Abstract
Description
technical field
[0001] The invention belongs to the field of resin lenses, in particular to a high-transmittance anti-blue light goggle lens and a preparation method thereof. Background technique
[0002] At present, with the advancement of science and technology, human beings have entered the information age, and major changes have taken place in the way of learning, working and living. Among them, the dependence on vision is getting higher and higher, and the burden of vision is getting heavier and heavier. People's study, work, and entertainment are increasingly inseparable from computers, TVs, mobile phones, etc. The display screens of these electronic products have high blue light radiation components, which can cause great damage to visual cells, and are an ever-changing source of light radiation.
[0003] Light wavelengths in the range of 400-700nm are visible to the human eye, those with wavelengths shorter than 400nm are ultraviolet rays, those with wavelengths lon...
Examples
Embodiment 1
[0038] High-transmittance anti-blue light goggles raw materials (parts by weight): 100 parts of resin monomer, 2 parts of ultraviolet absorber, 1 part of blue light absorber, 1 part of anti-reflection agent, and 1 part of initiator.
[0039] The resin monomer is a bisallyl diglycol dicarbonate monomer with a refractive index of 1.49.
[0040] The initiator is diisopropyl peroxydicarbonate.
[0041] The anti-reflection agent is titanium dioxide.
[0042] The blue light absorber is zirconia.
[0043] The ultraviolet absorber is a rare earth complex, and the rare earth complex is a binary rare earth complex.
[0044] The rare earth binary complex is prepared by the following method: Weigh 52.79g of europium carbonate and 134.55g of dibenzoylmethane, place it in a planetary ball mill for ball milling, select ceramic ball mill pots and ceramic balls, and the mass ratio of the ball to material is 20:1, the ball milling speed is 500 rpm, and the ball milling time is 4 hours to obt...
Embodiment 2
[0052] High-transmittance anti-blue light goggles raw materials (parts by weight): 100 parts of resin monomer, 2 parts of ultraviolet absorber, 1 part of blue light absorber, 1 part of anti-reflection agent, and 1 part of initiator.
[0053] The resin monomer is a bisallyl diglycol dicarbonate monomer with a refractive index of 1.49.
[0054] The initiator is diisopropyl peroxydicarbonate.
[0055] The anti-reflection agent is titanium dioxide.
[0056] The blue light absorber is modified zirconia.
[0057] The ultraviolet absorber is a rare earth complex, and the rare earth complex is a binary rare earth complex.
[0058] The rare earth binary complex is prepared by the following method: Weigh 52.79g of europium carbonate and 134.55g of dibenzoylmethane, place it in a planetary ball mill for ball milling, select ceramic ball mill pots and ceramic balls, and the mass ratio of the ball to material is 20:1, the ball milling speed is 500 rpm, and the ball milling time is 4 hou...
Embodiment 3
[0071] High-transmittance anti-blue light goggles raw materials (parts by weight): 100 parts of resin monomer, 2 parts of ultraviolet absorber, 1 part of blue light absorber, 1 part of anti-reflection agent, and 1 part of initiator.
[0072] The resin monomer is a bisallyl diglycol dicarbonate monomer with a refractive index of 1.49.
[0073] The initiator is diisopropyl peroxydicarbonate.
[0074] The anti-reflection agent is titanium dioxide.
[0075] The blue light absorber is modified zirconia.
[0076] The ultraviolet absorber is a rare earth complex, and the rare earth complex is a binary rare earth complex.
[0077] The rare earth binary complex is prepared by the following method: Weigh 52.79g of europium carbonate and 134.55g of dibenzoylmethane, place it in a planetary ball mill for ball milling, select ceramic ball mill pots and ceramic balls, and the mass ratio of the ball to material is 20:1, the ball milling speed is 500 rpm, and the ball milling time is 4 hou...