Method for producing pelletizing water and method for producing iron ore pellets
By determining the polymeric binder blending percentage in pelletizing water based on target viscosity, the method addresses the inefficiencies of adjusting components in existing technologies, ensuring stable production of iron ore pellets with consistent strength.
Patent Information
- Application Number
- CA3180993
- Authority / Receiving Office
- CA · CA
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-07
- Filing Date
- 2020-06-15
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2040-06-15
AI Technical Summary
Existing methods for producing iron ore pellets require time-consuming and labor-intensive adjustments of pelletizing water components to achieve the desired strength for green pellets, which varies with iron ore type and transport conditions, leading to inefficiencies.
A method for producing pelletizing water that determines the polymeric binder blending percentage based on target viscosity, using a formula that correlates viscosity with the drop number of green pellets, ensuring consistent strength regardless of iron ore type or transport conditions.
Enables easy determination of the polymeric binder percentage, stabilizing the production of iron ore pellets by controlling strength and preventing pulverization during transport.
Abstract
Description
7 2 DESCRIPTION METHOD FOR PRODUCING PELLETIZING WATER AND METHOD FOR PRODUCING IRON ORE PELLETS [TECHNICAL FIELD]
[0001] The present invention relates to a method for producing pelletizing water and a method for producing iron ore pellets. [BACKGROUND ART]
[0002] Iron ore pellets are a product which is obtained from iron ore powder in an order of several tens of µm, as a raw material, and is made with characteristics suitable for a blast furnace (for example, size, strength, reducibility, and the like) in order to improve quality. The iron ore pellets are produced through a pelletizing step and a firing step.
[0003] In the pelletizing step, an iron ore raw material in which moisture and grain size have been adjusted is charged into a pelletizer (for example, a pan pelletizer or the like) and rolled to make ball-shaped green pellets each having a diameter of about 10 mm. Furthermore, in the firing step, using a traveling grate furnace and a kiln furnace, the green pellets are dried and pre-fired and are then sintered at a temperature of about 1,200 °C.
[0004] In the green pellets produced in the pelletizing step, particles of the iron ore are cross-linked by water, whereby adhesion acts between the particles to keep the strength. That is to say, a bond between the particles is exhibited by surface tension of the water between the particles, and the adhesion between the particles is ensured by a value obtained from the surface tension and the number of contacts between the particles. Thus, the particles adhere to each other with a certain strength, but this adhesion is weaker than that of the iron ore pellets after the firing.
[0005] The green pellets having been thus produced with the pelletizer in the pelletizing step are transported to the traveling grate furnace for the firing step. For the transporting, for example, a plurality of conveyor belts are used, and the green pellets are transported while being transferred between these conveyor belts. At a transfer between the conveyor belts, a start of a conveyor belt on a downstream side is disposed below an end of a conveyor belt on an upstream side, and the green pellets are transferred by dropping from the conveyor belt on the upstream side onto the conveyor belt on the downstream side.
[0006] When the adhesion between the particles of the green pellets is insufficient, the Ŧ 1 1 I green pellets may be crumbled and pulverized by a drop impact. The pulverization of the green pellets may cause lowering of gas permeability in the traveling grate furnace and occurrence of a kiln ring in the kiln furnace, causing a problem in operations.
[0007] As a method for improving the adhesion of the green pellets, a method has been proposed in which pelletizing water, obtained by mixing an aqueous solution of polyalkylene glycol having a molecular weight of 1,000 to 20,000 with an aqueous solution of polyvinyl alcohol, is added to iron ore powder in a proportion of 0.001% by mass to 2% by mass of solid content, followed by pelletizing (see Japanese Unexamined Patent Application, Publication No. S48-095929).
[0008] According to the method for producing iron ore pellets disclosed in the patent application, permeability of the polyalkylene glycol and viscosity of the polyvinyl alcohol are utilized to improve crushing strength, a drop number (drop resistance), and the like of the green pellets. [PRIOR ART DOCUMENTS] [PATENT DOCUMENTS]
[0009] Patent Document 1: Japanese Unexamined Patent Application, Publication No. S48- 095929 [SUMMARY OF THE INVENTION] [PROBLEMS TO BE SOLVED BY THE INVENTION]
[0010] In a case in which the green pellets are transported, for example, by a plurality of conveyor belts, the number of transfers and a height difference at one transfer vary depending on equipment. Therefore, cracking strength (hereinafter also referred to simply as "strength") required for the green pellets varies. Furthermore, even when pelletizing water having the same concentration is used, the strength varies depending on the type of the iron ore. Thus, in the case of improving the strength of the green pellets by the above conventional method, components of the pelletizing water need to be adjusted each time the required strength, the iron ore to be used, or the like is changed. The component adjustment can be experimentally determined but requires time and effort, lowering operating efficiency.
[0011] The present invention was made in view of the foregoing circumstances, and an object of the present invention is to provide: a method for producing pelletizing water, the method enabling easily determining a polymeric binder-blending percentage of pelletizing water for obtaining strength required for green pellets; and a method for producing iron ore pellets. 3 7 1 1 [MEANS FOR SOLVING THE PROBLEMS]
[0012] As a result of intensive studies of the polymeric binder-blending percentage of the pelletizing water for obtaining the strength required for the green pellets, the present inventors found that regardless of the type and size of the iron ore and the type of the polymeric binder to be blended into water, a strength increment of the green pellets has a strong correlation with a viscosity of the pelletizing water, and completed the present invention.
[0013] That is to say, an aspect of the present invention is a method for producing pelletizing water to be added at a time of producing a pelletized product, the method including: a blending step of blending a polymeric binder into water, wherein in the blending step, a blending percentage of the polymeric binder with respect to the water is determined such that the pelletizing water after the blending satisfies a target viscosity.
[0014] In the method for producing pelletizing water, regardless of the type of the polymeric binder, the blending percentage of the polymeric binder is determined such that the pelletizing water after the blending satisfies the target viscosity. By using the pelletizing water which satisfies the target viscosity, the increment of the strength of the pelletized product can be controlled. The target viscosity can be calculated, for example, from a difference from the strength required for the pelletized product, by measuring beforehand the strength of the pelletized product in the case of using water as the pelletizing water. Accordingly, by using the method for producing pelletizing water, the polymeric binder- blending percentage of the pelletizing water for obtaining the strength required for the pelletized product can be easily determined.
[0015] It is preferred that the pelletized product is green pellets obtained by pelletizing iron ore, and that the target viscosity is defined by a drop number of the green pellets. By using the drop number, which is an indicator for the strength of the green pellets, to define the target viscosity, pulverization of the green pellets at a time of transporting can be inhibited.
[0016] When a drop number-control value of the green pellets is denoted by <com:Math><semantics>Dmin<annotation encoding="application / x-tex">D_{min}< / annotation>< / semantics>< / com:Math> [times] and the drop number of the green pellets in a case of using water as the pelletizing water is denoted by D<com:Sub>0< / com:Sub> [times], the target viscosity η [mPa·s] is preferably represented by the following formula 1. By using the following formula 1, the target viscosity can be easily defined, and thus the polymeric binder-blending percentage of the pelletizing water can be determined more easily. [Image disponible dans le document PDF, Image available in the PDF document] [0016a] In yet another aspect, the present invention provides a method for producing pelletizing water to be added at a time of producing a pelletized product, the method comprising: a blending step of blending a polymeric binder into water, wherein the polymeric binder comprises: a polymer which is a substance having a molecular weight of greater than or equal to 10<com:Sup>4< / com:Sup> and less than or equal to 10<com:Sup>8< / com:Sup>; and water, in the blending step, a blending percentage of the polymeric binder with respect to the water is determined such that the pelletizing water after the blending satisfies a target viscosity, the pelletized product is green pellets obtained by pelletizing iron ore, the target viscosity is defined by a drop number of the green pellets, a method for determining the blending percentage comprises: a drop number control value-setting step; a pelletizing water viscosity-determining step; a pelletizing water concentration-determining step; and a polymeric binder-blending amount-determining step, and in the drop number control value-setting step, when a drop number-control value of the green pellets is denoted by D<com:Sub>min< / com:Sub> [times] and the drop number of the green pellets in water is denoted by D<com:Sub>0< / com:Sub> [times], the target viscosity η [mPa·s] is represented by the following formula 1: [Image disponible dans le document PDF, Image available in the PDF document]
[0017] Another aspect of the present invention is a method for producing iron ore pellets, the method including: an adding step of adding pelletizing water to iron ore; a pelletizing step of pelletizing pelletizing water-containing iron ore obtained in the adding step; and a firing step of firing green pellets obtained in the pelletizing step, wherein as the pelletizing water, the pelletizing water obtained according to the method for producing pelletizing water of the present invention is used.
[0018] Since the method for producing iron ore pellets uses the pelletizing water obtained according to the method for producing pelletizing water of the present invention, the iron ore pellets can be stably produced.
[0019] The "viscosity" as referred to herein means a value measured according to JIS- Z8803:2011 by using a rotary viscometer. Furthermore, the "drop number of the green" pellets" as referred to herein means an average number of times until the green pellets are broken when free dropping of the green pellets onto an iron plate from a height of 500 mm is repeated. Specifically, the number of times until 12 green pellets are broken is measured, and an average value of 10 green pellets excluding the maximum and minimum is determined. It is to be noted that in addition to a case in which a green pellet is broken into greater than or equal to 2 pieces, a case of a visually detectable crack is included in the "broken" state. . [EFFECTS OF THE INVENTION]
[0020] As described above, according to the method for producing pelletizing water of the present invention, the polymeric binder-blending percentage of the pelletizing water for obtaining the strength required for the green pellets can be easily determined. Furthermore, according to the method for producing iron ore pellets of the present invention, the iron ore pellets can be stably produced. [BRIEF DESCRIPTION OF THE DRAWINGS]
[0021] FIG. 1 is a flowchart illustrating a method for producing iron ore pellets according to one embodiment of the present invention. FIG. 2 is a flowchart illustrating a method for producing pelletizing water according to an other embodiment of the present invention. FIG. 3 is a graph illustrating viscosities at a time of blending various types of polymers into water. FIG. 4 is a graph illustrating a relationship between the viscosity of pelletizing water and a drop number-improving effect. 4 4 FIG. 5 is a graph illustrating a relationship between the concentration and viscosity of pelletizing water in Examples. FIG. 6 is a graph illustrating a relationship between the polymeric binder-blending percentage and the drop number in the Examples. [DESCRIPTION OF EMBODIMENTS]
[0022] Hereinafter, embodiments of the present invention are described in detail with reference to the drawings as appropriate.
[0023] The method for producing iron ore pellets illustrated in FIG. 1 includes: an adding step S1; a pelletizing step S2; and a firing step S3.
[0024] Adding Step In the adding step S1, pelletizing water is added to iron ore.
[0025] The iron ore is fine powder having, for example, an average grain diameter of greater than or equal to 10 µm and less than or equal to 50 µm. Although surface properties of the iron ore differ greatly depending on the mining area and the crushing / transporting method, the surface properties of the iron ore are not particularly limited in the method for producing iron ore pellets.
[0026] As the pelletizing water, pelletizing water obtained according to the method for producing pelletizing water is used, the method itself being the other embodiment of present invention.
[0027] The method for producing pelletizing water is a method for producing pelletizing water to be added at a time of producing a pelletized product. In the method for producing iron ore pellets, the pelletized product is green pellets obtained by pelletizing iron ore.
[0028] As illustrated in FIG. 2, the method for producing pelletizing water includes a blending step S4.
[0029] Blending Step In the blending step S4, a polymeric binder is blended into water. It is to be noted that the polymeric binder may be blended with respect to moisture contained in the iron ore. That is to say, the adding of the pelletizing water to the iron ore and the blending in of the polymeric binder may be simultaneously performed.
[0030] ı • 1 1 A polymer used in the polymeric binder mainly means a substance having a molecular weight of greater than or equal to <com:Math><semantics>104<annotation encoding="application / x-tex">10^4< / annotation>< / semantics>< / com:Math> and less than or equal to <com:Math><semantics>108<annotation encoding="application / x-tex">10^8< / annotation>< / semantics>< / com:Math>, and preferably a substance having a molecular weight of greater than or equal to 10<com:Sup>4< / com:Sup> and less than or equal to 10<com:Sup>6< / com:Sup>. Examples of the polymeric binder include cornstarch, tapioca, potato, guar beans, and the like.
[0031] FIG. 3 illustrates a relationship between the concentration and the viscosity at the time of blending various types of polymers into water. When a polymer is thus blended (dissolved) into water, the viscosity of a solution of the polymer can be increased in accordance with the concentration. According to the method for producing pelletizing water, in the blending step S4, the blending percentage of the polymeric binder with respect to the water is determined such that the pelletizing water after the blending satisfies a target viscosity.
[0032] Specifically, the target viscosity is defined by a drop number of the green pellets. By using the drop number, which is an indicator for the strength of the green pellets, to define the target viscosity, pulverization of the green pellets at a time of transporting can be inhibited.
[0033] The present inventors have found that regardless of the type and size of the iron ore and the type of the polymeric binder to be blended into water, a strength increment of the green pellets has a strong correlation with the viscosity of the pelletizing water, and discovered that when a drop number-control value of the green pellets is denoted by Dmin [times] and the drop number of the green pellets in a case of using water as the pelletizing water is denoted by D<com:Sub>0< / com:Sub> [times], the target viscosity η [mPa·s] is represented by the following formula 1. By using the following formula 1, the target viscosity can be easily defined, and thus the polymeric binder-blending percentage of the pelletizing water can be determined more easily. [Image disponible dans le document PDF, Image available in the PDF document] • • • 1
[0034] The above formula 1 was derived from results of investigating the relationship between the viscosity and the drop number, wherein in the investigation, a pelletizing test was conducted using pelletizing water having a viscosity increased by blending a polymeric binder thereinto. The derivation of the above formula 1 is described below.
[0035] Three types of iron ores (iron ore 1, iron ore 2, and iron ore 3) having different properties were prepared. These iron ores differ in grain size. Table 1 shows a percentage 7 . 1 . of a grain diameter of less than or equal to <com:Math><semantics>4.7μm<annotation encoding="application / x-tex">4.7 \mu m< / annotation>< / semantics>< / com:Math>.
[0036] Table 1 [Image disponible dans le document PDF, Image available in the PDF document]
[0037] Firstly, by using water (viscosity: 1 mPa·s) as the pelletizing water, green pellets were produced from the three types of the iron ores. In the pelletizing, a pan pelletizer having a diameter of 0.4 m was used. Table 2 shows conditions for the pelletizing test.
[0038] Table 2 [Image disponible dans le document PDF, Image available in the PDF document]
[0039] For each of three types of green pellets produced from the three types of the iron ores, the drop number was measured. The viscosity was measured according to JIS- Z8803:2011 by using a rotary viscometer ("TVB-15 type viscometer", available from Toki Sangyo Co., Ltd.). It is to be noted that pure water was used as a solvent, and an angular velocity of a rotor was set to a constant value of 30 rpm. Furthermore, the measurement was performed at room temperature (greater than or equal to 23 °C and less than or equal to 25 °C).
[0040] The drop number of each of the green pellets in the case of using water as the pelletizing water is denoted by <com:Math><semantics>D0<annotation encoding="application / x-tex">D_0< / annotation>< / semantics>< / com:Math> [times]. <com:Math><semantics>D0<annotation encoding="application / x-tex">D_0< / annotation>< / semantics>< / com:Math> is a value which varies for each iron ore. Table 1 shows the value of <com:Math><semantics>D0<annotation encoding="application / x-tex">D_0< / annotation>< / semantics>< / com:Math> for each iron ore.
[0041] • i i Next, the viscosity of the pelletizing water was changed by blending the polymeric binder thereinto, and the pelletizing test was performed under similar conditions to measure a drop number <com:Math><semantics>Dx<annotation encoding="application / x-tex">D_x< / annotation>< / semantics>< / com:Math> of green pellets obtained. FIG. 4 illustrates a relationship between a difference <com:Math><semantics>ΔD<annotation encoding="application / x-tex">\Delta D< / annotation>< / semantics>< / com:Math> between <com:Math><semantics>Dx<annotation encoding="application / x-tex">D_x< / annotation>< / semantics>< / com:Math> and <com:Math><semantics>D0<annotation encoding="application / x-tex">D_0< / annotation>< / semantics>< / com:Math> (= <com:Math><semantics>Dx<annotation encoding="application / x-tex">D_x< / annotation>< / semantics>< / com:Math> - <com:Math><semantics>D0<annotation encoding="application / x-tex">D_0< / annotation>< / semantics>< / com:Math>; drop number-improving effect), and the viscosity η [mPa·s] of the pelletizing water. It is to be noted that the polymeric binder used was the polymeric binder A illustrated in FIG. 3.
[0042] According to the graph in FIG. 4, regardless of the type of the iron ore, the drop number-improving effect <com:Math><semantics>ΔD<annotation encoding="application / x-tex">\Delta D< / annotation>< / semantics>< / com:Math> has a correlation with the viscosity <com:Math><semantics>η<annotation encoding="application / x-tex">\eta< / annotation>< / semantics>< / com:Math> of the pelletizing water, and <com:Math><semantics>Dx<annotation encoding="application / x-tex">D_x< / annotation>< / semantics>< / com:Math> can be approximated according to the following formula 2. [Image disponible dans le document PDF, Image available in the PDF document] . . . 2
[0043] In actual operations, there is a drop number control value <com:Math><semantics>Dmin<annotation encoding="application / x-tex">D_{min}< / annotation>< / semantics>< / com:Math> [times], and the operations need to be conducted such that <com:Math><semantics>Dx<annotation encoding="application / x-tex">D_x< / annotation>< / semantics>< / com:Math> is greater than <com:Math><semantics>Dmin<annotation encoding="application / x-tex">D_{min}< / annotation>< / semantics>< / com:Math>; therefore, the operations need to be conducted such that the following formula 1 is always satisfied. [Image disponible dans le document PDF, Image available in the PDF document]
[0044] The above formula 1 was derived in the above-described manner. It is to be noted that the above formula 1 is an example and does not hinder the use of another approximate expression including a different coefficient or formula.
[0045] A method for determining the blending percentage of the polymeric binder with respect to the water in the case of using the above formula 1 such that the pelletizing water after the blending satisfies the target viscosity (method for determining the blending percentage) is described in detail.
[0046] The method for determining the blending percentage includes: a drop number control value-setting step; a pelletizing water viscosity-determining step; a concentration— viscosity correlation-extracting step; a pelletizing water concentration-determining step; and a polymeric binder-blending amount-determining step.
[0047] Drop number control value-setting step In the drop number control value-setting step, the drop number control value D<com:Sub>min< / com:Sub> is set as a target in accordance with a standard of each piece of production equipment for the iron ore pellets.
[0048] 3 ( . The drop number control value <com:Math><semantics>Dmin<annotation encoding="application / x-tex">D_{min}< / annotation>< / semantics>< / com:Math> is an amount determined by a transport path (the number of transfers and the height difference at each transfer) of the green pellets. In a case of renewal of the transport path, etc., <com:Math><semantics>Dmin<annotation encoding="application / x-tex">D_{min}< / annotation>< / semantics>< / com:Math> needs to be experimentally or analytically determined, but the same value can be continuously used as long as the transport path is maintained.
[0049] Pelletizing water viscosity-determining step In the pelletizing water viscosity-determining step, the target viscosity <com:Math><semantics>η<annotation encoding="application / x-tex">\eta< / annotation>< / semantics>< / com:Math> required is determined according to the above formula 1 by using the drop number control value D<com:Sub>min< / com:Sub> and the drop number <com:Math><semantics>D0<annotation encoding="application / x-tex">D_0< / annotation>< / semantics>< / com:Math>, which is determined by the iron ore to be used.
[0050] It is to be noted that in a case in which the drop number <com:Math><semantics>D0<annotation encoding="application / x-tex">D_0< / annotation>< / semantics>< / com:Math>, which is determined by the iron ore, has not been calculated, green pellets may be produced using water (viscosity: 1 mPa·s) as the pelletizing water, and the drop number of the green pellets may be measured for calculation.
[0051] Concentration-viscosity correlation-extracting step In the concentration-viscosity correlation-extracting step, a relationship between the concentration of the polymeric binder to be used and the viscosity of the pelletizing water is extracted.
[0052] Specifically, the viscosity is measured while changing the concentration of the polymeric binder, and the relationship therebetween is extracted. It is to be noted that in a case in which the concentration-viscosity correlation of the polymeric binder to be used has already been extracted, the result may be used, and thus this step can be omitted.
[0053] Pelletizing water concentration-determining step In the pelletizing water concentration-determining step, the concentration of the polymeric binder at which the target viscosity η determined in the pelletizing water viscosity- determining step is obtained is determined based on the result extracted in the concentration- viscosity correlation-extracting step.
[0054] Polymeric binder-blending amount-determining step In the polymeric binder-blending amount-determining step, the blending amount of the polymeric binder is determined such that the concentration of the pelletizing water is the concentration determined in the pelletizing water concentration-determining step.
[0055] In a case in which the iron ore retains sufficient water, the polymeric binder may be 3 1 i t added alone in accordance with the water retention amount. Conversely, in a case in which the iron ore does not retain water, pelletizing water in which the polymeric binder is blended into water to have the above concentration may be added. In an intermediate case, considering the water retention amount of the iron ore, the polymeric binder-blending amount is determined such that the concentration of the pelletizing water added reaches the above concentration.
[0056] Pelletizing Step In the pelletizing step S2, pelletizing water-containing iron ore obtained in the adding step S1 is pelletized.
[0057] Specifically, the pelletizing water-containing iron ore obtained by adding the pelletizing water in the adding step S1 is charged into a pelletizer (for example, a pan pelletizer or the like) and rolled to produce dirtball-shaped green pellets.
[0058] Firing Step In the firing step S3, the green pellets obtained in the pelletizing step S2 are fired.
[0059] In the firing step S3, a traveling grate furnace and a kiln furnace are used. In the traveling grate furnace, first the green pellets immediately following the pelletizing are placed on a metal pallet to form a packed bed, followed by transporting the packed bed and blowing a hot blast onto the packed bed to dry the green pellets. Next, while being rolled, the green pellets dried are pre-fired until reaching strength of a degree in which pulverization does not occur in firing. Furthermore, in the kiln furnace, the pre-fired pellets are sintered at a temperature of about 1,200 °C.
[0060] The pellets after the sintering are, for example, placed on the metal pallet and cooled by blowing with a cool blast. In this manner, the iron ore pellets can be produced.
[0061] Advantages In the method for producing pelletizing water, regardless of the type of the polymeric binder, the blending percentage of the polymeric binder is determined such that the pelletizing water after the blending satisfies the target viscosity. By using the pelletizing water which satisfies the target viscosity, the increment of the strength of the pelletized product can be controlled. The target viscosity can be calculated, for example, from a difference from the strength required for the pelletized product, by measuring beforehand the strength of the pelletized product in the case of using water as the pelletizing water. Accordingly, by using the method for producing pelletizing water, the polymeric binder- 3 4 . . . . . . . . . . . . . . . . . . . . blending percentage of the pelletizing water for obtaining the strength required for the pelletized product can be easily determined.
[0062] Furthermore, since the method for producing iron ore pellets uses the pelletizing water obtained according to the method for producing pelletizing water of the present invention, the iron ore pellets can be stably produced.
[0063] Other Embodiments It is to be noted that the present invention is not limited to the above-described embodiments.
[0064] In the above-described embodiments, the case in which the pelletized product is the green pellets obtained by pelletizing the iron ore has been described; however, the method for producing pelletizing water of the present invention can also be used to produce other pelletized products.
[0065] In the above-described embodiments, the case in which the target viscosity is defined by the drop number of the green pellets has been described; however, the target viscosity may be appropriately defined by other indicator(s) in accordance with the method for transporting the green pellets and the like. EXAMPLES
[0066] Hereinafter, the present invention is described further in detail by way of Examples; the present invention is not limited to the Examples.
[0067] Water was added to iron ore, and green pellets were produced using a pan pelletizer having a diameter of 6 m. As pelletizing conditions, an angle of 45°, a rotation speed of 8 rpm, a rim height of 760 mm, and a raw material feeding amount of 80 t / h were employed. The drop number of the green pellets produced was measured to determine <com:Math><semantics>D0<annotation encoding="application / x-tex">D_0< / annotation>< / semantics>< / com:Math>. The result was <com:Math><semantics>D0=5.2<annotation encoding="application / x-tex">D_0 = 5.2< / annotation>< / semantics>< / com:Math> [times].
[0068] The drop number control value <com:Math><semantics>Dmin<annotation encoding="application / x-tex">D_{min}< / annotation>< / semantics>< / com:Math> of a transport path of the green pellets, the transport path being constituted by conveyor belts with 7 transfers, was experimentally determined. The result was <com:Math><semantics>Dmin=7<annotation encoding="application / x-tex">D_{min} = 7< / annotation>< / semantics>< / com:Math> [times].
[0069] From the above results, the viscosity <com:Math><semantics>η<annotation encoding="application / x-tex">\eta< / annotation>< / semantics>< / com:Math> of the pelletizing water was determined according to the above formula 1. <com:Math><semantics>η≥14.3<annotation encoding="application / x-tex">\eta \ge 14.3< / annotation>< / semantics>< / com:Math> [mPa·s] was obtained. . 4 i i
[0070] Next, in order to use the polymer I in FIG. 3 as the polymeric binder, the concentration—viscosity correlation of the polymer I was examined. The viscosity was measured according to JIS-Z8803:2011 by using the rotary viscometer ("TVB-15 type viscometer", available from Toki Sangyo Co., Ltd.). It is to be noted that pure water was used as a solvent, and the angular velocity of the rotor was set to the constant value of 30 rpm. Furthermore, the measurement was performed at room temperature (greater than or equal to 23 °C and less than or equal to 25 °C). FIG. 5 illustrates the concentration— viscosity correlation.
[0071] From the concentration—viscosity correlation of the polymer I, a concentration R at which <com:Math><semantics>η≥14.3<annotation encoding="application / x-tex">\eta \ge 14.3< / annotation>< / semantics>< / com:Math> [mPa·s] is satisfied was calculated. R = 1.0 [% by mass] was determined.
[0072] Moisture contained in a raw material to be pelletized, the raw material including iron ore, was 80 g / kg-dry (8.0% by mass) per kg-dry of the raw material to be pelletized. Thus, 0.8 g / kg-dry (0.8% by mass) of the polymeric binder I per kg-dry of the raw material to be pelletized was added such that the polymeric binder concentration R of the pelletizing water was 1.0% by mass.
[0073] Green pellets were produced using the pelletizing water into which the polymeric binder I was thus blended. It is to be noted that for the pelletizing, the above-mentioned pan pelletizer having the diameter of 6 m was used.
[0074] With regard to the plurality of the green pellets produced, the drop number <com:Math><semantics>Dx<annotation encoding="application / x-tex">D_x< / annotation>< / semantics>< / com:Math> was measured. FIG. 6 illustrates the drop number <com:Math><semantics>Dx<annotation encoding="application / x-tex">D_x< / annotation>< / semantics>< / com:Math> together with the drop number <com:Math><semantics>D0<annotation encoding="application / x-tex">D_0< / annotation>< / semantics>< / com:Math> in the case of adding water to the iron ore to produce the green pellets.
[0075] The results in FIG. 6 indicate that by determining the blending percentage of the polymeric binder according to the method for producing pelletizing water of the present invention, green pellets having a drop number that is greater than or equal to the drop number control value D<com:Sub>min< / com:Sub> can be stably obtained. [INDUSTRIAL APPLICABILITY]
[0076] According to the method for producing pelletizing water of the present invention, the polymeric binder-blending percentage of the pelletizing water for obtaining the strength required for the green pellets can be easily determined. Furthermore, according to the method for producing iron ore pellets of the present invention, the iron ore pellets can be stably produced.
Claims
We claim: A method for producing pelletizing water to be added at a time of producing a pelletized product, the method comprising: a blending step of blending a polymeric binder into water, wherein the polymeric binder comprises: a polymer which is a substance having a molecular weight of greater than or equal to 10<com:Sup>4< / com:Sup> and less than or equal to 10<com:Sup>8< / com:Sup>; and water, in the blending step, a blending percentage of the polymeric binder with respect to the water is determined by: setting a drop number-control value of the pelletized product; determining a target viscosity of the pelletizing water; determining a concentration of the pelletizing water to obtain the target viscosity; and জ<com:Br / >কু ; . determining a blending amount of the polymeric binder based on the concentration determined, when the drop number-control value of the pelletized product is denoted by Dmin . . - [times] and a drop number of the pelletized product in water is denoted by D<com:Sub>0< / com:Sub> [times], the target viscosity η [mPa·s] is represented by the following formula 1: [Image disponible dans le document PDF, Image available in the PDF document] • • • 1 , and the pelletized product is green pellets obtained by pelletizing iron ore.
2. The method for producing pelletizing water according to claim 1, wherein said determining the concentration of the pelletizing water comprises measuring a viscosity of the pelletizing water while changing a concentration of the polymeric binder in the pelletizing water, thereby establishing a relationship between the concentration of the polymeric binder and the viscosity of the pelletizing water, and wherein the relationship is used to determine the concentration of the pelletizing water.
3. A method for producing iron ore pellets, the method comprising: an adding step of adding pelletizing water to iron ore; a pelletizing step of pelletizing water-containing iron ore obtained in the adding step; and a firing step of firing green pellets obtained in the pelletizing step, wherein the pelletizing water is obtained by the method defined by claim 1 or claim 2.