Non-Magnetic Substrate For Magnetic Disk, And Magnetic Disk
Patent Information
- Application Number
- LAP855
- Authority / Receiving Office
- LA · LA
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-11-24
- Filing Date
- 2018-04-02
- Publication Date
- 2025-04-25
AI Technical Summary
As magnetic disk substrates thin to increase storage capacity, they become more susceptible to vibrations from external shocks, leading to increased contact with other components and resulting in scratches, defects, and reduced durability.
A non-magnetic substrate with a metal film having a loss coefficient of 0.01 or more is applied to both main and end surfaces, with a thickness ratio of the film to the substrate body of 0.025 or more, enhancing vibration damping and reducing the amplitude of vibrations caused by external impacts.
This configuration effectively reduces vibrations and contact-related issues, minimizing scratches and defects on the magnetic disk, even at reduced substrate thicknesses, thereby enhancing the durability and performance of hard disk drive devices.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
Non-magnetic substrate for magnetic disk and magnetic disk
[0001] The present invention relates to a non-magnetic substrate for a magnetic disk and a magnetic disk.
[0002] Glass substrates and aluminum alloy substrates have traditionally been used as magnetic disk substrates. A magnetic film is formed on the main surface of these substrates to form a magnetic disk substrate. It is desirable for magnetic disks to have few surface defects, no hindrance to reading and writing information, and the ability to read and write large amounts of information.
[0003] For example, when an aluminum alloy substrate is used as a non-magnetic substrate for a magnetic disk, the surface of the aluminum alloy substrate is plated with NiP. However, in order to suppress surface defects after plating, an aluminum alloy substrate for a magnetic recording medium (hereinafter, sometimes abbreviated as "Al alloy substrate" or "Al-Mg alloy substrate") is known in which a metal film is formed on the substrate surface by physical vapor deposition (Patent Document 1).
[0004] Japanese Patent Application Laid-Open No. 2006-302358
[0005] The Al alloy substrate for magnetic recording media is said to be capable of reducing surface defects after NiP plating is formed on the substrate, thereby providing a magnetic disk substrate that can read and write large amounts of information without any problems.
[0006] In recent years, the hard disk drive industry has seen a slowdown in the rate at which recording density has improved, as the miniaturization of magnetic particles in magnetic disks has reached its limit. Meanwhile, demand for increased storage capacity in hard disk drives (hereinafter sometimes abbreviated as HDDs) is becoming increasingly intense due to big data analysis and other factors. Therefore, increasing the number of magnetic disks installed in a single hard disk drive is being considered.
[0007] To increase storage capacity by increasing the number of magnetic disks installed in a hard disk drive, it is necessary to reduce the thickness of the magnetic disk substrate, which accounts for the majority of the thickness of the magnetic disk, within the limited space within the magnetic disk drive. However, it has been found that reducing the thickness of the magnetic disk substrate reduces the substrate's rigidity, making it more susceptible to large vibrations and making it difficult to contain those vibrations. For example, cloud data centers use a huge number of hard disk drives, which require frequent replacement due to failure. It has been found that the impact of installing a new hard disk drive in a rack can cause failure or shorten the time until failure. Further detailed investigation revealed that when a hard disk drive is subjected to external impact, damage can occur even when the magnetic disk is not rotating because power is not yet supplied to the hard disk drive.
[0008] Unlike steady-state flutter vibrations caused by a rotating magnetic disk and the surrounding airflow, vibrations caused by external impacts decay over time. However, if the amplitude of these vibrations is large, they can come into contact with the ramp, which protrudes above the main surface of the magnetic disk to allow the magnetic head to retreat from the magnetic disk, scraping the ramp material and generating particles, and in some cases, causing scratches and defects on the magnetic disk surface. Furthermore, if the vibrations do not converge, the frequency of such contacts increases, making scratches, defects, and particles on the magnetic disk surface even more likely to occur. Currently, magnetic disk substrates are thick, making it difficult for vibrations caused by external impacts to have a significant amplitude that becomes a problem. Furthermore, because hard disk drive devices are equipped with a small number of magnetic disks, the distance (gap) between the magnetic disk and the ramp is relatively large. As a result, contact between the magnetic disk and the ramp is rare. However, in the future, as the storage capacity of hard disk drive devices increases, and the thickness of magnetic disk substrates is reduced to 0.700 mm or less, problems that did not previously occur, such as vibrations due to external impacts and the resulting contact with other components, as well as particles and scratches and dents on the magnetic disk caused by the contact, will no longer be negligible.
[0009] Therefore, an object of the present invention is to provide a non-magnetic substrate for a magnetic disk and a magnetic disk that can effectively reduce vibrations of the magnetic disk, which are different from flutter vibrations caused by external impacts, even if the thickness of the substrate is thin.
[0010] One aspect of the present invention is a non-magnetic substrate for a magnetic disk. The non-magnetic substrate includes: a substrate body having two opposing main surfaces; and a metal film formed on the main surfaces and made of a material with a loss factor of 0.01 or greater. The thickness (T+D) of the non-magnetic substrate, which is the sum of the thickness T of the substrate body and the thickness D of the metal film, is 0.700 mm or less, and the ratio D / T of the thickness D of the metal film to the thickness T of the substrate body is 0.025 or greater.
[0011] The metal film is preferably provided on each of the main surfaces and also on the end faces of the substrate body, and the thickness of the metal film on each of the main surfaces is preferably 80% or more of the thickness of the metal film on the end faces.
[0012] The thickness of the non-magnetic substrate is preferably 0.640 mm or less.
[0013] It is preferable that the non-magnetic substrate for a magnetic disk has a disk shape, and the disk shape has an outer diameter of 90 mm or more.
[0014] The Vickers hardness Hv of the metal film is 100 kgf / mm 2 ] or more.
[0015] The metal film is preferably formed on the main surface and the outer peripheral end face of the substrate body, and the maximum height Rz of the surface roughness of the outer peripheral end face of the substrate body that forms the interface with the metal film is 0.5 μm or more.
[0016] It is preferable that the metal film is formed on the main surface and the outer peripheral end face of the substrate body, and that the maximum height Rz of the surface roughness of the film at the outer peripheral end face of the non-magnetic substrate for a magnetic disk is smaller than the maximum height Rz of the surface roughness of the substrate body at the outer peripheral end face of the substrate body.
[0017] Another aspect of the present invention is a magnetic disk having at least a magnetic film on the surface of the non-magnetic substrate for a magnetic disk.
[0018] According to the above-described non-magnetic substrate for a magnetic disk and magnetic disk, vibrations of the magnetic disk caused by external impacts different from flutter vibrations can be effectively reduced even if the thickness of the magnetic disk substrate is thin.
[0019] 1 is a diagram illustrating an example of the external shape of a non-magnetic substrate for a magnetic disk according to an embodiment of the present invention, a diagram illustrating an example of an edge and a film of a non-magnetic substrate for a magnetic disk according to an embodiment of the present invention, and a diagram illustrating an example of vibration of the non-magnetic substrate for a magnetic disk according to an embodiment of the present invention.
[0020] The non-magnetic substrate for a magnetic disk of the present invention will be described in detail below. While the following description will be made using a glass substrate for a magnetic disk, the substrate body of the non-magnetic substrate for a magnetic disk may be a non-magnetic metal substrate in addition to a glass substrate. Materials for the glass substrate include aluminosilicate glass, soda-lime glass, and borosilicate glass. Amorphous aluminosilicate glass is particularly suitable because it can be chemically strengthened as needed and can produce a glass substrate for a magnetic disk with excellent main surface flatness and substrate strength. Materials for the metal substrate include, for example, aluminum alloys, titanium alloys, and single-crystal silicon. In the case of aluminum alloys, Al-Mg (aluminum-magnesium) alloys containing magnesium as a component can be used. Among these, aluminum alloys are particularly suitable.
[0021] FIG. 1 is a diagram showing the external shape of a non-magnetic substrate for a magnetic disk according to this embodiment. As shown in FIG. 1 , the non-magnetic substrate for a magnetic disk 1 (hereinafter simply referred to as non-magnetic substrate 1) according to this embodiment is a thin, disk-shaped substrate with an inner hole 2 formed therein. While the size of the non-magnetic substrate 1 is not critical, the non-magnetic substrate 1 is suitably applied to magnetic disk substrates with a nominal diameter of 2.5 inches or 3.5 inches, for example. For a magnetic disk substrate with a nominal diameter of 3.5 inches, the outer diameter (diameter) of the disk shape is preferably 90 mm or greater. Specifically, the nominal value of the outer diameter of the disk shape can be 95 mm or 97 mm. Even with such a large disk shape, the formation of a film (described below) on the main surface can reduce the generation of particles, scratches, and dents caused by magnetic disk vibration. Note that magnetic disk vibrations caused by external impacts, which differ from flutter vibrations, increase in magnitude as the outer diameter of the non-magnetic substrate 1 increases, and are more difficult to attenuate. Therefore, the non-magnetic substrate 1 according to this embodiment is particularly suitable for use with magnetic disks with a nominal diameter of 3.5 inches or greater.
[0022] 2 is a diagram illustrating an example of an edge and film of a non-magnetic substrate 1. As shown in FIG. 2, the non-magnetic substrate 1 has a substrate body 3 and a film 4. The substrate body 3 has a pair of main surfaces 3a, side wall surfaces 3b arranged in a direction perpendicular to the pair of main surfaces 3a, and a pair of chamfered surfaces 3c arranged between the pair of main surfaces 3a and the side wall surfaces 3b. The side wall surfaces 3b and the chamfered surfaces 3c are formed at the outer peripheral edge and the inner peripheral edge of the non-magnetic substrate 1.
[0023] When glass is used for the substrate body 3, the glass composition of the substrate body 3 is, for example, SiO 2 , 55-78%, Li 2 O, 0.1-1%, Na 2 The glass substrate 3 may contain 2 to 15% of SiO, and 10 to 25% in total of MgO, CaO, SrO, and BaO, and the molar ratio of the CaO content to the total content of MgO, CaO, SrO, and BaO (CaO / (MgO+CaO+SrO+BaO)) may be 0.20 or less (hereinafter referred to as glass 1). 2 The content of Al is 45-68%. 2 O 3 The content is 5 to 20%, SiO 2 and Al 2 O 3 The total content (SiO 2 +Al 2 O 3 ) is 60-80%, B 2 O 3 The content of MgO is 3 to 28%, the content of CaO is 0 to 18%, the total content of BaO and SrO (BaO + SrO) is 0 to 2%, the total content of alkaline earth metal oxides (MgO + CaO + SrO + BaO) is 12 to 30%, and the total content of alkali metal oxides (Li 2 O + Na 2 O+K 2 Alternatively, the glass may be an amorphous oxide glass containing 3.5 to 15% of Sn oxide and 0.05 to 2.00% of Ce oxide, and at least one oxide selected from the group consisting of Sn oxide and Ce oxide (hereinafter, this glass will be referred to as Glass 2).
[0024] As shown in FIG. 2 , a film 4 is provided on the main surface 3 a, side wall surface 3 b, and chamfered surface 3 c of the substrate body 3. The film 4 enhances the vibration-damping properties of the non-magnetic substrate 1. The film 4 is a metal film made of a metallic material with a loss factor of 0.01 or greater. The metallic material of the film 4 has a higher loss factor than the material of the substrate body 3. The loss factor values are measured at room temperature, e.g., 25°C. Hereinafter, the loss factor refers to the value at room temperature. Here, the loss factor of the film 4 is determined by a vibration test using the substrate body 3 and the non-magnetic substrate 1 with the film 4 formed on the substrate body 3 as test samples, and measuring the resonant frequency and half-width at the resonant frequency of the test samples. For example, a "Free Resonant Young's Modulus, Rigidity Modulus, and Internal Friction Measuring Device (JE Series)" manufactured by Nippon Technoplus Co., Ltd. can be used for the vibration test. The loss factor of the test sample can be determined from the resonant frequency and half-width of the test sample obtained in the vibration test. Furthermore, the loss factor of the film 4 can be calculated from the resonance frequency and loss factor of the non-magnetic substrate 1, the resonance frequency of the substrate body 3, the ratio of the thickness of the substrate body 3 to the thickness of the film 4, and the ratio of the density of the material of the substrate body 3 to the density of the metal material of the film 4, for example, according to the known formula shown below. 1 , η 1 and the resonance frequency of the substrate body 3 is f 3 The loss coefficient η of the film 4 is given by: a is the ratio of the total thickness of the film 4 to the thickness of the substrate body 3; and b is the ratio of the density of the metal material of the film 4 to the density of the material of the substrate body 3. 4 is α=(f 1 / f 3 ) 2 · (1 + a · b) as η 4 = α / (α-1) · η 1 It can be expressed as:
[0025] A Ni-P alloy containing Ni and P can be used as a material having the characteristics (loss factor) of the film 4. In the case of a Ni-P alloy, the P content can be set to 5 to 15 mass % so that the alloy is non-magnetic. For example, the P content can be set to 5 to 15 mass %. Also usable are Mg alloys, Al-Zn alloys, Mg-Zr alloys, etc. Note that the film formation method can be, for example, sputtering, electroless plating, electrolytic plating, etc. An appropriate method can be selected from these.
[0026] When the thickness of the substrate body 3 is defined as T and the thickness of the film 4 is defined as D, the thickness (T + D) of the non-magnetic substrate 1, including the substrate body 3 and the film 4, is 0.700 mm or less. The ratio D / T of the thickness D (= D1 + D2) of the film 4 provided on the main surface 3a to the thickness T of the substrate body 3 is 0.05 or greater. It is preferable that the thickness of the film 4 does not vary depending on the location on the main surface and is constant across the main surface. Since such a non-magnetic substrate 1 has a thickness of 0.700 mm or less, vibrations are easily generated in the non-magnetic substrate 1 due to external impacts, etc. However, even if such vibrations occur, the film 4 formed on the main surface 3a of the substrate body 3 can quickly damp the vibrations. Furthermore, it is preferable that the film 4 seamlessly covers the entire periphery of the metal body 1, including the end faces, since this particularly enhances the degree of vibration suppression. In this case, it is more preferable that the film 4 is harder than the substrate body 3. It is even more preferable that D1 and D2 are equal. In such a case, vibration modes that cause localized deformation are less likely to form, and the degree of vibration suppression is increased. Therefore, for example, the number of contacts with a ramp or an adjacent disk, the likelihood of contact, and the impact upon contact can be reduced. While the film 4 is formed on each of the two main surfaces 3 a in this embodiment, the present embodiment also includes a configuration in which the film 4 is formed on only one of the main surfaces 3 a. In this case, the thickness D of the film 4 is the thickness of the film 4 formed on one of the main surfaces 3 a.
[0027] A magnetic disk, formed by forming a magnetic film on a non-magnetic substrate 1, is fixed to the spindle of the hard disk drive at the bore 2 within the hard disk drive. For example, when a new hard disk drive is installed in a rack for replacement or when a hard disk drive is removed from the rack to be moved to another location, the hard disk drive may be subjected to external shocks during these operations. Such shocks cause vibrations in the non-magnetic substrate 1, with the bore 2 fixed by the spindle, displacing the main surface 3a around the bore 2 in the normal direction of the main surface 3a (thickness direction of the non-magnetic substrate 1). This vibration, as shown in Figure 3, differs from steady-state flutter vibrations that occur in a steady rotation state due to the rotating magnetic disk and the airflow around it; it is a vibration that decays over time. Figure 3 shows an example of vibration of the non-magnetic substrate 1. This vibration occurs whether the magnetic disk is rotating or stationary. Therefore, it is undesirable that this vibration continues for a long time, causing the magnetic disk formed from the non-magnetic substrate 1 to repeatedly come into contact with the ramp inside the hard disk drive device, resulting in scratches and defects on the surface of the magnetic disk, and furthermore, that this contact can cause the ramp material to be scraped off, generating particles.
[0028] However, since the non-magnetic substrate 1 is a film made of a material with a loss factor of 0.01 or more, and the ratio D / T of the thickness D (= D1 + D2) of the film 4 to the thickness T of the substrate body 3 is 0.025 or more, the vibration can be quickly damped. It is more preferable that the loss factor of the film 4 be 0.02 or more. On the other hand, there is no particular upper limit on the loss factor of the film 4, but a material with a loss factor that is too large may be a soft material whose crystals are easily broken. Therefore, a loss factor of 0.3 or less is preferable, for example, so that practical metal materials can be used.
[0029] If the ratio D / T is less than 0.025, the thickness D of the film 4 is not sufficiently thick relative to the thickness T of the substrate body 3, making it difficult to quickly damp vibrations in the non-magnetic substrate 1, and the film 4 cannot reduce the initial amplitude of vibrations on the main surface 3a. By setting the ratio D / T to 0.025 or more, the film 4 covering the main surface 3a is sufficiently thick, allowing for early damping of vibrations in the non-magnetic substrate 1 and reducing the initial amplitude of vibrations. The ratio D / T is preferably 0.03 or more, and more preferably 0.04 or more. While the upper limit of the ratio D / T is not limited in light of the above-mentioned problems, an excessively large ratio D / T increases the material cost of the film 4 and may increase the weight of the non-magnetic substrate 1, thereby increasing the power consumption of a hard disk drive device that rotates the magnetic disk. Therefore, the ratio D / T is preferably 0.15 or less.
[0030] The above effect can be achieved even if the film 4 is provided only on the main surface 3a, not on the sidewall surfaces 3b and chamfered surfaces 3c. However, as shown in FIG. 2, it is preferable to provide the film 4 on the end surfaces of the substrate body 3, i.e., the sidewall surfaces 3b and chamfered surfaces 3c, in addition to the main surface 3a. In this case, the thicknesses of the film 4 on the sidewall surfaces 3b and chamfered surfaces 3c are preferably greater than the thicknesses D1 and D2 of the film on the main surface 3a. The vibrations generated in the nonmagnetic substrate 1 are vibrations that displace in the normal direction of the main surface 3a. In conjunction with this displacement of the main surface 3a in the normal direction, the end surfaces of the substrate body 3 also displace in the normal direction of the main surface 3a. Suppressing such displacement can suppress the amount of displacement of the main surface 3a in the normal direction, i.e., the amplitude of vibration. Therefore, it is preferable to form the film 4 on the end surfaces of the substrate body 3, i.e., the sidewall surfaces 3b and chamfered surfaces 3c, in addition to the main surface 3a. In particular, it is preferable that the thicknesses of the film 4 on the sidewall surfaces 3b and the chamfered surfaces 3c be thicker than the thicknesses D1 and D2 of the film on the main surface 3a, respectively, in order to suppress the amplitude of vibration on the main surface 3a. In this case, the thicknesses D1 and D2 of the film 4 on the main surface 3a are preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more of the thickness of the film 4 on the sidewall surfaces 3b and the chamfered surfaces 3c (end surfaces), in order to efficiently suppress the amplitude of vibration. The closer the thicknesses D1 and D2 are to the thickness of the film 4 on the sidewall surfaces 3b and the chamfered surfaces 3c (end surfaces), the more preferable. The larger the above ratio is and the more uniform the thickness of the film 4 becomes over the entire surface of the non-magnetic substrate 1, the less likely a vibration mode that causes local deformation will be formed, and the more easily vibration will be suppressed.
[0031] The thinner the magnetic disk, the greater the amplitude of vibration, which increases the frequency of contact between the magnetic disk and other components within the hard disk drive, resulting in increased particle generation, scratches, and dents on the magnetic disk. However, in the case of the non-magnetic substrate 1, this problem is unlikely to occur even if the thickness is 0.640 mm or less. The thickness of the non-magnetic substrate 1 may be 0.570 mm or less, or even 0.52 mm or less, or even 0.400 mm or less. The thickness of the non-magnetic substrate 1 may be, for example, 0.635 mm, 0.550 mm, 0.500 mm, or 0.380 mm. From the perspective of mechanical durability, the lower limit of the thickness of the non-magnetic substrate 1 is preferably 0.2 mm or more. In principle, the thinner the non-magnetic substrate 1, the greater the problem of particle generation, and in some cases, the greater the problem of scratches and dents. However, in this embodiment, the effect of reducing particle generation, scratches, and dents is significant.
[0032] According to one embodiment, the Vickers hardness Hv of the film 4 is 100 [kgf / mm 2 By increasing the Vickers hardness Hv, defects such as scratches and dents are less likely to occur when the surface comes into contact with a ramp inside a hard disk drive device. The Vickers hardness Hv is preferably 100 [kgf / mm 2 If the thickness is less than 1 / 4, scratches or dents may occur when the surface comes into contact with the lamp inside the hard disk drive device, making the hard disk drive device more susceptible to failure.
[0033] According to one embodiment, the maximum height Rz (JIS B 0601:2001) of the surface roughness of the outer peripheral edge surface of the disk-shaped substrate body 3, which forms the interface with the film 4, is preferably 0.5 μm or more. The film 4 is formed on the substrate body 3, including the outer peripheral edge surface, and a cross-sectional image of the outer peripheral edge surface of the substrate body 3 can be acquired, thereby determining the maximum height Rz. Specifically, the outer peripheral edge surface of the non-magnetic substrate 1 on which the film 4 is formed is first cut using an ion polishing method along a plane passing through the center of the non-magnetic substrate 1 and perpendicular to the main surface, thereby creating a sample with an exposed cross section of the outer peripheral edge surface. A cross-sectional image of the outer peripheral edge surface is obtained at a magnification of, for example, 5000 times using a scanning electron microscope (SEM). From the image, the concave-convex curve of the surface of the substrate body 3, which forms the interface with the film 4, is obtained, for example, by binarizing the cross-sectional image or visually tracing it, and a 20 μm-wide region at any location on the concave-convex curve is extracted to determine the maximum height Rz.
[0034] The presence of a certain degree of surface unevenness at the interface of the substrate body 3 in contact with the film 4 enhances the vibration suppression by the film 4. It is presumed that this vibration suppression is due to the fact that the film 4 penetrates and bites into each other's recesses at the interface between the substrate body 3 and the film 4, increasing the adhesion between them, and the vibration suppression effect of the film 4 affects the substrate body 3. Furthermore, while increasing the thickness of the film 4 increases the film stress that causes film peeling, setting the maximum height Rz to 0.5 μm or more can prevent film peeling due to film stress. The outer peripheral end face has a smaller area and a more complex shape than the main surface, making it more susceptible to film peeling. The maximum height Rz of the surface roughness of the outer peripheral end face of the substrate body 3 is preferably 1.0 μm or more, and even more preferably 1.5 μm or more, in order to further enhance the vibration suppression described above. On the other hand, if the maximum height Rz is too large, the surface roughness of the film 4 after deposition (the surface roughness at the outer peripheral edge of the non-magnetic substrate 1) will increase in line with the surface roughness of the substrate body 3, making it easier for foreign matter to adhere to the outer peripheral edge during processing such as main surface polishing.Furthermore, foreign matter will also be more likely to adhere to the outer peripheral edge of the magnetic disk after the magnetic film is deposited, which may result in a decrease in the yield during the manufacture of the non-magnetic substrate 1 and hard disk drive devices.Note that the location of the outer peripheral edge where the maximum height Rz is 0.5 μm or more may be at least a portion of the outer peripheral edge, but in order to improve the suppression of vibration and prevent film peeling, it is preferable that it be both the side wall surface 3b and the chamfered surface 3c.On the other hand, if the maximum height Rz is too large on the main surface of the substrate body 3, defects may form and propagate during the initial formation of the film 4, causing defects such as recesses and cracks on the surface of the film 4. These defects cause corrosion and should be removed, but because they are deep-rooted and difficult to remove, their effects remain even after a magnetic film is formed to form a magnetic disk. Therefore, it is preferable that the maximum height Rz of the main surface of the substrate body 3 be, for example, 1 μm or less.
[0035] Furthermore, according to one embodiment, the maximum height Rz of the surface roughness of the film 4 at the outer peripheral edge of the non-magnetic substrate 1 is preferably smaller than the maximum height Rz of the surface roughness of the substrate body 3 at the outer peripheral edge of the substrate body 3 (the boundary surface in contact with the film 4). Regarding the maximum height Rz of the surface roughness of the film 4 at the outer peripheral edge of the non-magnetic substrate 1, for example, a stylus-type surface roughness and contour shape measuring instrument is used to determine the maximum height Rz of the surface roughness at multiple locations (e.g., three locations) on the outer peripheral edge under the following conditions, and the average value of these multiple locations is taken as the maximum height Rz of the surface roughness of the film 4. Note that the stylus movement (scanning) direction is the thickness direction of the non-magnetic substrate 1. Stylus shape: tip radius 2 μm, cone taper angle 60°; stylus load: 0.75 mN; stylus movement speed: 0.02 mm / sec; sampling length: 0.08 mm; filter λc: 0.08 mm; filter λs: 0.0008 mm.
[0036] If the maximum height Rz of the surface roughness of the film 4 at the outer peripheral edge of the non-magnetic substrate 1 is excessively large, it can easily cause foreign matter to adhere to the non-magnetic substrate 1, so a small maximum height Rz is preferable. The maximum height Rz is preferably 1.0 μm or less, and even more preferably 0.5 μm or less. The location on the outer peripheral edge of the non-magnetic substrate 1 where the maximum height Rz is limited may be at least a portion of the outer peripheral edge of the non-magnetic substrate 1. However, to enhance the vibration suppression effect and film peeling prevention effect, it is preferable that the location be the corresponding portion of the surface of the non-magnetic substrate 1 corresponding to the side wall surface 3b and the chamfered surface 3c. The surface roughness of the film 4 at the outer peripheral edge tends to mimic the surface roughness of the underlying substrate body 3. Therefore, if the surface roughness of the substrate body 3 is too large, additional processing such as edge polishing may be required after the film 4 is formed.
[0037] Such a non-magnetic substrate 1 is fabricated, for example, as follows. Here, as an example, a case where a glass substrate is used as the non-magnetic substrate 1 will be described. First, a glass blank, which will be the material for a plate-shaped magnetic disk glass substrate having a pair of main surfaces, is formed. Next, the glass blank is roughly ground. The glass blank is then shaped and edge polished. The glass substrate obtained from the glass blank is then finely ground using fixed abrasive grains. The glass substrate is then subjected to first polishing, chemical strengthening, and second polishing. Film formation and film polishing are then performed. In this embodiment, the glass substrate is fabricated according to the above-described sequence, but the above processes do not always need to be performed, and these processes may not be performed as appropriate. For example, among the above processes, edge polishing, fine grinding, first polishing, chemical strengthening, and second polishing may not be performed. Each process will be described below.
[0038] (a) Forming of Glass Blank For forming a glass blank, for example, a press forming method can be used. A circular glass blank can be obtained by the press forming method. Furthermore, it can be manufactured using known manufacturing methods such as a down-draw method, a re-draw method, and a fusion method. A disk-shaped glass substrate that serves as the base of a magnetic disk glass substrate can be obtained by appropriately shaping a plate-shaped glass blank manufactured by these known manufacturing methods.
[0039] (b) Rough grinding In rough grinding, grinding is performed on both main surfaces of the glass blank. For example, loose abrasive grains are used as the abrasive. In rough grinding, the glass blank is ground so as to approximate the target thickness dimension and flatness of the main surfaces. Note that rough grinding is performed depending on the dimensional accuracy or surface roughness of the formed glass blank, and may not be performed in some cases.
[0040] (c) Shape Processing Next, shape processing is performed. In shape processing, after molding the glass blank, a circular hole is formed using a known processing method to obtain a disk-shaped glass substrate with a circular hole. Then, the edge surfaces of the glass substrate are chamfered and the outer and inner diameters are adjusted by grinding. As a result, side wall surfaces 3b perpendicular to the main surfaces are formed on the edge surfaces of the glass substrate, and chamfered surfaces 3c inclined relative to the main surfaces 3a are formed between the side wall surfaces 3b and the main surfaces 3a on both sides.
[0041] (d) Edge Polishing Next, the edge of the glass substrate is polished. Edge polishing is a process in which, for example, a polishing liquid containing free abrasive grains is supplied between the polishing brush and the edge of the glass substrate (side wall surface 3b and chamfered surface 3c), and the polishing brush and the glass substrate are moved relative to each other. In edge polishing, the inner and outer peripheral edge surfaces of the glass substrate are polished to a mirror finish. Note that edge polishing may not be performed in some cases.
[0042] (e) Precision grinding Next, the main surfaces of the glass substrate are subjected to precision grinding. For example, a double-side grinding device with a planetary gear mechanism is used to grind the main surfaces 3a of the glass substrate. In this case, for example, fixed abrasive grains are provided on a surface plate for grinding. Alternatively, grinding can be performed using loose abrasive grains. Note that precision grinding may not be performed in some cases.
[0043] (f) First Polishing Next, the main surface 3a of the glass substrate is subjected to the first polishing. The first polishing uses a polishing pad attached to a surface plate using free abrasive grains. The first polishing removes cracks and distortions remaining on the main surface 3a after grinding with fixed abrasive grains, for example. The first polishing can reduce the surface roughness of the main surface 3a, for example, the arithmetic mean roughness Ra, while preventing the edge shape of the main surface 3a from excessively recessing or protruding. The free abrasive grains used in the first polishing are not particularly limited, but examples include cerium oxide abrasive grains or zirconia abrasive grains. Note that the first polishing may not be performed in some cases.
[0044] (g) Chemically strengthened glass substrates can be chemically strengthened as needed. Examples of chemical strengthening liquids include potassium nitrate, sodium nitrate, or a molten solution obtained by heating a mixture of these. By immersing the glass substrate in the chemical strengthening liquid, lithium ions and sodium ions in the glass composition on the surface of the glass substrate are replaced with sodium ions and potassium ions, respectively, which have relatively large ionic radii, in the chemical strengthening liquid. This results in the formation of a compressive stress layer in the surface layer, thereby strengthening the glass substrate. The timing of chemical strengthening can be determined as needed. However, polishing after chemical strengthening is particularly preferable, as it smooths the surface and removes foreign matter adhered to the surface of the glass substrate by chemical strengthening. In some cases, chemical strengthening may not be necessary.
[0045] (h) Second Polishing (Mirror Polishing) Next, the chemically strengthened glass substrate is subjected to a second polishing. The second polishing aims to mirror-polish the main surface 3a. The second polishing is performed using a polishing device with the same configuration as the first polishing. The second polishing uses different types and particle sizes of free abrasive grains compared to the first polishing, and a softer resin polisher is used as the polishing pad to perform mirror polishing. This reduces the roughness of the main surface 3a while preventing excessive depression or protrusion of the edge shape of the main surface 3a. The roughness of the main surface 3a is preferably 0.2 nm or less in arithmetic mean roughness Ra (JIS B 0601 2001). Since the main surface 3a of the substrate after the second polishing does not become the outermost surface of the non-magnetic substrate 1 having the film 4, the second polishing may not be performed in some cases.
[0046] (i) Film Formation: A film 4 is formed on the main surface 3a, sidewall surface 3b, and chamfered surface 3c of the fabricated glass substrate. The film 4 is formed by electrolytic plating, electroless plating, or the like. Before forming the film 4, pretreatment may be performed as needed to improve the adhesion of the film 4. The film 4 is formed on the main surface 3a, sidewall surface 3b, and chamfered surface 3c, and can have the same film thickness on all surfaces. After forming the film 4, an annealing treatment (heat treatment) of the film 4 is performed as needed to relieve internal stress in the formed film 4. It is preferable that the film 4 be nonmagnetic so as not to cause noise when finally formed into a magnetic disk.
[0047] (j) Film Polishing: After the film 4 is formed, the film 4 on the main surface 3a of the substrate body 3 is polished to reduce its surface roughness. The purpose of film polishing is mirror polishing. The roughness of the main surface after film polishing is preferably 0.2 nm or less in terms of arithmetic mean roughness Ra measured using an atomic force microscope (AFM). Film polishing can also be performed using a polishing device with a similar configuration to the first polishing. In film polishing, the type and particle size of the free abrasive grains are changed compared to the first polishing, and a resin polisher with a softer hardness is used as the polishing pad. Multiple polishing steps may be performed as necessary. In this case, the particle size of the free abrasive grains is reduced in later polishing steps to achieve more precise polishing. By polishing the film 4 formed on the main surface 3a in this manner and not polishing the film 4 on the sidewall surface 3b and chamfered surface 3c, the thickness of the film 4 on the sidewall surface 3b and chamfered surface 3c can be made thicker than the thickness of the film 4 on the main surface 3a. As described above, the film 4 formed on the side wall surface 3 b and the chamfered surface 3 c has the effect of suppressing the amplitude of vibration of the main surface 3 a of the non-magnetic substrate 1, so the thickness of the film 4 formed on the side wall surface 3 b and the chamfered surface 3 c is preferably set to a thickness that is thick enough to suppress the amplitude of vibration of the main surface 3 a. After film polishing, the glass substrate on which the film 4 has been formed is cleaned, and the non-magnetic substrate 1 for a magnetic disk is produced.
[0048] When the substrate body 3 is an Al alloy substrate, the substrate body 3 is fabricated, for example, by the following method. First, the Al alloy substrate that will become the substrate body 3 is machined to the required dimensions and shape by cutting. Then, to improve the shape accuracy and flatness of the substrate body 3, pressure and heat annealing is performed. Furthermore, the end faces (inner and outer peripheral end faces) of the substrate body 3 are ground and polished. To grind the end faces, as with a glass substrate, a rotary tool with abrasive grains attached is pressed against the machined end face of the substrate body 3, and while both are rotating, a grinding fluid is supplied from a nozzle to grind the end face of the substrate body 3. Furthermore, to reduce the surface roughness of the end faces, a polisher made of nonwoven fabric is attached to the surface of the rotary tool, and the end face of the substrate body 3 is polished while a polishing fluid containing dispersed abrasive grains is supplied. The chamfered surface of the substrate body 3 is formed by grinding using a formed grinding wheel whose end is pre-shaped to the chamfered shape of the rotary tool. Next, the main surfaces of the substrate body 3 are ground using a double-sided grinding machine, and then polished multiple times using a double-sided polishing machine with a polyurethane foam resin polisher and a polishing solution containing alumina abrasive grains or colloidal silica abrasive grains, and finally washed. The substrate body 3 may be subjected to a zincate treatment as a pretreatment for forming the film 4. After forming the film 4, an annealing treatment is appropriately performed to relieve the internal stress of the film 4. After the annealing treatment of the film 4, the main surfaces 3a are further polished. Polishing is performed multiple times depending on the needs of the substrate. After this, cleaning is performed, and the non-magnetic substrate 1 for a magnetic disk is produced.
[0049] In addition to the Ni-P alloy described above, the film 4 can be made of an Mg alloy, an Al-Zn alloy, an Mg-Zr alloy, or the like. Here, the material of the film 4 has a higher loss factor than the substrate body 3, with a loss factor of 0.01 or greater, in order to suppress vibrations of the non-magnetic substrate 1. However, according to one embodiment, the loss factor of the material of the film 4 is preferably 0.02 or greater, and more preferably 0.03 or greater. Furthermore, the loss factor of the substrate body 3 is preferably 0.002 or less, and more preferably 0.001 or less. The smaller the loss factor of the substrate body 3, the greater the vibration suppression effect of the film 4, so a substrate body 3 with a smaller loss factor is preferable. For amorphous aluminosilicate glass substrates used for magnetic disks, the loss factor is, for example, 0.001 or less. For Al-Mg alloy substrates for magnetic disks, the loss factor is, for example, 0.002 or less. Because the loss factor of the film 4 is sufficiently greater than the loss factor of the substrate body 3, forming the film 4 effectively suppresses vibrations. According to one embodiment, the Vickers hardness Hv of the material of the film 4 is set to 100 kgf / mm 2 ] or more, but 200 [kgf / mm 2 ] or more, and 400 [kgf / mm 2 ] or more is even more preferable.
[0050] Table 1 below shows the properties of materials that can be suitably used for the substrate body 3 and the film 4. The loss factors shown in Table 1 below were calculated using the above-mentioned method for calculating loss factors. The loss factor values are values at room temperature. The Vickers hardness Hv was measured using a micro Vickers hardness tester under the conditions of an indenter load of 10 gf for the film 4 because it is a thin film, and an indenter load of 300 gf for the substrate body 3.
[0051] In Table 1 above, the loss factors of aluminosilicate glasses were determined for several glasses, including those with the compositions of Glass 1 and Glass 2 described above. Note that a typical loss factor for Glass 2 is 0.0006. The Al-Mg alloy has a composition, in mass%, of 3.5-5% Mg, 0-0.05% Si, 0-0.1% Fe, 0-0.12% Cu, 0-0.3% Mn, 0-0.1% Cr, 0-0.5% Zn, 0-0.1% Ti, and the balance being Al. The Mg alloy has a composition, in mass%, of 91.57% Mg, 7.6% Al, 0.7% Zn, and 0.13% Mn. The Al-Zn alloy has a composition, in mass%, of 60% Al and 40% Zn. The composition of the Mg-Zr alloy is, in mass %, Mg: 99.4%, Zn: 0.6%, and the composition of the Ni-P alloy is, in mass %, Ni: 90%, P: 10%.
[0052] As can be seen from Table 1, it is preferable from the viewpoint of vibration suppression to use aluminosilicate glass or Al-Mg alloy as the material for the substrate body 3, and to use Ni-P alloy, Mg alloy, Al-Zn alloy, and Mg-Zr alloy as the material for the film 4. Furthermore, Ni-P alloy, Al-Zn alloy, and Mg-Zr alloy have a Vickers hardness Hv of 100 [kgf / mm 2 ] or more, which is high, and is more suitable as a material for the film 4, and particles, scratches, and dents are less likely to occur. In addition, it is understood that the Ni—P alloy has a particularly high Vickers hardness Hv, and is even more suitable as a material for the film 4.
[0053] (Experimental Example 1) Various substrates were fabricated to investigate the effects of the non-magnetic substrate 1. The substrate body of the non-magnetic substrate 1 was made of amorphous aluminosilicate glass and an aluminum alloy (Al-Mg alloy) satisfying the glass composition described above. When forming the film 4, a Ni-P alloy (P: 10% by mass, remainder Ni) was electrolessly plated to cover the entire surface of the substrate body 3 with a uniform thickness. The film 4 was then polished using a double-sided polishing machine, and 20% of the thickness of the film 4 was removed from each main surface. The final thickness of the film 4 was the same on both main surfaces, and each film 4 thickness was 80% of the thickness of the film 4 at the end face. The loss factor of the Ni-P alloy satisfied a value of 0.01 or greater. The fabricated non-magnetic substrate 1 had an outer diameter of 95 mm and an inner diameter (circular hole diameter) of 25 mm. Both the outer and inner peripheral end faces had chamfered surfaces at the junctions with the two main surfaces. The specifications of this chamfered surface were an angle of 45° with respect to the main surface, a length in the radial direction of 150 μm, and a length in the plate thickness direction of 150 μm. The roughness of the outer peripheral end surface was adjusted so that the maximum height Rz of both the surface of the substrate body 3 and the surface of the non-magnetic substrate 1 was 0.1 μm.
[0054] The magnetic disk obtained by forming a magnetic film on the fabricated non-magnetic substrate 1 was installed in an evaluation device modified from a hard disk drive. The evaluation device was equipped with a high-speed camera for observing the vibration of the magnetic disk, and it was possible to apply vibrations of any magnitude to the magnetic disk while monitoring the vibration of the magnetic disk with the high-speed camera. Note that the evaluation device did not rotate, but performed evaluations while the magnetic disk was stationary. This evaluation device was equipped with a ramp-like member made of PEEK (polyether ether ketone), so that when each magnetic disk was installed, a gap of 0.2 mm was left between both main surfaces. In other words, the gap between the ramps for the magnetic disk to fit was the thickness of the magnetic disk + 0.4 mm. Multiple evaluation devices with different specifications were prepared to maintain a constant gap even when the substrate thickness changed. The thickness of the magnetic film formed in the media process was approximately 100 nm or less, including the underlayer and soft magnetic layer, and therefore essentially negligible. Five magnetic disks were loaded into the evaluation device, and a portion of the main surface of each magnetic disk was sandwiched between the ramp members.
[0055] Using this evaluation device, impact tests were conducted in which a fixed impact was applied to the magnetic disks. The magnitude of the impact was optimized so that the magnetic disks of the comparative examples, which serve as the reference (100%) for the defect / foreign matter ratio in Tables 2 to 5, would collide with the ramp several times. Specifically, the impact in Table 2 was 140 G for 2 ms. Hereinafter, the impact time of 2 ms was constant, with 120 G in Table 2, 90 G in Table 3, and 70 G in Table 4. After the impact test, the number of particles and defects such as scratches and dents on the main surfaces of the assembled magnetic disks was visually inspected in a darkroom using a condenser lamp, and the numbers were counted on both sides of five disks. These particles, scratches, and dents were generated by the magnetic disks coming into contact with the ramp member or other disks within the device during the impact test. In Tables 2 to 5 below, the number of particles, scratches, and dents in Comparative Examples 1, 4, 7, and 10 is used as the reference (100%), and the number of particles, scratches, and dents in the examples and comparative examples is shown as a relative "defect / foreign matter ratio." The smaller the defect / foreign matter ratio, the fewer the number of particles, scratches, and dents. It is presumed that the smaller the defect / foreign matter ratio, the longer the life of the hard disk drive device will be due to the substantial effect of suppressing particles, etc. In the comparative examples and examples in Tables 2 to 5 below, the thickness of the substrate body 3 was kept constant, and the thickness of the film 4 was changed to variously change the ratio D / T.
[0056]
[0057]
[0058]
[0059]
[0060] Tables 2 and 3 show that Conventional Examples 1 and 2, in which the non-magnetic substrate 1 is thicker than 0.700 mm, do not experience any problems with particles, scratches, or dents, whereas Comparative Examples 1 and 3, in which the non-magnetic substrate 1 is thinner than 0.700 mm, do experience problems with particles, scratches, and dents. However, a comparison of Comparative Examples 2 and 3 with Examples 1 to 4, and a comparison of Comparative Examples 5 and 6 with Examples 5 to 8, shows that setting the D / T ratio to 0.025 or greater effectively reduces the number of particles, scratches, and dents. As shown in Tables 4 and 5, even when the non-magnetic substrate 1 is 0.520 mm thick, a comparison of Comparative Examples 8 and 9 with Examples 9 to 13, and a comparison of Comparative Examples 11 and 12 with Examples 14 to 18, shows that setting the D / T ratio to 0.025 or greater effectively reduces the number of particles, scratches, and dents. Furthermore, it can be seen that the reduction in the number of particles, scratches, and dents is greater than when the thickness is 0.640 mm. Furthermore, in Tables 2 to 5, when comparing examples (for example, Example 10 and Example 15) that have the same specifications except for the material of the substrate body 3, the defect and foreign matter ratio is lower when an Al alloy is used for the substrate body 3 than when glass is used. This means that when an Al alloy substrate is used as the substrate body 3, vibration suppression is greater than when glass is used. Note that the effect of suppressing vibration is more effective when the magnetic disk is likely to come into contact with the ramp, so the non-magnetic substrate 1 is particularly preferable for HDDs with a specification that the gap between the ramps for the magnetic disk to fit in is "the thickness of the magnetic disk + 0.4 mm or less."
[0061] (Experimental Example 2) Furthermore, various substrates were produced to investigate the surface roughness of the interface of the substrate body 3 in contact with the film 4 and the effect of vibration suppression. The non-magnetic substrate 1 produced in Experimental Example 2 had the same specifications for the substrate body 3 and film 4 as those of Experimental Example 1, except that the surface roughness of the outer peripheral edge face of the substrate body 3 was adjusted by appropriately changing the conditions for edge grinding and edge polishing. A magnetic disk obtained by forming a magnetic film on this non-magnetic substrate 1 was installed in the same evaluation device as in Experimental Example 1, and the same impact test as in Experimental Example 1 was performed to determine the defect / foreign matter ratio, thereby evaluating the effect of vibration suppression.
[0062] Examples 1, 5, and 13 in Tables 6 to 8 below are the same as Examples 1, 5, and 13 in Tables 2, 3, and 5. In these examples, the maximum height Rz, which is the surface roughness of the substrate body 3 at the interface where it contacts the film 4, is 0.1 μm. Using Examples 1, 5, and 13 as a reference, the maximum height Rz of the outer peripheral end face was adjusted without changing the type of substrate body 3, the presence or absence of film 4, the thickness of the non-magnetic substrate 1, and the D / T ratio. When fabricating the substrate body 3, the maximum height Rz was changed by changing the grinding wheel grit size and the polishing time of the outer peripheral end face during shaping. Therefore, in Table 6 below, examples in which the surface roughness of the outer peripheral end face was adjusted based on Example 1 are designated Examples 1A, 1B, and 1C. Similarly, in Tables 7 and 8, examples in which the surface roughness was adjusted based on Examples 5 and 13 are designated Examples 5A, 5B, 5C, and Examples 13A, 13B, and 13C.
[0063]
[0064]
[0065]
[0066] In all of the cases shown in Tables 6 to 8, it can be seen that by setting the maximum height Rz of the outer peripheral edge surface of the interface of the substrate body 3 in contact with the film 4 to 0.5 μm or more, the number of particles, scratches, and dents can be effectively reduced, and the vibration suppression effect is significant. It can also be seen that by setting the maximum height Rz to 1.0 μm or more, or even 1.5 μm or more, an even greater vibration suppression effect can be obtained. The above evaluation results clearly demonstrate the effects of the non-magnetic substrate 1 for magnetic disks.
[0067] The non-magnetic substrate for a magnetic disk and the magnetic disk of the present invention have been described in detail above, but the present invention is not limited to the above-mentioned embodiments and examples, and various improvements and modifications may be made without departing from the spirit and scope of the present invention.
[0068] REFERENCE SIGNS LIST 1 Non-magnetic substrate for magnetic disk 2 Inner hole 3 Substrate body 3a Main surface 3b Side wall surface 3c Chamfered surface 4 Film
Claims
1. A non-magnetic substrate for a magnetic disk, comprising: a substrate body having two opposing main surfaces; and a metal film of a material having a loss factor value of 0.01 or more provided on the main surfaces, wherein the thickness (T + D) of the non-magnetic substrate, which is the sum of the thickness T of the substrate body and the thickness D of the metal film, is 0.700 mm or less, and the ratio D / T of the thickness D of the metal film to the thickness T of the substrate body is 0.025 or more. The non-magnetic substrate for a magnetic disk is characterized by the above.
2. The metal film is provided on each of the main surfaces and further provided on the end surfaces of the substrate body. The thickness of the metal film on each of the main surfaces is 80% or more of the thickness of the metal film on the end surfaces. The non-magnetic substrate for a magnetic disk according to claim 1.
3. The thickness of the non-magnetic substrate is 0.640 mm or less. The non-magnetic substrate for a magnetic disk according to claim 1 or 2.
4. The non-magnetic substrate for a magnetic disk is in a disk shape, and the outer diameter of the disk shape is 90 mm or more. The non-magnetic substrate for a magnetic disk according to any one of claims 1 to 3.
5. The Vickers hardness Hv of the metal film is 100 [kgf / mm 2 . The non-magnetic substrate for a magnetic disk according to any one of claims 1 to 4.
6. The metal film is formed on the main surface and the outer peripheral end surface of the substrate body. The maximum height Rz of the surface roughness of the outer peripheral end surface of the substrate body that forms the interface with the metal film is 0.5 μm or more. The non-magnetic substrate for a magnetic disk according to any one of claims 1 to 5.
7. The metal film is formed on the main surface and the outer peripheral end surface of the substrate body. The maximum height Rz of the surface roughness of the film on the outer peripheral end surface of the non-magnetic substrate for a magnetic disk is smaller than the maximum height Rz of the surface roughness of the substrate body on the outer peripheral end surface of the substrate body. The non-magnetic substrate for a magnetic disk according to any one of claims 1 to 6.
8. A magnetic disk having at least a magnetic film on the surface of the non-magnetic substrate for a magnetic disk according to any one of claims 1 to 7.