or more carbon atoms may be any of linear, branched, and cyclic, and may have both a linear structure (linear structure, branched structure) and a cyclic structure.

[0062] Examples of the (meth)acrylic acid alkyl ester that forms the acrylic resin (A) include n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, undecyl (meth)acrylate, and lauryl (meth)acrylate.

[0063] The (meth)acrylic acid alkyl ester forming the acrylic resin (A) may be one type or two or more types, and when two or more types are used, the combination and ratio thereof can be selected arbitrarily. This is the same as saying that the structural unit (a1) in the acrylic resin (A) may be one type or two or more types, and when two or more types are used, the combination and ratio thereof can be selected arbitrarily.

[0064] The acrylic resin (A) may have, as the structural unit (a2), either a structural unit derived from acrylic acid or a structural unit derived from methacrylic acid, or may have both.

[0065] In the acrylic resin (A), the ratio of the amount of the structural unit (a1) to the total amount of the structural units ([amount of the structural unit (a1) in the acrylic resin (A) (parts by mass)] / [total amount of the structural units in the acrylic resin (A) (parts by mass)] × 100) is 50 to 99.5% by mass, and may be, for example, any of 65 to 99.5% by mass, 80 to 99.5% by mass, and 90 to 99.5% by mass, any of 50 to 95% by mass, and 50 to 80% by mass, or 65 to 95% by mass. When the ratio is equal to or greater than the lower limit, when the pressure-sensitive adhesive sheet is applied to an object, the pressure-sensitive adhesive sheet can maintain a high adhesive force to the object at a stage where the microcapsules are not destroyed, and a stable applied state can be maintained. When the ratio is equal to or less than the upper limit, the effect obtained by the acrylic resin (A) having a structural unit other than the structural unit (a1), such as the structural unit (a2), is further enhanced.

[0066] In the acrylic resin (A), the ratio of the amount of the structural unit (a2) to the total amount of the structural units ([amount of the structural unit (a2) in the acrylic resin (A) (parts by mass)] / [total amount of the structural units in the acrylic resin (A) (parts by mass)]×100) is 0.5 to 5% by mass, and may be, for example, any of 0.5 to 3.5% by mass and 0.5 to 2.5% by mass. When the ratio is equal to or greater than the lower limit, cohesive force can be imparted to the adhesive, and when the adhesive sheet is applied to an object, the adhesive state can be stably maintained at a stage where the microcapsules are not destroyed. When the ratio is equal to or less than the upper limit, the flexibility of the adhesive can be maintained, and when the adhesive sheet is applied to an object, the adhesive sheet can maintain high adhesive strength to the object at a stage where the microcapsules are not destroyed. In addition, the effect obtained by the acrylic resin (A) having a structural unit other than the structural unit (a2), such as the structural unit (a1), is further enhanced.

[0067] The acrylic resin (A) may or may not have a structural unit (a3) ​​that does not fall under either the structural unit (a1) or the structural unit (a2), as long as the effects of the present invention are not impaired. By making the acrylic resin (A) have the structural unit (a3), the properties of the acrylic resin (A) can be adjusted.

[0068] The monomer from which the structural unit (a3) ​​is derived is a monomer other than the above-mentioned (meth)acrylic acid alkyl ester in which the alkyl group constituting the alkyl ester has 4 or more carbon atoms, and (meth)acrylic acid, and is not particularly limited so long as it is copolymerizable with both the above-mentioned (meth)acrylic acid alkyl ester and (meth)acrylic acid.

[0069] Examples of the other monomers include (meth)acrylic acid alkyl esters in which the alkyl group constituting the alkyl ester has 1 to 3 carbon atoms; (meth)acrylic acid hydroxyalkyl esters; and other (meth)acrylic acid esters that do not fall into either the (meth)acrylic acid alkyl esters or the (meth)acrylic acid hydroxyalkyl esters.

[0070] Examples of the (meth)acrylic acid alkyl ester in which the alkyl group has 1 to 3 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and isopropyl (meth)acrylate. Examples of the hydroxyalkyl (meth)acrylate ester include compounds having a structure in which one hydrogen atom in the alkyl group constituting the alkyl ester is substituted with a hydroxyl group (e.g., hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, etc.) in either the alkyl (meth)acrylate ester in which the alkyl group has 4 or more carbon atoms or the alkyl (meth)acrylate ester in which the alkyl group has 1 to 3 carbon atoms. Examples of the other (meth)acrylic acid esters include aralkyl (meth)acrylic acid esters such as benzyl (meth)acrylate.

[0071] In the acrylic resin (A), the ratio of the amount of the structural unit (a3) ​​to the total amount of the structural units ([amount of the structural unit (a3) ​​in the acrylic resin (A) (parts by mass)] / [total amount of the structural units in the acrylic resin (A) (parts by mass)]×100) is preferably 0 to 49.5% by mass. The higher this ratio, the stronger the properties obtained by having the structural unit (a3) ​​in the acrylic resin (A). When the ratio is equal to or less than the upper limit, the effect obtained by having the structural units (a1) and (a2) in the acrylic resin (A) is enhanced.

[0072] In the acrylic resin (A), the proportion of the total amount of the structural units (a1), (a2), and (a3) ​​relative to the total amount of structural units (([amount of structural units (a1) in acrylic resin (A) (parts by mass)] + [amount of structural units (a2) in acrylic resin (A) (parts by mass)] + [amount of structural units (a3) ​​in acrylic resin (A) (parts by mass)]) / [total amount of structural units in acrylic resin (A) (parts by mass)] × 100) does not exceed 100% by mass.

[0073] The glass transition temperature of the acrylic resin (A) is −60 to −40° C. and may be, for example, any of −60 to −50° C., −50 to −40° C., and −57 to −47° C. When the glass transition temperature is in such a range, when the pressure-sensitive adhesive sheet is applied to an object, the pressure-sensitive adhesive sheet can maintain a stable applied state with high adhesive strength in the initial stage after application.

[0074] In this specification, the glass transition temperatures of the acrylic resin (A) are all values ​​calculated using the FOX formula. The glass transition temperatures of the homopolymers of the respective monomers used are shown below. [Glass transition temperature of homopolymer of monomer] Homopolymer of 2-ethylhexyl acrylate: -70℃ Butyl acrylate homopolymer: -52℃ Homopolymer of methyl acrylate: 8℃ Homopolymer of methyl methacrylate: 105℃ Acrylic acid homopolymer: 106℃ Homopolymer of methacrylic acid: 186℃

[0075] As described later, when producing the adhesive, it is preferable to use (blend) the acrylic resin (A) in the form of an emulsion. The emulsion of the acrylic resin (A) has good miscibility with the aqueous dispersion of microcapsules, and can disperse the microcapsules with high uniformity in the adhesive. The emulsion of the acrylic resin (A) can be obtained by synthesizing the acrylic resin (A) by a known emulsion polymerization method.

[0076] When the acrylic resin (A) is blended as an emulsion (acrylic resin emulsion) during the production of the pressure-sensitive adhesive, the ratio of the solid content to the total mass of the acrylic resin emulsion ([solid content of the acrylic resin emulsion (parts by mass)]) / [total mass of the acrylic resin emulsion (parts by mass)]×100) is preferably 40 to 65% by mass. By using an acrylic resin emulsion having such a ratio, a pressure-sensitive adhesive having the desired properties can be more easily produced. Here, the term "solid content" refers to a component that is solid at room temperature and normal pressure. In this specification, the above ratio may be simply referred to as "the ratio of the solid content of the acrylic resin emulsion."

[0077] <<Other Ingredients>> The adhesive of this embodiment may or may not contain other components that do not fall under either the microcapsules or the acrylic resin (A), as long as the effects of the present invention are not impaired. The other components contained in the pressure-sensitive adhesive can be arbitrarily selected depending on the purpose and are not particularly limited. The pressure-sensitive adhesive may contain only one type of other component, or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0078] The other components contained in the pressure-sensitive adhesive include, for example, a tackifier resin. By including a tackifier resin in the adhesive, the adhesive strength of the adhesive is improved, and further the application property of the adhesive becomes more stable.

[0079] As the tackifier resin, known resins can be used. The pressure-sensitive adhesive may contain only one type of tackifier resin, or may contain two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily. The tackifier resin is preferably a rosin-based resin, a terpene-based resin or an aromatic hydrocarbon resin, more preferably a rosin-based resin, and even more preferably a polymerized rosin ester resin.

[0080] In the pressure-sensitive adhesive, the ratio of the tackifier resin content to the acrylic resin (A) content ([tackifier resin content in pressure-sensitive adhesive (parts by mass)] / [acrylic resin (A) content in pressure-sensitive adhesive (parts by mass)]×100) is preferably 0 to 15% by mass.

[0081] As described later, in the production of the pressure-sensitive adhesive, it is preferable to use (blend) the tackifier resin in the form of its aqueous dispersion. It is also preferable to blend an emulsion of the acrylic resin (A), an aqueous dispersion of microcapsules, and an aqueous dispersion of the tackifier resin.

[0082] When the acrylic resin emulsion (emulsion of acrylic resin (A)) is used in producing the pressure-sensitive adhesive, the solvent (dispersion medium) such as water in the acrylic resin emulsion is an example of the other component. When an aqueous dispersion of the microcapsules is used in producing the pressure-sensitive adhesive, water (solvent, dispersion medium) in the aqueous dispersion is an example of the other component. When an aqueous dispersion of the tackifier resin is used in producing the PSA, water (solvent, dispersion medium) in the aqueous dispersion is an example of the other component.

[0083] In this specification, unless otherwise specified, not only a component capable of dissolving a solute in a solution, but also a component that serves as a dispersion medium in a dispersion liquid is referred to as a "solvent".

[0084] Among the other components contained in the pressure-sensitive adhesive, those that do not fall under either the tackifier resin or the solvent include, for example, additives such as neutralizers, leveling agents, defoamers, viscosity modifiers, preservatives, plasticizers, fillers, colorants, silane coupling agents, and crosslinking agents; and other resins that do not fall under either the acrylic resin (A) or the tackifier resin. These other components may be known.

[0085] When the pressure-sensitive adhesive contains the crosslinking agent, the crosslinking agent is capable of inter-particle crosslinking between dispersed particles of various copolymers in the pressure-sensitive adhesive. For example, when the copolymer has a structural unit derived from an ethylenically unsaturated monomer having a hydroxyl group, an isocyanate compound, a titanium alkoxide compound, a zirconium alkoxide compound, or the like can be used as a crosslinking agent. For example, when the copolymer has a structural unit derived from an ethylenically unsaturated monomer having a carbonyl group, amines, hydrazide compounds, etc. can be used as the crosslinking agent. For example, when the copolymer has a structural unit derived from an ethylenically unsaturated monomer having a carboxy group, a carbodiimide compound, an epoxy compound, an aziridine compound, a metal compound such as zinc oxide, or the like can be used as a crosslinking agent.

[0086] The other resins may be known resins. Examples of the other resin include acrylic resins having a glass transition temperature outside the range of −60 to −40° C. (less than −60° C., more than −40° C.) In particular, when the pressure-sensitive adhesive contains an acrylic resin having a glass transition temperature of more than −40° C., the pressure-sensitive adhesive has higher cohesive strength and adhesive strength.

[0087] In the adhesive, the ratio of the total content of the microcapsules and the acrylic resin (A) to the total content of components other than the solvent (([content of microcapsules in the adhesive (parts by mass)] + [content of acrylic resin (A) in the adhesive (parts by mass)]) / [total content of components other than the solvent in the adhesive (parts by mass)] × 100) is preferably 80 mass% or more, and may be, for example, any of 90 mass% or more, 95 mass% or more, and 97 mass% or more. When the ratio is equal to or more than the lower limit, when the adhesive sheet is attached to an object, a stable attached state can be maintained with high adhesive strength in the initial stage after attachment, and when the adhesive sheet is peeled off from the object, the adhesive sheet can be easily peeled off without requiring any special operation and without leaving an adhesive layer on the object. On the other hand, the proportion is 100% by mass or less.

[0088] <<Characteristics of adhesive>> When a dry film (0.06 g) obtained using the adhesive of this embodiment is immersed in ethyl acetate (200 mL) at 40° C. for 24 hours, and then the residue that remains undissolved is taken out and dried to obtain an insoluble component (sometimes referred to as "ethyl acetate insoluble component" in this specification), the ratio of the content of the insoluble component to the total mass of the dry adhesive film in the dry adhesive film ([amount of ethyl acetate insoluble component in the dry adhesive film (parts by mass)] / [total mass of the dry adhesive film (parts by mass)]×100) is preferably 30 to 60 mass%. When the ratio is equal to or greater than the lower limit, the cohesive strength of the adhesive is increased, the adhesive layer is more effectively prevented from protruding from the adhesive sheet, the processability of the adhesive sheet is improved, and the removability of the adhesive sheet is improved. When the ratio is equal to or less than the upper limit, the adhesive strength of the adhesive sheet (adhesive layer) is improved. Therefore, when the pressure-sensitive adhesive sheet is applied to an object, in the initial stage after application, the applied state can be maintained more stably with high adhesive strength. The dry film immersed in ethyl acetate can be formed by the method for forming a pressure-sensitive adhesive layer described later. That is, the dry film may be the pressure-sensitive adhesive layer in the pressure-sensitive adhesive sheet described later.

[0089] <<Adhesive manufacturing method>> The pressure-sensitive adhesive of the present embodiment can be produced by blending the microcapsules, the acrylic resin (A), and, if necessary, the other components, and thoroughly stirring these blended components. The order in which the components are mixed when producing the pressure-sensitive adhesive is not particularly limited. When blending the components, all the components may be added and then mixed, or some of the components may be added sequentially while being mixed, or all the components may be added sequentially while being mixed. Each component may be blended alone or as a mixture with other components. For example, when a solvent is blended, the solvent may be blended in a state where it is premixed with the microcapsules, the acrylic resin (A), or the other components other than the solvent, or it may be blended alone without being mixed with these components.

[0090] The temperature at which the components are mixed is not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately depending on the types of components, etc., but is usually preferably 15 to 30°C. The method for mixing the components during blending is not particularly limited, and can be appropriately selected from known methods such as a method for mixing by rotating a stirrer or stirring blade, a method for mixing using a mixer, a method for mixing by adding ultrasound, etc. The time for stirring the blended components may be appropriately adjusted depending on the total amount of adhesive to be produced, the stirring method, etc., and may be, for example, 10 minutes to 2 hours.

[0091] For example, as explained above, when producing the pressure-sensitive adhesive in which the ratio of the plasticizer (Z) content to the acrylic resin (A) content is 0.5 to 30 mass %, the amounts of microcapsules and acrylic resin (A) can be adjusted to achieve such a content ratio.

[0092] ◇Adhesive sheet An adhesive sheet according to one embodiment of the present invention comprises a substrate and an adhesive layer provided on the substrate, the adhesive layer being formed using the adhesive according to one embodiment of the present invention described above and containing the microcapsules. The adhesive sheet of this embodiment, having the adhesive layer, when applied to an object, can maintain a more stable attached state with high adhesive strength in the initial stage after application, and when the adhesive sheet is peeled off from the object, it can be peeled off more easily without the need for special operations and without leaving the adhesive layer on the object.

[0093] FIG. 1 is a cross-sectional view that illustrates an example of the pressure-sensitive adhesive sheet of the present embodiment. In addition, the figures used in the following explanation may show enlarged key parts for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones.

[0094] The adhesive sheet 1 shown here comprises a substrate 11 and an adhesive layer 12 provided on the substrate 11. The adhesive layer 12 is formed using the adhesive according to one embodiment of the present invention and contains the microcapsules. In Fig. 1, the microcapsules in the adhesive layer 12 are not shown. More specifically, in the adhesive sheet 1, one surface 11a of the substrate 11 (the surface on the adhesive layer 12 side) and one surface 12b of the adhesive layer 12 (the surface on the substrate 11 side) are in direct contact with each other. The other surface 12a of the pressure-sensitive adhesive layer 12 (the surface opposite to the substrate 11 side) is the exposed surface, and is the surface to be attached to the object to which the pressure-sensitive adhesive sheet 1 is to be attached.

[0095] The adhesive sheet of this embodiment is not limited to the adhesive sheet 1 shown in FIG. 1, and some of the configuration shown in FIG. 1 may be changed, deleted, or added, as long as the effects of the present invention are not impaired. For example, the adhesive sheet 1 shown in Fig. 1 includes a substrate 11 and an adhesive layer 12, but the adhesive sheet of the present embodiment may include other layers that do not correspond to either the substrate or the adhesive layer. The type and arrangement position of the other layer can be arbitrarily selected depending on the purpose, and is not particularly limited. For example, in the adhesive sheet 1 shown in Fig. 1, the other surface 12a of the adhesive layer 12 is an exposed surface, but may be provided with a known release paper or release film. However, in the pressure-sensitive adhesive sheet of the present embodiment, it is preferable that the substrate and the pressure-sensitive adhesive layer are provided in direct contact with each other.

[0096] <<Base material>> The material of the substrate of the pressure-sensitive adhesive sheet can be arbitrarily selected depending on the purpose, and is not particularly limited. Examples of materials for the substrate include papers such as waterproof paper, fine paper, art paper, coated paper, cast coated paper, resin coated paper, and synthetic paper; and synthetic resins such as polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyvinyl acetate, acrylic resin, AS resin, ABS resin, polyamide, polyacetal, polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyphenylene sulfide, polysulfone, polycarbonate, epoxy resin, melamine resin, phenolic resin, urea resin, polyurethane, and polyimide.

[0097] The substrate may consist of one layer (single layer), or may consist of two or more layers. When the substrate consists of multiple layers, the multiple layers may be the same or different, and the combination of the multiple layers is not particularly limited. Usually, a substrate consisting of one layer is sufficient.

[0098] In this specification, not only in the case of a substrate, "multiple layers may be the same or different from one another" means "all layers may be the same, all layers may be different, or only some layers may be the same", and further, "multiple layers are different from one another" means "at least one of the constituent materials and thicknesses of each layer is different from one another".

[0099] The thickness of the substrate is not particularly limited as long as the substrate is in the form of a sheet or film, but is preferably 10 to 300 μm, more preferably 20 to 200 μm, and particularly preferably 30 to 150 μm. When the thickness of the substrate is equal to or greater than the lower limit, the strength of the pressure-sensitive adhesive sheet is increased. When the thickness of the substrate is equal to or less than the upper limit, the substrate is prevented from becoming excessively thick, and, for example, the pressure-sensitive adhesive sheet becomes easier to handle. Here, the "thickness of the substrate" means the thickness of the entire substrate. For example, the thickness of a substrate consisting of multiple layers means the total thickness of all layers constituting the substrate.

[0100] As the substrate, a commercially available product or one produced by a known method may be used.

[0101] <<Adhesive layer>> The adhesive layer of the adhesive sheet is not particularly limited as long as it is formed using the adhesive according to one embodiment of the present invention and contains the microcapsules.

[0102] The adhesive layer may consist of one layer (single layer), or may consist of two or more layers. If it consists of multiple layers, these multiple layers may be the same or different, and the combination of these multiple layers is not particularly limited. Usually, a single pressure-sensitive adhesive layer is sufficient.

[0103] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is preferably 3 to 30 μm, more preferably 5 to 25 μm, and even more preferably 10 to 20 μm. When the thickness of the pressure-sensitive adhesive layer is equal to or greater than the lower limit, the structure of the pressure-sensitive adhesive layer can be more stably maintained. When the thickness of the pressure-sensitive adhesive layer is equal to or less than the upper limit, the pressure-sensitive adhesive layer can be prevented from becoming excessively thick, and, for example, the handleability of the pressure-sensitive adhesive sheet can be improved. Here, "the thickness of the adhesive layer" means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer consisting of multiple layers means the total thickness of all layers that make up the adhesive layer.

[0104] The thickness of the adhesive layer can be measured using a paper thickness measuring device. At this time, as described later in the Examples, a plurality of measurement points are arbitrarily selected on the surface of the adhesive layer so that there is no bias in these positions, the thickness of the adhesive layer is measured at these measurement points, and the average value of two or more measurement values ​​excluding the maximum and minimum values ​​among these measurement values ​​is calculated, and this average value can be used as the thickness of the adhesive layer. In this way, the thickness of the adhesive layer can be determined with higher accuracy. The measurement points are four or more (for example, 4 to 6). The thickness of the adhesive layer can also be measured in the state of a laminate in which the adhesive layer is laminated with some film or sheet. In that case, the thickness of the laminate is obtained by the above-mentioned method, and the thickness of the film or sheet before laminating the adhesive layer is also obtained by the above-mentioned method, and the thickness of the film or sheet is subtracted from the thickness of the laminate (calculating [thickness of the laminate]-[thickness of the film or sheet]), so that the thickness of the adhesive layer can be obtained with higher accuracy. In this case, the film or sheet can be, for example, a substrate, a release paper, or a release film constituting the adhesive sheet.

[0105] The mass of the film or sheet is measured in advance, the mass of the laminate is measured, and the mass of the film or sheet is subtracted from the mass of the laminate (calculating [mass of laminate]-[mass of film or sheet]), to determine the amount of the adhesive layer in the laminate. The amount of the adhesive layer is then divided by the surface area of ​​the adhesive layer (calculating [amount of adhesive layer] / [surface area of ​​adhesive layer]), to determine the amount of the adhesive layer per unit area on the film or sheet.

[0106] The ratio of the median diameter of the microcapsules to the thickness of the adhesive layer ([median diameter of microcapsules (μm)] / [thickness of adhesive layer (μm)]×100) is preferably 43 to 127%, more preferably 60 to 107%, and may be, for example, any one of 60 to 93% and 73 to 107%. When the ratio is equal to or greater than the lower limit, the adhesive force of the adhesive layer to the object can be more easily reduced without the need for special operations when peeling the adhesive sheet from the object after it has been affixed to the object, and the adhesive sheet can be more easily peeled off from the object without any adhesive layer remaining on the object. By ensuring that the ratio is equal to or less than the upper limit, when the pressure-sensitive adhesive sheet is applied to an object, the applied state can be maintained more stably with higher adhesive strength in the initial stage after application.

[0107] <<Manufacturing method of adhesive sheet>> The pressure-sensitive adhesive sheet of the present embodiment can be produced by providing a pressure-sensitive adhesive layer on a substrate. More specifically, the adhesive is applied to one side of a release paper or release film, and the applied adhesive is dried to form an adhesive layer on one side of the release paper or release film. One side of the substrate is then bonded to the exposed surface of the adhesive layer (the surface opposite the release paper or release film), thereby producing the adhesive sheet with the release paper or release film. The pressure-sensitive adhesive sheet can also be produced by coating one side of the substrate with the pressure-sensitive adhesive and drying the coated pressure-sensitive adhesive to form a pressure-sensitive adhesive layer on one side of the substrate. In this case, a pressure-sensitive adhesive sheet with release paper or release film can be produced by laminating one side of a release paper or release film to the exposed surface of the pressure-sensitive adhesive layer (the surface opposite to the substrate).

[0108] In any of the above manufacturing methods, the adhesive can be applied by a known method using an apparatus such as an air knife coater, curtain coater, die coater, blade coater, roll coater, gate roll coater, bar coater, rod coater, gravure coater, gravure offset coater, etc.; a wire bar coater, etc.

[0109] In any of the above manufacturing methods, the pressure-sensitive adhesive can be dried by a known method such as air drying or heated air drying (heat drying). Drying conditions such as drying temperature and drying time can be appropriately set depending on the drying method. For example, the drying temperature may be 80 to 120° C., and the drying time may be 1 minute to 24 hours. EXAMPLES

[0110] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the examples shown below.

[0111] [Example 1] <<Adhesive manufacturing>> <Production of Microcapsules> The desired microcapsules were produced by the interfacial polycondensation method described below. That is, polyvinyl alcohol ("JP-24" manufactured by Japan Vinyl Acetate & Poval Co., Ltd.) (8.6 g) was added to distilled water (171.4 g), and the mixture was stirred at 50°C for 1 hour to form a solution, which was then cooled to 25°C to obtain an aqueous polyvinyl alcohol solution (the first solution) having a concentration of 4.8% by mass.

[0112] Separately, at room temperature, a TDI-TMP adduct (Mitsui Chemicals, Inc., "Takenate (registered trademark) D-103") (25 g) and polymeric MDI (Tosoh Corporation, "Millionate MR-200", NCO content 31.3% by mass) (5 g) were added to a plasticizer (Z)-1 (ADEKA Corporation, "ADEKA Cizer RS-700") (65 g) shown in Table 1, and the mixture was stirred until it became transparent, thereby obtaining a mixed solution in which all of these components were dissolved (the second solution).

[0113] At room temperature, the entire amount of the mixed solution was added to the entire amount of the polyvinyl alcohol aqueous solution, and the resulting mixed solution was stirred for 3 minutes at a rotation speed of 3000 rpm using a homogenizer (manufactured by Primix Corporation) to obtain an emulsion (the emulsification process).

[0114] To the entire amount of the obtained emulsion, 1,3-bisaminomethylcyclohexane (Tokyo Chemical Industry Co., Ltd.) (6.8 g) and distilled water (40 g) were added, and the reaction solution was stirred at 80°C and 500 rpm for 2 hours with an anchor blade to carry out interfacial polycondensation (the polycondensation process described above).

[0115] As a result of the above, microcapsules having an outer shell made of polyurea containing a polycondensate of 1,3-bisaminomethylcyclohexane and a TDI-TMP adduct, and a polycondensate of 1,3-bisaminomethylcyclohexane and polymeric MDI, and encapsulating the plasticizer (Z)-1 as a core material, were obtained as an aqueous dispersion.

[0116] <Evaluation of Microcapsules> [Evaluation of microcapsule formation] The aqueous dispersion obtained above was coated on fine paper and dried in an oven at 105° C. for 1 minute. The dried product was then observed at 1000x magnification using a scanning electron microscope (SEM, manufactured by JEOL Ltd.). The degree of shell formation was then confirmed to evaluate the formability of the microcapsules according to the following criteria. The results are shown in Table 1. [Evaluation Criteria] A: The outer shell is formed normally, and the microcapsules are formed normally. B: The outer shell is not formed normally and no microcapsules are formed.

[0117] [Measurement of median diameter of microcapsules] The median diameter of the microcapsules was measured using a particle size distribution analyzer (Sysmex Corporation, "CDA-1000X") and the aqueous dispersion obtained above. The results are shown in Table 1.

[0118] [Calculation of the ratio of the thickness of the outer shell of a microcapsule to the particle diameter of the microcapsule] The dried product on the fine paper obtained in the above "Evaluation of microcapsule formability" was immersed in liquid nitrogen for 20 seconds to cool, and then cut into pieces using a cutter. Next, the cross section of the cut piece was observed at a magnification of 1000 times using a scanning electron microscope (manufactured by JEOL Ltd.). Then, 30 cut microcapsules were randomly selected from the acquired image data, and the thickness of the outer shell and the particle diameter of these microcapsules were measured. Then, for all of these 30 microcapsules, the ratio of the thickness of the outer shell of the microcapsule to the particle diameter of the microcapsule was calculated. Furthermore, of these 30 calculated values, the top 18 calculated values ​​(18 calculated values ​​from the largest calculated value to the 18th largest calculated value) and the bottom two calculated values ​​(the smallest calculated value and the second smallest calculated value) were excluded, and the average of the remaining 10 calculated values ​​was calculated, and this average was adopted as the ratio of the thickness of the outer shell of the microcapsule to the particle diameter of the microcapsule in this microcapsule. The results are shown in the column "[Thickness of the outer shell of the microcapsule (μm)] / [Particle diameter of the microcapsule (μm)]×100(%)" in Table 1.

[0119] <Synthesis of acrylic resin (A)-1> An emulsion was obtained by adding octyl thioglycolate (0.09 parts by mass) as a molecular weight regulator, Newcol 707SF (aqueous solution of polyoxyethylene polycyclic phenyl ether sulfate salt, active ingredient 30%, manufactured by Nippon Nyukazai Co., Ltd.) (5.0 parts by mass) as an emulsifier, and ion-exchanged water (24.5 parts by mass) to 2-ethylhexyl acrylate (30 parts by mass), butyl acrylate (64 parts by mass), methyl methacrylate (5 parts by mass), and acrylic acid (1 part by mass), and stirring. The obtained emulsion was placed in a dropping funnel. Deionized water (24.5 parts by mass) was charged into a four-neck flask equipped with a stirrer, a cooling tube, a thermometer, and the dropping funnel, the air inside the flask was replaced with nitrogen gas, the internal temperature was raised to 78°C with stirring, and a 3% by mass aqueous potassium persulfate solution (2.1 parts by mass) was added. After 5 minutes, the dropping of the emulsion obtained above was started from the dropping funnel, and in parallel with this, a 3% by mass aqueous potassium persulfate solution (6.3 parts by mass) was dropped from another dropping port over 3 hours. After the dropping was completed, the contents were aged for 4 hours while stirring while maintaining the internal temperature of the four-neck flask at 78°C, then cooled, neutralized with aqueous ammonia, and diluted with water to obtain an emulsion of acrylic resin (A)-1 with a solid content of 55% by mass. The glass transition temperature (Tg) of the acrylic resin (A-1) is shown in Table 1.

[0120] <Adhesive manufacturing> At room temperature, the water dispersion of the microcapsules obtained above, an emulsion of acrylic resin (A)-1, and a water dispersion of tackifier resin "Super Ester E-788" (Arakawa Chemical Industry Co., Ltd., water dispersion of polymerized rosin ester, solid content 50 mass%) were mixed. At this time, the ratio of the amount of the microcapsules to the amount of the acrylic resin (A)-1 (total amount of components other than water in the water dispersion) was 10 mass%. In addition, the ratio of the amount of the tackifier resin to the amount of the acrylic resin (A)-1 was 7.2 mass%. Furthermore, a defoamer, a leveling agent, and a preservative were added to the obtained mixture, and a viscosity adjuster was added to adjust the viscosity of the mixture to 4000 mPa·s (measured at 60 rpm using a BL type viscometer and a #4 rotor). An aqueous adhesive was obtained. In the dried coating of the obtained adhesive, the ratio of the content of the insoluble components in ethyl acetate to the total mass of the dried coating was 45 mass%.

[0121] <<Manufacture of adhesive sheets>> The adhesive obtained above was coated on the release-treated surface of a release paper and dried by heating at 105° C. for 2 minutes to form an adhesive layer (thickness 15 μm) on the release paper. The thickness of the adhesive layer was measured by the following method. That is, five measurement points were arbitrarily selected on the surface of the laminate of the release paper and the adhesive layer so that there was no bias in these positions. Then, using a paper thickness measuring device ("MEI-11" manufactured by Citizen Co., Ltd.), the thickness of the laminate was measured at these five measurement points, and the average value of the three measurement values ​​excluding the maximum and minimum values ​​was calculated, and this average value was adopted as the thickness of the laminate. Separately, the thickness (average value of the three thickness measurements of the release paper) of the release paper before the adhesive layer was laminated was also measured, in the same manner as for the laminate, and the thickness of the adhesive layer was determined by subtracting the thickness of the release paper from the thickness of the laminate (calculating [laminate thickness] - [release paper thickness]).

[0122] Next, using a high-quality paper (thickness 65 μm) as a substrate, the exposed surface of the adhesive layer (the surface opposite to the release paper side) was attached to one surface of the high-quality paper to obtain an adhesive sheet with release paper, which comprises the high-quality paper, the adhesive layer provided on the high-quality paper, and the release paper on the surface of the adhesive layer opposite to the high-quality paper side. This adhesive sheet with release paper was left to stand for 24 hours under conditions of a temperature of 23° C. and a relative humidity of 50% (50% RH).

[0123] Cross sections were randomly cut from the obtained pressure-sensitive adhesive sheet with release paper and examined, and it was found that the pressure-sensitive adhesive layer normally contained the medium-sized microcapsules as previously confirmed.

[0124] <<Evaluation of adhesive sheets>> <Calculation of [median diameter of microcapsule] / [thickness of adhesive layer]> The value of [median diameter of microcapsules] / [thickness of adhesive layer] was calculated. The results are shown in the column of "Proportion (%) of median diameter to thickness of adhesive layer" in Table 1.

[0125] <Evaluation of the initial adhesive performance of adhesive sheets> [Measurement of initial adhesive strength of adhesive sheet] A piece measuring 25 mm×100 mm was cut from the pressure sensitive adhesive sheet after the above-mentioned static storage, and the release paper was removed to prepare a test piece. The entire exposed surface of the newly formed pressure sensitive adhesive layer (the surface opposite to the fine paper side) in this test piece was placed on one surface of a polyethylene terephthalate (PET) film (thickness 100 μm) fixed to a metal plate. Then, a roll having a mass of 2 kg was rolled back and forth once in the longitudinal direction of the test piece on the laminate of the test piece and the PET film to sufficiently bond the test piece and the PET film. In this manner, a laminate sheet for evaluation was prepared.

[0126] Next, the wood-free paper in the test piece of this evaluation laminate sheet was immediately peeled off from the PET film. At this time, the peeling speed was set to 300 mm / min, and the 180° peeling was performed so that the angle between the two peeled surfaces generated by the peeling was 180°. The peeling force at this 180° peeling was then measured, and this was adopted as the initial adhesive force of the adhesive sheet, and its level was judged according to the following criteria. The results are shown in Table 1. [Judgment criteria] A: The initial adhesive strength of the adhesive sheet is 7N / 25mm or more, which is extremely high. B: The initial adhesive strength of the adhesive sheet is 6 N / 25 mm or more and less than 7 N / 25 mm, and the initial adhesive strength is high. C: The initial adhesive strength of the adhesive sheet is less than 6 N / 25 mm, and the initial adhesive strength is low.

[0127] [Determination of initial peeling pattern of substrate] Furthermore, the two peeled surfaces were observed, and the initial peeling mode of the substrate (free-quality paper) was judged according to the following criteria. The results are shown in Table 1. [Judgment criteria] A: The substrate peeled off due to cohesive failure of the adhesive layer or destruction of the substrate, which is a preferable peeling mode and reflects the high initial adhesive strength of the adhesive sheet, and the initial adhesive performance of the adhesive sheet is high as intended. B: The substrate peeled off due to interfacial peeling between the adhesive layer and the PET film, which is an undesirable peeling pattern and reflects the low initial adhesive strength of the adhesive sheet, and the initial adhesive performance of the adhesive sheet is low, contrary to the purpose.

[0128] <Evaluation of adhesive performance of adhesive sheets during dismantling> [Measurement of adhesive strength when dismantling adhesive sheet] Separately, a test piece identical to the one obtained above was prepared, and the entire exposed surface of the adhesive layer in this test piece (the surface opposite to the fine paper side) was attached to one surface of a polyethylene terephthalate (PET) film (thickness 100 μm). The corner of a metal plate was brought into contact with the exposed surface of the PET film in the laminate of the test piece and the PET film obtained in this way, and the metal plate was moved three times along the longitudinal direction of the test piece while applying a pressure of about 10 MPa, thereby scraping the laminate. It was previously confirmed that the pressure of 10 MPa was sufficient to destroy the microcapsules in the adhesive layer. Next, the laminate after being rubbed with this metal plate was left to stand and stored at room temperature for 60 minutes. Next, the exposed surface of the PET film of the laminate after the static storage was fixed to a metal plate, and the peel strength was measured in the same manner as in the measurement of the initial adhesive strength of the adhesive sheet. This was used as the adhesive strength of the adhesive sheet when dismantled, and its level was judged according to the following criteria. The results are shown in Table 1. In this specification, the removal of the laminated structure between the adhesive layer and the object by peeling the adhesive layer from the object at any desired timing is sometimes referred to as "dismantling." [Judgment criteria] A: The adhesive strength of the adhesive sheet when disassembled is less than 5.5N / 25mm, which is extremely low. B: The adhesive strength of the adhesive sheet when disassembled is 5.5 N / 25 mm or more but less than 6.5 N / 25 mm, which means the adhesive strength when disassembled is low. C: The adhesive strength of the adhesive sheet when disassembled is 6.5N / 25mm or more, and the adhesive strength when disassembled is high.

[0129] [Determination of peeling pattern when dismantling the substrate] Furthermore, the two peeled surfaces were observed, and the peeling pattern when the base material (fine paper) was dismantled was judged according to the following criteria. The results are shown in Table 1. [Judgment criteria] A: The substrate is peeled off due to interfacial peeling between the adhesive layer and the PET film, which is a preferable peeling pattern and reflects the low adhesive strength of the adhesive sheet when disassembled. The adhesive performance of the adhesive sheet when disassembled is low as intended. B: The substrate peeled off due to cohesive failure of the adhesive layer or destruction of the substrate, which is an undesirable peeling pattern and reflects the high adhesive strength of the adhesive sheet when disassembled. The adhesive performance of the adhesive sheet when disassembled is high, contrary to the intended purpose.

[0130] In Table 1, "[Microcapsule content] / [Acrylic resin (A) or other acrylic resin (A') content] x 100 (mass%)" means "the ratio (mass%) of the microcapsule content to the acrylic resin (A) or other acrylic resin (A') content in the adhesive." This is the same in Table 2 and subsequent tables. In Table 1, "[Content of tackifier resin] / [Content of acrylic resin (A) or other acrylic resin (A')] x 100 (mass%)" means "the ratio (mass%) of the content of tackifier resin to the content of acrylic resin (A) or other acrylic resin (A') in the adhesive." This also applies to Table 2 and subsequent tables. In Table 1, "[Amount of ethyl acetate insoluble components in the dry adhesive coating] / [Total mass of the dry adhesive coating] × 100 (mass %)" means "the ratio of the content of ethyl acetate insoluble components in the dry adhesive coating to the total mass of the dry adhesive coating." This also applies to Table 2 and subsequent tables.

[0131] <<Production of adhesives, production and evaluation of microcapsules, production of adhesives, and production and evaluation of adhesive sheets>> [Example 2] Microcapsules were produced and evaluated in the same manner as in Example 1, except that the amount of distilled water used was changed from 171.4 g to 172.8 g, and the amount of polyvinyl alcohol used was changed from 8.6 g to 7.2 g. The obtained microcapsules were different from those obtained in Example 1 in terms of their median diameter. A pressure-sensitive adhesive was produced in the same manner as in Example 1, except that these microcapsules (more specifically, the water dispersion of the microcapsules) were used. Furthermore, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 1.

[0132] [Example 3] Microcapsules were produced and evaluated in the same manner as in Example 1, except that the amount of distilled water used was changed from 171.4 g to 173.7 g, and the amount of polyvinyl alcohol used was changed from 8.6 g to 6.3 g. The obtained microcapsules were different from those obtained in Example 1 in terms of their median diameter. A pressure-sensitive adhesive was produced in the same manner as in Example 1, except that these microcapsules (more specifically, the water dispersion of the microcapsules) were used. Furthermore, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 1.

[0133] [Example 4] Microcapsules were produced and evaluated in the same manner as in Example 1, except that the amount of distilled water used was changed from 171.4 g to 174.6 g, and the amount of polyvinyl alcohol used was changed from 8.6 g to 5.4 g, and the microcapsules were produced and evaluated in the same manner as in Example 1. The obtained microcapsules were different from the microcapsules obtained in Example 1 in terms of their median diameter. A pressure-sensitive adhesive was produced in the same manner as in Example 1, except that these microcapsules (more specifically, the water dispersion of the microcapsules) were used. Furthermore, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 1.

[0134] [Example 5] Microcapsules were produced and evaluated in the same manner as in Example 1, except that when producing the microcapsules, plasticizer (Z)-2 ("Ricksizer C-101" manufactured by Ito Oil Mills) (65 g) shown in Table 2 was used instead of plasticizer (Z)-1, and the rotation speed of the homogenizer in the emulsification process was changed from 3000 rpm to 6000 rpm. A pressure-sensitive adhesive was produced in the same manner as in Example 1, except that these microcapsules (more specifically, the water dispersion of the microcapsules) were used. Furthermore, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 2.

[0135] [Example 6] Microcapsules were produced and evaluated in the same manner as in Example 5, except that the rotation speed of the homogenizer in the emulsification step was changed from 6000 rpm to 3000 rpm. A pressure-sensitive adhesive was produced in the same manner as in Example 1, except that these microcapsules (more specifically, the water dispersion of the microcapsules) were used. Furthermore, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 2.

[0136] [Example 7] Microcapsules were produced and evaluated in the same manner as in Example 5, except that the rotation speed of the homogenizer in the emulsification step was changed from 6000 rpm to 2000 rpm. A pressure-sensitive adhesive was produced in the same manner as in Example 1, except that these microcapsules (more specifically, the water dispersion of the microcapsules) were used. Furthermore, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 2.

[0137] [Example 8] Microcapsules were produced and evaluated in the same manner as in Example 5, except that the rotation speed of the homogenizer in the emulsification step was changed from 6000 rpm to 1500 rpm. A pressure-sensitive adhesive was produced in the same manner as in Example 1, except that these microcapsules (more specifically, the water dispersion of the microcapsules) were used. Furthermore, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 2.

[0138] [Example 9] <<Adhesive manufacturing>> <Synthesis of acrylic resin (A)-2> Acrylic resin (A)-2 was synthesized in the same manner as in the case of the above acrylic resin (A)-1, except that 2-ethylhexyl acrylate (78 parts by mass), methyl acrylate (20 parts by mass) and acrylic acid (2 parts by mass) were used instead of 2-ethylhexyl acrylate (30 parts by mass), butyl acrylate (64 parts by mass), methyl methacrylate (5 parts by mass) and acrylic acid (1 part by mass). In the obtained emulsion of acrylic resin (A)-2, the solid content was 55% by mass. The glass transition temperature of acrylic resin (A-2) is shown in Table 3.

[0139] <Adhesive manufacturing> At room temperature, the aqueous dispersion of the microcapsules, the emulsion of the acrylic resin (A)-2, and the aqueous dispersion of the tackifier resin "Super Ester E-788" (Arakawa Chemical Industries, Inc., aqueous dispersion of polymerized rosin ester, solid content 50% by mass) were mixed. At this time, the ratio of the amount of the microcapsules mixed (total amount of components other than water in the aqueous dispersion) to the amount of the acrylic resin (A)-2 mixed was 10% by mass. In addition, the ratio of the amount of the tackifier resin mixed to the amount of the acrylic resin (A)-2 mixed was 12.7% by mass. Furthermore, a defoamer, a leveling agent, and a preservative were added to the obtained mixture, and a viscosity modifier was added to adjust the viscosity of the mixture to 4000 mPa·s (measured at 60 rpm using a BL type viscometer and a #4 rotor), thereby obtaining an aqueous adhesive. The insoluble content in ethyl acetate of the dried coating of the obtained adhesive was 53% by mass.

[0140] <<Production and evaluation of adhesive sheets>> An adhesive sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive obtained above was used. The results are shown in Table 3.

[0141] <<Production of adhesives, production and evaluation of microcapsules, production of adhesives, and production and evaluation of adhesive sheets>> [Example 10] Microcapsules were produced and evaluated in the same manner as in Example 1, except that the amount of distilled water used was changed from 171.4 g to 172.8 g, and the amount of polyvinyl alcohol used was changed from 8.6 g to 7.2 g. The obtained microcapsules were different from those obtained in Example 1 in terms of their median diameter. Then, except for using these microcapsules (more specifically, an aqueous dispersion of microcapsules) and using an emulsified acrylic resin (A)-2 instead of the emulsified acrylic resin (A)-1, an adhesive was produced in the same manner as in Example 1. At this time, the ratio of the total amount of components other than water added in the aqueous dispersion to the amount of acrylic resin (A)-2 was 10 mass%. Furthermore, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 3.

[0142] [Example 11] Microcapsules were produced and evaluated in the same manner as in Example 5, except that the rotation speed of the homogenizer in the emulsification step was changed from 6000 rpm to 3000 rpm. Then, except for using these microcapsules (more specifically, an aqueous dispersion of microcapsules) and using an emulsified acrylic resin (A)-2 instead of the emulsified acrylic resin (A)-1, an adhesive was produced in the same manner as in Example 1. At this time, the ratio of the total amount of components other than water added in the aqueous dispersion to the amount of acrylic resin (A)-2 was 10 mass%. Furthermore, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 3.

[0143] [Comparative Example 1] <<Adhesive manufacturing>> <Production of Microcapsules> Sodium hydroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (0.7 g) and styrene-maleic anhydride copolymer (manufactured by Monsanto Co., Ltd. "Scriptet (registered trademark) 520") (5.1 g) were added to distilled water (159.2 g), and the mixture was stirred at 80°C for 2 hours and then cooled to 25°C to obtain an aqueous solution of styrene-maleic acid copolymer with a concentration of 3.5 mass%.

[0144] Separately, at room temperature, distilled water (20 g) was added to a 37% by mass aqueous formaldehyde solution (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) (7.0 g) to obtain an aqueous formaldehyde solution with a concentration of 9.6% by mass, and a small amount of dilute sodium hydroxide solution was added thereto to adjust the pH of the aqueous formaldehyde solution to 9.0.

[0145] Melamine monomer (Tokyo Chemical Industry Co., Ltd.) (3.4 g) was added to the entire amount of the aqueous formaldehyde solution at room temperature, and the mixture was stirred at 80° C. for 10 minutes to obtain a melamine-formaldehyde mixed solution.

[0146] At room temperature, plasticizer (Z)-2 (65 g) was added to the entire amount of the styrene-maleic acid copolymer aqueous solution, and the resulting mixture was stirred for 3 minutes at a rotation speed of 3,500 rpm using a homogenizer (manufactured by Primix Corporation) to obtain an emulsion.

[0147] The entire amount of the melamine-formaldehyde mixed liquid was added to the entire amount of the obtained emulsion, and the reaction liquid was stirred at 80° C. and 500 rpm for 2 hours with an anchor blade to carry out polycondensation. Next, the reaction liquid was cooled to 25° C., and then a small amount of dilute aqueous sodium hydroxide solution was added thereto to adjust the pH of the reaction liquid to 7.0.

[0148] As a result, microcapsules having an outer shell made of melamine and encapsulating the plasticizer (Z)-2 as a core substance were obtained as an aqueous dispersion.

[0149] <Evaluation of Microcapsules> The microcapsules obtained above were evaluated in the same manner as in Example 1. The results are shown in Table 4.

[0150] <Production of adhesive, and production and evaluation of adhesive sheets> Except for using the water dispersion of microcapsules obtained above, an adhesive was produced and evaluated in the same manner as in Example 1. When producing the adhesive, the ratio of the amount of microcapsules to the amount of acrylic resin (A)-1 (total amount of components other than water in the water dispersion) was 10 mass % in the same manner as in Example 1. In addition, the ratio of the amount of tackifier resin to the amount of acrylic resin (A)-1 was 7.2 mass %. The content of the insoluble matter in ethyl acetate of the dried coating of the obtained adhesive was 45 mass %. Then, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 4.

[0151] <<Production of adhesives, production and evaluation of microcapsules, production of adhesives, and production and evaluation of adhesive sheets>> [Comparative Example 2] As in Comparative Example 1, microcapsules were produced as an aqueous dispersion. A pressure-sensitive adhesive was produced in the same manner as in Example 1, except that the aqueous dispersion of the microcapsules was used, and the emulsion of the acrylic resin (A)-2, which was the same as that obtained in Example 9, was used instead of the emulsion of the acrylic resin (A)-1. At this time, the ratio of the amount of the microcapsules to the amount of the acrylic resin (A)-2 (the total amount of the components other than water in the aqueous dispersion) was 10% by mass, as in Example 9. In addition, the ratio of the amount of the tackifier resin to the amount of the acrylic resin (A)-2 was 12.7% by mass. The content of the insoluble matter in ethyl acetate of the dried coating of the obtained pressure-sensitive adhesive was 53% by mass. Then, an adhesive sheet was produced and evaluated in the same manner as in Example 1, except that this adhesive was used. The results are shown in Table 4.

[0152] [Comparative Example 3] <<Adhesive manufacturing>> <Synthesis of other acrylic resin (A')-1> Other acrylic resin (A')-1 was synthesized in the same manner as in the case of the above acrylic resin (A)-1, except that 2-ethylhexyl acrylate (99 parts by mass) and acrylic acid (1 part by mass) were used instead of 2-ethylhexyl acrylate (30 parts by mass), butyl acrylate (64 parts by mass), methyl methacrylate (5 parts by mass) and acrylic acid (1 part by mass). In the obtained emulsion of other acrylic resin (A')-1, the solid content was 55% by mass. The glass transition temperature of other acrylic resin (A')-1 is shown in Table 4.

[0153] <Adhesive manufacturing> At room temperature, the aqueous dispersion of the microcapsules, the emulsion of the other acrylic resin (A')-1, and the aqueous dispersion of the tackifier resin "Super Ester E-788" (Arakawa Chemical Industry Co., Ltd., aqueous dispersion of polymerized rosin ester, solid content 50% by mass) were mixed. At this time, the ratio of the amount of the microcapsules to the amount of the other acrylic resin (A')-1 (total amount of components other than water in the aqueous dispersion) was 10% by mass. In addition, the ratio of the amount of the tackifier resin to the amount of the other acrylic resin (A')-1 was 7.2% by mass. Furthermore, a defoamer, a leveling agent, and a preservative were added to the obtained mixture, and a viscosity modifier was added to adjust the viscosity of the mixture to 4000 mPa·s (measured at 60 rpm using a BL type viscometer and a #4 rotor), thereby obtaining an aqueous adhesive. The insoluble content in ethyl acetate of the dried coating of the obtained adhesive was 42% by mass.

[0154] <<Production and evaluation of adhesive sheets>> An adhesive sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive obtained above was used. The results are shown in Table 4.

[0155] [Comparative Example 4] <<Adhesive manufacturing>> <Synthesis of other acrylic resin (A')-2> Other acrylic resin (A')-2 was synthesized in the same manner as in the case of the above acrylic resin (A)-1, except that 2-ethylhexyl acrylate (30 parts by mass), butyl acrylate (64 parts by mass), methyl methacrylate (5 parts by mass) and acrylic acid (1 part by mass) were used instead of 2-ethylhexyl acrylate (75 parts by mass), methyl acrylate (19.5 parts by mass), methacrylic acid (3.5 parts by mass) and acrylic acid (2 parts by mass), and the amount of octyl thioglycolate used was changed from 0.09 parts by mass to 0.03 parts by mass. In the obtained emulsion of other acrylic resin (A')-2, the solid content was 55% by mass. The glass transition temperature of other acrylic resin (A')-2 is shown in Table 4.

[0156] <Adhesive manufacturing> At room temperature, the aqueous dispersion of the microcapsules, the emulsion of the other acrylic resin (A')-2, and the aqueous dispersion of the tackifier resin "Super Ester E-788" (Arakawa Chemical Industry Co., Ltd., aqueous dispersion of polymerized rosin ester, solid content 50% by mass) were mixed. At this time, the ratio of the amount of the microcapsules mixed (total amount of components other than water in the aqueous dispersion) to the amount of the other acrylic resin (A')-2 was 10% by mass. In addition, the ratio of the amount of the tackifier resin mixed to the amount of the other acrylic resin (A')-2 was 12.7% by mass. Furthermore, a defoamer, a leveling agent, and a preservative were added to the obtained mixture, and a viscosity modifier was added to adjust the viscosity of the mixture to 4000 mPa·s (measured at 60 rpm using a BL type viscometer and a #4 rotor). A water-based adhesive was obtained. The insoluble content in ethyl acetate of the dried coating of the obtained adhesive was 65% by mass.

[0157] <<Production and evaluation of adhesive sheets>> An adhesive sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive obtained above was used. The results are shown in Table 4.

[0158] [Comparative Example 5] <<Adhesive manufacturing>> <Synthesis of other acrylic resin (A')-3> Other acrylic resin (A')-3 was synthesized in the same manner as in the case of the above acrylic resin (A)-1, except that butyl acrylate (79 parts by mass), methyl methacrylate (20 parts by mass) and acrylic acid (1 part by mass) were used instead of 2-ethylhexyl acrylate (30 parts by mass), butyl acrylate (64 parts by mass), methyl methacrylate (5 parts by mass) and acrylic acid (1 part by mass). In the obtained emulsion of other acrylic resin (A')-3, the solid content was 55% by mass. The glass transition temperature of other acrylic resin (A')-3 is shown in Table 5.

[0159] <Adhesive manufacturing> At room temperature, the aqueous dispersion of the microcapsules, the emulsion of the other acrylic resin (A')-3, and the aqueous dispersion of the tackifier resin "Super Ester E-788" (Arakawa Chemical Industry Co., Ltd., aqueous dispersion of polymerized rosin ester, solid content 50% by mass) were mixed. At this time, the ratio of the amount of the microcapsules to the amount of the other acrylic resin (A')-3 (total amount of components other than water in the aqueous dispersion) was 10% by mass. In addition, the ratio of the amount of the tackifier resin to the amount of the other acrylic resin (A')-3 was 7.5% by mass. Furthermore, a defoamer, a leveling agent, and a preservative were added to the obtained mixture, and a viscosity modifier was added to adjust the viscosity of the mixture to 4000 mPa·s (measured at 60 rpm using a BL type viscometer and a #4 rotor), thereby obtaining an aqueous adhesive. The insoluble content in ethyl acetate of the dried coating of the obtained adhesive was 65% by mass.

[0160] <<Production and evaluation of adhesive sheets>> An adhesive sheet was produced and evaluated in the same manner as in Example 1, except that the adhesive obtained above was used. These results are shown in Table 5.

[0161] [Table 1]

[0162] [Table 2]

[0163] [Table 3]

[0164] [Table 4]

[0165] [Table 5]

[0166] As is clear from the above results, in Examples 1 to 11, the initial adhesive strength of the adhesive sheet was high, which reflected the preferred initial peeling mode of the substrate, and the initial adhesive performance of the adhesive sheet was high. On the other hand, in Examples 1 to 11, the adhesive strength of the adhesive sheet upon dismantling was low, which reflected the preferred peeling mode of the substrate upon dismantling, and the adhesive performance of the adhesive sheet upon dismantling was low. That is, the pressure-sensitive adhesive sheets of Examples 1 to 11 were able to maintain a stable attached state with high adhesive strength at the initial stage after being attached to the object. On the other hand, at the stage of peeling off from the object at any desired time, the adhesive strength of these pressure-sensitive adhesive sheets was reduced by merely rubbing with a hard object such as a metal plate, and they could be easily peeled off without leaving any adhesive layer on the object.

[0167] In Examples 1 to 11, the glass transition temperature of the acrylic resin (A) was -55.9 to -52.4°C, the amount of the structural unit (a1) in the acrylic resin (A) was 78 to 94 mass%, the amount of the structural unit (a2) was 1 to 2 mass%, the outer shell of the microcapsule was made of polyurea, and the microcapsules encapsulated a plasticizer (Z) that was liquid at room temperature.

[0168] Of these, in Examples 2, 3, 6, 7, and 9 to 11, both the initial adhesive strength and the adhesive strength during dismantling of the adhesive sheets were within the most preferred ranges, and both the initial adhesive performance and the adhesive performance during dismantling were particularly excellent. The ratio of the median diameter of the microcapsules to the thickness of the adhesive layer was 50 to 120% in Examples 1 to 11 (the median diameter of the microcapsules was 7.5 to 18 μm), whereas it was 70 to 100% in Examples 2, 3, 6, 7, and 9 to 11 (the median diameter of the microcapsules was 10 to 15 μm).

[0169] In the pressure-sensitive adhesives of Examples 1 to 11, the ratio of the content of the plasticizer (Z) to the content of the acrylic resin (A) was 5.9 to 6.1% by mass. In the dried adhesive coatings of Examples 1 to 11, the content of components insoluble in ethyl acetate relative to the total mass was 45 to 53 mass %. In the pressure-sensitive adhesives of Examples 1 to 11, the ratio of the tackifier resin content to the acrylic resin (A) content was 7.2 to 12.7% by mass. In the microcapsules of Examples 1 to 11, the ratio of the thickness of the outer shell of the microcapsule to the particle diameter of the microcapsule was 11.3 to 12.9%.

[0170] In contrast, in Comparative Examples 1 and 2, the adhesive strength of the adhesive sheet when dismantled was high, and reflecting this, the peeling mode when the substrate was dismantled was not preferable, and the adhesive performance of the adhesive sheet when dismantled was high. That is, in the adhesive sheets of Comparative Examples 1 and 2, when peeled from the object at any desired timing, the adhesive strength did not decrease even when rubbed with a hard object such as a metal plate, and the adhesive layer remained on the object, making it difficult to peel off. In Comparative Examples 1 and 2, the outer shell of the microcapsules was made of melamine.

[0171] In Comparative Example 3, the initial adhesive strength of the adhesive sheet was low, which reflected the initial peeling manner of the substrate being unfavorable, and the initial adhesive performance of the adhesive sheet was low. That is, the adhesive sheet of Comparative Example 3 was unable to maintain a stable attached state with high adhesive strength in the initial stage after attachment to the object. In Comparative Example 3, instead of the acrylic resin (A), another acrylic resin (A') was used, and its glass transition temperature was -69.1°C.

[0172] In Comparative Example 4, similarly to Comparative Examples 1 and 2, the adhesive strength of the adhesive sheet when dismantled was high, and reflecting this, the peeling mode when the substrate was dismantled was not preferable, and the adhesive performance of the adhesive sheet when dismantled was high. That is, when the adhesive sheet of Comparative Example 4 was to be peeled off from the object at any desired timing, the adhesive strength did not decrease even when rubbed with a hard object such as a metal plate, and the adhesive layer remained on the object, making it difficult to peel off. In Comparative Example 4, an acrylic resin (A') was used instead of the acrylic resin (A), and in the acrylic resin (A') the proportion of the structural unit (a2) was 5.5 mass %.

[0173] In Comparative Example 5, the initial adhesive strength of the adhesive sheet was low, and reflecting this, the initial peeling mode of the substrate was not favorable, resulting in low initial adhesive performance of the adhesive sheet, as in Comparative Example 3. In other words, the adhesive sheet of Comparative Example 5 was unable to maintain a stable attached state with high adhesive strength in the initial stage after attachment to an object. In Comparative Example 5, instead of the acrylic resin (A), another acrylic resin (A') was used, and its glass transition temperature was -30.9°C. [Industrial Applicability]

[0174] INDUSTRIAL APPLICABILITY The present invention can be used as an adhesive sheet that has high adhesive strength in the initial stage after application to an object, and can have its adhesive strength reduced at any timing after application. [Explanation of symbols]

[0175] REFERENCE SIGNS LIST 1... adhesive sheet, 11... substrate, 11a... one surface of substrate, 12... adhesive layer

Claims

1. An adhesive having microcapsules dispersed therein, The pressure-sensitive adhesive contains an acrylic resin (A) having a glass transition temperature of −60 to −40° C., The acrylic resin (A) has a structural unit (a1) derived from an alkyl (meth)acrylate ester and a structural unit (a2) derived from (meth)acrylic acid, the number of carbon atoms in the alkyl group constituting the alkyl ester in the (meth)acrylic acid alkyl ester is 4 or more; In the acrylic resin (A), the ratio of the amount of the structural unit (a1) to the total amount of structural units is 50 to 99.5 mass%, In the acrylic resin (A), the ratio of the amount of the structural unit (a2) to the total amount of structural units is 0.5 to 5 mass%, The outer shell of the microcapsule is made of polyurea, The microcapsules encapsulate a plasticizer (Z) that is liquid at room temperature.

2. The pressure-sensitive adhesive according to claim 1, wherein the ratio of the content of the plasticizer (Z) to the content of the acrylic resin (A) in the pressure-sensitive adhesive is 0.5 to 30 mass %.

3. A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer, The pressure-sensitive adhesive sheet includes a substrate and the pressure-sensitive adhesive layer provided on the substrate, 3. An adhesive sheet, wherein the adhesive layer is formed using the adhesive according to claim 1 or 2 and contains the microcapsules.

4. The pressure-sensitive adhesive sheet according to claim 3, wherein a ratio of the median diameter of the microcapsules to a thickness of the pressure-sensitive adhesive layer is 65 to 105%.

Citation Information

Patent Citations

  • Acrylic tacky agent composition and double-side tacky tape

    JP1995034051A

  • Bonding agent

    JP2001214148A

Cited By

  • Water-based binder as well as preparation method and application thereof

    CN120173535A