A technology of curbstone and recycled materials, applied in the field of curbstone repairing recycled materials and its bonding, can solve the problems of low compressive strength, waste of resources, limited resources, etc., and achieve the goal of reducing aging rate, processing cost and demoulding time Effect
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2018-09-18
- Estimated Expiration
- Not applicable · inactive patent
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of curb stone processing, in particular to a regenerated material for curb stone repair and a bonding method thereof. Background technique:
[0002] Curb stone refers to the boundary stone used on the edge of the road surface, also known as curb stone or curb stone, curb stone. Curb stones are used to distinguish roadways, sidewalks, green spaces, isolation belts and other parts of the road on the road surface, and play a role in ensuring the safety of pedestrians and vehicles and ensuring the tidy edges of the road surface.
[0003] Currently, curbs are usually prefabricated from ordinary concrete or cut from natural stones, such as curbs made of granite and marble. Curb stone cut from natural stone is not only difficult to obtain materials and construction, but also has limited resources and damages natural resources, so it has not been widely used in recent years. However, although the price of curb st...
Examples
Embodiment 1
[0035] (1) Crushing of waste ore: First, use a pulverizer to make the waste ore into coarse particles with a particle size of 1-3cm, then crush the coarse particles into fine particles with a particle size of 0.05-0.5cm, and then crush the fine particles into particles with a particle size of 0.25-1mm Fine powder, that is, curb stone recycled material;
[0036] (2) Formability activation of recycled materials: add 100kg of the above-mentioned curbstone recycled materials into water, stir to make it completely submerged, add 3kg of coagulant after soaking for 12 hours, stir evenly, and continue soaking for 12 hours;
[0037] (3) Preparation of auxiliary materials: short cotton wool, marble powder, phosphate starch-vegetable glue copolymer adhesive, polyethylene oxide, nano-SiO 2 colloidal particles, phosphate starch, active agent, deionized water; auxiliary materials weigh 80kg ;
[0038] The weight ratio of short cotton linters, marble powder, phosphate starch-vegetable glue ...
Embodiment 2
[0055] (1) Crushing of waste ore: First, use a pulverizer to make the waste ore into coarse particles with a particle size of 1-3cm, then crush the coarse particles into fine particles with a particle size of 0.05-0.5cm, and then crush the fine particles into particles with a particle size of 0.25-1mm Fine powder, that is, curb stone recycled material;
[0056] (2) Formability activation of recycled materials: add 100kg of the above-mentioned road calculus recycled materials into water, stir to make it fully submerged, add 5kg of coagulant after soaking for 12 hours, stir evenly, and continue soaking for 12 hours;
[0057] (3) Preparation of auxiliary materials: short cotton wool, marble powder, phosphate starch-vegetable glue copolymer adhesive, polyethylene oxide, nano-SiO 2 colloidal particles, phosphate starch, active agent, deionized water; auxiliary materials weigh 80kg ;
[0058] The weight ratio of short cotton linters, marble powder, phosphate starch-vegetable glue c...
Embodiment 3
[0075] (1) Crushing of waste ore: First, use a pulverizer to make the waste ore into coarse particles with a particle size of 1-3cm, then crush the coarse particles into fine particles with a particle size of 0.05-0.5cm, and then crush the fine particles into particles with a particle size of 0.25-1mm Fine powder, that is, curb stone recycled material;
[0076] (2) Formability activation of recycled materials: add 100kg of the above-mentioned road calculus recycled materials into water, stir to make it fully submerged, add 5kg of coagulant after soaking for 12 hours, stir evenly, and continue soaking for 12 hours;
[0077] (3) Preparation of auxiliary materials: short cotton wool, marble powder, phosphate starch-vegetable glue copolymer adhesive, polyethylene oxide, nano-SiO 2 colloidal particles, phosphate starch, active agent, deionized water; auxiliary materials weigh 80kg ;
[0078] The weight ratio of short cotton linters, marble powder, phosphate starch-vegetable glue c...