Resin metal laminated material and producing method thereof

The resin-metal laminate material with a metal oxide layer bond addresses weak bonding issues, providing a strong, lightweight, and reliable joint suitable for stressed applications through direct bonding and efficient manufacturing.

JP2024179023APending Publication Date: 2024-12-26HIROTEC CORP +2

Patent Information

Application Number
JP2023097506
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-06-14
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

Existing resin-metal laminates face issues with weak bonding interfaces, especially when subjected to large stress or requiring long-term reliability, and current methods either fail to provide strong joints over large areas or cause local damage.

Method used

A resin-metal laminate material where the resin layer and metal layer are directly bonded via a metal oxide layer, with the top and bottom layers being resin layers, ensuring a strong and reliable bond without mechanical fastening, and a manufacturing method involving pulsed laser treatment and heat pressing.

Benefits of technology

The laminate achieves a lightweight, reliable bond with excellent corrosion resistance and insulation properties, suitable for applications with large external stress, and allows for efficient large-area joining.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024179023000001_ABST
    Figure 2024179023000001_ABST
Patent Text Reader

Abstract

To provide a resin metal joint having long reliability by covering a front surface and a back surface with a resin layer, capable of using in the use where a resin layer and a metal layer are jointed strongly and large external stress is applied on a joint surface, without using a mechanical joint such as rivet coupling or the like, and a simple and efficient producing method thereof.SOLUTION: A resin metal laminated material in which a resin layer and a metal layer are laminated, having a joint region in which the resin layer and the metal layer are directly joined via a metal oxide layer, and the top layer and the bottom layer are resin layers. The top resin layer and the bottom resin layer are preferably made of different resins.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a resin-metal laminate material in which a resin layer and a metal layer are laminated, and a method for producing the same. [Background technology]

[0002] Resin materials are lightweight, do not conduct heat or electricity well, and have excellent corrosion resistance. On the other hand, metal materials are generally strong and have characteristics such as excellent heat resistance and dimensional stability. If resin and metal materials could be combined, a composite material could be obtained that utilizes the advantages of each material. However, it is difficult to effectively join resin and metal materials, which have different bonding styles. Therefore, when strong joining is required, mechanical joining such as riveting is mainly used.

[0003] However, the use of rivets etc. not only increases the weight of the structure, but also poses various problems such as corrosion from the gap between the resin material and the metal material, breakage due to stress concentration at the mechanical fastening part, etc. In response to this, when integrating a thin metal foil with a resin material, it has been proposed to directly join the metal foil and the resin material.

[0004] For example, Patent Document 1 (JP 2020-82388 A) discloses a conductive metal resin laminate comprising a metal foil and, on at least one side thereof, a resin layer containing a conductive filler made of a non-metallic material, organic fibers, and a resin.

[0005] The conductive metal resin laminate described in Patent Document 1 is said to have improved moldability and processability by comprising a metal foil and, on at least one surface of the metal foil, a resin layer containing a conductive filler made of a non-metallic material, organic fibers, and a resin.

[0006] Furthermore, Patent Document 2 (JP 2008-221739 A) discloses a resin-metal laminate comprising a resin composition containing a polyaryl ketone resin (A) and a thermoplastic resin (B) having a glass transition temperature of 180 to 350°C in a mass ratio of (A) / (B) = 95 / 5 to 5 / 95, and having a metal layer (Y) having a thickness of 0.1 to 300 μm on at least one side of a resin layer (X) having a thickness of 0.5 to 15 mm, and wherein the maximum peak height Ry (measured in accordance with JIS B0601-1994) of the outer surface of the metal layer (Y) is in the range of 0.1 to 4 μm.

[0007] The resin-metal laminate described in Patent Document 2 above is a resin plate that has excellent heat resistance and cutting processability, as well as low water absorption and low expansion, and is said to be capable of providing a resin-metal laminate that can be preferably used for electronic and electrical equipment parts, equipment and machine tool members, automobile parts, etc.

[0008] Furthermore, in Patent Document 3 (WO 2021 / 230025), the present inventors have disclosed a method for directly bonding a metal material and a thermoplastic resin material, which comprises: a first step of irradiating the surface of the metal material with a pulsed laser in an oxidizing atmosphere to form a surface-modified region; a second step of abutting the thermoplastic resin material against the surface-modified region to form a bonding interface; and a third step of raising the temperature of the bonding interface by laser irradiation to achieve bonding, wherein in the first step, metal oxide particle clusters are formed in the surface-modified region by continuously bonding metal oxide particles having particle sizes of 5 to 500 nm, and the maximum height (Sz) of the surface of the metal oxide particle clusters is 50 nm to 3 μm.

[0009] In the direct metal-thermoplastic resin bonding method described in Patent Document 3, the dissociation of molecular bonds in the thermoplastic resin material in the third step is promoted by metal oxide particle clusters, making it possible to efficiently obtain a strong bonded joint. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Japanese Patent Publication No. 2020-82388 [Patent Document 2] Japanese Patent Application Laid-Open No. 2008-221739 [Patent Document 3] International Publication No. 2021 / 230025 Summary of the Invention [Problem to be solved by the invention]

[0011] However, the conductive metal resin laminate described in Patent Document 1 is obtained by a method for manufacturing a conductive metal resin laminate that includes a step of placing a conductive metal resin laminate manufacturing sheet on at least one surface of a metal foil and applying pressure, and the conductive metal resin laminate manufacturing sheet and the metal foil are not firmly bonded, so the conductive metal resin laminate cannot be used in applications where a relatively large stress is applied to the bonding interface or in applications where long-term reliability is required.

[0012] Furthermore, the resin-metal laminate described in Patent Document 2 is obtained by a known heat pressing method (compression molding method) or a heat pressing method in which the laminate is sandwiched between multiple heated rolls, seamless belts, or hot plates, and, like the conductive metal-resin laminate described in Patent Document 1, the resin layer and the metal foil are not firmly bonded, and therefore cannot be used in applications in which a relatively large stress is applied to the bonding interface or in applications requiring long-term reliability.

[0013] In other words, the conductive metal resin laminate described in Patent Document 1 and the resin metal laminate described in Patent Document 2 are not intended for use in applications where large stress is applied to the bonding interface. Furthermore, these resin metal laminates have a thin metal layer formed on the surface of a relatively thick resin material, and currently there are no highly reliable resin metal laminates in which the periphery of a metal material is covered with a resin layer.

[0014] On the other hand, the metal-thermoplastic resin direct joining method described in Patent Document 3 can obtain a strong joint, but it is a technology for obtaining a joint between a metal member and a resin member, and since the joining is achieved by locally raising the temperature of the joining interface by laser irradiation, the area of ​​the joining interface formed is relatively small, and it cannot be used to produce a resin-metal joined body, which requires joining of a resin layer and a metal layer over a large area.

[0015] In view of the problems in the conventional techniques as described above, an object of the present invention is to provide a resin-metal joined body in which a resin layer and a metal layer are firmly joined without using mechanical joining such as riveting, which can be used in applications in which a large external stress is applied to the joining interface, and which has long-term reliability and in which the front and back surfaces are covered with a resin layer, and a simple and efficient method for producing the same. [Means for solving the problem]

[0016] In order to achieve the above-mentioned object, the inventors have conducted extensive research into the structure of resin-metal laminates and the state of the bonding interface, and have discovered that it is extremely effective to firmly and directly bond a resin plate to the front and back surfaces of a metal plate via a metal oxide layer, thereby arriving at the present invention.

[0017] That is, the present invention provides: A resin-metal laminated material in which a resin layer and a metal layer are laminated, a bonding region in which the resin layer and the metal layer are directly bonded via a metal oxide layer; the uppermost layer and the lowermost layer are the resin layers; The present invention provides a resin-metal laminate material characterized by the above.

[0018] In the resin-metal laminate of the present invention, the resin layer and the metal layer are firmly and directly bonded via a metal oxide layer, and the top and bottom layers are resin layers. As a result, the weight of the structure can be reduced while utilizing the excellent corrosion resistance, heat insulating properties, and electrical insulation properties of the resin layer. Furthermore, for example, by using a carbon fiber reinforced resin layer (CFRP layer) as the resin layer, high strength can be achieved. On the other hand, since there is a metal layer firmly bonded to the resin layer inside, the excellent mechanical properties and environmental resistance of the metal layer can be utilized. The side (outer periphery) of the resin-metal laminate may be in a state where the laminated surfaces of the resin layer and the metal layer are exposed, or, for example, a resin layer wider than the metal layer may be laminated and the resin layers may be sealed by crimping or the like.

[0019] Here, the metal layer in the present invention is made of a metal plate or metal sheet, and does not include, for example, a non-dense metal material such as a mesh-like material. That is, in the resin-metal laminate of the present invention, a strong bonding interface between the resin layer and the metal layer via the metal oxide layer is essential, and it is different from composite materials having a relatively weak bonding interface, such as those formed by impregnating a mesh-like metal material with a resin material.

[0020] The metal oxide layer in the resin-metal laminate of the present invention can be formed by irradiating the metal layer with a pulsed laser in the atmosphere. The metal oxide layer may be formed on the entire surface of the metal layer, but is preferably formed selectively in the bonding region.

[0021] In addition, in the resin-metal laminate of the present invention, it is preferable that the resin layer of the uppermost layer and the resin layer of the lowermost layer are made of different resins. By providing different resin layers for the uppermost and lowermost layers, the mechanical and chemical properties of the resin-metal laminate can be optimized according to the desired application. For example, if chemical stability is required for the outermost surface and lightweight and high mechanical properties are required for the resin-metal laminate as a whole, a fluororesin layer can be provided on one surface of an aluminum alloy plate (metal layer) and a carbon fiber reinforced resin layer (CFRP layer) can be provided on the other surface.

[0022] In the resin-metal laminate of the present invention, it is preferable that the bonding region is formed in the entire region where the resin layer and the metal layer contact each other. By forming the bonding region in the entire region where the resin layer and the metal layer contact each other, peeling between the resin layer and the metal layer can be suppressed.

[0023] Furthermore, in the resin-metal laminate of the present invention, it is preferable that the resin layer contains a fluororesin layer. Fluororesins have excellent chemical resistance, abrasion resistance, flame retardancy, and water and oil repellency, and have characteristic electrical properties such as low dielectric constant and dielectric loss tangent. Therefore, by including a fluororesin layer in the resin layer, the resin-metal laminate can be suitably used in related industries such as medical devices, food, and pharmaceuticals. Because fluororesins have a stable and inactive molecular structure, adhesion between fluororesins and metals is extremely difficult. However, in the resin-metal laminate of the present invention, the resin layer and metal layer are firmly bonded via a metal oxide layer, so the resin layer can be a fluororesin layer.

[0024] Furthermore, in the resin-metal laminate of the present invention, it is preferable that a shear tensile test of the resin layer and the metal layer does not result in a fracture at the bonding interface. In the resin-metal laminate of the present invention, the metal layer and the resin layer are firmly and directly bonded via the metal oxide layer, so that even when a large external stress is applied to the bonding interface, the fracture at the interface is suppressed. Here, the method of the shear tensile test of the resin layer and the metal layer is not particularly limited. For example, the resin layer and the metal layer may be partially cut to form a region consisting only of the resin layer and the metal layer, and then the region may be chucked and a shear stress may be applied.

[0025] In addition, the resin-metal laminate of the present invention has a thickness of the metal layer (T m The metal layer in the resin-metal laminate of the present invention is not a thin film intended to impart electrical properties, but also plays a role in improving the mechanical properties of the resin-metal laminate, and preferably has a thickness of 0.05 to 3.0 mm.

[0026] By making the thickness of the metal layer 0.05 mm or more, the mechanical properties of the metal layer can be utilized. Here, since the metal layer and the resin layer are firmly and directly bonded via the metal oxide layer, even if the thickness of the metal layer is 0.05 mm or more, interfacial fracture is suppressed when external stress is applied to the resin-metal laminate. On the other hand, by making the thickness of the metal layer 3.0 mm or less, the weight increase of the resin-metal laminate due to an increase in the proportion of the metal layer can be suppressed. The thickness of the metal layer is preferably 0.1 to 2.0 mm, more preferably 0.2 to 1.0 mm, and most preferably 0.3 to 0.5 mm.

[0027] Furthermore, in the resin-metal laminate of the present invention, the thickness of the metal layer (T m ) and the thickness of the resin layer (T R ) is T R ≦T m ≦20T R It is preferable that the thickness of the metal layer (T m ) to the thickness of the resin layer (T R ) or more, the mechanical properties of the metal layer can be fully reflected in the resin-metal laminate. m ) to the thickness of the resin layer (T R ) is 20 times or less, it is possible to suppress the weight increase of the resin-metal laminate material due to the increase in the proportion of the metal layer. R ≦T m ≦20T R By satisfying the above, the advantages of laminating metal and resin layers can be maximized. m ) and the thickness of the resin layer (T R ) is 2T R ≦T m ≦10T R It is more preferable to satisfy 3T. R ≦T m ≦5T R It is most preferable that

[0028] The present invention also provides a first step of irradiating one surface and the other surface of a metal plate with a pulsed laser to form a surface-modified region having a metal oxide layer; a second step of contacting a resin plate with the surface-modified region on the one surface and the surface-modified region on the other surface to form a bonded interface; a third step of heating the entire surface of the interface to be joined using an external heating means and pressing the interface to be joined using a pressing means to form a joining interface; Also provided is a method for producing a resin-metal laminate material, characterized by:

[0029] In the method for producing a resin-metal laminate of the present invention, a surface-modified region having a metal oxide layer is formed on both sides of a metal plate, and the metal plate is sandwiched between resin plates, and the entire surface of the joining interface is heated and pressed, thereby easily and efficiently obtaining a resin-metal laminate having a strong resin-metal joining interface.

[0030] In the method for producing a resin-metal laminate of the present invention, it is preferable to arrange the resin plates made of different resins in the uppermost and lowermost layers. By arranging different types of resin plates in the uppermost and lowermost layers, resin-metal laminates having a variety of lamination combinations can be produced simply and efficiently.

[0031] In the method for producing a resin-metal laminate of the present invention, it is preferable that the bonding interface is formed in the entire region on both sides of the metal plate. By contacting the resin plate with the entire region on both sides of the metal plate and applying pressure, it is possible to apply uniform pressure to the bonding interfaces on one surface and the other surface of the metal plate, and also to bond two resin plates to the metal plate in a single bonding process.

[0032] Furthermore, in the manufacturing method of the resin-metal laminate of the present invention, it is preferable to use at least one fluororesin plate. Because fluororesins have a stable and inactive molecular structure, it is extremely difficult to bond fluororesins to metals. However, in the resin-metal laminate of the present invention, the resin layer and the metal layer are firmly bonded via a metal oxide layer, so the resin layer can be a fluororesin layer. In addition, in the third step, the entire surface of the bonded interface is heated using an external heating means, and the bonded interface is pressed using a pressing means, so that a large-area bonded interface can be efficiently formed.

[0033] In the method for producing a resin-metal laminate of the present invention, it is preferable to use a metal plate having a thickness of 0.05 to 3.0 mm. m ) and the thickness of the resin plate (T R ) is T R ≦T m ≦20T R By combining a metal plate and a resin plate with an appropriate thickness, a uniform pressure can be applied to the joining interface between the metal plate and the resin plate by pressing in the third step, and a good joining interface can be formed.

[0034] In the third step, the temperature of the entire surface of the interface to be joined is increased using an external heating means, and the interface to be joined is pressed using a pressing means, thereby efficiently forming a large-area joining interface. The external heating means and pressing means are not particularly limited as long as they do not impair the effects of the present invention, and various conventionally known means can be used, but it is preferable to perform heating and pressurization in an autoclave, for example. [Effects of the Invention]

[0035] According to the present invention, it is possible to provide a resin-metal joined body in which a resin layer and a metal layer are firmly joined without using mechanical joining such as riveting, which can be used in applications where a large external stress is applied to the joining interface, and which has long-term reliability and in which the front and back surfaces are covered with resin layers, and a simple and efficient method for producing the same. [Brief explanation of the drawings]

[0036] [Figure 1] 1 is a schematic diagram showing several embodiments of a resin-metal laminate material of the present invention. [Figure 2] FIG. 2 is a schematic cross-sectional view of the resin-metal laminate material 1 of FIG. [Figure 3] 1 is a schematic diagram of a shear tensile test of a resin layer 4 and a metal layer 2. FIG. [Figure 4] 1 is a process diagram of a method for producing a resin-metal laminate material of the present invention. [Figure 5] 1 shows the autoclave molding conditions used in the examples. [Figure 6] 1 is a photograph showing the appearance of the resin-metal laminate material obtained in Example 1. [Figure 7] 1 shows the results of a shear tensile test of the resin-metal laminate obtained in Example 1. [Figure 8] 1 is a photograph showing the appearance of the resin-metal laminate material obtained in Example 2. [Figure 9] 3 is a cross-sectional photograph of the resin-metal laminate obtained in Example 2. DETAILED DESCRIPTION OF THE INVENTION

[0037] Representative embodiments of the resin-metal laminate and its manufacturing method of the present invention will be described in detail below with reference to the drawings, but the present invention is not limited to these. In the following description, the same or equivalent parts will be designated by the same reference numerals, and duplicated explanations may be omitted. Furthermore, since the drawings are intended to conceptually explain the present invention, the dimensions and ratios of the components shown may differ from the actual ones.

[0038] 1. Resin-metal laminated material Schematic diagrams showing several embodiments of the resin-metal laminate material of the present invention are shown in Figure 1. Figure 1 (a) shows a resin-metal laminate material consisting of a resin layer / metal layer / resin layer, Figure 1 (b) shows a resin-metal laminate material consisting of a resin layer / metal layer / resin layer in which the resin layers are of different types, and Figure 1 (c) shows a resin-metal laminate material consisting of a resin layer / metal layer / resin layer / metal layer / resin layer. Note that the number of resin layers and metal layers stacked is not limited to these, and any number of layers can be used.

[0039] In the resin metal laminate material 1 shown in FIG. 1(a), one surface and the other surface of the metal layer 2 are entirely coated with a resin layer 4. Because the front and back surfaces of the resin metal laminate material 1 that come into contact with the external environment are coated with the resin layer 4, the resin metal laminate material 1 can be suitably used, for example, in applications requiring environmental resistance. Furthermore, because the front and back surfaces of the resin metal laminate material 1 are coated with the resin layer 4, high vibration damping properties can also be exhibited. Since chemical stability can be imparted by using a fluororesin for the resin layer 4, for example, a resin metal laminate material 1 made of fluororesin / aluminum alloy / fluororesin can be used as a tray for medical use or chemical processing, etc.

[0040] 1(b), the resin metal laminate material 1 is configured such that one surface and the other surface of the metal layer 2 are entirely covered with a resin layer 4, and the resin layer 4 covering one surface and the resin layer 4 covering the other surface are made of different types of resin. For example, by using a fluororesin for the resin layer 4 covering one surface and a carbon fiber reinforced plastic (CFRP) for the resin layer 4 covering the other surface, the laminate material can be suitably used as a lightweight structural material that requires high strength and environmental resistance.

[0041] The resin metal laminate material 1 shown in FIG. 1(c) is composed of two metal layers 2 and three resin layers 4, with the resin layer 4 being the outermost surface. Similar to the resin metal laminate material 1 shown in FIG. 1(a), the front and back surfaces of the resin metal laminate material 1 that come into contact with the external environment are covered with the resin layer 4, making the resin metal laminate material 1 suitable for use in applications requiring environmental resistance, for example. Furthermore, because the front and back surfaces of the resin metal laminate material 1 are covered with the resin layer 4, it is also possible to achieve high vibration-damping properties. Furthermore, the five-layer structure allows for more precise design of the various properties of the resin metal laminate material 1.

[0042] In order to explain in detail the state of the bonding interface between the metal layer 2 and the resin layer 4 in the resin-metal laminate 1, a schematic cross-sectional view of the resin-metal laminate 1 in FIG. 1(a) is shown in FIG. 2. A metal oxide layer 6 is formed on the entire surface of one surface and the other surface of the metal layer 2, and the resin layer 4 is directly bonded to the metal layer 2 via the metal oxide layer 6. Here, "directly bonded" means that the resin layer 4 is bonded to the metal layer 2 without using adhesives, bolts, etc.

[0043] Furthermore, although the metal oxide layer 6 is formed on the entire surface of the metal layer 2, it is not necessary for the entire surface of the metal layer 2 to be densely covered with the metal oxide layer 6, and it is sufficient if, for example, a dotted or linear metal oxide layer 6 is formed on the entire surface of the metal layer 2. More specifically, it is preferable that the metal oxide layer 6 occupies 20% or more of the area of ​​the interface to be joined.

[0044] 2, for the sake of explanation, the metal oxide layer 6 is depicted as being relatively thick, but in reality, the metal oxide layer 6 is extremely thin, having a thickness of approximately 10 to 500 nm. The metal oxide layer 6 is preferably a metal oxide particle cluster formed by continuously bonding metal oxide particles having a particle size of 5 to 500 nm, and is preferably a metal oxide particle cluster having a maximum height (Sz) of 50 nm to 3 μm.

[0045] By setting the maximum height (Sz) of the surface of the metal oxide particle clusters, which form the bonding interface on the metal layer 2 side, to 50 nm to 3 μm, it is possible to ensure adhesion between the metal oxide particle clusters and the resin layer 4. By setting the maximum height (Sz) of the surface of the metal oxide particle clusters to 50 nm or more, it is possible to improve the strength of the bonding portion by filling with the resin layer 4, and by setting it to 3 μm or less, it is possible to prevent the resin layer 4 from not being filled and remaining as voids. The maximum height (Sz) of the surface of the metal oxide particle clusters is more preferably 100 nm to 2 μm, and most preferably 200 nm to 1 μm.

[0046] The particle size of the metal oxide particles is preferably 50 to 200 nm. By setting the particle size of the metal oxide particles to 50 nm or more, it becomes easy to set the maximum surface height (Sz) of the metal oxide particle cluster to 50 nm or more. Furthermore, by setting the particle size of the metal oxide particles to 200 nm or less, it becomes easy to set the maximum surface height (Sz) of the metal oxide particle cluster to 3 μm or less. In addition, by setting the particle size of the metal oxide particles to 50 to 200 nm, it becomes possible to promote dissociation of C—F bonds of the fluororesin material on the surface of the metal oxide particles, for example, when the fluororesin material is heated.

[0047] In addition, in the resin metal laminate material 1, the thickness of the metal layer 2 (T m ) is 0.05 to 3.0 mm. By making the thickness of the metal layer 2 0.05 mm or more, the mechanical properties of the metal layer 2 can be utilized. Here, since the metal layer 2 and the resin layer 4 are firmly and directly bonded via the metal oxide layer 6, even if the thickness of the metal layer 2 is 0.05 mm or more, interfacial fracture is suppressed when external stress is applied to the resin-metal laminate material 1. On the other hand, by making the thickness of the metal layer 2 3.0 mm or less, an increase in the weight of the resin-metal laminate material 1 due to an increase in the proportion of the metal layer 2 can be suppressed. The thickness of the metal layer 2 is preferably 0.1 to 2.0 mm, more preferably 0.2 to 1.0 mm, and most preferably 0.3 to 0.5 mm.

[0048] In addition, the thickness of the metal layer 2 (Tm ) and the thickness of resin layer 4 (T R ) is T R ≦T m ≦20T R It is preferable that the thickness (T m ) to the thickness of resin layer 4 (T R ) or more, the mechanical properties of the metal layer 2 can be sufficiently reflected in the resin-metal laminate material 1. On the other hand, m ) to the thickness of resin layer 4 (T R ) or less, it is possible to suppress an increase in the weight of the resin-metal laminate material 1 due to an increase in the proportion of the metal layer 2. That is, T R ≦T m ≦20T R By satisfying the above condition, it is possible to maximize the merit of laminating the metal layer 2 and the resin layer 4. m ) and the thickness of resin layer 4 (T R ) is 2T R ≦T m ≦10T R It is more preferable to satisfy 3T. R ≦T m ≦5T R It is most preferable that

[0049] The metal material used for the metal layer 2 is not particularly limited as long as it does not impair the effects of the present invention, and various conventionally known metal materials can be used, such as stainless steel, titanium, titanium alloys, aluminum, aluminum alloys, magnesium, magnesium alloys, copper, and copper alloys. From the viewpoint of specific strength, aluminum, aluminum alloys, titanium, and titanium alloys are preferred, and from the viewpoint of corrosion resistance, stainless steel, titanium, and titanium alloys are preferred. Furthermore, in order to control the conductivity as a structural material, copper or a copper alloy is preferred.

[0050] Various thermoplastic resins can be used for the resin layer 4. The thermoplastic resin is not particularly limited as long as it does not impair the effects of the present invention, and conventionally known general-purpose plastics, engineering plastics, and super-engineering plastics can be suitably used. More specifically, for example, polyethylene (PE), polypropylene (PP), polystyrene (PS), polyacetal (POM), polyvinyl chloride (PVC), polyethylene terephthalate (PET), ABS resin (ABS), polyamide (PA), polycarbonate (PC), PET (Polyethylene Terephthalate), and various carbon fiber reinforced plastics (CFRP) and glass fiber reinforced plastics (GFRP) can be used.

[0051] In the resin-metal laminate 1, it is preferable that a shear tensile test of the resin layer 4 and the metal layer 2 does not result in a fracture at the bonding interface. In the resin-metal laminate 1, the metal layer 2 and the resin layer 4 are firmly and directly bonded via the metal oxide layer 6, so that even when a large external stress is applied to the bonding interface, the fracture at the interface is suppressed. Here, the method for the shear tensile test of the resin layer 4 and the metal layer 2 is not particularly limited. For example, as shown in FIG. 3, the resin layer 4 and the metal layer 2 may be partially cut to form a region consisting only of the resin layer 4 and the metal layer 2, and then the region may be chucked and a shear stress (L) may be applied.

[0052] 2. Manufacturing method of resin-metal laminated material 4 is a process diagram of the method for producing a resin-metal laminate of the present invention. The method for producing a resin-metal laminate of the present invention includes a first step (S01) of forming a surface-modified region having a metal oxide layer, a second step (S02) of forming a joining interface, and a third step (S03) of forming a joining interface. Each step will be described in detail below.

[0053] (1) First step (S01: Surface modified region formation step) The first step (S01) is a step for obtaining a surface-modified region that contributes to the formation of a strong bonded interface. In the surface-modified region, metal oxide particle clusters are formed by continuously bonding metal oxide particles having particle diameters of 5 to 500 nm, and the maximum height (Sz) of the metal oxide particle clusters is preferably formed to be 50 nm to 3 μm.

[0054] By setting the maximum surface height (Sz) of the metal oxide particle clusters at the joining interface on the metal plate side that will become metal layer 2 to 50 nm to 3 μm, it is possible to ensure adhesion between the metal oxide particle clusters and the resin plate that will become resin layer 4 in the third step (S03). Setting the maximum surface height (Sz) of the metal oxide particle clusters to 50 nm or more allows the strength of the joint to be improved by filling with resin material, while setting it to 3 μm or less prevents voids from remaining without being filled with resin material. A more preferred maximum surface height (Sz) of the metal oxide particle clusters is 100 nm to 2 μm, and the most preferred maximum height (Sz) is 200 nm to 1 μm.

[0055] The particle size of the metal oxide particles is preferably 50 to 200 nm. By setting the particle size of the metal oxide particles to 50 nm or more, it becomes easy to set the maximum surface height (Sz) of the metal oxide particle cluster to 50 nm or more. Furthermore, by setting the particle size of the metal oxide particles to 200 nm or less, it becomes easy to set the maximum surface height (Sz) of the metal oxide particle cluster to 3 μm or less. In addition, by setting the particle size of the metal oxide particles to 50 to 200 nm, it becomes possible to promote the dissociation of the bond of the resin material when the resin material is heated on the surface of the metal oxide particles.

[0056] In the first step (S01), specifically, a pulsed laser is irradiated onto the surface of a metal material in an oxidizing atmosphere. The laser used in the first step is not particularly limited as long as it does not impair the effects of the present invention, and various conventionally known lasers can be used. For example, a semiconductor laser that can efficiently heat a metal material can be preferably used.

[0057] The irradiation energy of one pulse of the pulsed laser is preferably 0.2 to 1.0 mJ. By setting the irradiation energy of one pulse of the pulsed laser to 0.2 to 1.0 mJ, metal oxide particle clusters are formed in the irradiated region in which metal oxide particles having particle diameters of 5 to 500 nm are continuously bonded together, and the maximum surface height (Sz) of the metal oxide particle clusters can be set to 50 nm to 3 μm.

[0058] Furthermore, the type of oxidizing atmosphere is not particularly limited as long as it does not impair the effects of the present invention, and it is sufficient that the atmosphere be one in which metal oxide particle clusters are formed on the surface of the metal plate by irradiation with a pulsed laser, for example, the treatment may be carried out in air.

[0059] The surface-modified region may be formed on the interface between the metal plates, and preferably occupies at least 20% of the area of ​​the interface. By forming the surface-modified region at least 20% of the area of ​​the interface, high joint strength and reliability can be ensured for the entire joint. The surface-modified region may be formed in a planar shape, or may have an appropriate pattern, such as a line shape.

[0060] (2) Second process (S02: bonded interface formation process) The second step (S02) is a step of bringing the metal plate, on which the surface modified region has been formed in the first step (S01), into contact with the resin plate to form a joining interface.

[0061] Here, the resin metal laminate material 1 may have a structure in which the metal plate and the resin plate are continuously integrated by the bonding interface formed between them, and any number of metal plates and resin plates can be laminated.

[0062] The metal plate used as the metal layer 2 is not particularly limited as long as it does not impair the effects of the present invention, and various conventionally known metal plates can be used, such as stainless steel, titanium, titanium alloys, aluminum, aluminum alloys, magnesium, magnesium alloys, copper, copper alloys, etc., but from the viewpoint of specific strength, it is preferable to use aluminum, aluminum alloys, titanium, and titanium alloys, and from the viewpoint of corrosion resistance, etc., it is preferable to use stainless steel, titanium, and titanium alloys.

[0063] Furthermore, various thermoplastic resins can be used for the resin plate that becomes the resin layer 4. The thermoplastic resin is not particularly limited as long as it does not impair the effects of the present invention, and conventionally known general-purpose plastics, engineering plastics, and super-engineering plastics can be suitably used. More specifically, for example, polyethylene (PE), polypropylene (PP), polystyrene (PS), polyacetal (POM), polyvinyl chloride (PVC), polyethylene terephthalate (PET), ABS resin (ABS), polyamide (PA), polycarbonate (PC), PET (Polyethylene Terephthalate), and various carbon fiber reinforced plastics (CFRP) and glass fiber reinforced plastics (GFRP) can be used.

[0064] It is also preferable to use at least one fluororesin plate. Fluororesin has a stable and inactive molecular structure, making it extremely difficult to bond fluororesin to metal. However, in the resin-metal laminate of the present invention, the resin layer 4 and the metal layer 2 are firmly bonded via the metal oxide layer 6, so the resin layer 4 can be a fluororesin layer. In addition, in the third step (S03), the temperature of the entire surface of the bonded interface is increased using an external heating means, and the bonded interface is pressed using a pressing means, so that a large-area bonded interface can be efficiently formed.

[0065] It is also preferable to cover one surface and the other surface of the metal plate with different types of resin plates. By disposing different types of resin plates on one surface and the other surface of the metal plate, resin-metal laminate materials 1 having a variety of layer combinations can be produced simply and efficiently.

[0066] Here, the thickness of the metal plate (T m ) is set to 0.05 to 3.0 mm, and the thickness of the metal plate (T m ) and the thickness of the resin plate (T R ) is T R ≦T m ≦20T R By designing the resin metal laminate material 1 so as to satisfy the above, it is possible to obtain a good resin metal laminate material 1 simply and efficiently.

[0067] By making the thickness of the metal plate 0.05 mm or more, the mechanical properties of the metal plate can be utilized. Here, since the metal plate and the resin plate are firmly and directly bonded via the metal oxide layer 6, even if the thickness of the metal plate is 0.05 mm or more, interfacial fracture is suppressed when external stress is applied to the resin-metal laminate material 1. On the other hand, by making the thickness of the metal plate 3.0 mm or less, an increase in the weight of the resin-metal laminate material 1 due to an increase in the proportion of the metal layer 2 can be suppressed. The thickness of the metal plate is preferably 0.1 to 2.0 mm, more preferably 0.2 to 1.0 mm, and most preferably 0.3 to 0.5 mm.

[0068] Also, the thickness of the metal plate (T m ) and the thickness of the resin plate (T R ) is T R ≦T m ≦20T R It is preferable that the thickness of the metal plate (T m ) to the thickness of the resin plate (T R ) or more, the mechanical properties of the metal plate can be sufficiently reflected in the resin-metal laminate material 1. m ) to the thickness of the resin plate (T R ) or less, it is possible to suppress an increase in the weight of the resin-metal laminate material 1 due to an increase in the proportion of the metal layer 2. That is, T R ≦Tm ≦20T R By satisfying the above, the advantages of laminating metal sheets and resin sheets can be maximized. m ) and the thickness of the resin plate (T R ) is 2T R ≦T m ≦10T R It is more preferable to satisfy 3T. R ≦T m ≦5T R It is most preferable that

[0069] (3) Third process (S03: bonding interface formation process) The third step (S03) is a step of simultaneously heating and pressing the entire surface of the interface to be bonded formed in the second step (S02) using an external heating means and pressing means, thereby achieving bonding.

[0070] By using an external heating means to heat the entire surface of the bonded interface and using a pressing means to press the bonded interface, a large-area bonded interface can be efficiently formed. The external heating means and pressing means are not particularly limited as long as they do not impair the effects of the present invention, and various conventionally known means can be used. For example, it is preferable to heat and pressurize using an autoclave. By using an autoclave, it is possible to produce a resin-metal laminate (uniform and high-strength bonding over a large area), which is difficult to achieve by partial heating using laser irradiation. On the other hand, when heating the bonded interface using laser irradiation, for example, it is not possible to heat the entire surface of the bonded interface simultaneously and uniformly, so it cannot be used to produce a resin-metal laminate.

[0071] The temperature and applied pressure at the interface to be joined may be set appropriately depending on the type, size, shape, etc. of the metal and resin materials. For example, when laminating a 0.1 mm thick fluororesin plate on one surface of a 0.3 mm thick aluminum alloy plate and a polypropylene matrix CFRP plate on the other surface, the temperature may be maintained at 150 to 250°C and 0.1 to 1.0 MPa for approximately 20 minutes.

[0072] Furthermore, it is preferable to form a bonding interface in the entire region on both sides of the metal plate material. By abutting the resin plate against the entire region on both sides of the metal plate material and applying pressure, it is possible to apply uniform pressure to the bonding interfaces on one surface and the other surface of the metal plate material, and also to bond two resin plates to the metal plate in a single bonding process.

[0073] Representative embodiments of the present invention have been described above, but the present invention is not limited to these, and various design modifications are possible, all of which are included in the technical scope of the present invention. [Example]

[0074] Example 1 Using the manufacturing method of the resin-metal laminate of the present invention, a fluororesin plate (ETFE: tetrafluoroethylene-ethylene copolymer) was bonded to the entire surface of one side of an aluminum alloy plate (A5052), and a CFRP plate with a polypropylene matrix was bonded to the entire surface of the other side, thereby obtaining the resin-metal laminate of the present invention.

[0075] The aluminum alloy plate has a thickness of 0.3 mm, a width of 100 mm, and a length of 100 mm. The fluororesin plate has a thickness of 0.1 mm, and the CFRP plate has a thickness of 0.14 mm (four layers laminated), and the width and length of the plate are the same as those of the aluminum alloy plate. The thickness of the aluminum alloy plate, which is a metal plate, is in the range of 0.05 to 3.0 mm, and the thickness of the aluminum alloy plate (T m ) and the thickness of each resin layer (T R ) is T R ≦T m ≦20T R It meets the following criteria.

[0076] The entire surfaces of one and the other of the aluminum alloy plates, which would become the bonding interface, were irradiated with laser in the atmosphere to form a surface-modified region (first step). The laser used was a YLP pulse laser manufactured by IPG, with an average output of 50 W (energy per pulse: 1 mJ) and a laser dot diameter of 59 μm. The laser dot spacing was 30 μm in the X-axis direction and 70 μm in the Y-axis direction.

[0077] Next, a fluororesin plate and a CFRP plate were placed on the surface-modified region (second step), and the joining interface was heated and pressurized using an autoclave (third step) to obtain a resin-metal laminate. The autoclave used was a DLF-4020 manufactured by Hanyuda Iron Works, and the autoclave molding conditions shown in Figure 5 were applied. The holding temperature was 200°C, the applied pressure was 0.5 MPa, and the holding time was 20 minutes or more.

[0078] A photograph of the appearance of the obtained resin-metal laminate is shown in Figure 6. The resin and metal plates were not peeled off, and the entire resin-metal laminate was distorted, indicating that the resin / metal bonded interface was extremely strong. In addition, the fluororesin plate and CFRP plate were bonded to the entire surface of the aluminum alloy plate, and cross-sectional observation revealed no defects such as peeling or voids at the bonded interfaces between the resin and aluminum alloy plates.

[0079] Next, the plates were machined as shown in Figure 3, and the bond strength of the fluororesin plate / aluminum alloy plate and the shear tensile strength of the CFRP plate / aluminum alloy plate were evaluated using a tensile testing machine. No fracture was observed at the bond interface in either case. Figure 7 shows the relationship between test force and stroke when a shear tensile test was performed on the bond interface of the fluororesin plate / aluminum alloy plate. The maximum test force reached 48 N, and after the fluororesin elongated and the load decreased, fracture occurred at the fluororesin. The shear tensile test was performed in accordance with JIS Z0237, using a Shimadzu AGS-X10KN testing machine. The test piece width was 25 mm.

[0080] Example 2 A resin metal laminate of the present invention was obtained in the same manner as in Example 1, except that CFRP plates were joined to the entire surfaces of one surface and the other surface of an aluminum alloy plate (A5052).

[0081] A photograph of the appearance of the obtained resin-metal laminate is shown in Figure 8, and a cross-sectional photograph is shown in Figure 9. The CFRP plate is bonded to the entire surface of the aluminum alloy plate, and no defects such as delamination or voids are observed at the bonding interface between the CFRP plate and the aluminum alloy plate. Furthermore, when the same type of resin plate is bonded to both sides of the aluminum alloy plate, no distortion of the resin-metal laminate is observed.

[0082] From the above results, it can be seen that by using the method for producing a resin-metal laminate of the present invention, the resin layer and the metal layer are firmly joined without using mechanical joining such as riveting, and a resin-metal joined body having long-term reliability can be obtained, which can be used even in applications where large external stress is applied to the joining interface. [Explanation of symbols]

[0083] 1. Resin-metal laminated material, 2...metal layer, 4. Resin layer, 6···Metal oxide layer.

Claims

1. A resin-metal laminate material in which a resin layer and a metal layer are laminated, a bonding region in which the resin layer and the metal layer are directly bonded to each other via a metal oxide layer; the uppermost layer and the lowermost layer being the resin layer; A resin-metal laminate material characterized by:

2. the uppermost resin layer and the lowermost resin layer are made of different resins; The resin-metal laminate material according to claim 1 ,

3. the bonding region is formed in the entire region where the resin layer and the metal layer are in contact with each other; The resin-metal laminate material according to claim 1 or 2,

4. The resin layer includes a fluororesin layer; The resin-metal laminate material according to claim 1 or 2,

5. In a shear tensile test of the resin layer and the metal layer, no fracture occurs at the bonding interface; The resin-metal laminate material according to claim 1 or 2,

6. The thickness of the metal layer (T m ) is 0.05 to 3.0 mm; The resin-metal laminate material according to claim 1 or 2,

7. The thickness of the metal layer (T m ) and the thickness of the resin layer (T R ) is T R ≦T m ≦20T R To satisfy the following: The resin-metal laminate material according to claim 1 or 2,

8. A first step of irradiating one surface and another surface of a metal plate with a pulsed laser to form a surface modified region having a metal oxide layer; a second step of contacting a resin plate with the surface-modified region on the one surface and the surface-modified region on the other surface to form a bonded interface; a third step of heating the entire surface of the bonded interface by using an external heating means and pressing the bonded interface by using a pressing means to form a bonded interface; A method for producing a resin-metal laminate material, comprising the steps of:

9. disposing the resin plates made of different resins as the top layer and the bottom layer; The method for producing a resin-metal laminate according to claim 8, further comprising the steps of:

10. forming the bonding interface in all areas of the one surface and the other surface; The method for producing a resin-metal laminate according to claim 8 or 9, characterized in that

11. Use at least one fluororesin plate; The method for producing a resin-metal laminate according to claim 8 or 9, characterized in that

12. The thickness of the metal layer (T m ) is 0.05 to 3.0 mm; The method for producing a resin-metal laminate according to claim 8 or 9, characterized in that

13. The thickness of the metal plate (T m ) and the thickness of the resin plate (T R ) is T R ≦T m ≦20T R To satisfy the following: The method for producing a resin-metal laminate according to claim 8 or 9, characterized in that

14. using an autoclave for the external heating means and the pressing means; The method for producing a resin-metal laminate according to claim 8 or 9, characterized in that

Citation Information

Patent Citations

  • Plastic metal laminate

    JP2008221739A

  • Conductive metal resin laminate and molded body thereof

    JP2020082388A

  • Method of bonding thermoplastic resin and metal

    WO2021230025A1

Cited By

  • --CMC omitted

    KR1020240029971A