Fumed silica for rubber composition and method of compressing fumed silica

Fumed silica with enhanced tap density and pore structure addresses dispersion issues in rubber compositions, improving wear resistance and fuel efficiency by reducing blending times and maintaining productivity.

JP2024180223APending Publication Date: 2024-12-26TOKUYAMA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023136383
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-15
Filing Date
2023-08-24
Publication Date
2024-12-26

AI Technical Summary

Technical Problem

Existing methods for blending dry silica in rubber compositions face issues with low tap density leading to poor dispersion and increased productivity loss due to the need for multiple divisions, resulting in reduced wear resistance and fuel efficiency.

Method used

The use of fumed silica with increased tap density and a controlled pore structure, combined with specific surface area and silanol group density, allows for improved dispersion and reduced blending times, using methods like ball milling, vibration milling, and uniaxial compression pressing.

Benefits of technology

This approach enables sufficient dispersion of fumed silica in rubber components, enhancing wear resistance and fuel efficiency while maintaining productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024180223000001
    Figure 2024180223000001
  • Figure 2024180223000002
    Figure 2024180223000002
  • Figure 2024180223000003
    Figure 2024180223000003
Patent Text Reader

Abstract

To provide fumed silica which can be sufficiently dispersed in a rubber component even with a small number of times of divisional compounding, and a method for compressing the fumed silica.SOLUTION: Fumed silica for rubber compositions has a) a tapped density of 200 g / L or more, b) a pore peak radius of 22 nm or greater obtained by applying the BJH method to the adsorption isotherm from nitrogen adsorption; and c) a pore volume of 1.6 mL / g or more. The BET specific surface area of the fumed silica for rubber compositions is preferably 180 m2 / g or more and 500 m2 / g or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fumed silica for use in a rubber composition and a method for compressing the fumed silica, and more particularly to a fumed silica that is easily and sufficiently dispersed in a rubber component and a method for compressing the fumed silica. [Background technology]

[0002] In addition to being fuel-efficient, automobile tires are required to have a long life. To achieve a long life, it is necessary to improve the wear resistance and heat aging resistance of tires. To improve the wear resistance, carbon black has been blended as a reinforcing filler into rubber compositions for tires.

[0003] On the other hand, it is known that wet silica is effective in improving fuel economy, but the abrasion resistance when wet silica is blended is inferior to that when carbon black is blended. Therefore, when wet silica is used as a reinforcing filler, a part of the carbon black blended amount is replaced by wet silica, and the amount of carbon black blended is relatively reduced, so that it is known that a decrease in the abrasion resistance of the rubber material for tires is unavoidable.

[0004] Patent Document 1 proposes replacing a part of wet silica with dry silica, and describes that dry silica can improve fuel economy and suppress deterioration of rubber hardness more than wet silica. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2016-104840 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in Patent Document 1, it is believed that the dry silica is blended in a bulky state. When such bulky (low tap density) dry silica is blended using a Banbury mixer, which is a general kneading device for rubber compositions, there is a problem that the dry silica flows out without being mixed into the rubber component. Therefore, it is necessary to divide and blend the planned amount of dry silica. However, there is a problem that the productivity decreases as the number of divisions increases.

[0007] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a fumed silica which can be sufficiently dispersed in a rubber component even with a small number of times of divided blending, and a method for compressing the fumed silica. [Means for solving the problem]

[0008] The present inventors have found that even if fumed silica with a high tap density is simply used, aggregated particles of several tens of μm may occur in unvulcanized or vulcanized rubber. Based on this finding, the present inventors have found that by not only increasing the tap density but also making the pore structure of the surface of the fumed silica into a specific structure, the fumed silica can be sufficiently dispersed even if it is distributed and mixed in the rubber component only a small number of times, and have completed the present invention.

[0009] Based on the above, the aspects of the present invention are as follows.

[0010] [1] A fumed silica for rubber compositions having a tap density of 200 g / L or more, a pore peak radius of 22 nm or more, obtained by applying the BJH method to an adsorption isotherm by nitrogen adsorption, and a pore volume of 1.6 mL / g or more. [2] The BET specific surface area of ​​fumed silica for rubber compositions is 180m 2 / g or more 500m 2 / g or less. [3] The fumed silica for rubber compositions according to [1] or [2], wherein the fumed silica for rubber compositions is an untreated fumed silica for rubber compositions.

[0011] [4] A method for compressing fumed silica, in which fumed silica having a tap density of less than 200 g / L is subjected to uniaxial compression pressing to obtain compressed fumed silica having a tap density of 200 g / L or more. Effect of the Invention

[0012] According to the present invention, it is possible to provide fumed silica which can be sufficiently dispersed in a rubber component even with a small number of times of divided blending, and a method for compressing the fumed silica. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will now be described in detail based on specific embodiments in the following order. 1. Fumed silica for rubber compositions 2. Method of compressing fumed silica 2.1. When using a ball mill 2.2. When using a vibration mill 2.3.When using a uniaxial opposed compression press 3. Rubber composition 3.1. Diene rubber 3.2.Silane coupling agents 3.3. Amount of each ingredient 3.4.Other Ingredients 4. Method for producing rubber composition

[0014] (1. Fumed silica for rubber compositions) The fumed silica for rubber compositions according to the present embodiment is fumed silica used for compounding in rubber compositions, and is particularly preferably used in rubber compositions for tires. Fumed silica is fine particle silicon dioxide produced by high-temperature hydrolysis of silicon tetrachloride in an oxyhydrogen flame. Therefore, fumed silica is also called dry silica, as its production method differs from that of wet silica produced by wet methods such as precipitation and gelation. Among wet silica, precipitated silica, which is generally used as a rubber reinforcing material, has a specific surface area of ​​200 m2 / g, while for fumed silica it is 400m 2 / g is used as a reinforcing material for silicone rubber, etc. Therefore, because of its high specific surface area, the primary particle size of the primary aggregate (smallest constituent) of fumed silica is smaller than that of precipitated silica. The particles of fumed silica are aggregated and fused together in a beaded shape, forming bulky aggregates.

[0015] In this embodiment, the tap density of the fumed silica for rubber compositions is 200 g / L or more. Since the fumed silica is bulky as described above, the tap density of the fumed silica is usually lower than 200 g / L in many cases. Therefore, when the tap density of the fumed silica is low (when the fumed silica is bulky), the fumed silica for rubber compositions according to this embodiment is preferably fumed silica (compressed fumed silica) in which the tap density is increased by compressing the fumed silica.

[0016] Since the tap density of the fumed silica for rubber compositions is 200 g / L or more, the fumed silica for rubber compositions can be sufficiently dispersed in a rubber composition for tires even when the fumed silica for rubber compositions is blended with a rubber component and kneaded. In addition, even when a Banbury mixer is used, which is difficult to knead with bulky components, the bulkiness is suppressed, so that the fumed silica can be sufficiently kneaded with other components.

[0017] The tap density of the fumed silica for rubber compositions is preferably 250 g / L or more, and more preferably 300 g / L or more. The upper limit of the tap density is not particularly limited, but is, for example, 320 g / L or less from the viewpoint of production.

[0018] In the present embodiment, the bulkiness of the fumed silica for rubber compositions may be evaluated by a parameter other than the tap density. For example, it may be evaluated by the apparent density measured by the tamp method specified in JIS K5101-12-2.

[0019] The apparent density by the tamp method of the fumed silica for rubber compositions is preferably 150 g / L or more and 250 g / L or less, and more preferably 170 g / L or more and less than 200 g / L. A detailed method for measuring the apparent density by the tamp method will be described in the examples.

[0020] The method of compressing fumed silica will be described in detail later, but examples of the method of compressing fumed silica include a method of compressing with a ball mill and a method of compressing with a vibration mill. In these methods, the fumed silica is compressed between balls or between a ball and a mill container. When such compression is performed with a small contact area using a hard material, agglomerated particles with low dispersibility (for example, particles with a particle size of 20 μm or more) may be generated due to a mechanochemical reaction. As a result, agglomerated particles due to poor dispersion of fumed silica may occur in the rubber composition, even though the tap density of the fumed silica is high and the number of divided blends is small.

[0021] The inventors speculate that such low dispersibility is due to the fact that compression forms pores on the surface of the fumed silica that are too small for the silane coupling agent, which improves the wettability between the rubber component and the fumed silica and acts as a cross-linker, to penetrate, slowing down the rate at which the silane coupling agent penetrates into the fumed silica aggregates, and as a result, the coupling agent is unable to react uniformly enough.

[0022] Therefore, the fumed silica for rubber compositions according to the present embodiment has a pore peak radius of 22 nm or more and a pore volume of 1.6 mL / g or more, which are obtained by applying the BJH method to an adsorption isotherm by nitrogen adsorption. The fumed silica for rubber compositions, in which the pores on the surface of the fumed silica are controlled as described above, can sufficiently react with a silane coupling agent even if it has a high tap density, and can suppress the generation of aggregated particles.

[0023] The pore peak radius is preferably 30 nm or more, more preferably 50 nm or more, while the upper limit of the pore peak radius is not particularly limited, and is, for example, 85 nm.

[0024] The pore volume is preferably 2 mL / g or more, more preferably 4 mL / g, while the upper limit of the pore volume is not particularly limited, and is, for example, 6 mL / g.

[0025] The above pore peak radius and pore volume are physical property values ​​obtained by applying the BJH method to the adsorption isotherm by nitrogen adsorption. The adsorption isotherm by nitrogen adsorption can be obtained by measurement and analysis under conditions where a sample is degassed at 150°C to a pressure of 1 Pa or less and nitrogen is adsorbed at liquid nitrogen temperature.

[0026] In this embodiment, the BET specific surface area of ​​the fumed silica for rubber compositions is 180 m 2 / g or more, and 2 / g or more is more preferable, and 250m 2 When the BET specific surface area of ​​the fumed silica for a rubber composition is within the above range, the number of silanol groups that serve as reaction points with a diene rubber or a silane coupling agent can be sufficiently secured in the fumed silica for a rubber composition.

[0027] The upper limit of the BET specific surface area of ​​the fumed silica for rubber compositions is not particularly limited, but may be, for example, 500 m 2 / g. If the BET specific surface area of ​​the fumed silica for rubber compositions is too small, the flame temperature during the production of the fumed silica must be increased, and the structure specific to the fumed silica is lost, which tends to make it difficult to produce the fumed silica stably. If the BET specific surface area of ​​the fumed silica for rubber compositions is too large, it tends to make it difficult to produce the fumed silica stably. The BET specific surface area mentioned above is a specific surface area measured by the nitrogen adsorption BET method.

[0028] Fumed silica has siloxane bonds, but on the surface of the fumed silica, in addition to the siloxane groups, there are silanol groups in which a hydroxy group is bonded to a silicon atom. The density of silanol groups on the surface of fumed silica (surface silanol group density) is lower than that of wet silica due to differences in the manufacturing method. In this embodiment, the surface silanol group density of the fumed silica for rubber compositions is 3 / nm 2 The surface silanol group density is within the above range, and while maintaining the amount of silanol groups that are reaction sites with coupling agents, it is possible to prevent the decrease in wettability with rubber due to moisture adsorption on the silica surface, and thus further fine dispersion can be expected. In addition, it is expected that the aggregation of silica during the compression process, which is likely to increase due to the high adsorption of moisture, can be prevented.

[0029] The surface silanol group density may be measured by, for example, the Karl Fischer method, the Igros method, or active hydrogen titration using a Grignard reagent.

[0030] In addition, silanol groups are prone to adsorb water. Therefore, surface treatment is sometimes performed to reduce the reactivity with water by reacting the silanol groups with other substances. Surface-treated fumed silica is called surface-treated fumed silica, and fumed silica that has not been surface-treated is called untreated fumed silica.

[0031] In this embodiment, the surface-treated fumed silica and the untreated fumed silica are distinguished by the modification hydrophobicity (M value) shown below. The modification hydrophobicity (M value) is a value obtained by a measurement method utilizing the fact that the surface-treated fumed silica floats in water but is completely suspended in methanol. The method described in the examples of International Publication No. 2004 / 099075 can be used to measure the M value. When the surface-treated fumed silica and the untreated fumed silica are expressed using the M value, the M value of the surface-treated fumed silica is 1 or more, and the M value of the untreated fumed silica is less than 1.

[0032] In this embodiment, from the viewpoint that the silane coupling agent has a bulky molecular structure and can react in sufficient amount with the silica surface, it is preferable that the fumed silica for rubber compositions is untreated fumed silica for rubber compositions in which the moisture content that induces self-condensation of the coupling agent is small but the silanol groups, which are reaction sites, are sufficiently secured.

[0033] (2. Method of compressing fumed silica) The fumed silica for rubber compositions according to the present embodiment has a tap density of 200 g / L or more. However, due to its manufacturing method, the fumed silica is bulky and has a low tap density. Therefore, the fumed silica for rubber compositions having a tap density of 200 g / L or more is generally obtained by compressing the fumed silica.

[0034] As described above, the method of compressing fumed silica includes, for example, a method of compressing with a ball mill, a method of compressing with a vibration mill, etc. However, in the normal compression method, the pores on the surface of the fumed silica become too small by compression, and it is considered that the speed at which the silane coupling agent penetrates and diffuses into the silica aggregate particles becomes slow in the small pores.

[0035] Therefore, the surface of the fumed silica may be partially coated before compression so that the pore peak radius and pore volume after compression satisfy the above-mentioned range. For example, a surfactant, wax, etc. can be used for the coating. As the surfactant, a nonionic surfactant is preferable. As the nonionic surfactant, a fatty acid surfactant such as coconut oil fatty acid N-methylethanolamide, and an alkylamine ether surfactant such as N,N',N'-tris(2-hydroxyethyl)-N-alkyl(C14-C18))1,3-diaminopropane, an alkyldiamine EO adduct, are exemplified. In addition, as the wax, a hydrocarbon wax is preferable, for example, paraffin wax. As the paraffin wax, a general paraffin wax having a melting point of about 60 to 80°C, a paraffin wax usually used as an anti-aging agent for tires, etc. are preferable. Examples of coating methods include a method in which molten wax is sprayed from a one-fluid or two-fluid nozzle into a mixer in which fumed silica is mixed and stirred, and a method in which fumed silica and fine powder wax particles are mixed and then heated to a temperature equal to or higher than the melting point of the wax to melt the wax and diffuse it over the silica surface.

[0036] When a uniaxial opposed compression press, a ball mill or a vibration mill is used as a method for compressing the fumed silica, it is preferable to employ the compression treatment conditions shown below.

[0037] (2.1. When using a ball mill) When the ball diameter is small, the curvature is small, so the compressive force by the balls tends to be a point load, and when the ball diameter is large, the compressive force by the balls tends to be a surface load. Therefore, the ball diameter in the ball mill is preferably 27 to 60 mm, and more preferably 32 to 45 mm. When the ball diameter is too small, the impact force due to the concentration of the load during crushing and compression is too strong, and the pore structure on the surface of the fumed silica tends to change and not satisfy the above-mentioned range. When the ball diameter is too large, the number of balls packed with the same volume is reduced, so the collision frequency is low, which increases the crushing time and may increase the production cost.

[0038] The rotation speed of the ball mill is preferably 50 to 600 rpm, more preferably 200 to 400 rpm. If the rotation speed is too low, the balls do not fall but simply roll on the pot wall, and the impact force during pulverization is insufficient, which may result in a failure to increase the tap density of the fumed silica. If the rotation speed is too low, it is necessary to extend the pulverization time in order to increase the tap density of the fumed silica to 200 g / L or more, which may result in a decrease in productivity and an increase in production costs. If the rotation speed is too high, the pulverization efficiency may decrease.

[0039] The ball filling rate in the ball mill is preferably 10 to 80%, more preferably 20 to 50%. If the ball filling rate is too low, the tap density of the fumed silica may not be high due to insufficient grinding efficiency. If the ball filling rate is too low, the grinding time must be extended to make the tap density of the fumed silica 200 g / L or more, which may reduce productivity and increase production costs. If the ball filling rate is too high, the amount of material filled may decrease, resulting in reduced grinding efficiency.

[0040] (2.2. Using a Vibration Mill) The ball diameter or rod diameter in the vibration mill is preferably 27 mm or more, more preferably 32 to 60 mm. If the ball diameter or rod diameter is too small, the impact during grinding is too strong, and the pore structure on the surface of the fumed silica changes, tending not to satisfy the above-mentioned range. If the ball diameter is too large, the gap between the balls is large and the collision frequency is low, so the grinding time becomes long, and there is a risk of increasing the production cost.

[0041] The vibration frequency in the vibration mill is preferably 600 to 2000 CPM, more preferably 800 to 1500 CPM. If the vibration frequency is too low, the tap density of the fumed silica may not be high due to insufficient impact force during pulverization. If the vibration frequency is too low, the pulverization time must be extended to make the tap density of the fumed silica 200 g / L or more, which may reduce productivity and increase production costs. If the vibration frequency is too high, the impact force may be large, and stable pulverization may not be possible.

[0042] The ball filling rate in the vibration mill is preferably 30 to 90%, more preferably 30 to 50%. If the ball filling rate is too low, the tap density of the fumed silica may not be high due to insufficient grinding efficiency. If the ball filling rate is too low, the grinding time must be extended to make the tap density of the fumed silica 200 g / L or more, which may decrease productivity and increase production costs. If the ball filling rate is too high, the grinding efficiency may decrease.

[0043] (2.3. When using a uniaxial compression press) The uniaxial opposed compression press is a device that compresses the powder by the uniaxial compression force between the opposing pressure rolls by pushing the powder between the opposing pressure rolls with a degassing screw or the like. If the clearance between the rolls can be kept small enough, a uniform uniaxial compression force is continuously applied to the powder. On the other hand, in ball mill compression, the compression force tends to be a single point load, and there is a possibility that the same aggregated powder may be repeatedly compressed many times. Therefore, by using a uniaxial opposed compression press, the distribution of the apparent density of the compressed powder is smaller than that of devices such as a vibration mill or a ball mill. In addition, it is possible to prevent an increase in silanol groups due to mechanochemical effects. When adjusting the degree of compression of the powder, the bulk density can be adjusted by adjusting the amount of powder supplied by the degassing screw, the pressure applied between the rolls, and the roll rotation speed. In general, a high bulk density product is easily obtained by slowing the roll rotation speed, increasing the pressure between the rolls, and slowing the roll rotation speed. If a low bulk density product is required, the opposite conditions should be selected.

[0044] (3. Rubber Composition) In the present embodiment, the rubber composition includes the above-mentioned fumed silica for rubber compositions, a diene rubber, and a silane coupling agent. The rubber composition preferably further includes a diol. The rubber composition is preferably a rubber composition for tires.

[0045] (3.1. Diene rubber) The diene rubber contained in the rubber composition is preferably at least one selected from natural rubber, isoprene rubber, butadiene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, butyl rubber, ethylene-propylene-diene rubber, and chloroprene rubber. The content of each of the above rubbers constituting the diene rubber may be appropriately determined depending on the application. Among these, at least one selected from natural rubber and styrene-butadiene rubber is preferable.

[0046] Examples of natural rubber include natural rubber (NR) and modified natural rubbers such as epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), deproteinized natural rubber (DPNR), and high-purity natural rubber (HPNR). These natural rubbers may be used alone or in combination of two or more. In this embodiment, NR is preferred as the natural rubber.

[0047] Examples of styrene-butadiene rubber (SBR) include unmodified solution-polymerized SBR (S-SBR), unmodified emulsion-polymerized SBR (E-SBR), and modified SBRs thereof (modified S-SBR, modified E-SBR).

[0048] (3.2. Silane coupling agents) The hydrophobic diene rubber and the fumed silica for rubber compositions having hydrophilic silanol groups have low affinity, and are difficult to mix during kneading. Therefore, by blending a silane coupling agent, a crosslinked structure between the diene rubber and the fumed silica for rubber compositions is easily formed via the silane coupling agent, and the fumed silica for rubber compositions is easily dispersed uniformly in the diene rubber. As a result, the presence of coarse fumed silica that is not dispersed in the rubber component in the rubber composition can be suppressed.

[0049] The silane coupling agent is not particularly limited as long as it is one that is normally used in rubber compositions. In this embodiment, a sulfur-containing silane coupling agent is preferred. As the sulfur-containing silane coupling agent, a sulfide-based silane coupling agent, a mercapto-based silane coupling agent, a thioester-based silane coupling agent, etc. are preferred. As the sulfide-based silane coupling agent, bis-(3-triethoxysilylpropyl) tetrasulfide, bis(3-triethoxysilylpropyl) disulfide, 3-trimethoxysilylpropyl benzothiazole tetrasulfide, etc. are exemplified. As the mercapto-based silane coupling agent, γ-mercaptopropyl triethoxysilane, mercapto-thiocarboxylate oligomer, etc. are exemplified. As the thioester-based silane coupling agent, 3-octanoylthiopropyl triethoxysilane, etc. are exemplified.

[0050] (3.3. Diol) The diol is a dihydric alcohol and a hydrocarbon having two hydroxyl groups. Although the Mooney viscosity of the tire rubber composition is reduced by blending the diol, the A hardness of the tire rubber material is increased, so that the amount of fumed silica blended can be reduced. As a result, the fuel economy and abrasion resistance of the tire rubber material are improved. Furthermore, blending the diol together with the above-mentioned silane coupling agent provides a tire rubber material with good heat aging resistance. Note that the above-mentioned effects tend not to be obtained with monohydric alcohols and alcohols having trihydric or higher hydricities.

[0051] In this embodiment, preferred examples of diols include propylene glycol, 1,3-propanediol, dipropylene glycol, diethylene glycol, and polyethylene glycol having a degree of polymerization of about 200 to 1000, and propylene glycol, 1,3-propanediol, dipropylene glycol, diethylene glycol, and polyethylene glycol having a degree of polymerization of 300 to 500 are more preferred.

[0052] (3.4. Amount of each ingredient) The amount of the fumed silica for rubber composition according to the present embodiment is preferably 10 parts by mass or more and 70 parts by mass or less per 100 parts by mass of diene rubber. By setting the amount of the fumed silica for rubber composition within the above range, a rubber composition in which the fumed silica for rubber composition is sufficiently dispersed can be obtained. If the amount of the fumed silica for rubber composition is too large, the fumed silica is not sufficiently dispersed in the rubber component, and a good kneaded product tends not to be obtained.

[0053] The amount of the fumed silica for the rubber composition is more preferably 20 parts by mass or more, and even more preferably 32 parts by mass or more, per 100 parts by mass of the diene rubber. On the other hand, the amount of the fumed silica for the rubber composition is more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less, per 100 parts by mass of the diene rubber.

[0054] From the viewpoint of increasing the wettability of the fumed silica surface to rubber and increasing the dispersibility of the fumed silica, the amount of the silane coupling agent (the content of the silane coupling agent in the rubber composition for tires) is set to 0.50 μmol / m with respect to the BET specific surface area per 1 g of the fumed silica. 2 More than 3.9 μmol / m 2 It is preferable that:

[0055] By the amount of the silane coupling agent being within the above range, the diene rubber and the fumed silica for rubber composition are sufficiently dispersed, and a rubber composition in which the fumed silica for rubber composition is sufficiently dispersed in the rubber component can be obtained. If the amount of the silane coupling agent is too large, the coupling agent acts as a plasticizer, and the viscosity of the rubber composition becomes too low, so that the fumed silica is not sufficiently dispersed in the rubber component, and a good kneaded product tends not to be obtained. In addition, the hardness of the rubber after vulcanization also tends to decrease, so that the amount of filler required to obtain the same hardness tends to increase, and fuel efficiency tends to deteriorate.

[0056] The amount of silane coupling agent blended is 0.7 μmol / m2 relative to the specific surface area of ​​fumed silica. 2 More preferably, it is equal to or greater than this.

[0057] The amount of the diol to be added may be determined according to the specific surface area of ​​the fumed silica, in the same manner as the silane coupling agent, in order to reduce the viscosity of the kneaded rubber. The amount of the diol to be added (the content of the diol in the rubber composition) is 3 μmol / m2 relative to the BET specific surface area per gram of the fumed silica. 2 More than 14μmol / m 2 The following is the result.

[0058] The amount of the compound is 3.4 μmol / m 2 It is preferable that the concentration is 6.8 μmol / m or more. 2 More preferably, the amount is 11 μmol / m 2 It is preferable that:

[0059] (3.5. Other Ingredients) In this embodiment, the rubber composition may contain components to be blended in the rubber composition in addition to the above-mentioned components (diene rubber, fumed silica for rubber composition, and silane coupling agent). An example of such a component is a lubricant. Blending the lubricant improves the kneadability of each component, and a rubber composition in which each component is well dispersed is easily obtained.

[0060] Examples of lubricants include stearic acid and process oil. A lubricant may be used alone or in combination of two or more. Examples of process oils include aromatic oils, paraffin oils, naphthenic oils, etc., which are made of mineral oils and synthetic oils. These may be used alone or in combination of two or more.

[0061] The amount of the lubricant (the amount of the lubricant in the rubber composition) is not limited. For example, the amount of the lubricant is preferably 2 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the diene rubber. Furthermore, the amount of the lubricant is more preferably 4 parts by mass or more and even more preferably 30 parts by mass or less per 100 parts by mass of the diene rubber.

[0062] If the amount of lubricant is too small, the viscosity becomes high and kneadability becomes poor, and the fumed silica for rubber compositions may not be sufficiently dispersed in the diene rubber, whereas if the amount of lubricant is too large, shear is not applied during kneading, and the fumed silica for rubber compositions may not be sufficiently dispersed in the diene rubber.

[0063] Furthermore, the rubber composition may contain a reinforcing filler other than the fumed silica for rubber compositions. Examples of the reinforcing filler include carbon black, wet silica, clay, mica, talc, calcium carbonate, aluminum hydroxide, aluminum oxide, and titanium oxide. When the reinforcing filler is blended, an appropriate amount of a filler coupling agent can also be blended. The blending amount of the reinforcing filler is not limited within the range in which the effects of the present invention can be obtained, and may be a general blending amount.

[0064] Furthermore, the rubber composition may contain various additives such as zinc oxide, antioxidants, plasticizers, processing aids, liquid polymers, thermosetting resins, etc. The amounts of these additives to be blended are not limited as long as the effects of the present invention can be obtained, and may be general amounts.

[0065] (4. Method for producing rubber composition) The rubber composition is obtained by kneading the diene rubber, the fumed silica for rubber compositions, the silane coupling agent, and, if necessary, other components.

[0066] In this embodiment, the rubber composition may be produced by kneading certain components to prepare a master batch, and then blending and kneading the remaining components into the master batch, or by kneading all of the components together.

[0067] When preparing the master batch, it is preferable to knead the above-mentioned diene rubber, the above-mentioned fumed silica for a rubber composition, the above-mentioned silane coupling agent, and, if necessary, other components to prepare the master batch.

[0068] After the master batch is prepared, other components are blended and kneaded into the master batch to obtain a rubber composition. In this embodiment, since fumed silica for rubber compositions having a tap density of 200 g / L or more is blended, a rubber composition in which the fumed silica is sufficiently dispersed in the rubber components can be obtained even by kneading using a Banbury mixer, for example.

[0069] The kneading conditions may be set so that each component is thoroughly kneaded.

[0070] The above rubber composition is suitable as a rubber composition for tires. By using the rubber composition according to the present embodiment as a rubber composition for tires, a rubber material for tires excellent in fuel economy, abrasion resistance, and heat aging resistance can be obtained. The rubber material for tires is a material obtained by vulcanizing the rubber composition for tires.

[0071] Such rubber material for tires can be suitably used for tires for passenger cars, trucks, buses, etc. It can be suitably used for each component of tires, particularly for treads, base treads, sidewalls, clinches, etc.

[0072] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES

[0073] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0074] (Experiment 1) (Preparation of Rubber Composition for Tires) In experiment 1, the diene rubber was SBR rubber. The following components (A) to (D) and (E-1) to (E-4) were charged into a 0.6 L Banbury mixer type Plastomill BB600 manufactured by Toyo Seiki Co., Ltd. so that the compounding amount per 100 parts by mass of SBR rubber was the compounding amount shown in Table 1. After charging, the rotor rotation speed was adjusted within the range of 20 to 100 rpm so that the temperature of the kneaded material was within the range of 140 to 150°C, and the kneading was continued for 5 minutes after the temperature was reached. The air cylinder pressure was 0.5 MPa. After the kneading was completed, the mixture was cooled to room temperature and taken out to obtain a master batch.

[0075] The amounts of diene rubber and other additives were calculated so that the fill factor after mixing would be 70%, and the components were added to the Plastomill and mixed. The filler was added twice. (A) Diene rubber (A-1) SBR (Asahi Kasei S-SBR E-581) (A-2) BR (ENEOS BR01) (B) Filler (B-1) Carbon black (Tokai Carbon, Seast 6, nitrogen adsorption BET specific surface area: 120 m 2 / g, tap density: 400g / L) (B-2) Wet silica (Tosoh Silica, Nipsil AQ, nitrogen adsorption BET specific surface area: 200 m 2 / g, tap density: 300g / L, silanol group density: 6 / nm 2 , Pycnometer method true density: 2.1g / cm3 ) (B-3) Hydrophilic fumed silica (Tokuyama, Reolosil QS-40, nitrogen adsorption BET specific surface area: 380 m 2 / g, tap density 50g / L, silanol group density 2.3 / nm 2 , Pycnometer method true density: 2.2g / cm 3 ) (B-4) Hydrophilic fumed silica (Tokuyama, Leoloseal QS-30C, nitrogen adsorption BET specific surface area: 300 m 2 / g, tap density: 100g / L, silanol group density: 2.1 / nm 2 , Pycnometer method true density: 2.2g / cm 3 ) (BM-1)~(BM-3) Fumed silica compressed by ball mill (BC-1)~(BC-4) Fumed silica compressed by uniaxial opposed compression press (C) Silane coupling agent (C-1) Polysulfide coupling agent (EVONIK Si69) (D) Diol (D-1) 1,3-Propanediol (E) Other ingredients (E-1) Lubricant (stearic acid, NOF Corp., Beads Stearic Acid YR) (E-2) Lubricant (zinc oxide, Seido Chemical, zinc oxide type 2) (E-3) Anti-aging agent (Seiko Chemical, Ozonone 6C) (E-4) Process oil (Fuji Kosan, Aromax 3 (TDAE Oil))

[0076] [Preparation of ball-milled fumed silica] The fumed silica compressed by a ball mill was prepared as follows. That is, about 200 g of the fumed silica (B-4) was put into a 7 L ball mill made of alumina (filling rate of alumina balls with a ball diameter of φ32 mm is 30%) and ground at room temperature at a rotation speed of 300 rpm for about 3 hours to obtain compressed fumed silica (BM-1) with a tap density of 200 g / L. By extending the ball milling time to 5 hours and 8 hours, respectively, compressed fumed silica (BM-2) with a tap density of 250 g / L and compressed fumed silica (BM-3) with a tap density of 320 g / L were obtained.

[0077] [Preparation of uniaxially compressed fumed silica] The fumed silica compressed by a uniaxial opposed compression press was prepared as follows. That is, the fumed silica (B-4) was compressed by a Freund Turbo WP-230×80 compactor as a uniaxial opposed compression press. The roller clearance was fixed at 0.5 mm, the roller rotation speed at 10 rpm, and the compression pressure applied to the roll at 0.3 T / cm, and the degree of vacuum of the screw feeder that feeds the powder to the roller was changed from -10 kPa to -45 kPa to obtain compressed fumed silica with different tap densities of the powder. The tap densities of the obtained compressed fumed silica were 200 g / L (BC-1), 250 g / L (BC-2), 320 g / L (BC-3), and 385 g / L (BC-4), respectively.

[0078] The tap density of the filler was measured as follows. First, a 1 L resin graduated cylinder was placed on an electronic balance, the tare was subtracted, and about 1 L of filler was filled and the weight M1 (g) was recorded. After that, the cylinder was manually tapped 30 times from a height of about 10 cm, after which the volume V1 (ml) was measured and the tap density ρ1 was calculated from the following formula. The results are shown in Table 1. Tap density ρ1 = 1000 × M1 / V1 (g / L)

[0079] The apparent density of the filler by the tamp method was measured as follows. Each filler was passed through a sieve with a mesh size of 500 μm, dried at 105°C for 2 hours, and then cooled in a desiccator. 200 ± 10 mL of filler was filled into the measuring cylinder of the tamp volume meter, and the weight of the filler M2 (g) was recorded. After that, the measuring cylinder was rotated 1250 times by the cam of the tamp volume meter, and the volume V2 (mL) was measured, and the apparent density ρ2 by the tamp method was calculated from the following formula. Other conditions were measured in accordance with JIS5101-12-2. The results are shown in Table 1. Apparent density by tamp method ρ2 = 1000 × M2 / V2 (g / L)

[0080] The nitrogen adsorption BET specific surface area of ​​each filler was measured by the nitrogen adsorption BET method using a Microtrac BELSOP MINI X. The results are shown in Table 1.

[0081] The surface silanol group density of the fumed silica ((B-3), (B-4), (BM-1) to (BM-3), (BC-1) to (BC-4)) was measured using a Kyoto Electronics Manufacturing Co., Ltd. MKC-610 coulometric titration device equipped with an ADP-512 moisture vaporizer. That is, the temperature was raised to 130°C in the low-temperature side furnace of the moisture vaporizer, and the moisture amount equivalent to the silica drying loss was measured by coulometric titration using the MKC-610 model. Then, the moisture amount equivalent to the ignition loss was measured in the high-temperature side furnace heated to 1000°C in the same manner by coulometric titration. The moisture amount equivalent to the ignition loss generated from 130°C to 1000°C was converted to silanol group density using the following formula. The results are shown in Table 1. Silanol group density (pcs / nm 2 )=668.9 × H2O(%) / specific surface area(m 2 / g)

[0082] The pore peak radius and pore volume of the fumed silica ((B-3), (B-4), (BM-1) to (BM-3), (BC-1) to (BC-4)) were measured as follows. Using a BELSOP MINI X manufactured by Microtrac, nitrogen was adsorbed at liquid nitrogen temperature onto a sample that had been degassed at 150°C to a pressure of 1 Pa or less to obtain an adsorption isotherm. The pore peak radius and pore volume were calculated from the obtained adsorption isotherm based on the BJH theory using the analysis software provided with the BELSOP MINI X. The results are shown in Table 1.

[0083] [Table 1]

[0084] The above-obtained master batch and the following (E-5), (E-6) and (E-7) were added and mixed by a 6-inch roll tester to obtain a rubber composition for tires. The amount of sulfur was set to the amount shown in Table 2, taking into account the amount of sulfur contained in other added components. (E-5) Sulfur (Tsurumi Chemical Industry, 5% oil-containing fine sulfur) (E-6) Vulcanization accelerator (Sansera CM-G N-cyclohexyl-2-benzothiazole sulfenamide (CBS), manufactured by Sanshin Chemical Industry Co., Ltd.) (E-7) Vulcanization accelerator (Sansera DG 1,3-diphenylguanidine (DPG), manufactured by Sanshin Chemical Industry Co., Ltd.)

[0085] [Table 2]

[0086] Test specimens were prepared for the resulting rubber composition for tires to carry out the following evaluations. The resulting test specimens were used to evaluate the following physical properties.

[0087] (Processability: Mooney viscosity) The Mooney viscosity (ML1+4 100°C) of the obtained test piece of the rubber composition for tires was measured in accordance with JIS K6300-1 using a Mooney viscometer (VR-1132 manufactured by Ueshima Seisakusho). When the Mooney viscosity is low, the processability of the rubber composition for tires tends to be good. The results are shown in Table 2.

[0088] (Preparation of tire rubber material test pieces) The resulting rubber composition for tires was then press-vulcanized at 160°C for T90+1 minutes to obtain a rubber material for tires. Test pieces for the following evaluations were prepared from the resulting rubber material for tires. The following physical properties were evaluated using the resulting test pieces.

[0089] (A hardness) The hardness (Shore A hardness) of the test pieces of the obtained rubber material for tires was measured by a durometer in accordance with JIS K6253 Type A. Since the target A hardness of the rubber material for tires is 65, it is preferable that the A hardness of the test pieces is also around 65. In Comparative Examples 3 to 5, the tap density of the filler was low, so that the amount of filler mixed per time (mixing volume) was large, and the filler was not kneaded with other components in the mixer and flowed out from the mixer. Therefore, in Comparative Examples 3 to 5, only a smaller amount of filler could be mixed than the planned amount. As a result, the A hardness of the obtained rubber material was very low, making it unsuitable as a rubber material for tires. The results are shown in Table 2.

[0090] (Fuel efficiency: tan δ at 60℃) The obtained test pieces of the rubber material for tires were measured under the following conditions using a dynamic viscoelasticity tester (VR-7130 manufactured by Ueshima Seisakusho) in accordance with JIS K6394. Tan δ (60°C) was calculated from the measured value at 60°C. Measurement temperature: 60℃ Static strain: 10% Dynamic Distortion: ±2% Frequency: 10Hz

[0091] The rolling resistance index was calculated by the following formula, taking the calculated tan δ (60° C.) of Standard Example 1 (Comparative Example 1) as 1.0. The larger the index, the better the rolling resistance. The results are shown in Table 2. (Rolling resistance index) = (tan δ of standard example 1 (60°C)) / (tan δ of example (60°C))

[0092] (Wear resistance: FPS wear amount) For the test pieces of the obtained rubber material for tires, the FPS abrasion amount was measured using an FPS abrasion tester (AB-2012 manufactured by Ueshima Seisakusho) under the conditions of a temperature of 35°C, a load of 40N, a slip rate of 10%, and a test time of 2 minutes. The volume loss was calculated from the FPS abrasion amount, and the abrasion index was calculated using the following formula, with the loss amount of Standard Example 1 (Comparative Example 1) being set at 1.0. The higher the index, the better the abrasion resistance. The results are shown in Table 2. (Wear index) = (loss amount of control example 1) / (loss amount of example)

[0093] (Heat aging resistance) The obtained rubber composition for tires was vulcanized at 160°C for T90+1 minutes using a 2mm thick mold, and the obtained vulcanized rubber sheet was punched out with a JIS No. 3 dumbbell to obtain a sample. The sample was thermally aged for 5 days (120 hours) in a gear oven set at a temperature of 80°C, and then the strength at break (break strength) was measured together with an unaged sample using a tensile tester according to JIS K6251. The ratio of the unaged break strength to the break strength after aging was taken as an index of heat aging resistance. The heat resistance index was calculated using the following formula. When the heat resistance index is 1 or more, the heat aging resistance is excellent, and when the heat resistance index is less than 1, the break strength decreases due to thermal degradation, so the heat aging resistance is poor. The results are shown in Table 2. (Heat resistance index)={(breaking strength after heat aging) / (breaking strength of unaged sample)}

[0094] Furthermore, for the samples before the heat aging test, the strength index was calculated by the following formula, taking the breaking strength of Control Example 1 (Comparative Example 1) as 1.00. The higher the strength index, the better the strength. The results are shown in Table 2. (Strength index)=(Breaking strength of Example) / (Breaking strength of Reference Example 1)

[0095] From Table 2, it was confirmed that when the diene rubber is an SBR rubber, by using fumed silica for rubber compositions having the above-mentioned physical properties as a filler, a rubber material for tires having good properties can be obtained while reducing the number of times of mixing the fumed silica for rubber compositions. On the other hand, it was confirmed that when the number of times of mixing a filler with a low tap density is reduced, only a smaller amount of the filler than the planned amount can be mixed, and a rubber material having the desired hardness cannot be obtained.

[0096] (Experiment 2) In experiment 2, the diene rubber was natural rubber. (A-3) shown below, and (B) to (D), (E-1) to (E-4) shown above were charged into a 0.6 L Banbury mixer type Plastomill BB600 manufactured by Toyo Seiki Co., Ltd. so that the compounding amount per 100 parts by mass of natural rubber was the compounding amount shown in Table 3. After charging, a master batch was prepared under the same conditions as in experiment 1. The filler (B), silane coupling agent (C), diol (D), and other components (E-1) to (E-4) other than (A-3) were the same as those used in experiment 1. Therefore, the physical properties of the fillers used in experiment 2 are as shown in Table 1. (A) Diene rubber (A-3) Vietnamese natural rubber: SVR

[0097] The above-obtained master batch, the above-mentioned (E-5) and the below-mentioned (E-8) were added and mixed by a 6-inch roll tester to obtain a rubber composition for tires. The amount of sulfur was set to the amount shown in Table 3, taking into consideration the amount of sulfur contained in other added components. The other component (E-5) was the same as the component used in Experiment 1. (E) Other ingredients (E-8) Vulcanization accelerator (Sansera NS-G N-(tert-butyl)-2-benzothiazole sulfenamide (TBBS), manufactured by Sanshin Chemical Industry Co., Ltd.)

[0098] Test pieces were prepared from the obtained rubber composition for tires by the same method as in Experiment 1, and the physical properties were evaluated by the same method and conditions as in Experiment 1. The results are shown in Table 3. Furthermore, the obtained rubber composition for tires was vulcanized under the same conditions as in Experiment 1 to obtain a rubber material for tires. Test pieces were prepared from the obtained rubber material for tires by the same method as in Experiment 1, and the physical properties were evaluated by the same method and conditions as in Experiment 1. The results are shown in Table 3.

[0099] [Table 3]

[0100] From Table 3, it was confirmed that even when the diene rubber is natural rubber, by using fumed silica for rubber compositions having the above-mentioned physical properties as a filler, a rubber material for tires having good properties can be obtained while reducing the number of times of mixing the fumed silica for rubber compositions. On the other hand, it was confirmed that when the number of times of mixing a filler with a low tap density is reduced, only a smaller amount of the filler than the planned amount can be mixed, and a rubber material having the desired hardness cannot be obtained. [Industrial Applicability]

[0101] The fumed silica according to the present invention is obtained by compressing the bulky fumed silica into a form that does not generate dust. Therefore, by using the fumed silica according to the present invention, in addition to adding it to the rubber composition for tires, it is expected to prevent dust generation and shorten the process time by being quickly caught in the medium when adding it to silicone rubber, clear rubber for shoes, and paint other than tires.

Claims

1. A fumed silica for a rubber composition having a tap density of 200 g / L or more, a pore peak radius of 22 nm or more obtained by applying the BJH method to an adsorption isotherm by nitrogen adsorption, and a pore volume of 1.6 mL / g or more.

2. The BET specific surface area of ​​the fumed silica for rubber compositions is 180 m 2 / g or more 500m 2 The fumed silica for a rubber composition according to claim 1, wherein the molecular weight of the fumed silica is 1 / g or less.

3. 3. The fumed silica for rubber compositions according to claim 1, wherein the fumed silica for rubber compositions is an untreated fumed silica for rubber compositions.

4. A method for compressing fumed silica, comprising the steps of: subjecting fumed silica having a tap density of less than 200 g / L to uniaxial compression pressing to obtain compressed fumed silica having a tap density of 200 g / L or more.

Citation Information