Film and laminate

The film with a resin base material and oxygen-LAICP treatment addresses the adhesion issues in laminated films by optimizing the carbon and oxygen element ratios, resulting in enhanced mechanical properties and improved performance in applications like antireflection films.

WO2025013853A1PCT designated stage expired Publication Date: 2025-01-16NITTO DENKO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/024744
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-11
Filing Date
2024-07-09
Publication Date
2025-01-16

AI Technical Summary

Technical Problem

Existing laminated films, particularly hard coat films, face issues with insufficient adhesion between the base film and the antireflection layer, which affects the overall performance and durability of the composite material.

Method used

A film with a resin base material that satisfies specific carbon and oxygen element ratios measured by X-ray photoelectron spectroscopy, combined with an oxygen-LAICP treatment, enhances the adhesion between the resin base material and the inorganic layer, ensuring better bonding and improved mechanical properties.

Benefits of technology

The enhanced adhesion significantly improves the mechanical strength and durability of the film, leading to improved performance in applications such as antireflection films and laminates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024024744_16012025_PF_FP_ABST
    Figure JP2024024744_16012025_PF_FP_ABST
Patent Text Reader

Abstract

A film (1) is constituted by a resin substrate (2). In the film (1), an elemental carbon ratio C90, an elemental oxygen ratio O90, an elemental carbon ratio C15, and an elemental oxygen ratio O15 which are measured in a prescribed first test satisfy a formula (1) below, or an elemental carbon ratio C15 and an elemental oxygen ratio O15 which are measured in a prescribed second test satisfy a formula (2) below. (1): O15 / C15>O90 / C90, (2): O15 / C15>0.3
Need to check novelty before this filing date? Find Prior Art

Description

Films and Laminates

[0001] The present invention relates to a film and a laminate, and more particularly to a film and a laminate including the film.

[0002] In order to achieve weight reduction and high performance in electronics products, composite materials that combine organic and inorganic materials have been developed. For example, a laminated film that includes an organic substrate film and an inorganic layer on the substrate film is known as a composite material.

[0003] As such a laminate film, for example, a hard coat film having a film substrate and a hard coat layer in this order, an inorganic oxide primer layer, and an antireflection film having an antireflection layer in this order have been proposed (see, for example, Patent Document 1).

[0004] In Patent Document 1, the hard coat layer is subjected to a plasma treatment before a primer layer is formed on the hard coat layer. Such a treatment can remove dirt and moisture from the surface of the hard coat film (hard coat layer) and improve the adhesion between the hard coat film and the antireflection layer.

[0005] Japanese Patent Application Laid-Open No. 2022-65437

[0006] However, the substrate film (hard coat film) of Patent Document 1 has a drawback in that it has insufficient adhesion, and therefore the substrate film (hard coat film) is required to have even better adhesion.

[0007] The present invention provides a film having excellent adhesion and a laminate including the film.

[0008] The present invention [1] is a film made of a resin substrate, and the carbon element ratio C measured by the following first test 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 is a film that satisfies the following formula (1): 15 / C 15 >O 90 / C90 (1) First test: (1) Using X-ray photoelectron spectroscopy, the photoelectron take-off angle was adjusted to 90° with respect to one surface in the thickness direction of the resin substrate, and the carbon element ratio C 90 and oxygen element ratio O 90 (2) Using X-ray photoelectron spectroscopy, the photoelectron take-off angle is adjusted to 15° with respect to one surface in the thickness direction of the resin substrate, and the carbon element ratio C 15 and oxygen element ratio O 15 Measure.

[0009] The present invention [2] is characterized in that the resin substrate is made of a substrate layer, and in the first test, the carbon element ratio C 90 and the oxygen element ratio O 90 is measured by adjusting the photoelectron take-off angle to 90° with respect to one surface in the thickness direction of the base material layer, and the carbon element ratio C 15 and the oxygen element ratio O 15 The film includes the film according to the above [1], which is measured by adjusting the photoelectron take-off angle to 15° with respect to one surface in the thickness direction of the base layer.

[0010] The present invention [3] is a method for manufacturing a cured resin substrate, the resin substrate including a base layer and a cured resin layer in this order toward one side in the thickness direction, and the carbon element ratio C 90 and the oxygen element ratio O 90 is measured by adjusting the photoelectron take-off angle to 90° with respect to one surface in the thickness direction of the cured resin layer, and the carbon element ratio C 15 and the oxygen element ratio O 15 The film includes the film according to the above [1], which is measured by adjusting the photoelectron take-off angle to 15° with respect to one surface in the thickness direction of the cured resin layer.

[0011] The present invention [4] includes the film according to the above [3], wherein the cured resin layer contains an acrylic urethane resin.

[0012] The present invention [5] is a film made of a resin substrate, and the carbon element ratio C measured by the following second test 15 and oxygen element ratio O 15 is a film that satisfies the following formula (2): 15 / C15 >0.3 (2) Second test: Using X-ray photoelectron spectroscopy, the photoelectron take-off angle was adjusted to 15° with respect to one surface in the thickness direction of the resin substrate, and the carbon element ratio C 15 and oxygen element ratio O 15 Measure.

[0013] The present invention [6] is characterized in that the resin substrate is made of a substrate layer, and in the second test, the carbon element ratio C 15 and the oxygen element ratio O 15 The film includes the film according to the above [5], which is measured by adjusting the photoelectron take-off angle to 15° with respect to one surface in the thickness direction of the base layer.

[0014] The present invention [7] is a method for manufacturing a cured resin substrate, the resin substrate including a base layer and a cured resin layer in this order toward one side in the thickness direction, and the carbon element ratio C 15 and the oxygen element ratio O 15 The film includes the film according to the above [5], which is measured by adjusting the photoelectron take-off angle to 15° with respect to one surface in the thickness direction of the cured resin layer.

[0015] The present invention [8] includes the film according to the above [7], wherein the cured resin layer contains an acrylic urethane resin.

[0016] The present invention [9] includes a laminate comprising the film according to any one of the above [1] to [8] and an inorganic layer in that order toward one side in the thickness direction.

[0017] The present invention

[10] includes the laminate according to the above [9], wherein the inorganic layer is an anti-reflection layer, and the anti-reflection layer includes a plurality of layers having refractive indices different from one another along the thickness direction.

[0018] The present invention

[11] includes the laminate according to the above [9], wherein the inorganic layer is a conductive layer.

[0019] The film of the present invention has a carbon element ratio C measured by a predetermined first test. 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15satisfies the following formula (1), or the carbon element ratio C measured by a predetermined second test 15 and oxygen element ratio O 15 However, the following formula (2) is satisfied. Therefore, the adhesion can be improved. 15 / C 15 >O 90 / C 90 (1) O 15 / C 15 >0.3 (2)

[0020] The laminate of the present invention includes the film of the present invention and an inorganic layer in this order toward one side in the thickness direction, and therefore has excellent adhesion between the film and the inorganic layer.

[0021] Fig. 1 shows a first embodiment of a film of the present invention. Fig. 2 shows a perspective view illustrating the positional relationship between a low inductance antenna and a resin substrate. Fig. 3 is a cross-sectional view illustrating the positional relationship between a low inductance antenna and a resin substrate. Fig. 4 shows a second embodiment of a film of the present invention. Fig. 5 shows an embodiment of a laminate of the present invention. Fig. 6 shows an embodiment of a laminate in which the inorganic layer is an antireflection layer.

[0022] The film of the present invention comprises a resin substrate.

[0023] In the following description, a first embodiment in which the resin substrate is composed of a substrate layer, and a second embodiment in which the resin substrate has a substrate layer and a cured resin layer in this order toward one side in the thickness direction will be described in detail.

[0024] The film of the present invention has a carbon element ratio C measured by the following first test. 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 satisfies the following formula (1), or the carbon element ratio C measured by the following second test 15 and oxygen element ratio O 15 satisfies the following formula (2): 15 / C 15 >O 90 / C 90 (1) O 15 / C 15>0.3 (2)

[0025] The first test is (1) using X-ray photoelectron spectroscopy, adjusting the photoelectron take-off angle to 90° with respect to one surface in the thickness direction of the resin substrate, and measuring the carbon element ratio C 90 and oxygen element ratio O 90 Then, (2) using X-ray photoelectron spectroscopy, the photoelectron take-off angle was adjusted to 15° with respect to one surface in the thickness direction of the resin substrate, and the carbon element ratio C 15 and oxygen element ratio O 15 This is a test that measures:

[0026] The second test is performed by X-ray photoelectron spectroscopy, adjusting the photoelectron take-off angle to 15° with respect to one surface in the thickness direction of the resin substrate, and measuring the carbon element ratio C 15 and oxygen element ratio O 15 This is a test that measures:

[0027] Although details will be described later, in the first embodiment, in the first test, the carbon element ratio C 90 and oxygen element ratio O 90 is measured by adjusting the photoelectron take-off angle to 90° with respect to one surface in the thickness direction of the substrate layer, and the carbon element ratio C 15 and oxygen element ratio O 15 is measured with the photoelectron take-off angle adjusted to 15° with respect to one surface in the thickness direction of the substrate layer (such a first test is referred to as a 1A test).

[0028] In addition, although details will be described later, in the first embodiment, in the second test, the carbon element ratio C 15 and oxygen element ratio O 15 is measured with the photoelectron take-off angle adjusted to 15° with respect to one surface in the thickness direction of the substrate layer (such a second test is referred to as a second A test).

[0029] In addition, although details will be described later, in the second embodiment, in the first test, the carbon element ratio C 90 and oxygen element ratio O 90 is measured by adjusting the photoelectron take-off angle to 90° with respect to one surface in the thickness direction of the cured resin layer, and the carbon element ratio C 15 and oxygen element ratio O 15is measured by adjusting the photoelectron take-off angle to 15° with respect to one surface in the thickness direction of the cured resin layer (such a first test is referred to as a 1B test).

[0030] In addition, although details will be described later, in the second embodiment, in the second test, the carbon element ratio C 15 and oxygen element ratio O 15 is measured by adjusting the photoelectron take-off angle to 15° with respect to one surface in the thickness direction of the cured resin layer (such a second test is referred to as Test 2B).

[0031] 1. First Embodiment A first embodiment of the film of the present invention will be described with reference to FIG.

[0032] In Figure 1, the up-down direction of the paper surface is the up-down direction (thickness direction). The upper side of the paper surface is the upper side (one side in the thickness direction). The lower side of the paper surface is the lower side (the other side in the thickness direction). The left-right direction and the depth direction of the paper surface are surface directions perpendicular to the up-down direction. Specifically, they conform to the directional arrows in each figure.

[0033] The film 1 has a film shape (including a sheet shape) with a predetermined thickness. The film 1 extends in a plane direction perpendicular to the thickness direction. The film 1 has a flat upper surface and a flat lower surface. The film 1 is preferably flexible.

[0034] The film 1 preferably has transparency. Specifically, the total light transmittance (JIS K 7375-2008) of the film 1 is, for example, 80% or more, or preferably 85% or more.

[0035] The thickness of the film 1 is, for example, 10 μm or more, preferably 20 μm or more, more preferably 35 μm or more, and from the viewpoint of handleability in the roll-to-roll system described below, for example, 200 μm or less, preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 60 μm or less. A carrier film may be attached to the back surface of the film 1 to ensure the transportability and handleability of the film 1 in the roll-to-roll process.

[0036] The thickness of the film 1 can be measured using a dial gauge (manufactured by PEACOCK, "DG-205").

[0037] The film 1 is made of a resin substrate 2 .

[0038] <Resin Substrate> The resin substrate 2 is composed of a substrate layer 3 .

[0039] The base layer 3 has a film shape and is preferably flexible.

[0040] The substrate layer 3 may be, for example, a polymer film.

[0041] Examples of polymer film materials include polyester resins, (meth)acrylic resins, olefin resins, polycarbonate resins, polyethersulfone resins, polyarylate resins, melamine resins, polyamide resins, polyimide resins, cellulose resins, and polystyrene resins. Examples of polyester resins include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of (meth)acrylic resins include polymethyl methacrylate. Examples of olefin resins include polyethylene, polypropylene, and cycloolefin polymers. Examples of cellulose resins include triacetyl cellulose.

[0042] The polymer film is preferably made of a cellulose resin, and more preferably made of triacetyl cellulose.

[0043] The thickness of the base layer 3 is, from the viewpoint of ensuring mechanical strength, for example, 10 μm or more, preferably 20 μm or more, more preferably 30 μm or more, and from the viewpoint of handleability in the roll-to-roll method described later, for example, 200 μm or less, preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less.

[0044] The thickness of the base material layer 3 can be measured using a dial gauge (manufactured by PEACOCK, "DG-205").

[0045] The base layer 3 preferably has transparency. Specifically, the total light transmittance (JIS K 7375-2008) of the base layer 3 is, for example, 80% or more, or preferably 85% or more.

[0046] <Carbon element ratio C 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 > Film 1 has a carbon element ratio C measured by the following 1A test 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 satisfies the following formula (1A), or the carbon element ratio C measured by the following 2A test 15 and oxygen element ratio O 15 satisfies the following formula (2A): 15 / C 15 >O 90 / C 90 (1A) O 15 / C 15 >0.3 (2A)

[0047] The first A test is a test in which (1) the carbon element ratio C was measured by X-ray photoelectron spectroscopy with the photoelectron take-off angle adjusted to 90° with respect to one surface in the thickness direction of the base layer 3. 90 and oxygen element ratio O 90 Then, (2) using X-ray photoelectron spectroscopy, the photoelectron take-off angle was adjusted to 15° with respect to one surface in the thickness direction of the base layer 3, and the carbon element ratio C 15 and oxygen element ratio O 15 This is a test that measures:

[0048] The second A test is performed by X-ray photoelectron spectroscopy, adjusting the photoelectron take-off angle to 15° with respect to one surface in the thickness direction of the base layer 3, and measuring the carbon element ratio C 15 and oxygen element ratio O 15 This is a test that measures:

[0049] Carbon element ratio C measured by the above-mentioned 1A test 90 , oxygen element ratio O 90 , carbon element ratio C15 and oxygen element ratio O 15 satisfies the above formula (1A), or the carbon element ratio C measured by the above 2A test 15 and oxygen element ratio O 15 However, if the above formula (2A) is satisfied, the adhesion can be improved.

[0050] On the other hand, the carbon element ratio C measured by the above-mentioned 1A test 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 does not satisfy the above formula (1A) and the carbon element ratio C measured by the above 2A test 15 and oxygen element ratio O 15 However, if the above formula (2A) is not satisfied, the adhesion will decrease.

[0051] Preferably, the carbon element ratio C measured by the above test 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 satisfies the above formula (1A) and the carbon element ratio C measured by the above 2A test 15 and oxygen element ratio O 15 satisfies the above formula (2A). This makes it possible to further improve the adhesion.

[0052] To satisfy the above formula (1A) and / or formula (2A), the surface of the resin substrate 2 is subjected to an oxygen-LAICP treatment (described below). In the oxygen-LAICP treatment, for example, the conveying speed of the resin substrate 2 (described below), the type of LA 21 (described below), the oxygen concentration in the vacuum chamber during the oxygen-LAICP treatment (described below), the pressure in the vacuum chamber during the oxygen-LAICP treatment (described below), the frequency and magnitude of the high-frequency power applied to the LA 21 during the oxygen-LAICP treatment (described below), and the plasma current density during the oxygen-LAICP treatment (described below) are adjusted.

[0053] Carbon element ratio C 90 is, for example, 50 atomic % or more, and, for example, 80 atomic % or less.

[0054] Oxygen element ratio O 90 is, for example, 10 atomic % or more, and, for example, 50 atomic % or less.

[0055] Carbon element ratio C 15 is, for example, 50 atomic % or more, and, for example, 80 atomic % or less.

[0056] Oxygen element ratio O 15 is, for example, 10 atomic % or more, and, for example, 50 atomic % or less.

[0057] <Film Treatment Method> The film treatment method includes a first step of preparing a resin substrate 2 and a second step of performing plasma treatment on one surface in the thickness direction of the resin substrate 2. This method is preferably performed using a roll-to-roll system. In such a case, the conveying speed is, for example, 0.1 m / min or more and, for example, 20.0 m / min or less.

[0058] [First Step] In the first step, a resin substrate 2 is prepared. Specifically, a substrate layer 3 is prepared.

[0059] [Second Step] In the second step, one surface in the thickness direction of the resin film 2 (substrate layer 3) is subjected to plasma treatment.

[0060] Specifically, the plasma treatment may be a treatment using inductively coupled plasma of an oxygen-containing gas (oxygen-LAICP treatment) generated by applying high frequency power to a low inductance antenna.

[0061] The low inductance antenna means an antenna that has a low inductance of 7.5 μH or less and that can generate inductively coupled plasma by applying high frequency power.

[0062] 2 and 3, the low inductance antennas 21 (LA21) are supported by fixtures 22 and arranged in a state where they are covered with cover blocks 23 (omitted in FIG. 3) (a case where the number of LA21 is four is illustrated as an example.) The multiple LA21 are arranged in a line so as to be aligned in the running direction of the resin film 2 and in a direction perpendicular to the running direction (the width direction of the resin film 2).

[0063] The LA 21 is formed of a conductor. Examples of the conductor include copper and silver, and preferably copper. The LA 21 may be covered with an insulator. Examples of the insulator include glass and quartz.

[0064] The LA 21 is electrically connected to a high frequency power source (RF power source) via an impedance matching box.

[0065] The LA21 has an open loop shape. The open loop shape of the LA21 can reduce the inductance of the LA21. Therefore, the open loop shape of the LA21 can suppress an increase in voltage due to an increase in power applied to the LA21. This can suppress abnormal discharge during plasma treatment. Suppressing abnormal discharge can suppress damage to the resin substrate 2 being plasma treated.

[0066] Specifically, the LA 21 has a U-shape with two free ends. For each LA 21, the two free ends are fixed to the fixture 22 so as to be aligned in the width direction of the resin substrate 2. More specifically, the LA 21 is fixed to the fixture 22 via a feedthrough 24, as shown in FIG. 3 .

[0067] The LA 21 also has extensions 21a on the side opposite to the two free ends. The extensions 21a extend in the width direction of the resin film 2. Each extension 21a may extend in the running direction of the resin film 2 (two LAs 21 may be arranged in this manner).

[0068] The LA 21 extends from the fixture 22 toward the resin film 2. The LA 21 extends in a direction perpendicular to the fixture 22. The extension length d of the LA 21 from the fixture 22 1 is, for example, 30 mm or more and, for example, 150 mm or less.

[0069] The maximum length d of LA21 in the surface direction of the resin film 2 2 is, for example, 50 mm or more and, for example, 150 mm or less.

[0070] The distance d between the LA 21 and the resin substrate 2 3is, for example, 50 mm or more and, for example, 200 mm or less.

[0071] Preferably, the extension length d 1 and separation distance d 3 is the same as.

[0072] Extension length d 1 Separation distance d 3 The ratio (d 3 / d 1 ) is, for example, 0.5 or more and, for example, 3.5 or less.

[0073] In the running direction of the resin film 2, the center distance d between adjacent LA 21 4 The number of LAs 21 (rows) spaced apart in the running direction of the resin film 2 may be 1, 2, or 3, or may be 4 or more if necessary, depending on the running speed of the resin film 2 (i.e., the plasma treatment time).

[0074] In the width direction of the resin base material 2, the center-to-center distance d between adjacent LA 21 5 is, for example, 200 mm or less, or, for example, 500 mm or less. 5 By adjusting the above, the uniformity of the plasma density in the width direction of the resin substrate 2 can be controlled.

[0075] Preferably, the center distance d 4 and center distance d 5 is the same as.

[0076] The centers of the extensions 21a of the four LAs 21 preferably form a square with the vertices as vertices. Such a set of LAs 21 can generate high-density plasma with high in-plane uniformity. For example, the high-frequency antenna for plasma generation described in JP 2013-258153 A can be used as the LAs 21.

[0077] The LA 21 may have a coil shape instead of an open loop shape.

[0078] The cover block 23 includes a block body 23A and multiple partition plates 23B. The block body 23A has multiple storage spaces 23a. Each storage space 23a stores one LA 21. The partition plates 23B are arranged to close the storage spaces 23a. The storage spaces 23a are sealed spaces. In the cover block 23, the block body 23A is made of, for example, aluminum. Examples of aluminum include aluminum A5052. The partition plates 23B are made of an insulating material. Examples of insulating materials include quartz and glass. The separation distance d' (shown in FIG. 3) between the traveling resin substrate 2 and the cover block 23 is, for example, 50 mm or more and, for example, 200 mm or less. Such a cover block 23 helps to avoid damage and contamination of LA21 due to plasma treatment without excessively reducing the plasma conversion efficiency due to the power applied to LA21, and also helps to suppress damage to the resin substrate 2 being plasma treated.

[0079] In the oxygen-LAICP treatment, the LA 21 is placed in a vacuum chamber, and the resin substrate 2 is transported thereinto, and oxygen is supplied into the vacuum chamber.

[0080] From the viewpoint of improving adhesion, the oxygen concentration in the vacuum chamber is, for example, 30 vol% or more, more preferably 50 vol% or more, and even more preferably 80 vol% or more. Also, from the viewpoint of improving adhesion, the oxygen concentration in the vacuum chamber is, for example, 100 vol% or less, preferably 95 vol% or less, and more preferably 90 vol% or less.

[0081] In addition, an inert gas or an active gas other than oxygen may be introduced into the vacuum chamber. Examples of the inert gas include rare gases (argon, krypton, and xenon). Examples of the active gas include nitrogen and water vapor.

[0082] The pressure inside the vacuum chamber during the oxygen-LAICP treatment is, for example, 0.1 Pa or more, preferably 0.2 Pa or more, more preferably 0.3 Pa or more, and for example, 7.0 Pa or less, preferably 5.0 Pa or less, more preferably 3.0 Pa or less, and even more preferably 1.0 Pa or less. The pressure can be adjusted by the amount of oxygen supplied to the vacuum chamber.

[0083] Furthermore, the frequency of the high frequency power applied to LA21 during the oxygen-LAICP treatment is, for example, 1 MHz or more, preferably 3 MHz or more, more preferably 5 MHz or more, and even more preferably 10 MHz or more, and is, for example, 100 MHz or less, preferably 80 MHz or less, and more preferably 60 MHz or less.

[0084] The high frequency power is, for example, 1.0 kW or more, preferably 1.5 kW or more, more preferably 1.8 kW or more, and for example, 10 kW or less, preferably 8 kW or less, more preferably 6 kW or less.

[0085] In the oxygen-LAICP treatment, the plasma current density at the intermediate position between the LA 21 and the resin substrate 2 is, for example, 1.0 mA / cm 3 or more, preferably 2.0 mA / cm 3 More preferably, 3.0 mA / cm 3 More preferably, 4.0 mA / cm 3 or more, for example, 10 mA / cm 3 Preferably, 8 mA / cm or less 3 More preferably, 5 mA / cm or less 3 The following is the result.

[0086] The plasma current density can be adjusted by the amount of oxygen introduced, the frequency of the high frequency power, and the high frequency power.

[0087] In this way, one surface in the thickness direction of the resin film 2 (substrate layer 3) is subjected to plasma treatment.

[0088] 2. Second Embodiment A second embodiment of the film of the present invention will be described with reference to FIG.

[0089] In the second embodiment, the same components and steps as those in the first embodiment are denoted by the same reference numerals, and detailed descriptions thereof will be omitted. Furthermore, the second embodiment can achieve the same effects as those in the first embodiment, unless otherwise specified.

[0090] The film 1 is made of a resin substrate 2 .

[0091] <Resin substrate> The resin substrate 2 includes a substrate layer 3 and a cured resin layer 4 in this order toward one side in the thickness direction. Specifically, the resin substrate 2 includes the substrate layer 3 and the cured resin layer 4 disposed directly on the upper surface (one surface in the thickness direction) of the substrate layer 3. The resin substrate 2 preferably includes the substrate layer 3 and the cured resin layer 4.

[0092] [Substrate Layer] The substrate layer 3 is a substrate for ensuring the mechanical strength of the film 1 .

[0093] The base layer 3 is disposed on the entire lower surface of the cured resin layer 4 so as to be in contact with the lower surface of the cured resin layer 4. The base layer 3 is the bottom layer of the film 1.

[0094] [Cured Resin Layer] The cured resin layer 4 has a film shape. The cured resin layer 4 is disposed on the entire upper surface of the base layer 3 so as to be in contact with the upper surface of the base layer 3. The cured resin layer 4 is the uppermost layer of the film 1.

[0095] Examples of the cured resin layer 4 include a hard coat layer, an easy-adhesion layer, and an anti-blocking (AB) layer. A hard coat layer is preferably used as the cured resin layer 4. The hard coat layer is an abrasion protection layer that makes the film 1 less susceptible to scratches.

[0096] The hard coat layer is a cured product of a hard coat composition containing a curable resin.

[0097] Examples of the curable resin include polyester resin, acrylic urethane resin, acrylic resin (excluding acrylic urethane resin), urethane resin (excluding acrylic urethane resin), amide resin, silicone resin, epoxy resin, and melamine resin. As the curable resin, acrylic urethane resin is preferably used. That is, the hard coat layer preferably contains acrylic urethane resin. When the hard coat layer contains acrylic urethane resin, the carbon element ratio C 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 However, it can be adjusted so as to fully satisfy the formula (1B) and the formula (2B) described later.

[0098] The curable resins may be used alone or in combination of two or more.

[0099] Examples of the curable resin include an ultraviolet-curable resin and a thermosetting resin. The curable resin is preferably an ultraviolet-curable resin. If the curable resin is an ultraviolet-curable resin, the curable resin can be cured without heating, thereby improving the production efficiency of the film 1.

[0100] In the hard coat composition, the content of the curable resin is, for example, 80 mass % or more, preferably 90 mass % or more, and for example, 99 mass % or less, preferably 95 mass % or less.

[0101] The hard coat composition optionally contains particles, an initiator (thermal polymerization initiator, photopolymerization initiator) and a leveling agent.

[0102] Examples of the particles include inorganic particles and organic particles. Examples of the inorganic particles include inorganic oxide particles. Examples of the inorganic oxide particle material include silica, alumina, titania, zirconia, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide. Examples of the organic particle material include polymethyl methacrylate, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate.

[0103] The content ratio of inorganic particles is preferably low. The lower the content ratio of inorganic particles, the more light scattering caused by inorganic particles can be suppressed and the production cost can be reduced. In terms of visibility (described later), the content ratio of inorganic particles in the hard coat composition is, for example, 20 mass% or less, preferably 10 mass% or less, more preferably 5 mass% or less, even more preferably 1 mass% or less, particularly preferably 0.5 mass% or less, most preferably 0.2 mass% or less, even 0.1 mass% or less, or even 0.0 mass%.

[0104] The hard coat composition can be diluted, if necessary, with a solvent, such as butyl acetate, ethyl acetate, toluene, and cyclopentanone.

[0105] When the hard coat composition is diluted with a solvent, the solids concentration is, for example, 10% by mass or more, preferably 30% by mass or more, and for example, 70% by mass or less, preferably 60% by mass or less.

[0106] As will be described in detail later, the hard coat layer is formed by applying a hard coat composition to one surface in the thickness direction of the substrate layer 3, and drying and curing it as necessary.

[0107] The hard coat layer preferably has transparency. Specifically, the total light transmittance (JIS K 7375-2008) of the hard coat layer is, for example, 80% or more, or preferably 85% or more.

[0108] The thickness of the cured resin layer 4 is, for example, 0.5 μm or more, preferably 2 μm or more, more preferably 3 μm or more, and for example, 30 μm or less, preferably 25 μm or less, more preferably 20 μm or less.

[0109] <Carbon element ratio C 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 > Film 1 has a carbon element ratio C measured by the following 1B test 90 , oxygen element ratio O 90, carbon element ratio C 15 and oxygen element ratio O 15 satisfies the following formula (1B), or the carbon element ratio C measured by the following 2B test 15 and oxygen element ratio O 15 satisfies the following formula (2B): 15 / C 15 >O 90 / C 90 (1B) O 15 / C 15 >0.3 (2B)

[0110] The first B test is (1) using X-ray photoelectron spectroscopy, the photoelectron take-off angle is adjusted to 90° with respect to one surface in the thickness direction of the cured resin layer 4, and the carbon element ratio C 90 and oxygen element ratio O 90 Then, (2) using X-ray photoelectron spectroscopy, the photoelectron take-off angle was adjusted to 15° with respect to one surface in the thickness direction of the cured resin layer 4, and the carbon element ratio C 15 and oxygen element ratio O 15 This is a test that measures:

[0111] The second B test is performed by X-ray photoelectron spectroscopy, adjusting the photoelectron take-off angle to 15° with respect to one surface in the thickness direction of the cured resin layer 4, and measuring the carbon element ratio C 15 and oxygen element ratio O 15 This is a test that measures:

[0112] Carbon element ratio C measured by the above-mentioned 1B test 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 satisfies the above formula (1B), or the carbon element ratio C measured by the above 2B test 15 and oxygen element ratio O 15 However, if the above formula (2B) is satisfied, the adhesion can be improved.

[0113] On the other hand, the carbon element ratio C measured by the above-mentioned 1B test 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O15 does not satisfy the above formula (1B) and the carbon element ratio C measured by the above 2B test 15 and oxygen element ratio O 15 However, if the above formula (2B) is not satisfied, the adhesion will decrease.

[0114] Preferably, the carbon element ratio C measured by the above-mentioned Test 1B 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 satisfies the above formula (1B) and the carbon element ratio C measured by the above 2B test 15 and oxygen element ratio O 15 satisfies the above formula (2B). This makes it possible to further improve the adhesion.

[0115] To satisfy the above formula (1B) and / or formula (2B), the surface of the resin substrate 2 is subjected to an oxygen-LAICP treatment. In the oxygen-LAICP treatment, for example, the conveyance speed of the resin substrate 2, the type of LA 21, the oxygen concentration in the vacuum chamber during the oxygen-LAICP treatment, the pressure in the vacuum chamber during the oxygen-LAICP treatment, the frequency and magnitude of the high-frequency power applied to the LA 21 during the oxygen-LAICP treatment, and the plasma current density during the oxygen-LAICP treatment are adjusted.

[0116] <Film Manufacturing Method> The film manufacturing method includes a first step of preparing a resin substrate 2 and a second step of performing a plasma treatment on one surface in the thickness direction of the resin substrate 2. This method is preferably performed using a roll-to-roll system. In such a case, the conveying speed is, for example, 0.1 m / min or more and, for example, 20.0 m / min or less. The following description will be given in detail of the case where the cured resin layer 4 is a hard coat layer.

[0117] [First Step] In the first step, the resin substrate 2 is prepared.

[0118] Specifically, first, the base layer 3 is prepared.

[0119] Next, a hard coat layer (cured resin layer 4) is disposed on one surface in the thickness direction of the substrate layer 3. To dispose the hard coat layer on one surface in the thickness direction of the substrate layer 3, a hard coat composition is applied to one surface in the thickness direction of the substrate layer 3, and then dried and cured as necessary to form the hard coat layer.

[0120] As for the drying conditions, the drying temperature is, for example, 50° C. or more and, for example, 120° C. or less, and the drying time is, for example, 10 seconds or more and, for example, 10 minutes or less.

[0121] When the hard coat composition contains an ultraviolet-curable resin, the curable resin is cured by ultraviolet irradiation. Examples of the light source for ultraviolet irradiation include a high-pressure mercury lamp and an LED light. The cumulative irradiation amount of ultraviolet light is, for example, 100 mJ / cm. 2 or more, for example, 500 mJ / cm 2 The following is the result.

[0122] When the hard coat composition contains a thermosetting resin, the thermosetting resin is cured by heating. The heating temperature is, for example, 100° C. or higher and, for example, 150° C. or lower. The heating time is, for example, 10 seconds or higher and, for example, 10 minutes or shorter.

[0123] In this way, the hard coat layer (cured resin layer 4) is disposed on one surface of the substrate layer 3 in the thickness direction, and the resin substrate 2 is prepared.

[0124] [Second Step] In the second step, one surface in the thickness direction of the resin substrate 2 (cured resin layer 4) is subjected to plasma treatment in the same procedure as in the first embodiment, thereby producing the film 1.

[0125] <Laminate> As shown in Fig. 5 , the laminate 10 includes a film 1 (specifically, the film 1 of the first embodiment or the film 1 of the second embodiment) and an inorganic layer 11, arranged in this order toward one side in the thickness direction (note that Fig. 5 shows a case where the film 1 is the film 1 of the second embodiment). Specifically, the laminate 10 includes the film 1 and the inorganic layer 11 disposed directly on the upper surface (one side in the thickness direction) of the film 1. The laminate 10 preferably includes the film 1 and the inorganic layer 11.

[0126] [Film] The film 1 is disposed over the entire lower surface of the inorganic layer 11 so as to be in contact with the lower surface of the inorganic layer 11. The film 1 is the bottom layer in the laminate 10.

[0127] [Inorganic Layer] The inorganic layer 11 has a film shape. The inorganic layer 11 is disposed on the entire upper surface of the film 1 so as to be in contact with the upper surface of the film 1. The inorganic layer 11 is the uppermost layer in the laminate 10.

[0128] Examples of the inorganic layer 11 include an anti-reflection layer and a conductive layer. Hereinafter, the cases where the inorganic layer 11 is an anti-reflection layer and a conductive layer will be described in detail.

[0129] (When the Inorganic Layer is an Antireflection Layer) With reference to FIG. 6, the case where the inorganic layer 11 is an antireflection layer will be described in detail.

[0130] When the inorganic layer 11 is an anti-reflection layer, the laminate 10 is an anti-reflection film.

[0131] The antireflection layer includes multiple layers with different refractive indices along the thickness direction. Specifically, the antireflection layer alternates between high-refractive-index layers with relatively high refractive indexes and low-refractive-index layers with relatively low refractive indexes in the thickness direction. In the antireflection layer, the net reflected light intensity is attenuated by interference between reflected light at multiple interfaces in the multiple thin layers (high-refractive-index layers, low-refractive-index layers) included therein. Furthermore, the antireflection layer can exhibit interference that attenuates the reflected light intensity by adjusting the optical film thickness (product of refractive index and thickness) of each thin layer. Such an antireflection layer includes high-refractive-index layers 12 and low-refractive-index layers 13 alternately arranged in order toward one side in the thickness direction.

[0132] The antireflection layers (specifically, the high-refractive-index layer 12 and the low-refractive-index layer 13) preferably contain one selected from the group consisting of a metal, an alloy, a metal oxide, a metal nitride, and a metal fluoride, and more preferably contain one selected from the group consisting of a metal, a metal oxide, and a metal nitride, which enables the antireflection layers to suppress the reflection intensity of external light.

[0133] Examples of metals include silicon, nickel, chromium, aluminum, tin, gold, silver, platinum, zinc, titanium, tungsten, zirconium, niobium, and palladium. Examples of alloys include alloys of the above metals. Examples of metal oxides include metal oxides of the above metals. Examples of metal nitrides include metal nitrides of the above metals. Examples of metal fluorides include metal nitrides of metal fluorides of the above metals.

[0134] In particular, the material used for the anti-reflection layer is selected depending on the desired refractive index.

[0135] Specifically, the high refractive index material constituting the high refractive index layer 12 is, for example, niobium oxide (Nb 2 O 5 ), titanium oxide, zirconium oxide, indium tin oxide (ITO), and antimony-doped tin oxide (ATO). As the high refractive index material, indium tin oxide (ITO) is preferably used.

[0136] The low refractive index material constituting the low refractive index layer 13 is, for example, silicon dioxide (SiO 2 ), and magnesium fluoride. As the low refractive index material, silicon dioxide (SiO 2 ) are listed.

[0137] In the antireflection layer, the high refractive index layer 12 has a thickness of, for example, 1 nm or more, or preferably 3 nm or more, and for example, 15 nm or less, or preferably 10 nm or less.

[0138] The thickness of the low refractive index layer 13 is thicker than the thickness of the high refractive index layer 12, and is, for example, greater than 15 nm and is, for example, 50 nm or less, preferably 30 nm or less.

[0139] The ratio of the thickness of the low refractive index layer 13 to the thickness of the high refractive index layer 12 (thickness of the low refractive index layer 13 / thickness of the high refractive index layer 12) is, for example, more than 1, preferably 2 or more, more preferably 3 or more, and for example, 10 or less, preferably 5 or less.

[0140] The thickness of the antireflection layer is, for example, 20 nm or more, and, for example, 300 nm or less, preferably 250 nm or less, and more preferably 200 nm or less.

[0141] When the inorganic layer 11 is an anti-reflection layer, the laminate 10 can be produced by disposing the anti-reflection layer on one surface of the film 1 in the thickness direction by a known sputtering method.

[0142] In the antireflection layer, the number of high refractive index layers and low refractive index layers is not particularly limited.

[0143] (When the inorganic layer is a conductive layer) When the inorganic layer 11 is a conductive layer, the laminate 10 is a transparent conductive film.

[0144] Examples of materials for the conductive layer include metals and metal oxides. Examples of metals include copper, silver, gold, nickel, chromium, and alloys thereof. Examples of metal oxides include indium-containing conductive oxides and antimony-containing conductive oxides. Examples of indium-containing conductive oxides include indium tin composite oxide (ITO), indium zinc composite oxide (IZO), indium gallium composite oxide (IGO), and indium gallium zinc composite oxide (IGZO). Examples of antimony-containing conductive oxides include antimony tin composite oxide (ATO).

[0145] The conductive layer has a thickness of, for example, 1 nm or more, preferably 5 nm or more, and for example, 100 nm or less.

[0146] When the inorganic layer 11 is a conductive layer, the laminate 10 can be produced by disposing the conductive layer on one surface of the film 1 in the thickness direction by a known sputtering method.

[0147] <Effects> In the first embodiment, the film 1 has a carbon element ratio C 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15satisfies the above formula (1A), or the carbon element ratio C measured by the above 2A test 15 and oxygen element ratio O 15 satisfies the above formula (2A), and therefore, the adhesion can be improved.

[0148] In the second embodiment, the film 1 has a carbon element ratio C 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 satisfies the above formula (1B), or the carbon element ratio C measured by the above 2B test 15 and oxygen element ratio O 15 satisfies the above formula (2B), and therefore, the adhesion can be improved.

[0149] Specifically, in X-ray photoelectron spectroscopy, the smaller the photoelectron take-off angle, the shallower the detection depth relative to the surface of the film 1 (specifically, the base layer 3 or the cured resin layer 4), whereas the larger the photoelectron take-off angle, the deeper the detection depth relative to the surface of the film 1 (the base layer 3 or the cured resin layer 4).

[0150] That is, the carbon element ratio C 15 is the carbon element ratio based on a relatively shallow detection depth, and the carbon element ratio C 90 is the carbon element ratio based on a relatively deep detection depth.

[0151] In other words, the carbon element ratio C 15 is the carbon element ratio derived from the vicinity of the surface of the film 1 (substrate layer 3 or cured resin layer 4), and the carbon element ratio C 90 is the carbon element ratio derived from the inside of the film 1 (substrate layer 3 or cured resin layer 4).

[0152] Similarly, the oxygen element ratio O 15 is the oxygen element ratio derived from the vicinity of the surface of the film 1 (substrate layer 3 or cured resin layer 4), and the oxygen element ratio O 90 is the oxygen element ratio derived from the inside of the film 1 (substrate layer 3 or cured resin layer 4).

[0153] Satisfying the above formula (1A) or (1B) means that the oxygen element ratio is higher near the surface of the film 1 (substrate layer 3 or cured resin layer 4) than inside the film 1 (substrate layer 3 or cured resin layer 4).

[0154] This suggests that oxygen modification has been applied to the surface of the film 1 (substrate layer 3 or cured resin layer 4), which results in a chemical bond between the film 1 (substrate layer 3 or cured resin layer 4) and the inorganic layer 11 via oxygen, improving adhesion.

[0155] The laminate 10 includes the film 1 and the inorganic layer 11 in this order toward one side in the thickness direction, so that the film 1 and the inorganic layer 11 have excellent adhesion to each other.

[0156] The present invention will be described in more detail below with reference to examples and comparative examples. It should be noted that the present invention is in no way limited to these examples and comparative examples. The specific numerical values ​​of the blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values ​​(numeric values ​​defined as "equal to or less than") or lower limit values ​​(numeric values ​​defined as "equal to or greater than" or "exceeding") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the "Description of the Invention" above.

[0157] Example 1 <Film Production> [First Step] In the first step, a resin substrate was prepared. Specifically, a long TAC film (triacetyl cellulose film, length 100 m, width 340 mm, thickness 40 μm) was first prepared as a substrate layer.

[0158] Next, a hard coat layer (cured resin layer) was disposed on one surface in the thickness direction of the substrate layer. Specifically, first, 100 parts by mass (solid content equivalent) of a butyl acetate solution of ultraviolet-curable acrylic urethane resin (product name "Luxidia 17-806", solid content concentration 80% by mass, manufactured by DIC Corporation), 5 parts by mass of a photopolymerization initiator (product name "Omnirad 907", manufactured by IGM Resins), 0.03 parts by mass of a leveling agent (product name "GRANDIC PC4100", manufactured by DIC Corporation), and butyl acetate as a solvent were mixed to adjust the solid content concentration to 75% by mass. Next, cyclopentanone was added as a solvent to prepare a hard coat composition (solid content concentration 50% by mass).

[0159] Next, a hard coat composition was applied to one surface of the substrate layer in the thickness direction to form a coating film. Next, this coating film was dried by heating and then cured by ultraviolet irradiation. As a result, a hard coat layer (thickness: 5 μm) was disposed on one surface of the substrate layer in the thickness direction.

[0160] The heating temperature was 100° C. and the heating time was 60 seconds. For ultraviolet irradiation, a high-pressure mercury lamp was used as a light source, and ultraviolet rays with a wavelength of 365 nm were irradiated onto the coating film, with an integrated irradiation light amount of 300 mJ / cm 2 It was decided.

[0161] In this way, a resin substrate was prepared.

[0162] [Second Step] In the second step, a plasma treatment was performed on one surface in the thickness direction of the resin substrate (hard coat layer).

[0163] Specifically, the resin substrate was transported into a vacuum chamber by a roll-to-roll method under vacuum at a transport speed of 1.0 m / min, and the resin substrate (hard coat layer) was subjected to plasma treatment.

[0164] The plasma treatment was an oxygen-LAICP treatment, and the low inductance antenna shown in Figures 2 and 3 was used.

[0165] In the low inductance antenna, the extension length d 1 is 88 mm, and the maximum length d 2 is 100 mm, and the separation distance d 3is 112 mm, and the center distance d 4 is 290 mm, and the center distance d 5 is 280 mm, and the separation distance d' is 100 mm. Each low inductance antenna is electrically connected to a high frequency power source (RF power source, frequency 13.56 MHz) via an impedance matching box.

[0166] The ultimate vacuum of the vacuum chamber is 1.0 x 10 -4 After evacuating the apparatus until the pressure reached 0.5 Pa, oxygen gas (oxygen concentration 100% by volume) was introduced into the vacuum chamber, and the pressure in the vacuum chamber was set to 0.5 Pa. A high-frequency power of 5.0 kW was applied to the four low-inductance antennas by a high-frequency power supply, thereby forming an inductively coupled plasma of an oxygen-containing gas around the antennas (the resin substrate (hard coat layer) was treated with this plasma). The plasma current density at the midpoint between the low-inductance antennas and the resin substrate was 4.2 mA / cm. 3 It was decided.

[0167] This produced a film.

[0168] <Production of Laminate> An anti-reflection layer was formed on one surface of the film in the thickness direction by sputtering.

[0169] Specifically, after evacuating the vacuum chamber, 1.0 × 10 -4 The pressure was reduced to 100 Pa, and argon gas was introduced as a sputtering gas. An ITO target (SnO ratio 10 mass%, length 600 mm × width 150 mm × thickness 5 mm, single cathode system) was used as a target to deposit a high refractive index layer (ITO film, thickness 5 nm) (input power 1.0 kW, film deposition chamber pressure: 0.3 Pa, DC discharge). Next, a pure Si target (length 600 mm × width 50 mm × thickness 5 mm, dual cathode system) was used as a target to deposit a low refractive index layer (SiO 2 A film (thickness: 20 nm) was placed on the substrate (power input: 3.0 kW, film formation pressure: 0.3 Pa, O 2 / Ar=0.3, MFAC power supply 60kHz).

[0170] In this way, a laminate was produced.

[0171] Comparative Example 1 <Production of Film> A resin substrate was prepared according to the same procedure as in the first step of Example 1.

[0172] In the second step, one surface in the thickness direction of the resin substrate (hard coat layer) was subjected to a bombardment treatment with argon ions.

[0173] Specifically, the resin substrate was transported into a vacuum chamber by a roll-to-roll method under vacuum at a transport speed of 1.0 m / min.

[0174] The vacuum chamber is equipped with a pair of planar electrodes for generating plasma: a cathode electrode and an anode electrode (both rectangular electrodes made of SUS304). The pair of planar electrodes are arranged parallel to the resin substrate passing through the vacuum chamber, with a gap of 50 mm between them. The anode electrode is positioned 35 mm away from the resin substrate and is grounded outside the vacuum chamber. The cathode electrode is positioned facing the hard coat layer surface of the resin substrate and is electrically connected to a high-frequency power source (RF power source, 13.56 MHz) via an impedance matcher. The length of each electrode in the film running direction is 110 mm, and the length in the width direction is 430 mm.

[0175] The ultimate vacuum of the vacuum chamber is 1.0 x 10 -4 After evacuating the apparatus until the pressure reached 0.5 Pa, argon gas was introduced as an inert gas into the vacuum chamber, and the pressure inside the vacuum chamber was adjusted to 0.5 Pa. Capacitively coupled plasma (CCP) was generated by applying 550 W of power between the planar electrodes using a high-frequency power supply. In this plasma environment, the surface of the resin substrate (hard coat layer) was bombarded with argon ions.

[0176] <Production of Laminate> A laminate was prepared according to the same procedure as in Example 1.

[0177] <Evaluation> [Carbon element ratio C 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15Measurement of 1B Test and 2B Test were carried out on the films of each Example and Comparative Example.

[0178] The film was cut out from the center portion in the width direction (340 mm width) into a piece of about 1 cm square and used as a sample.

[0179] Specifically, in the first B test, (1) X-ray photoelectron spectroscopy was used to measure the carbon element ratio C 90 and oxygen element ratio O 90 Next, (2) X-ray photoelectron spectroscopy was used to measure the carbon element ratio C 15 and oxygen element ratio O 15 was measured.

[0180] In the second B test, the carbon element ratio C was measured by X-ray photoelectron spectroscopy with the photoelectron take-off angle adjusted to 15° with respect to one surface in the thickness direction of the hard coat layer. 15 and oxygen element ratio O 15 was measured.

[0181] The conditions for X-ray photoelectron spectroscopy are as follows: {Conditions} Apparatus: "KRATOS ULTRA2" (Shimadzu Corporation) X-ray source: Monochrome Al Kα X-ray setting: 700×300 μm [5 mA, 75 W] Charge neutralization: Yes

[0182] The results are shown in Table 1. 15 / C 15 " and "O 90 / C 90 " indicates.

[0183] [Adhesion] The laminates of each Example and Comparative Example were cut into 50 mm x 50 mm pieces to prepare samples. Next, the treated surface of the sample was scored at 1 mm intervals to form a grid of 100 squares, and then placed in a weathering tester under the following conditions. {Conditions} SUV irradiation conditions Temperature and humidity conditions: 85°C, 45% Rh Light source used: metal halide lamp Irradiation conditions: 150 mW / cm 2 (290-450 nm) Input time: 32.5 hours

[0184] Next, 2 mL of isopropyl alcohol was continuously dropped onto the surface of the anti-reflection layer to prevent it from drying out, and a polyester wiper (Anticon Gold, manufactured by Sanplatec) fixed to a 20 mm square SUS jig was slid over the grid (load: 1.5 kg, 1000 strokes). A grid where the anti-reflection layer had peeled off over an area of ​​¼ or more of the grid's area was counted as "peeling." The adhesion was evaluated based on the following criteria. The results are shown in Table 1. {Criteria} ◯: 5 or fewer grids were "peeled off." ×: More than 5 grids were "peeled off."

[0185]

[0186] The above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and should not be interpreted as limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.

[0187] The film and laminate of the present invention are suitable for use, for example, in the production of anti-reflection films.

[0188] REFERENCE SIGNS LIST 1 film 2 resin substrate 3 substrate layer 4 cured resin layer 10 laminate 11 inorganic layer

Claims

1. A film made of a resin substrate, having a carbon element ratio C measured by the following first test: 90 , oxygen element ratio O 90 , carbon element ratio C 15 and oxygen element ratio O 15 A film that satisfies the following formula (1): 15 / C 15 >O 90 / C 90 (1) First test: (1) Using X-ray photoelectron spectroscopy, the photoelectron take-off angle was adjusted to 90° with respect to one surface in the thickness direction of the resin substrate, and the carbon element ratio C 90 and oxygen element ratio O 90 (2) Using X-ray photoelectron spectroscopy, the photoelectron take-off angle is adjusted to 15° with respect to one surface in the thickness direction of the resin substrate, and the carbon element ratio C 15 and oxygen element ratio O 15 Measure.

2. The resin substrate is made of a substrate layer, and in the first test, the carbon element ratio C 90 and the oxygen element ratio O 90 is measured by adjusting the photoelectron take-off angle to 90° with respect to one surface in the thickness direction of the base layer, 15 and the oxygen element ratio O 15 The film according to claim 1 , wherein the photoelectron take-off angle is adjusted to 15° with respect to one surface in the thickness direction of the base layer.

3. The resin substrate has a substrate layer and a cured resin layer in this order toward one side in the thickness direction, and in the first test, 90 and the oxygen element ratio O 90 is measured by adjusting the photoelectron take-off angle to 90° with respect to one surface in the thickness direction of the cured resin layer, 15 and the oxygen element ratio O 15 The film according to claim 1 , wherein the photoelectron take-off angle is adjusted to 15° with respect to one surface in the thickness direction of the cured resin layer.

4. The film of claim 3, wherein the cured resin layer comprises an acrylic urethane resin.

5. A film made of a resin substrate, having a carbon element ratio C measured by the following second test 15 and oxygen element ratio O 15 A film that satisfies the following formula (2). 15 / C 15 >0.3 (2) Second test: Using X-ray photoelectron spectroscopy, the photoelectron take-off angle was adjusted to 15° with respect to one surface in the thickness direction of the resin substrate, and the carbon element ratio C 15 and oxygen element ratio O 15 Measure.

6. The resin substrate is made of a substrate layer, and in the second test, the carbon element ratio C 15 and the oxygen element ratio O 15 The film according to claim 5 , wherein the photoelectron take-off angle is adjusted to 15° with respect to one surface in the thickness direction of the base layer.

7. The resin substrate has a substrate layer and a cured resin layer in this order toward one side in the thickness direction, and in the second test, 15 and the oxygen element ratio O 15 The film according to claim 5 , wherein the photoelectron take-off angle is adjusted to 15° with respect to one surface in the thickness direction of the cured resin layer.

8. The film of claim 7, wherein the cured resin layer comprises an acrylic urethane resin.

9. A laminate comprising the film according to any one of claims 1 to 8 and an inorganic layer in that order toward one side in the thickness direction.

10. The laminate according to claim 9, wherein the inorganic layer is an anti-reflection layer, and the anti-reflection layer comprises a plurality of layers having mutually different refractive indices along the thickness direction.

11. The laminate according to claim 9, wherein the inorganic layer is a conductive layer.

Citation Information

Patent Citations

  • Hydrophilization of hydrophobic polymers

    JP1997512294A

  • Manufacture of metal element-containing thin film laminate

    JP2000185362A

  • Method for surface treatment of polymeric materials using hydrogen ion assisted reaction

    JP2003509558A

  • Improved method for modifying polymer surfaces

    JP2005511876A

  • Hard coat film

    JP2011043606A