Environment-friendly low-temperature-bending-resistant pressure-sensitive adhesive tape and preparation method therefor

By using a combination of bio-based acrylate copolymer and functional resin in the folding screen tape, the problems of poor low-temperature bending performance and easy adhesive residue at high temperatures of the existing tape are solved, achieving high-efficiency performance of the environmentally friendly adhesive layer, and The interpenetrating network structure is formed through chemical cross-linking, which meets the bonding needs of flexible foldable mobile phones and improves environmental pollution problems.

WO2024221970A1PCT designated stage expired Publication Date: 2024-10-31SUZHOU SHIHUA NEW MATERIAL TECH

Patent Information

Application Number
PCT/CN2023/138745
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2023-12-14
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing folding screen tapes have poor bending performance under low temperature conditions and are prone to adhesive residue at high temperatures. Moreover, the use of acrylic pressure-sensitive adhesives produced in the petrochemical industry causes environmental pollution, making it difficult to meet the bonding needs of flexible foldable mobile phones.

Method used

An environmentally friendly low-temperature bending pressure-sensitive tape is designed. Its adhesive layer contains bio-based acrylate copolymer, functional resin and curing agent. It generates high and low glass transition temperatures through two-phase separation to ensure low-temperature flexibility and high-temperature cohesion. And through chemical cross-linking, an interpenetrating network structure is formed to provide good adhesion properties.

Benefits of technology

It achieves good bending performance under low temperature conditions and no glue residue at high temperatures, and no glue spillage when slitting. The use of bio-based raw materials improves the problems of refractory degradation and high pollution of petroleum-based tapes, and satisfies the bonding of flexible foldable mobile phones. need.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023138745_31102024_PF_FP_ABST
    Figure CN2023138745_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of high polymer materials and particularly to an environment-friendly low-temperature-bending-resistant pressure-sensitive adhesive tape and a preparation method therefor. According to the present invention, a bio-based acrylate adhesive layer with both an extremely low glass transition temperature and a high glass transition temperature is designed on the basis of the need for low-temperature bending resistance, high-temperature viscosity, and cohesion required by flexible foldable mobile phones, and the regulation of a bio-based acrylate copolymer monomer, molecular weight, a functional resin, and a cross-linking agent allows the adhesive layer to meet certain modulus and adhesiveness requirements, and to meet a bio-based acrylate copolymer adhesive layer's requirements of low-temperature flexibility, high-temperature cohesiveness, high-temperature stripping without residual glue, and slitting without glue overflow; additionally, an easily biodegradable bio-based raw material is used for the adhesive layer, ameliorating the problem that petroleum-based adhesive layers are difficult to degrade, highly pollutive, and highly toxic.
Need to check novelty before this filing date? Find Prior Art

Description

Environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape and preparation method thereof Technical Field

[0001] The present invention relates to the technical field of polymer materials, in particular to an environmentally friendly low-temperature-resistant bending pressure-sensitive adhesive tape and a preparation method thereof. Background Art

[0002] With the continuous advancement of full-screen technology, the screen-to-body ratio of most mobile phones has exceeded 90%, approaching its limit. Increasing the screen size without increasing the phone's size is difficult, and excessive screen size can lead to problems such as inconvenience in operation and portability. Following the full-screen era, consumer electronics innovation will continue, and mobile phone appearances are likely to diversify. With the advancement of science and technology and market demand, flexible foldable phones debuted at the Mobile World Congress in 2019. Due to their portability and versatility, combining the advantages of mobile phones and tablets, they became an instant market hit, with market attention and demand growing year by year. To meet current consumer demand, leading manufacturers have invested heavily in recent years in promoting the development of foldable screen technology.

[0003] Whether folding outward or inward, flexible foldable phones present a series of new requirements for screen flexibility. Conventional screen and under-screen bonding also require upgrades to ensure the screen maintains reliable adhesion and appearance after withstanding the horizontal stress of hundreds of thousands of repeated folds and aging in high and low temperature environments. To meet the requirements of foldable functionality, the adhesive tape used to bond the phone's internal components will experience long periods of folding and frequent folding during actual use, requiring the tape to provide excellent adhesion and flex resistance.

[0004] The folding screen tape in the existing technology generally includes a 50μm release layer, a 25μm adhesive layer, a 25-50μm TPU / foam core material, a 25μm adhesive layer, and a 50μm release layer. The TPU core material has a large low-temperature fracture strength and elastic modulus, and its bending resistance is relatively poor, making it difficult to meet the connection requirements of the internal components of the folding screen. The foam core material is prone to creases after being bent at low temperatures, affecting the appearance of the folding screen. The elastic modulus of the adhesive layer is extremely low, and it is easy to leave residual glue at high temperatures, and it is easy to overflow glue when cutting. In addition, the tape prepared by the existing technology is relatively thick, and the process requires multiple coatings, which not only affects the appearance but also increases costs.

[0005] Currently, the acrylic pressure-sensitive adhesive (PSA) industry primarily relies on acrylate monomers produced by the petrochemical industry. As disposable products for daily use, PSAs are in high demand, inevitably accelerating the depletion of petroleum resources. Petroleum resources are non-renewable or difficult to regenerate, and overexploitation inevitably leads to the depletion of Earth's resources. Furthermore, petrochemical-derived PSAs biodegrade slowly and are difficult to degrade if directly discarded or landfilled. The environmental impact of these non-degradable waste adhesives is becoming increasingly severe, leading to an urgent need for the development of environmentally friendly, biodegradable PSAs. However, the types of natural raw materials that can be used in PSA products are limited. This requires not only a high degree of natural origin, but also the superior performance of petroleum-based adhesive tapes, or even better. The production of bio-based acrylate monomers is generally based on the catalytic esterification of plant-derived alcohols with acrylic acid. Bio-based alcohols are typically derived from natural products such as vegetable oils and borneol. These raw materials are abundant and highly renewable, aligning with sustainable development strategies. Bio-derived acrylate monomers have different structural units in their side chain groups from petroleum-based products, but they are equally reactive, so similar synthetic processes can be used to prepare bio-based acrylate adhesives.

[0006] The adhesive layer used in current flexible foldable mobile phones generally has an extremely low elastic modulus to achieve its low-temperature bendability, which makes it easy for glue to overflow during cutting and for residual glue to remain at high temperatures. The viscosity is significantly reduced under high temperature and high humidity. Summary of the Invention

[0007] The object of the present invention is to provide an environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: an environmentally friendly low-temperature resistant bending pressure-sensitive tape and a preparation method thereof.

[0009] An environmentally friendly, low-temperature-resistant, bendable pressure-sensitive tape, characterized in that: the pressure-sensitive tape comprises a first release layer, an adhesive layer, and a second release layer; the first release layer is provided on one side of the adhesive layer, and the second release layer is provided on the other side;

[0010] The adhesive layer contains at least two glass transition temperatures, the first glass transition temperature is between -70 and -30°C, and the second glass transition temperature is between 0 and 65°C; if the first glass transition temperature of the adhesive layer is less than -70°C, it will be too soft to affect the cohesion of the adhesive layer, and it is easy to leave residual glue at high temperatures, and it is easy for glue to overflow during cutting; if the first glass transition temperature of the adhesive layer is greater than -30°C, it will be too hard and not flexible enough at low temperatures, resulting in poor bending at low temperatures; if the second glass transition temperature of the adhesive layer is less than 0°C, it will affect the high-temperature cohesion of the adhesive layer, and it is easy to leave residual glue at high temperatures; if the second glass transition temperature of the adhesive layer is greater than 65°C, it will be too hard to affect the low-temperature flexibility, resulting in poor bending at low temperatures.

[0011] Furthermore, the adhesive layer comprises the following components: a bio-based acrylate copolymer, a functional resin, and a curing agent;

[0012] Adding a functional resin to the bio-based acrylate copolymer utilizes the difference in polarity to generate two-phase separation, ensuring the simultaneous existence of high and low glass transition temperature parts, thereby achieving its low-temperature flexibility and high-temperature resistance;

[0013] The adhesive layer provides good low-temperature flexibility and high-temperature cohesion by adhering to the adhered object, and has no adhesive residue during high-temperature peeling and no adhesive overflow during cutting.

[0014] The glass transition temperature of the bio-based acrylate copolymer is between -80 and -40°C. If the glass transition temperature of the bio-based acrylate copolymer is less than -80°C, it will be too soft, affecting the cohesion of the adhesive layer, and it will easily leave residual glue at high temperatures and overflow glue during cutting. If the glass transition temperature of the bio-based acrylate copolymer is greater than -40°C, it will be too hard and lack low-temperature flexibility, resulting in poor bending at low temperatures.

[0015] The glass transition temperature of the functional resin is between 0 and 55°C;

[0016] The mass ratio of the bio-based acrylate copolymer to the functional resin is (50:50) to (95:5);

[0017] The amount of the curing agent used is 0.5-2.5 wt % of the bio-based acrylate copolymer.

[0018] Furthermore, the bio-based acrylate copolymer is polymerized by a main monomer and an auxiliary monomer, wherein the main monomer is one or more of bio-based n-butyl acrylate, 2-ethylhexyl acrylate, 2-octyl acrylate, n-octyl acrylate, isooctyl acrylate, isononyl acrylate, isooctyl acrylate, 2-propylheptyl acrylate, alkoxylated tetrahydrofuran acrylate, methoxyethyl acrylate, caprolactone acrylate, ethoxyethoxyethyl acrylate, methoxypolyethylene glycol acrylate, tridecyl acrylate, hexadecyl acrylate, heptadecyl acrylate, isooctyl methacrylate, lauryl methacrylate, and dodecyl methacrylate; and the auxiliary monomer is one or more of methyl acrylate, acrylic acid, acrylamide, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, methacrylic acid, and methacrylamide.

[0019] Furthermore, in the bio-based acrylate copolymer, the mass ratio of the main monomer to the auxiliary monomer is (90:10) to (99.9:0.1).

[0020] Furthermore, the functional resin is any one or more of polyester resin, polyacrylic resin, and epoxy resin; the hydroxyl group, carboxyl group, epoxy group in the resin and the carboxyl group or hydroxyl group on the molecular chain segment of the bio-based acrylate copolymer are chemically cross-linked with the cross-linking agent to form an interpenetrating network structure, providing an adhesive layer for support and ensuring high-temperature cohesion of the adhesive layer.

[0021] Furthermore, the weight-average molecular weight of the bio-based acrylate copolymer is between 180,000 and 1,000,000. If the weight-average molecular weight of the bio-based acrylate copolymer is less than 180,000, the cohesion is too low, which affects the high-temperature cohesion and causes problems of residual glue and overflow. If the weight-average molecular weight of the bio-based acrylate copolymer is greater than 1,000,000, it is too high and affects the low-temperature flexibility.

[0022] Furthermore, the storage modulus of the adhesive layer is between 0 and 200 KPa at -20°C. If the storage modulus of the adhesive layer is ≥200 KPa at -20°C, poor low-temperature bending may occur due to the adhesive layer being too hard and lacking low-temperature flexibility.

[0023] Furthermore, the storage modulus of the adhesive layer is between 8 and 25 KPa at 65°C; if the storage modulus of the adhesive layer is less than 8 KPa at 65°C, the high-temperature residual adhesive peeling force is easily reduced due to too low high-temperature cohesion, and adhesive overflow is easy to occur during cutting; if the storage modulus of the adhesive layer is greater than 25 KPa at 65°C, the adhesive layer is too hard and lacks flexibility.

[0024] Furthermore, at 65° C., the adhesive layer has a ratio of loss modulus to storage modulus (tanθ) between 0.3 and 0.8.

[0025] Furthermore, the peeling force between any side of the adhesive layer and the mirror steel plate at 65° C. is between 5.0 and 8.0 N / inch.

[0026] A method for preparing an environmentally friendly low-temperature-resistant bending pressure-sensitive adhesive tape comprises the following steps:

[0027] S1: Take the functional monomer and auxiliary monomer of the bio-based acrylate copolymer, mix them evenly to obtain a bio-based acrylate mixed monomer, add a solvent and an initiator, heat and stir under nitrogen protection, and keep warm for 3-5 hours to obtain a bio-based acrylate copolymer solution;

[0028] S2: Take a functional resin, add toluene to obtain a functional resin solution, add the bio-based acrylate copolymer solution, mix evenly, add a diluent solvent, mix evenly, add a curing agent, mix for 20-50 minutes, let it stand for defoaming, and obtain a bio-based acrylate adhesive solution;

[0029] S3: applying a bio-based acrylate adhesive to the release surface of the first release layer, drying the adhesive layer, laminating the dried adhesive layer with the release surface of the second release layer, and curing the adhesive layer to obtain an environmentally friendly low-temperature resistant bending pressure-sensitive tape;

[0030] The adhesive layer has a first glass transition temperature of -80 to -30°C, and a second glass transition temperature of 0 to 65°C.

[0031] Furthermore, the main monomer of the bio-based acrylate copolymer is one or more of bio-based n-butyl acrylate, 2-ethylhexyl acrylate, 2-octyl acrylate, n-octyl acrylate, isooctyl acrylate, isononyl acrylate, isooctyl acrylate, 2-propylheptyl acrylate, alkoxylated tetrahydrofuran acrylate, methoxyethyl acrylate, caprolactone acrylate, ethoxyethoxyethyl acrylate, methoxypolyethylene glycol acrylate, tridecyl acrylate, hexadecyl acrylate, heptadecyl acrylate, isooctyl methacrylate, lauryl methacrylate, and dodecyl methacrylate; and the auxiliary monomer is one or more of methyl acrylate, acrylic acid, acrylamide, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, methacrylic acid, and methacrylamide.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention proposes an environmentally friendly double-sided adhesive tape with low low-temperature flexibility and good bending resistance, but not easy to leave residual adhesive at high temperatures and no adhesive overflow during cutting, which is used for folding screens for bonding mobile phone screens to conductive graphite or metal sheets. Based on the requirements of low-temperature bending resistance and high-temperature adhesion and cohesion required by flexible foldable mobile phones, the present invention designs a bio-based acrylate adhesive layer with both extremely low glass transition temperature and high glass transition temperature, so that the adhesive layer meets certain modulus and adhesion requirements, and meets the requirements of low-temperature flexibility, high-temperature cohesion, no residual adhesive during high-temperature peeling, and no adhesive overflow during cutting of the bio-based acrylate copolymer adhesive layer. In addition, the adhesive layer uses bio-based raw materials that are easily biodegradable, which improves the problems of difficult degradation, high pollution, and high toxicity of petroleum-based adhesive layers. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:

[0035] FIG1 is a schematic diagram of the structure of the bio-based double-sided adhesive tape of the present invention;

[0036] FIG2 is a graph showing performance changes of the adhesive layer at different temperatures according to Example 4 of the present invention;

[0037] In the figure: 1-first release layer; 2-adhesive layer; 3-second release layer. DETAILED DESCRIPTION

[0038] The following will clearly and completely describe the technical solutions in the embodiments of the present invention in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.

[0039] 1. Preparation method of bio-based acrylate copolymer solution (A1-A5), the specific steps are as follows:

[0040] The raw materials were weighed by mass, and a bio-based acrylate mixed monomer was added to a reactor with reflux condensation. 1 / 2 of the total mass of the mixed monomer, 1 / 2 of the total mass of the solvent, and 1 / 4 of the total mass of the initiator were heated and stirred under nitrogen protection at a temperature of 85°C. After the reaction started, 1 / 2 of the total mass of the initiator, the remaining bio-based acrylate mixed monomer and 1 / 2 of the total mass of the solvent were evenly added dropwise within 60 minutes. The reaction was continued at a temperature of 80°C for 2 hours. Finally, the remaining initiator was added and the temperature was kept warm for 4 hours to obtain a bio-based acrylate copolymer solution.

[0041] Specifically, the bio-based comonomer is selected from one or more of 2-ethylhexyl acrylate (2-EHA), heptadecyl acrylate (C17A), n-octyl acrylate (OA), methyl acrylate (MA), and acrylic acid (AA); the initiator is azobisisobutyronitrile (AIBN); and the solvent is selected from ethyl acetate (EAC) and toluene (Tol). The resulting acrylate copolymer solution is then tested for weight-average molecular weight (Mw) and glass transition temperature (Tg).

[0042] The specific formula of the bio-based acrylate copolymer solution (mass ratio of the added materials) is shown in Table 1.

[0043] Table 1

[0044]

[0045] 2. Preparation method of bio-based acrylate copolymer solution (A6-A7), the specific steps are as follows:

[0046] The raw materials were weighed by mass, and the bio-based acrylate mixed monomers were added into a reactor with reflux condensation. 4 / 5 of the total mass of the mixed monomers, 2 / 5 of the total mass of the solvent, and 1 / 3 of the total mass of the initiator were heated and stirred under nitrogen protection. After the reaction was carried out at 70°C for 120 minutes, 1 / 6 of the total mass of the initiator and the remaining 1 / 5 of the total mass of the bio-based acrylate mixed monomers and the solvent were evenly added dropwise within 120 minutes. The reaction was continued at 70°C for 3 hours. Finally, the remaining initiator was added and kept warm for 3 hours. Finally, the remaining solvent was added to obtain a bio-based acrylate copolymer solution.

[0047] Specifically, the bio-based comonomers used were one or more of 2-ethylhexyl acrylate (2-EHA), n-octyl acrylate (OA), methyl acrylate (MA), and acrylic acid (AA); the initiators were azobisisobutyronitrile (AIBN) and dibenzoyl peroxide (BPO); and the solvent was ethyl acetate (EAC) or toluene (Tol). The resulting acrylate copolymer solution was tested for weight-average molecular weight (Mw) and glass transition temperature (Tg).

[0048] The specific formula of the bio-based acrylate copolymer solution (mass ratio of the added materials) is shown in Table 2.

[0049] Table 2

[0050]

[0051] 3. Preparation of bio-based acrylic adhesive

[0052] Take a functional resin and add toluene to obtain a functional resin concentration of 50% to obtain a functional resin solution. The bio-based acrylate copolymer solution prepared in step 1 is mixed with the functional resin solution in a certain proportion to obtain 100 parts by weight of a bio-based acrylate masterbatch. A diluent solvent is added to the obtained masterbatch and stirred for 30 minutes to mix evenly. Finally, a curing agent is added and stirred for 30 minutes to mix evenly. The mixture is allowed to stand for defoaming to obtain a bio-based acrylate adhesive solution.

[0053] The mass ratios of the above components in the specific examples and comparative examples are shown in Table 3.

[0054] The functional resin in Table 3 is selected from any one of polyester resin (B1), polyester resin (B2), polyester resin (B3), acrylic resin (B4), and epoxy resin (B5). Polyester resin (B1) is provided by Toyobo, with a product number of 280 and a Tg of 68°C; polyester resin (B2) is provided by Toyobo, with a product number of GK-680 and a Tg of 10°C; polyester resin (B3) is provided by Mitsubishi Chemical, with a product number of TP249 and a Tg of 36°C; acrylic resin (B4) is provided by Mitsubishi Chemical, with a product number of BR116 and a Tg of 48°C; epoxy resin (B5) is provided by Nan Ya, with a product number of NPES-901 and a Tg of 60°C.

[0055] The curing agent isocyanate was provided by Toyo Ink, product number BHS8515, with a solid content of 5%.

[0056] The dilution solvent used was ethyl acetate, which was provided by Jiangsu Sopo.

[0057] Table 3

[0058]

[0059] 6. Preparation of environmentally friendly tape for folding screens

[0060] A bio-based acrylate adhesive was applied to the release surface of the first release layer (1) using a comma blade coater. The adhesive was then placed in a 100°C oven for 2 minutes to evaporate the solvent, forming a bio-based adhesive layer with a thickness of 25 μm. The dried adhesive layer (2) was then laminated to the release surface of the second release layer (3). The coated eco-friendly foldable screen tape was then cured at room temperature (25°C) for 7 days to obtain the eco-friendly foldable screen tape. After curing, the tape was left at room temperature for 24 hours before physical property testing.

[0061] The first release layer 1 is a release film 1, provided by Yaoyang New Materials, with a thickness of 50 μm and a release force of 15-20 g / inch;

[0062] The second release layer 3 is a release film 2 provided by Jiangyin Huamei Technology, with a thickness of 20 μm and a release force of 3-6 g / inch.

[0063] experiment

[0064] If the test conditions are not clearly stated, the following tests are conducted at 23°C-50%RH.

[0065] The weight average molecular weight (Mw) of the acrylate copolymer was determined using a Waters E2695 gel permeation chromatograph. Test conditions: mobile phase: tetrahydrofuran; column temperature: 40° C.; mobile phase flow rate: 1.0 mL / min.

[0066] A bio-based acrylate adhesive coating was applied to a 50 μm release film using a comma roller scraper. The film was then dried in a 100°C oven for 5 minutes to obtain a dry adhesive film. Rheological tests were performed using a TA HR-10 rotational rheometer. The loss modulus G'' and storage modulus G' of the adhesive layer were measured by temperature scanning at a temperature of -100-150°C, a heating rate of 5°C / min, a strain of 0.1%, and a frequency of 1 Hz.

[0067] A comma roller scraper was used to scrape a bio-based acrylate adhesive onto a 50 μm release film. The film was then dried in a 100°C oven for 5 minutes to obtain a dry adhesive film. Rheological testing was performed using a TA HR-10 rotational rheometer from the United States. The apex of the peak of the loss factor tanθ curve of the adhesive layer, measured at a temperature of -100-150°C, a heating rate of 5°C / min, a strain of 0.1%, and a frequency of 1 Hz, was recorded as the glass transition temperatures Tg1 and Tg2 of the adhesive layer.

[0068] Using a comma roller, apply the acrylate copolymer solution onto a 50μm release film. Dry the film in a 100°C oven for 5 minutes to obtain a 25μm thick dry film. The glass transition temperature (Tg) of the dry film was then determined using a Netzsch DSC200F3 measuring instrument. The test temperature range was -100-120°C, with a heating rate of 5°C / min.

[0069] At 23°C, either side of a 150mm long × 25mm wide tape strip was reinforced with a 50μm thick D03 standard BOPET film from Yihua Toray, and the other side was bonded to a stainless steel mirror plate (150mm long × 50mm wide × 2mm thick and surface roughness: 10nm±10nm) that meets the requirements of GB / T2792 peel test steel plate material. A 2kg roller was used to roll the strip back and forth on the stainless steel mirror plate at a speed of 300mm / min. After standing for 20 minutes at -30°C / 65°C, a 180° peel strength test was performed using a tensile machine at a peel speed of 300mm / min. Three samples were tested, and the arithmetic average of the three test results was taken as the peel force result.

[0070] If the ratio of the residual adhesive area on the mirror-finished stainless steel plate after the tape strip peel test at 65°C to the area where the tape strip was peeled from the plate is ≤5%, the sample is considered to have excellent adhesive residue. If the ratio of the residual adhesive area on the mirror-finished stainless steel plate after the tape strip peel test at 65°C to the area where the tape strip was peeled from the plate is greater than 5%, the sample is considered to have poor adhesive residue. Adhesive residue refers to the phenomenon where the adhesive layer has cohesively failed, with both the substrate and the plate surface covered by the damaged adhesive layer.

[0071] The performance test results of the bio-based adhesive layers of the comparative examples and embodiments are listed in Table 4.

[0072] Table 4

[0073]

[0074] Conclusion: From the comparison in Table 4, it can be concluded that in Example 1, the Tg of the bio-based acrylate copolymer is relatively low, resulting in poor cohesion of the adhesive layer at high temperature and the problem of residual adhesive.

[0075] In Example 2, the Tg of the bio-based acrylate copolymer is relatively high, resulting in an excessively high low-temperature storage modulus of the adhesive layer.

[0076] In Example 3, the molecular weight of the bio-based acrylate copolymer is relatively low, the adhesive layer has poor cohesion at high temperature and low peeling strength, and is prone to adhesive residue.

[0077] In Examples 4-6, the functional resin polyester resin B3 is added to the bio-based acrylate copolymers A4-A6, and the high and low temperature modulus and peel strength of the adhesive layer meet the requirements without residual adhesive.

[0078] In Example 7, the molecular weight of the bio-based acrylate copolymer is relatively high, the high-temperature modulus of the adhesive layer is high, and the high-temperature peel strength is too high, which affects the reworkability.

[0079] In Example 8, the functional resin polyester resin B1 was added to the bio-based acrylate copolymer A4, and the high-temperature modulus of the adhesive layer was too high, and the adhesive surface was too hard and had no adhesiveness.

[0080] In Example 9, the functional resin polyester resin B2 was added to the bio-based acrylate copolymer A4, and the high-temperature modulus of the adhesive layer was too low, and the high-temperature peeling strength was insufficient.

[0081] In Example 10, the amount of functional resin B2 added was too high, the high / low temperature modulus of the adhesive layer was too high, and the adhesive surface was too hard and non-sticky.

[0082] In Example 11, the addition amount of the functional resin B2 was too low, the high-temperature modulus of the adhesive layer was low, and the high-temperature peeling force was insufficient.

[0083] In Example 12, the functional resin acrylic resin B4 is added to the bio-based acrylate copolymer A4, and the high and low temperature modulus and peel strength of the adhesive layer meet the requirements without residual adhesive.

[0084] In Example 13, the functional resin B5 was added to the bio-based acrylate copolymer A4, but the high-temperature modulus of the adhesive layer was too high, and the adhesive surface was too hard and non-sticky.

[0085] No functional resin was added to the formulations of Comparative Examples 1-2. The adhesive layer had low high-temperature peeling strength, poor cohesion, and easy adhesive residue. By increasing the crosslinking agent, the high-temperature peeling strength was still low, but the low-temperature modulus was too high and the low-temperature flexibility was poor.

[0086] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art will be able to modify the technical solutions described in the aforementioned embodiments or substitute equivalents for some of the technical features. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.

Claims

1. An environmentally friendly low-temperature resistant bending pressure-sensitive tape, characterized in that: The pressure-sensitive adhesive tape comprises a first release layer (1), an adhesive layer (2), and a second release layer (3); the first release layer (1) is arranged on one side of the adhesive layer (2), and the second release layer (3) is arranged on the other side; The adhesive layer (2) has at least two glass transition temperatures, the first glass transition temperature is between -70 and -30°C, and the second glass transition temperature is between 0 and 65°C.

2. The environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape according to claim 1, characterized in that: The adhesive layer (2) comprises the following components: a bio-based acrylate copolymer, a functional resin, and a curing agent; The glass transition temperature of the bio-based acrylate copolymer is between -80 and -40°C; The glass transition temperature of the functional resin is between 0 and 55°C; The mass ratio of the bio-based acrylate copolymer to the functional resin is (50:50) to (95:5); The amount of the curing agent used is 0.5-2.5wt% of the bio-based acrylate copolymer.

3. The environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape according to claim 2, characterized in that: The bio-based acrylate copolymer is polymerized by a main monomer and an auxiliary monomer. The main monomer is one or more of bio-based n-butyl acrylate, 2-ethylhexyl acrylate, 2-octyl acrylate, n-octyl acrylate, isooctyl acrylate, isononyl acrylate, isobutyl acrylate, 2-propylheptyl acrylate, alkoxylated tetrahydrofuran acrylate, methoxyethyl acrylate, caprolactone acrylate, ethoxyethoxyethyl acrylate, methoxypolyethylene glycol acrylate, tridecyl acrylate, hexadecyl acrylate, heptadecyl acrylate, isooctyl methacrylate, lauryl methacrylate, and dodecyl methacrylate; the auxiliary monomer is one or more of methyl acrylate, acrylic acid, acrylamide, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, methacrylic acid, and methacrylamide.

4. The environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape according to claim 3, characterized in that: In the bio-based acrylate copolymer, the mass ratio of the main monomer to the auxiliary monomer is (90:10) to (99.9:0.1).

5. The environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape according to claim 2, characterized in that: The functional resin is any one or more of polyester resin, polyacrylic resin and epoxy resin.

6. The environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape according to claim 2, characterized in that: The weight average molecular weight of the bio-based acrylate copolymer is between 180,000 and 1,000,000.

7. The environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape according to claim 1, characterized in that: The adhesive layer (2) has a storage modulus between 0 and 200 KPa at -20°C; The adhesive layer (2) has a storage modulus between 8 and 25 KPa at 65°C; When the temperature of the adhesive layer (2) is 65° C., the ratio of the loss modulus to the storage modulus (tanθ) is between 0.3 and 0.

8.

8. The environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape according to claim 1, characterized in that: The peeling force of any side of the adhesive layer (2) from the mirror steel plate at 65° C. is between 5.0 and 8.0 N / inch.

9. A method for preparing an environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape, characterized in that: The following steps are involved: S1: Take the functional monomer and auxiliary monomer of the bio-based acrylate copolymer, mix them evenly to obtain a bio-based acrylate mixed monomer, add a solvent and an initiator, heat and stir under nitrogen protection, and keep warm for 3-5 hours to obtain a bio-based acrylate copolymer solution; S2: Take a functional resin, add toluene to obtain a functional resin solution, add the bio-based acrylate copolymer solution, mix evenly, add a diluent solvent, mix evenly, add a curing agent, mix for 20-50 minutes, let stand to defoam, and obtain a bio-based acrylate adhesive glue solution; S3: applying a bio-based acrylic adhesive liquid on the release surface of the first release layer (1), drying the adhesive layer (2) after drying and compounding the release surface of the second release layer (3), and aging the adhesive layer to obtain an environmentally friendly low-temperature resistant bending pressure-sensitive tape; The first glass transition temperature of the adhesive layer (2) is between -80 and -30°C, and the second glass transition temperature is between 0 and 65°C.

10. The method for preparing an environmentally friendly low-temperature resistant bending pressure-sensitive adhesive tape according to claim 9, characterized in that: The main monomer of the bio-based acrylic ester copolymer is one or more of bio-based n-butyl acrylate, 2-ethylhexyl acrylate, 2-octyl acrylate, n-octyl acrylate, isooctyl acrylate, isononyl acrylate, isodecyl acrylate, 2-propylheptyl acrylate, alkoxylated tetrahydrofuran acrylate, methoxyethyl acrylate, caprolactone acrylate, ethoxyethoxyethyl acrylate, methoxypolyethylene glycol acrylate, tridecyl acrylate, hexadecyl acrylate, heptadecyl acrylate, isooctyl methacrylate, lauryl methacrylate, and dodecyl methacrylate; the auxiliary monomer is one or more of methyl acrylate, acrylic acid, acrylamide, 2-hydroxyethyl acrylate, 4-hydroxybutyl acrylate, methacrylic acid, and methacrylamide.

Citation Information

Patent Citations

  • Pressure sensitive adhesive composite with wide temperature applicable range and preparation method thereof

    CN101705066A

  • A pressure-sensitive adhesive for BOPP protective film and its preparation method

    CN102260477A

  • Pressure sensitive adhesive composition and product thereof

    CN105505263A

  • Optical pressure-sensitive adhesive and preparation method thereof

    CN105694773A

  • Renewable pressure-sensitive adhesive and preparation method thereof

    CN110776856A

Cited By

  • Dual-curable high-viscosity folding OCA adhesive, adhesive film and preparation method

    CN118389101A

  • Semi-interpenetrating dual-network organogel OCA optical adhesive applied to folding display equipment, preparation method of semi-interpenetrating dual-network organogel OCA optical adhesive and folding display equipment

    CN119242226A

  • Ultralow-temperature double-faced adhesive tape and manufacturing process thereof

    CN119463716A