Reverse osmosis membrane preparation method and reverse osmosis membrane prepared thereby

By building artificial water channels in reverse osmosis membrane, the scarcity and high cost of natural aquatic channel proteins are solved, and a high-throughput and high desalination rate reverse osmosis membrane is achieved, reducing operating pressure and achieving energy saving and consumption reduction effect .

WO2024250573A1PCT designated stage expired Publication Date: 2024-12-12VONTRON TECH CO LTD

Patent Information

Application Number
PCT/CN2023/131577
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-06-08
Filing Date
2023-11-14
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

The application of natural aquaporin in reverse osmosis membranes has problems such as scarce yield, difficulty in collecting, high cost, poor stability and difficult to scale, which limits its application in reverse osmosis membrane technology.

Method used

By pretreating the porous polymer-supported base film with a silane coupling agent and contacting the catalyst and substances that can form artificial water channels, artificial water channels are formed through self-assembly, and high-throughput, high desalination is prepared by combining interfacial polymerization reaction. rate reverse osmosis membrane.

Benefits of technology

The reverse osmosis membrane with high throughput and high desalination rate is achieved, which reduces the operating pressure, achieves the purpose of energy saving and consumption reduction, and overcomes the application shortcomings of natural aquaporin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023131577_12122024_PF_FP_ABST
    Figure CN2023131577_12122024_PF_FP_ABST
Patent Text Reader

Abstract

A reverse osmosis membrane preparation method and a reverse osmosis membrane prepared thereby. The preparation method comprises the following steps: forming a porous polymer support-layer base membrane; pretreating the porous polymer support-layer base membrane by using an aqueous solution containing a silane coupling agent; enabling the pretreated porous polymer support-layer base membrane to be in contact with a solution containing a catalyst and a substance capable of forming an artificial water channel, so as to form the artificial water channel by means of self-assembly; sequentially enabling the pretreated porous polymer support-layer base membrane having the artificial water channel to be in contact with a water-phase solution containing an amine monomer, and an oil-phase solution containing an acyl chloride monomer, thereby forming a polyamide functional layer; and performing post-treatment to obtain a reverse osmosis membrane. By means of the method, a reverse osmosis membrane having high flux and a high desalinization rate can be prepared, and the prepared reverse osmosis membrane can effectively reduce the operation pressure in the running process thereof, thereby achieving the objectives of energy saving and consumption reduction.
Need to check novelty before this filing date? Find Prior Art

Description

Method for preparing reverse osmosis membrane and reverse osmosis membrane prepared thereby

[0001] Citation of Related Applications

[0002] This disclosure claims priority to invention patent application number 202310675890.5, filed in China on June 8, 2023, entitled “Method for preparing reverse osmosis membrane and reverse osmosis membrane prepared thereby”, and the entire contents of that patent application are incorporated herein by reference. Technical Field

[0003] The present disclosure relates to the technical field of reverse osmosis membranes, and in particular to a reverse osmosis membrane with an artificial water channel and a preparation method thereof. Background Art

[0004] As one of the key technologies to solve the current global water resource problems, reverse osmosis technology has received unprecedented attention worldwide. Although reverse osmosis membranes have been widely used in the fields of electricity, metallurgy, petrochemicals, medicine, food, municipal engineering, sewage reuse and seawater desalination, there is still a prominent contradiction in meeting the huge demand for reverse osmosis membrane applications and the limitations of existing desalination technologies. Among them, improving the comprehensive performance of reverse osmosis membranes with water flux and desalination rate as the core is an enduring research topic.

[0005] Aquaporins are naturally occurring proteins found throughout the body. They form pores in cell membranes, controlling the flow of water in and out of cells while simultaneously removing all ions. In recent years, numerous research institutions and market players have initiated research into incorporating aquaporins into reverse osmosis membrane manufacturing. Natural aquaporins are widely used in reverse osmosis membranes.

[0006] Patent Document 1 (CN108176241B) provides a composite nanofiltration membrane containing aquaporin and a method for preparing the same. The method comprises: step S1, placing aquaporin vesicles and a polyamine aqueous monomer solution on the surface of a porous support layer to obtain a surface-treated porous support layer, wherein the polyamine aqueous monomer solution comprises a polyamine, a surfactant, an acid acceptor, and water; step S2, performing a second surface treatment on the surface-treated porous support layer using a polyacyl chloride oil-phase monomer solution to obtain a composite nanofiltration preliminary membrane; and step S3, drying the composite nanofiltration preliminary membrane to obtain a composite nanofiltration membrane. The composite nanofiltration membrane comprises a porous support layer and a polymerized polyamide layer, wherein the aquaporin vesicles are dispersed in the polyamide layer. This not only protects the activity of the aquaporin but also ensures the strength of the composite nanofiltration membrane, significantly improving the water flux of the membrane and enhancing the membrane's anti-fouling ability.

[0007] Patent Document 2 (CN103463997B) discloses a method for preparing a composite membrane containing aquaporin. The method involves self-polymerizing dopamine onto the surface of a basement membrane. This polydopamine-attached basement membrane then reacts with the amino groups of a phosphatidylethanolamine membrane containing aquaporin, thereby producing the composite membrane. This patented technology belongs to the field of nanofiltration membrane technology.

[0008] Patent document 3 (CN103721572B) discloses a method for preparing a phospholipid biomimetic membrane containing water channel protein. A composite membrane with an electronegative surface is prepared by layer-by-layer assembly, and then a positively charged phospholipid vesicle solution wrapped with water channel protein is spread on the composite membrane through electrostatic binding to form a phospholipid bilayer membrane. This patented technology belongs to the field of nanofiltration membrane technology.

[0009] Patent Document 4 (CN104144737B) discloses a thin film composite membrane based on aquaporin, in which a thin selective layer of natural amphiphilic vesicles is supported by a microporous substrate, wherein the amphiphilic substance is selected from block copolymers, including triblock copolymers of the hydrophile-hydrophobe-hydrophile ABA or ABC type or diblock copolymers of the hydrophile-hydrophobe AB type.

[0010] Patent document 5 (CN106731908A) discloses a composite reverse osmosis membrane containing aquaporin and a preparation method thereof. The preparation method of the reverse osmosis membrane comprises modifying the surface of a polysulfone support membrane, grafting amino functional groups, and allowing the amino groups to participate in the interfacial polymerization reaction of polyamide, so that the connection between the polysulfone support layer and the polyamide active layer is a chemical bond force, thereby enhancing the bonding force between the two, thereby effectively extending the life of the composite reverse osmosis membrane.

[0011] Patent Document 6 (CN106928324A) discloses a method for increasing the expression activity of aquaporins in vesicles. The method comprises the phosphorylation of aquaporins and the preparation of a phospholipid vesicle system solution in the first step, and the introduction of phosphorylated aquaporins in the second step. The phosphorylation of aquaporins increases the expression activity of aquaporins, and the phosphorylated aquaporins are then embedded in vesicles and applied to reverse osmosis membranes. When the water flux and salt rejection rate are achieved at the same level, the ratio of aquaporins to vesicles is greatly reduced.

[0012] Patent Document 7 (CN107474119B) discloses antibacterial aquaporin vesicles, which are used to prepare antibacterial aquaporin reverse osmosis membranes. The antibacterial aquaporin vesicles are prepared by encapsulating aquaporins in quaternized ABA or AB amphiphilic block copolymers. These vesicles are then directly added to the reverse osmosis membrane, preserving the surface structure of the polyamide functional layer while simplifying the preparation process for the antibacterial aquaporin reverse osmosis membrane.

[0013] Patent Document 8 (CN108602025B) discloses an RO membrane or FO membrane having a high water permeability and salt-blocking performance, comprising a covering layer composed of a phospholipid bilayer membrane formed on the surface of a porous membrane body. The membrane is a selectively permeable membrane having a porous membrane with a pore size of 5 nm to 50 nm and a covering layer composed of a phospholipid bilayer formed on the surface of the porous membrane. The phospholipid bilayer contains phospholipids, amphotericin B, and ergosterol, with amphotericin B being included as a channel substance.

[0014] Patent Document 9 (CN108697984B) discloses a self-assembled nanostructure formed between a transmembrane protein such as aquaporin and polyalkyleneimine, and a separation membrane comprising the nanostructure.

[0015] Patent document 10 (CN110382094A) discloses a selective permeable membrane, which comprises a selective permeable support membrane and a lipid membrane formed on the surface of the support membrane and containing a channel substance. The support membrane has a flow rate of 20 L / (m 2 h) and a permeation flux of 1% to 20%.

[0016] Patent Document 11 (CN111545084A) discloses a method for preparing a composite nanofiltration membrane containing aquaporin. The method comprises: S1, placing aquaporin vesicles and a polyamine aqueous monomer solution on the surface of a porous support layer to obtain a surface-treated porous support layer, wherein the polyamine aqueous monomer solution comprises a polyamine, a surfactant, an acid acceptor, and water; S2, preparing a phosphate buffer solution with a pH of 5.5-8; and S3, dissolving tannic acid and polyetheramine in the phosphate buffer solution to prepare tannic acid and polyetheramine solutions, respectively, each with a concentration of 0.1-0.5 g / L. This invention involves alternating deposition of tannic acid and polyetheramine on a porous polymer base membrane, resulting in a nanofiltration membrane with a stable selective layer structure, which is beneficial for improving membrane stability. Furthermore, the polyethylene glycol segments in the polyetheramine can reduce protein adhesion, improving the membrane's anti-fouling properties.

[0017] Patent document 12 (CN112058097B) discloses a method for preparing a forward osmosis membrane material. The material is composed of a four-layer structure, comprising a basement membrane, a dopamine cushion layer, a phospholipid bilayer containing water channel proteins, and a polymer protective layer. The forward osmosis membrane prepared by this invention has a dense non-porous structure, efficient interception, and high mechanical strength and acid and alkali resistance, capable of achieving a removal effect of more than 99% of monovalent ions; it has good stability, a high water flux recovery rate after cleaning the membrane, strong anti-pollution ability, and can effectively alleviate concentration polarization, with a long operating time. Water channel proteins have a single water molecule selective permeability, and their water molecule transmission rate exceeds that of any current nanoporous material, which can ensure a substantial increase in the water flux of the composite membrane.

[0018] Patent Document 13 (CN113543871A) discloses a method for producing a membrane containing proteoliposomes having protein water channels. The method may include providing a porous substrate, depositing a solution containing proteoliposomes on the porous substrate, and then contacting the porous substrate with an aqueous monomer solution and an organic monomer solution to form a selective layer on the porous substrate encapsulating the proteoliposomes. The method may include depositing an aqueous monomer solution, then depositing a solution containing proteoliposomes, and then depositing an organic monomer solution to form the selective layer.

[0019] The application of natural water channel proteins in reverse osmosis membranes has the following problems: first, the source is very rare. Although proteins with channel functions are widely present in nature, so far, 13 different types of channel proteins have been found in mammals alone, but proteins with channel functions only exist in specific parts of the animal body and the output is extremely small; second, it is difficult to separate and purify. Because natural water channel proteins exist in the animal body, therefore, collection, separation, purification, and enrichment are extremely difficult, and face great technical challenges; third, the material cost is high. Due to the low output and difficulty in purification and separation, the material cost of natural water channel proteins is extremely high; fourth, the stability is poor, easy to deteriorate and inactivate, extremely sensitive to environmental changes, and difficult to adapt to complex and changeable water quality environments; fifth, it is difficult to synthesize artificially. Since the mechanism of formation of natural water channel proteins is still unclear, it is extremely difficult to synthesize artificially. In summary, natural water channel protein technology is difficult to be applied to reverse osmosis membrane technology on a large scale.

[0020] The counterpart to natural aquaporins is artificial water channels, which are still in their infancy and relatively rarely used in reverse osmosis membranes. Artificial water channel technology uses simpler techniques to synthesize substances with functions similar to those of natural aquaporins. Synthetic biomimetic approaches offer the potential to construct artificial single-molecule or supramolecular structures that mimic biological functions while offering structural simplicity, ease of synthesis, relatively low cost, high stability, good tunability, and adjustable compatibility with membrane substrates.

[0021] Patent document 14 (CN112717715A) discloses a polyvinylamine membrane with nano-hydrophilic channels and its preparation and application. The preparation process includes: first, preparing polyvinylamine by free radical polymerization-hydrolysis of N-vinylformamide, reacting a small amount of amino groups in the polyvinylamine with an acyl chloride compound with a hydrophobic comb-like side chain, and after the reaction is completed, coating it on a polyacrylonitrile ultrafiltration membrane by a solution coating method, and allowing it to stand for microphase separation to prepare a pervaporation composite membrane.

[0022] Patent Document 15 (CN113600036A) discloses a method for preparing a high-flux composite nanofiber membrane with artificial water channels. This method uses single-walled carbon nanotubes as the artificial water channels and electrostatically loads them onto the surface of an electrospun nanofiber membrane substrate via electrostatic spraying, resulting in a composite nanofiber membrane with high permeability. The resulting composite nanofiber membrane exhibits high permeability and good biodegradability.

[0023] Patent document 16 (CN114728241A) discloses a composite biomimetic membrane having artificial water channels, wherein the artificial water channel protein used is formed by a supramolecular aggregate composed of a self-organized lamellar phase containing imidazole-tetrad type artificial water channels.

[0024] Patent Document 17 (CN112295411B) discloses a modified polyamide membrane and a method for preparing the same. The method comprises the following steps: (1) applying a solution containing a pyrimidine or purine compound to the surface of a nascent polyamide membrane; (2) heating the polyamide membrane coated with the pyrimidine or purine compound to complete the reaction; and (3) applying a solution of purine or a pyrimidine compound to the polyamide membrane after the reaction to complete base pairing, thereby obtaining a polyamide membrane modified with pyrimidine and purine compounds. This method is simple and easy to operate, and the resulting polyamide membrane not only has improved salt rejection and flux, but also has improved boron removal performance and chlorine resistance.

[0025] Summary of the Invention

[0026] Problems to be solved by the invention

[0027] The purpose of the present disclosure is to solve the above problems existing in the prior art and provide a method for preparing a reverse osmosis membrane and a reverse osmosis membrane prepared thereby. The method effectively solves the problems of natural water channel proteins, such as rare production, difficulty in collection, high cost, poor stability, and difficulty in large-scale application in reverse osmosis membrane preparation technology, by constructing artificial water channels.

[0028] Solutions for solving problems

[0029] In order to achieve the above objectives, the inventors of the present invention conducted intensive research and found that by pre-treating the porous polymer support base membrane with a silane coupling agent, the artificial water channel material to be introduced subsequently can be more efficiently immobilized on the surface of the base membrane. By utilizing a catalyst, the material that can form artificial water channels can form artificial water channels through self-assembly on the surface of the base membrane, and then an ultra-thin functional layer can be prepared through interfacial polymerization reaction. A reverse osmosis membrane with high flux and high desalination rate can be prepared. The prepared reverse osmosis membrane can effectively reduce the operating pressure during its operation, thereby achieving the purpose of energy saving and consumption reduction.

[0030] One aspect of the present disclosure relates to a method for preparing a reverse osmosis membrane, comprising the following steps:

[0031] (1) preparing a polymer solution as a casting solution, applying the casting solution to a non-woven fabric, and then solidifying the casting solution in a coagulation bath to form a film, thereby forming a porous polymer support layer base film;

[0032] (2) pre-treating the porous polymer support layer base membrane obtained in (1) using an aqueous solution containing a silane coupling agent;

[0033] (3) contacting the pretreated porous polymer support layer base membrane obtained in (2) with a solution containing a catalyst and a substance capable of forming artificial water channels to form artificial water channels by self-assembly;

[0034] (4) contacting the pretreated porous polymer support layer base membrane having artificial water channels obtained in (3) with an aqueous solution containing an amine monomer and an oily solution containing an acyl chloride monomer in sequence, thereby forming a polyamide functional layer;

[0035] (5) After post-treatment, a reverse osmosis membrane is obtained.

[0036] The preparation method disclosed herein, wherein the polymer is one or more of bisphenol A type polysulfone, polyethersulfone, polyarylsulfone, polydiazine ether sulfone ketone, polyaryl ether sulfone ketone, polyaryl ether nitrile ketone, polyacrylonitrile and sulfonated polyethersulfone.

[0037] The preparation method disclosed herein, wherein the silane coupling agent is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltri(2-methoxyethoxy)silane, and 3-aminopropylmethyldiethoxysilane.

[0038] The preparation method disclosed herein, wherein the substance capable of forming an artificial water channel has one of the following molecular structures: I, II, and III:

[0039] wherein R is a straight-chain or branched alkyl group having 1 to 8 carbon atoms, and X is O or S.

[0040] In the preparation method disclosed herein, the catalyst is one or more of selenium dioxide, selenium disulfide, potassium permanganate, and potassium dichromate.

[0041] The preparation method disclosed herein, wherein the amine monomer is o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, s-phenylenediamine, polyetheramine, 3-fluoroaniline, 3-chloroaniline, aminopiperazine, 2,3-diaminopyridine, 2,6-diaminopyridine, 2,5-diaminobenzenesulfonic acid, N-phenyl-p-phenylenediamine, 1,4-phenylenediamine, m-phenylenediamine, 2,4-diaminotoluene, 2,5-diaminotoluene, 2,6-diaminotoluene, 2,4-diaminoanisole, 3,4'-diaminoanisole, One or more of aminodiphenyl ether, 1,2-propylenediamine, 1,3-propylenediamine, diisobutylamine, 1,2-cyclohexanediamine, n-hexylamine, heptylamine, cycloheptylamine, 1,8-octanediamine, decylamine, dodecylamine, N-ethylethylenediamine, N-butylethylenediamine, 4,5-dimethyl-1,2-phenylenediamine, 1,5-diaminonaphthalene, N,N-diethyl-p-phenylenediamine, 2-hydroxyethylpropylamine, 1,3-diamino-2-propanol and 3,3',5,5'-tetramethylbenzidine.

[0042] The preparation method disclosed herein, wherein the acyl chloride monomer is trimesoyl chloride, pyromellitoyl chloride, terephthaloyl chloride, isophthaloyl chloride, o-chlorobenzoyl chloride, oxalyl chloride, 3-bromopropionyl chloride, undecanoyl chloride, dodecanoyl chloride, n-valeryl chloride, 3-fluorobenzoyl chloride, 4-methoxybenzoyl chloride, 4-phenylbenzoyl chloride, p-fluorobenzoyl chloride, isovaleryl chloride, succinoyl chloride, 1,7-pimeloyl chloride, ethyl malonate chloride, m-methylbenzoyl chloride, 2-methoxybenzoyl chloride, 4-methylbenzoyl chloride, One or more of oxybenzoyl chloride, 4-phenylbenzoyl chloride, 3,4-dimethoxybenzoyl chloride, cyclopentylcarbonyl chloride, cyclopropylcarbonyl chloride, heptanoyl chloride, 3-phenylpropionyl chloride, o-fluorobenzenesulfonyl chloride, p-ethylbenzoyl chloride, perfluorooctanesulfonyl chloride, 2,4,6-trichlorobenzoyl chloride, 4-bromo-2-fluorobenzoyl chloride, 3,5-difluorobenzoyl chloride, 2,5-difluorobenzoyl chloride, 3,4-dichlorobenzoyl chloride, 4-n-propylbenzoyl chloride, n-butyryl chloride and 2-nitrobenzoyl chloride.

[0043] Another aspect of the present disclosure relates to a reverse osmosis membrane, which includes a porous polymer support layer base membrane and a polyamide functional layer in sequence, wherein the porous polymer support layer base membrane includes a polymer porous support layer formed on a non-woven fabric layer, and is characterized in that there is an artificial water channel between the porous polymer support layer base membrane and the polyamide functional layer, and the artificial water channel is formed by self-assembly of substances that can form artificial water channels.

[0044] The reverse osmosis membrane of the present disclosure, wherein the substance capable of forming an artificial water channel has one of the following molecular structures I, II and III:

[0045] wherein R is a straight-chain or branched alkyl group having 1 to 8 carbon atoms, and X is O or S.

[0046] Effects of the Invention

[0047] The reverse osmosis membrane preparation method disclosed herein effectively addresses the problems of natural aquaporins, such as their low production, difficulty in collection, high cost, poor stability, and difficulty in large-scale application in reverse osmosis membrane preparation, by constructing artificial water channels. The resulting reverse osmosis membrane exhibits high flux and high salt rejection rates, and can effectively reduce operating pressure during operation, thereby achieving energy conservation and cost reduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] FIG1 shows a schematic diagram of an artificial water channel formed by the method disclosed herein, wherein the left figure is a schematic diagram of a single water channel, and the right figure is a schematic diagram of multiple water channels (also known as water cluster channels). DETAILED DESCRIPTION

[0049] Various exemplary embodiments, features, and aspects of the present disclosure are described in detail below. The word "exemplary" is used herein to mean "serving as an example, embodiment, or illustration." Any embodiment described herein as "exemplary" is not necessarily to be construed as superior or preferred over other embodiments.

[0050] In addition, numerous specific details are provided in the following detailed description to better illustrate the present disclosure. Those skilled in the art will appreciate that the present disclosure can be practiced without certain specific details. In other instances, methods, means, equipment, and steps well known to those skilled in the art are not described in detail in order to highlight the main points of the present disclosure.

[0051] Unless otherwise stated, the units used in this specification are international standard units, and the numerical values ​​and numerical ranges appearing in this disclosure should be understood to include the inevitable systematic errors in industrial production.

[0052] In this specification, the use of "may" includes both the meaning of performing a certain process and the meaning of not performing a certain process.

[0053] In this specification, references to "some specific / preferred embodiments," "other specific / preferred embodiments," "embodiments," etc., mean that the specific elements (e.g., features, structures, properties, and / or characteristics) described in connection with the embodiments are included in at least one embodiment described herein, and may or may not be present in other embodiments. In addition, it should be understood that the elements may be combined in various embodiments in any suitable manner.

[0054] In this specification, the numerical range expressed using "a numerical value A to a numerical value B" means a range including the endpoints A and B.

[0055] In this specification, when "normal temperature" or "room temperature" is used, the temperature may be 10-40°C.

[0056] The present disclosure relates to a method for preparing a reverse osmosis membrane, which comprises the following steps:.

[0057] (1) preparing a polymer solution as a casting solution, applying the casting solution to a non-woven fabric, and then solidifying the casting solution in a coagulation bath to form a film, thereby forming a porous polymer support layer base film;

[0058] (2) pre-treating the porous polymer support layer base membrane obtained in (1) using an aqueous solution containing a silane coupling agent;

[0059] (3) contacting the pretreated porous polymer support layer base membrane obtained in (2) with a solution containing a catalyst and a substance capable of forming artificial water channels to form artificial water channels by self-assembly;

[0060] (4) contacting the pretreated porous polymer support layer base membrane having artificial water channels obtained in (3) with an aqueous solution containing an amine monomer and an oily solution containing an acyl chloride monomer in sequence, thereby forming a polyamide functional layer;

[0061] (5) After post-treatment, a reverse osmosis membrane is obtained.

[0062] The technical concept of the present disclosure is to use a silane coupling agent to pretreat the porous polymer support base membrane, so that the artificial water channel material to be introduced subsequently can be more efficiently fixed on the surface of the base membrane. By using a catalyst, the material that can form artificial water channels forms artificial water channels through self-assembly on the surface of the base membrane, and then an ultra-thin functional layer is prepared through interfacial polymerization reaction. A reverse osmosis membrane with high flux and high desalination rate can be prepared. The prepared reverse osmosis membrane can effectively reduce the operating pressure during its operation, thereby achieving the purpose of energy saving and consumption reduction.

[0063] In the preparation method disclosed herein, the polymer is one or more of bisphenol A type polysulfone, polyethersulfone, polyarylsulfone, polydiazine ether sulfone ketone, polyaryl ether sulfone ketone, phthalazine polyaryl ether nitrile ketone, polyacrylonitrile and sulfonated polyethersulfone.

[0064] Preferably, the polymer concentration is 15 wt% to 35 wt% based on the total weight of the polymer solution, more preferably 15 wt% to 25 wt%. If the polymer concentration is less than 15 wt%, the resulting membrane has a larger pore size, higher pure water flux, and lower mechanical strength. If the polymer concentration is greater than 35 wt%, the resulting membrane has a smaller pore size and lower pure water flux. Both low and high polymer concentrations are detrimental to membrane performance.

[0065] Preferably, the polymer is added to a solvent and stirred until the polymer is completely dissolved to form a homogeneous solution. The solution temperature is set to 120°C to 180°C. After the polymer is completely dissolved, the polymer solution is placed in a vacuum drying oven for degassing and kept at 25°C. Preferably, the solvent used is one or more of N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), and N-methyl-2-pyrrolidone.

[0066] The polymer solution is coated on the non-woven fabric as a casting liquid, and the porous polymer support layer base membrane is prepared through three steps of immersion precipitation phase conversion in a coagulation bath, cleaning and heat treatment.

[0067] Preferably, the coagulation bath is pure water. There is no special limitation on the material of the non-woven fabric, which can be polyester (PET), polypropylene (PP), acrylic (PAN) and polyvinyl chloride (PVC), etc. The coagulation bath temperature is, for example, 13°C, the washing water temperature is, for example, 25°C, and the heat treatment temperature is, for example, 80°C.

[0068] Preferably, the average pore size of the prepared porous polymer support layer base membrane is 5 to 30 nm, more preferably 8 to 15 nm, and the pore ratio is preferably 5% to 20%, more preferably 8% to 10%.

[0069] In the preparation method disclosed herein, the silane coupling agent is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltri(2-methoxyethoxy)silane, and 3-aminopropylmethyldiethoxysilane.

[0070] Preferably, the concentration of the silane coupling agent is 0.01 wt% to 5 wt%, more preferably 0.5 wt% to 1 wt%, based on the total weight of the aqueous solution containing the silane coupling agent. There is no particular limitation on the time for pretreatment with the aqueous solution containing the silane coupling agent, which can be 5 s to 10 min, preferably 15 s to 30 s. After pretreatment, the solution is rinsed with deionized water for later use.

[0071] In the preparation method disclosed herein, the substance capable of forming an artificial water channel has one of the following molecular structures: I, II, and III:

[0072] wherein R is a straight-chain or branched alkyl group having 1 to 8 carbon atoms, and X is O or S.

[0073] Preferably, R is a linear alkyl group having 1 to 8 carbon atoms, and more preferably, R is butyl, pentyl, hexyl, heptyl, or octyl.

[0074] In the above molecular structures I, II, and III, R serves as a hydrophobic group in the molecule, and the middle part is a urea group (when X is O) or a thiourea group (when X is S) structure. The urea group or thiourea group mainly serves as a molecular skeleton, and the -NH groups on the urea groups between molecules are self-assembled through hydrogen bonding. The third part is a polyol structure with 2 or 3 hydroxyl groups, which are connected at the head by hydrogen bonding to form a single water channel or multiple water (also known as water cluster) channels.

[0075] Molecular structure I self-assembles through hydrogen bonding to form the following structure:

[0076] Molecular structure II self-assembles through hydrogen bonding to form the following structure:

[0077] Molecular structure III self-assembles through hydrogen bonding to form the following structure:

[0078] In the above molecular structures I, II, and III, the structural part formed by hydrogen bonds between the alcoholic hydroxyl groups is the water molecule channel, which is divided into a single water channel or a multiple water (also known as a water cluster) channel according to the width of the water molecule transmission path, as shown in Figure 1, where the left figure is a schematic diagram of a single water channel and the right figure is a schematic diagram of a multiple water channel (also known as a water cluster channel).

[0079] The pretreated porous polymer support layer base membrane is contacted with a solution containing a catalyst and a substance capable of forming artificial water channels, so as to form artificial water channels through self-assembly.

[0080] Preferably, the pretreated porous polymer support layer base membrane is immersed in a solution containing a catalyst and a substance that can form artificial water channels. There is no special restriction on the immersion time and the solution temperature, which can be 5s to 24h, and the solution temperature can be 10 to 40°C, preferably 15°C to 30°C.

[0081] The solution may further contain a solvent. Preferably, the solvent is one or more of water, methanol, ethanol, chloroform, and carbon tetrachloride.

[0082] In the preparation method disclosed herein, the catalyst is one or more of selenium dioxide, selenium disulfide, potassium permanganate, and potassium dichromate. The catalyst acts to oxidize the methyl and methylene groups in molecular structures I, II, and III, converting them into more active aldehyde or carboxyl groups, thereby reacting with the silane coupling agent.

[0083] Preferably, the concentration of the substance capable of forming artificial water channels is 0.01 mol / L to 0.5 mol / L, more preferably 0.05 mol / L to 0.2 mol / L.

[0084] Preferably, the solvent is evaporated by reduced pressure evaporation in a pressure range of 0.1 to 0.5 standard atmospheres, i.e., 0.01 MPa to 0.05 MPa, while maintaining the temperature at 30°C to 40°C and the evaporation time at 0.5h to 12h. Under these conditions, a substance that can form an artificial water channel is deposited, and after evaporation is completed, deionized water is used for washing and standby use.

[0085] In the preparation method disclosed herein, the amine monomer is o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, s-phenylenediamine, polyetheramine, 3-fluoroaniline, 3-chloroaniline, aminopiperazine, 2,3-diaminopyridine, 2,6-diaminopyridine, 2,5-diaminobenzenesulfonic acid, N-phenyl-p-phenylenediamine, 1,4-phenylenediamine, m-phenylenediamine, 2,4-diaminotoluene, 2,5-diaminotoluene, 2,6-diaminotoluene, 2,4-diaminoanisole, 3,4'-diaminoanisole, One or more of aminodiphenyl ether, 1,2-propylenediamine, 1,3-propylenediamine, diisobutylamine, 1,2-cyclohexanediamine, n-hexylamine, heptylamine, cycloheptylamine, 1,8-octanediamine, decylamine, dodecylamine, N-ethylethylenediamine, N-butylethylenediamine, 4,5-dimethyl-1,2-phenylenediamine, 1,5-diaminonaphthalene, N,N-diethyl-p-phenylenediamine, 2-hydroxyethylpropylamine, 1,3-diamino-2-propanol and 3,3',5,5'-tetramethylbenzidine.

[0086] In the preparation method disclosed herein, the acyl chloride monomers are trimesoyl chloride, pyromellitoyl chloride, terephthaloyl chloride, isophthaloyl chloride, o-chlorobenzoyl chloride, oxalyl chloride, 3-bromopropionyl chloride, undecanoyl chloride, dodecanoyl chloride, n-valeryl chloride, 3-fluorobenzoyl chloride, 4-methoxybenzoyl chloride, 4-phenylbenzoyl chloride, p-fluorobenzoyl chloride, isovaleryl chloride, succinoyl chloride, 1,7-pimeloyl chloride, ethyl malonate chloride, m-methylbenzoyl chloride, 2-methoxybenzoyl chloride, 4-methylbenzoyl chloride, One or more of oxybenzoyl chloride, 4-phenylbenzoyl chloride, 3,4-dimethoxybenzoyl chloride, cyclopentylcarbonyl chloride, cyclopropylcarbonyl chloride, heptanoyl chloride, 3-phenylpropionyl chloride, o-fluorobenzenesulfonyl chloride, p-ethylbenzoyl chloride, perfluorooctanesulfonyl chloride, 2,4,6-trichlorobenzoyl chloride, 4-bromo-2-fluorobenzoyl chloride, 3,5-difluorobenzoyl chloride, 2,5-difluorobenzoyl chloride, 3,4-dichlorobenzoyl chloride, 4-n-propylbenzoyl chloride, n-butyryl chloride and 2-nitrobenzoyl chloride.

[0087] Preferably, the pretreated porous polymer support layer base membrane with artificial water channels obtained as described above is immersed in an aqueous solution containing an amine monomer as an aqueous phase monomer for 5s to 60s, and after being taken out, the excess solution on the surface is blown away with nitrogen; then it is immersed in an oil phase solution containing an acyl chloride monomer as an oil phase monomer for 5s to 60s and naturally dried.

[0088] Preferably, based on the total weight of the aqueous solution, the concentration of the amine monomer is 0.5 wt % to 9.0 wt %.

[0089] In the preparation method disclosed herein, preferably, an acid absorbent (also known as a pH adjuster) is added to the aqueous solution to adjust the pH value of the solution to a range of 8 to 10. More preferably, the pH adjuster is a combination of camphorsulfonic acid / triethylamine, and the concentration of the pH adjuster is 0.5 wt%-5 wt% based on the total weight of the aqueous solution. The pH adjuster is used to absorb excess acid generated by interfacial polymerization and promote a continuous forward reaction of interfacial polymerization.

[0090] Preferably, the acyl chloride monomer is one or more of trimesoyl chloride, pyromellitoyl chloride, terephthaloyl chloride, o-chlorobenzoyl chloride, and isophthaloyl chloride, and the concentration of the acyl chloride monomer is 0.01 wt% to 5 wt% based on the total weight of the oil phase solution. Preferably, the solvent in the oil phase solution is one or more of ethylcyclohexane, n-hexane, n-heptane, ISOPAR G, and ISOPAR E.

[0091] In the preparation method of the present application, the post-treatment is preferably performed by washing with deionized water to remove the solvent and unreacted monomers, followed by drying. There is no particular restriction on the drying temperature, typically 50-100°C; and there is no particular restriction on the drying time, typically 5-60 minutes.

[0092] Preferably, a rinsing component is added to the deionized water. The rinsing component is one or more of citric acid, sodium citrate, sodium carbonate, and sodium bicarbonate. The concentration of the rinsing component is 0.5 wt% to 20 wt%, more preferably 5 wt% to 10 wt%. The solution temperature is preferably 30°C to 80°C, more preferably 50°C to 70°C. There is no particular limitation on the rinsing time. Preferably, the rinsing time is 5 seconds to 10 minutes, more preferably 30 seconds to 2 minutes.

[0093] The present disclosure also provides a reverse osmosis membrane, which includes a porous polymer support layer base membrane and a polyamide functional layer in sequence, wherein the porous polymer support layer base membrane includes a polymer porous support layer formed on a non-woven fabric layer, wherein there is an artificial water channel between the porous polymer support layer base membrane and the polyamide functional layer, and the artificial water channel is formed by self-assembly of substances that can form artificial water channels.

[0094] According to the reverse osmosis membrane of the present disclosure, the substance capable of forming an artificial water channel has one of the following molecular structures I, II and III:

[0095] wherein R is a straight-chain or branched alkyl group having 1 to 8 carbon atoms, and X is O or S.

[0096] The descriptions of the molecular structure I, the molecular structure II, and the molecular structure III are the same as those in the above-mentioned method for producing a reverse osmosis membrane.

[0097] The reverse osmosis membrane prepared by the present invention has been significantly improved in water molecule transport and salt retention. The artificial water channel layer embedded between the porous polymer support base membrane and the polyamide functional layer can transport up to 2×10 8 Water molecules / second / channel, while intercepting most of the ions. Its water molecule transmission efficiency is close to that of natural aquaporin, which effectively improves the permeability selectivity of the reverse osmosis membrane.

[0098] At present, most natural water channel proteins have disadvantages such as scarce sources, difficulty in enrichment and purification, high cost, difficulty in adapting to the harsh application environment of reverse osmosis membranes, and difficulty in artificial synthesis. The substances used in the present disclosure that can form artificial water channels have the advantages of large-scale production, low cost, controllable process, and stable structure, which overcome the application disadvantages of natural water channel proteins; compared with existing reverse osmosis membranes (referred to as RO membranes), the reverse osmosis membranes prepared in the present disclosure have higher flux due to the artificial water channels contained therein, and at least ensure that the desalination rate is not lower than that of existing reverse osmosis membranes. Therefore, the reverse osmosis membranes prepared by the present disclosure have the characteristics of high flux and high desalination rate, effectively reducing the operating pressure of the reverse osmosis membrane, and achieving the purpose of energy saving and consumption reduction.

[0099] Example

[0100] The embodiments of the present disclosure will be described in detail below with reference to the examples. However, those skilled in the art will appreciate that the following examples are intended only to illustrate the present disclosure and should not be construed as limiting the scope of the present disclosure. Where specific conditions are not specified in the examples, the experiments were performed under conventional conditions or the conditions recommended by the manufacturer. Where the manufacturer of the reagents or instruments is not specified, all are commercially available conventional products.

[0101] Comparative Example

[0102] Step 1: Preparation of porous polymer support layer membrane

[0103] The polymer is dissolved in a solvent and allowed to stand for degassing. The solution is then applied to a non-woven fabric and placed in a coagulation bath to achieve phase separation between the solvent and polymer, resulting in a porous base membrane. The solvent is N,N-dimethylformamide (DMF); the polymer is bisphenol A polysulfone at 18 wt%. The coagulation bath is pure water at 12°C, and the non-woven fabric is made of polyester (PET).

[0104] Step 2: Preparation of reverse osmosis membrane

[0105] The base film prepared in step 1 was first immersed in an aqueous solution containing aqueous monomers for 10 seconds, removed and the excess solution blown off with nitrogen. It was then immersed in an oily solution containing oily monomers for 20 seconds. Finally, it was removed, rinsed with deionized water, and dried in an oven at 80°C. The aqueous monomers were m-phenylenediamine (4 wt%), and the acid absorbents were 2 wt% camphorsulfonic acid / 1 wt% triethylamine. The oily monomers were trimesoyl chloride (0.15 wt%), and the solvent was ethylcyclohexane.

[0106] Step 3: Diaphragm post-processing

[0107] The membrane sheet after step 2 was immersed in a water tank containing a rinsing solution to remove excess monomers and solvents. The rinsing component was citric acid with a concentration of 8 wt %, a temperature of 70° C., and a rinsing time of 2 min.

[0108] Example 1

[0109] Step 1: Preparation of porous polymer support layer membrane

[0110] The polymer is dissolved in a solvent and allowed to stand for degassing. The solution is then applied to a nonwoven fabric and passed through a coagulation bath to phase separate the solvent and polymer, resulting in a porous base membrane. The solvent is N,N-dimethylformamide (DMF); the polymer is bisphenol A polysulfone at 18 wt%. The coagulation bath is pure water at 12°C, and the nonwoven fabric is made of polyester (PET).

[0111] Step 2: Pretreatment of porous polymer support layer with silane coupling agent

[0112] The porous polymer support layer base membrane prepared in step 1 was pretreated using an aqueous solution containing a silane coupling agent. The silane coupling agent used was 3-aminopropyltriethoxysilane with a concentration of 0.5 wt %. The pretreatment was performed for 20 seconds. After the pretreatment was completed, the base membrane was rinsed with deionized water for use.

[0113] Step 3: Self-assembly of artificial water channels on the porous polymer support layer

[0114] The porous polymer support layer membrane from step 2 was immersed in a solution containing N,N'-1,2-dihydroxymethyl octyl urea artificial water channel molecules of molecular structure type I for 30 minutes at a temperature of 30°C. The solution contained 2.5g / L selenium dioxide and 0.1mol / L N,N'-1,2-dihydroxymethyl octyl urea, and the solvent was water. The solvent was evaporated by reduced pressure evaporation at a pressure of 0.02MPa while maintaining the temperature at 35°C for 5 hours to deposit the artificial water channel molecules under these conditions. After evaporation, the membrane was rinsed with deionized water for later use.

[0115] Step 4: Preparation of a reverse osmosis membrane with an ultrathin functional layer by interfacial polymerization on the base membrane assembled with artificial water channels

[0116] The base film, having completed step 3, was first immersed in an aqueous solution containing the aqueous monomer for 10 seconds, removed and purged with nitrogen to remove excess solution. It was then immersed in an oily solution containing the oily monomer for 20 seconds. Finally, it was removed, rinsed with deionized water, and dried in an oven at 80°C. The aqueous monomer consisted of 4% m-phenylenediamine, and the acid absorbent consisted of 2% camphorsulfonic acid and 1% triethylamine. The oily monomer consisted of 0.15% trimesoyl chloride, and the solvent was ethylcyclohexane.

[0117] Step 5: Diaphragm post-processing

[0118] The membrane sheet after step 4 was immersed in a water tank containing a rinsing solution to remove excess monomers and solvents. The rinsing component was citric acid with a concentration of 8 wt %, a temperature of 70° C., and a rinsing time of 2 minutes.

[0119] Example 2

[0120] Step 1 and step 2 are the same as step 1 and step 2 in Example 1.

[0121] Step 3: Self-assembly of artificial water channels on the porous polymer support layer

[0122] The porous polymer support layer membrane from step 2 was immersed in a solution containing N,N'-1,3-dihydroxymethylpropane octyl urea artificial water channel molecules of molecular structure II for 30 minutes at a temperature of 30°C. The solution contained 2.5g / L selenium dioxide and 0.1mol / L N,N'-1,3-dihydroxymethylpropane octyl urea, and the solvent was water. The solvent was evaporated by reduced pressure evaporation at a pressure of 0.02MPa while maintaining the temperature at 35°C for 5 hours to deposit the artificial water channel molecules under these conditions. After evaporation, the membrane was rinsed with deionized water for later use.

[0123] Step 4 and step 5 are the same as step 4 and step 5 in Example 1.

[0124] Example 3

[0125] Step 1 and step 2 are the same as step 1 and step 2 in Example 1.

[0126] Step 3: Self-assembly of artificial water channels on the porous polymer support layer

[0127] The porous polymer support layer base membrane completed in step 2 is immersed in a solution containing N, N'-2, 3-bis(hydroxymethyl)ethanol octyl urea artificial water channel molecules of molecular structure III, the immersion time is 30 minutes, the solution temperature is 30 ° C, the solution contains 2.5g / L selenium dioxide, 0.15mol / LN, N'-2, 3-bis(hydroxymethyl)ethanol octyl urea, the solvent is an ethanol / water mixture with a volume ratio of 80 / 2, the solvent is evaporated by reduced pressure evaporation, the pressure is 0.02MPa, while maintaining the temperature at 35 ° C, the evaporation time is 5h, the artificial water channel molecules are deposited under this condition, and after evaporation, it is washed with deionized water for use.

[0128] Step 4 and step 5 are the same as step 4 and step 5 in Example 1.

[0129] Example 4

[0130] Step 1 and step 2 are the same as step 1 and step 2 in Example 1.

[0131] Step 3: Self-assembly of artificial water channels on the porous polymer support layer

[0132] The porous polymer support layer base membrane completed in step 2 is immersed in a solution containing artificial water channel molecules of molecular structure type II N,N'-1,3-propylenedihydroxymethyl octyl urea, the immersion time is 30 minutes, the solution temperature is 30°C, the solution contains 2.5g / L selenium dioxide, 0.15mol / LN,N'-1,3-propylenedihydroxymethyl octyl urea, and the solvent is an ethanol / water mixture with a volume ratio of 80 / 20. The solvent is evaporated by reduced pressure evaporation with a pressure of 0.02MPa while maintaining the temperature at 35°C for 5 hours. Under this condition, artificial water channel molecules are deposited. After evaporation, deionized water is used to wash the solution for use.

[0133] Step 4 and step 5 are the same as step 4 and step 5 in Example 1.

[0134] Example 5

[0135] Step 1 and step 2 are the same as step 1 and step 2 in Example 1.

[0136] Step 3: Self-assembly of artificial water channels on the porous polymer support layer

[0137] The porous polymer support layer base membrane completed in step 2 was immersed in a solution containing N,N'-1,3-propylenedihydroxymethylbutyl urea artificial water channel molecules of molecular structure II, the immersion time was 30 minutes, the solution temperature was 30°C, the solution components included 2.5g / L selenium dioxide, 0.15mol / LN,N'-1,3-propylenedihydroxymethylbutyl urea, and the solvent was an ethanol / water mixture with a volume ratio of 80 / 20. The solvent was evaporated by reduced pressure evaporation with a pressure of 0.02MPa while maintaining the temperature at 35°C for 5 hours. Under this condition, artificial water channel molecules were deposited. After evaporation, the solution was washed with deionized water for use.

[0138] Step 4 and step 5 are the same as step 4 and step 5 in Example 1.

[0139] Example 6

[0140] Step 1 and step 2 are the same as step 1 and step 2 in Example 1.

[0141] Step 3: Self-assembly of artificial aquaporins on the porous polymer support layer

[0142] The porous polymer support layer base membrane completed in step 2 is immersed in a solution containing N,N'-1,3-propylenedihydroxymethylpentyl urea artificial water channel molecules of molecular structure II, the immersion time is 30 minutes, the solution temperature is 30°C, the solution contains 2.5g / L selenium dioxide, 0.15mol / LN,N'-1,3-propylenedihydroxymethylpentyl urea, and the solvent is an ethanol / water mixture with a volume ratio of 80 / 20. The solvent is evaporated by reduced pressure evaporation with a pressure of 0.02MPa while maintaining the temperature at 35°C for 5 hours. Under this condition, artificial water channel molecules are deposited. After evaporation, deionized water is used to wash the solution for use.

[0143] Step 4 and step 5 are the same as step 4 and step 5 in Example 1.

[0144] Example 7

[0145] Step 1 and step 2 are the same as step 1 and step 2 in Example 1.

[0146] Step 3: Self-assembly of artificial water channels on the porous polymer support layer

[0147] The porous polymer support layer base membrane completed in step 2 is immersed in a solution containing N,N'-1,3-propylenedihydroxymethylhexylurea artificial water channel molecules of molecular structure II, the immersion time is 30 minutes, the solution temperature is 30°C, the solution contains 2.5g / L selenium dioxide, 0.15mol / LN,N'-1,3-propylenedihydroxymethylhexylurea, and the solvent is an ethanol / water mixture with a volume ratio of 80 / 20. The solvent is evaporated by reduced pressure evaporation with a pressure of 0.02MPa while maintaining the temperature at 35°C for 5 hours. Under this condition, artificial water channel molecules are deposited. After evaporation, deionized water is used to wash the solution for use.

[0148] Step 4 and step 5 are the same as step 4 and step 5 in Example 1.

[0149] Example 8

[0150] Step 1 and step 2 are the same as step 1 and step 2 in Example 1.

[0151] Step 3: Self-assembly of artificial water channels on the porous polymer support layer

[0152] The porous polymer support layer base membrane completed in step 2 is immersed in a solution containing N,N'-2,3-bis(hydroxymethyl)ethanol octyl urea artificial water channel molecules of molecular structure III, the immersion time is 30 minutes, the solution temperature is 30°C, the solution contains 2.5g / L selenium disulfide, 0.2mol / LN,N'-2,3-bis(hydroxymethyl)ethanol octyl urea, and the solvent is an ethanol / water mixture with a volume ratio of 80 / 20. The solvent is evaporated by reduced pressure evaporation with a pressure of 0.02MPa while maintaining the temperature at 35°C for 5 hours. Under this condition, artificial water channel molecules are deposited. After evaporation, the solution is washed with deionized water for standby use.

[0153] Step 4 and step 5 are the same as step 4 and step 5 in Example 1.

[0154] Diaphragm performance test

[0155] The reverse osmosis membranes prepared in the comparative example and Examples 1 to 8 were tested for initial performance under 150 psi pressure and a 2000 ppm NaCl solution at a pH of 6-7. The membrane flux and salt rejection were measured at various solution temperatures. The run time was 30 minutes at a temperature of 25±3°C. The salt concentrations of both the produced and raw water were measured. The salt rejection of the membranes was calculated as: (1 - (produced water salt concentration / influent salt concentration)) × 100. The results are shown in Table 1 below.

[0156] Table 1

[0157] From the results shown in Table 1, it can be seen that compared with the control example, the performance of the membranes obtained in all embodiments is significantly improved, the flux is increased by 40% to 65%, and the rejection rate is slightly increased by 0.05% to 0.18%. Therefore, under the same pressure conditions, the permeation efficiency is higher, achieving the expected energy saving and consumption reduction purpose of the present disclosure.

[0158] It should be noted that, although the technical solutions of the present disclosure are described with specific examples, those skilled in the art will appreciate that the present disclosure should not be limited thereto.

[0159] While various embodiments of the present disclosure have been described above, the foregoing description is intended to be illustrative, non-exhaustive, and not limited to the disclosed embodiments. Many modifications and variations will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments. The terminology used herein is selected to best explain the principles of the embodiments, their practical applications, or technological improvements in the marketplace, or to enable others skilled in the art to understand the embodiments disclosed herein.

[0160] Industrial applicability

[0161] The reverse osmosis membrane preparation method disclosed herein effectively addresses the problems of natural aquaporins, such as their low production, difficulty in collection, high cost, poor stability, and difficulty in large-scale application in reverse osmosis membrane preparation, by constructing artificial water channels. The resulting reverse osmosis membrane exhibits high flux and high salt rejection rates, and can effectively reduce operating pressure during operation, thereby achieving energy conservation and cost reduction.

Claims

1. A method for preparing a reverse osmosis membrane, characterized in that: The following steps are involved: (1) preparing a polymer solution as a casting solution, applying the casting solution to a non-woven fabric, and then solidifying the casting solution in a coagulation bath to form a film, thereby forming a porous polymer support layer base film; (2) pretreating the porous polymer support layer base membrane obtained in (1) using an aqueous solution containing a silane coupling agent; (3) contacting the pretreated porous polymer support layer base membrane obtained in (2) with a solution containing a catalyst and a substance capable of forming an artificial water channel to form an artificial water channel by self-assembly; (4) contacting the pretreated porous polymer support layer base membrane having artificial water channels obtained in (3) with an aqueous solution containing an amine monomer and an oil solution containing an acyl chloride monomer in sequence, thereby forming a polyamide functional layer; (5) After post-treatment, a reverse osmosis membrane is obtained.

2. The preparation method according to claim 1, wherein the polymer is one or more of bisphenol A type polysulfone, polyethersulfone, polyarylsulfone, polynaphthylidene ether sulfone ketone, polyaryl ether sulfone ketone, naphthalene biphenyl polyaryl ether nitrile ketone, polyacrylonitrile and sulfonated polyethersulfone.

3. The preparation method according to claim 1 or 2, wherein the silane coupling agent is one or more of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-glycidyloxypropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyltri(2-methoxyethoxy)silane, and 3-aminopropylmethyldiethoxysilane.

4. The preparation method according to claim 1 or 2, wherein the substance capable of forming an artificial water channel has one of the following molecular structures I, II and III: Wherein R is a straight or branched alkyl group having 1 to 8 carbon atoms, and X is O or S.

5. The preparation method according to claim 1 or 2, wherein the catalyst is one or more of selenium dioxide, selenium disulfide, potassium permanganate, and potassium dichromate.

6. The preparation method according to claim 1 or 2, wherein the amine monomer is o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, s-phenylenediamine, polyetheramine, 3-fluoroaniline, 3-chloroaniline, aminopiperazine, 2,3-diaminopyridine, 2,6-diaminopyridine, 2,5-diaminobenzenesulfonic acid, N-phenyl-p-phenylenediamine, 1,4-phenylenediamine, m-phenylenediamine, 2,4-diaminotoluene, 2,5-diaminotoluene, 2,6-diaminotoluene, 2,4-diaminoanisole, 3, One or more of 4'-diaminodiphenyl ether, 1,2-propylenediamine, 1,3-propylenediamine, diisobutylamine, 1,2-cyclohexanediamine, n-hexylamine, heptylamine, cycloheptylamine, 1,8-octanediamine, decylamine, dodecylamine, N-ethylethylenediamine, N-butylethylenediamine, 4,5-dimethyl-1,2-phenylenediamine, 1,5-diaminonaphthalene, N,N-diethyl-p-phenylenediamine, 2-hydroxyethylpropylamine, 1,3-diamino-2-propanol and 3,3',5,5'-tetramethylbenzidine.

7. The preparation method according to claim 1 or 2, wherein the acyl chloride monomer is trimesoyl chloride, pyromellitoyl chloride, terephthaloyl chloride, isophthaloyl chloride, o-chlorobenzoyl chloride, oxalyl chloride, 3-bromopropionyl chloride, undecanoyl chloride, dodecanoyl chloride, n-valeryl chloride, 3-fluorobenzoyl chloride, 4-methoxybenzoyl chloride, 4-phenylbenzoyl chloride, p-fluorobenzoyl chloride, isovaleryl chloride, succinoyl chloride, 1,7-heptanedioyl chloride, ethyl malonate chloride, m-methylbenzoyl chloride, 2-methoxybenzoyl chloride , 4-methoxybenzoyl chloride, 4-phenylbenzoyl chloride, 3,4-dimethoxybenzoyl chloride, cyclopentylcarbonyl chloride, cyclopropylcarbonyl chloride, heptanoyl chloride, 3-phenylpropionyl chloride, o-fluorobenzenesulfonyl chloride, p-ethylbenzoyl chloride, perfluorooctanesulfonyl chloride, 2,4,6-trichlorobenzoyl chloride, 4-bromo-2-fluorobenzoyl chloride, 3,5-difluorobenzoyl chloride, 2,5-difluorobenzoyl chloride, 3,4-dichlorobenzoyl chloride, 4-n-propylbenzoyl chloride, n-butyryl chloride and 2-nitrobenzoyl chloride.

8. A reverse osmosis membrane, comprising a porous polymer support layer base membrane and a polyamide functional layer in sequence, wherein the porous polymer support layer base membrane comprises a polymer porous support layer formed on a non-woven fabric layer, characterized in that: There are artificial water channels between the porous polymer support layer base membrane and the polyamide functional layer, and the artificial water channels are formed by self-assembly of substances that can form artificial water channels.

9. The reverse osmosis membrane according to claim 8, wherein the substance capable of forming an artificial water channel has one of the following molecular structures I, II and III: Wherein R is a straight or branched alkyl group having 1 to 8 carbon atoms, and X is O or S.

Citation Information

Patent Citations

  • Composite reverse osmosis membrane and preparation method thereof

    CN105080352A

  • High-performance reverse-osmosis composite membrane and preparation method thereof

    CN109351191A

  • Preparation method of anti-pollution composite reverse osmosis membrane and anti-pollution composite reverse osmosis membrane prepared thereby

    CN114432900A

  • Composite biomimetic membrane with artificial water channel

    CN114728241A

  • Preparation method of composite membrane and composite membrane

    CN115121128A

Cited By

  • Nano-bubble induced amphiphilic compound self-assembled polyamide composite membrane as well as preparation method and application of nano-bubble induced amphiphilic compound self-assembled polyamide composite membrane

    CN120984124A