Color paste and processing technology thereof
By developing dye pastes with particle sizes below 200nm and combining dye, dispersant and comprehensive additive technologies, we have solved the problems of traditional dye pollution and water consumption, achieved an efficient and environmentally friendly dyeing process, and reduced the pollution of cleaning water. and dyeing time.
Patent Information
- Application Number
- CN201811146780.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-09-29
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2038-09-29
AI Technical Summary
Traditional dyes produce a large amount of impurities and auxiliary residues during the dyeing process, resulting in cleaning water pollution, water consumption and time-consuming, and affecting the color fastness of fabrics, making it difficult to achieve low pollution, energy conservation and environmental protection.
Develop a color paste with a particle size below 200nm, which contains dyes, dispersants and comprehensive additives. It reduces the particle size and impurity content through rough grinding and fine grinding, and is directly combined with fibers during the dyeing process to achieve water dispersion. Self-circulating and efficient dyeing, using deionized water and a combination of specific additives to improve stability and environmental protection.
It effectively reduces the cleaning process and water volume, reduces dyeing time, improves the color fastness and environmental performance of dyes, reduces pollution and energy consumption, realizes self-circulation and reuse of dyeing water, and reduces costs.
Smart Images

Figure CN108867106B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a color paste and a processing technology thereof, belonging to the technical field of dyeing or printing processing of fabrics. Background Art
[0002] The dyeing of fabrics, fibers, etc. mainly consists of pre-treatment, dyeing / printing, and post-treatment processes. Among them, the post-treatment includes at least four cleaning steps: alkali washing, water washing, acid washing, and water washing. The main reason for multiple cleanings is that the conventional dyes are composite finished products. In addition to the dyes themselves, they also contain a large amount of impurities, fillers, dispersants, and auxiliaries. These ingredients are used to maintain the stability of the performance and specifications of the dyes on the one hand, and on the other hand, they are based on considerations such as color fastness and dyeing rate. For commercial purposes, they must be added in large quantities. Therefore, in the dyeing process, dye is the main active ingredient of dyeing, and impurities, fillers, dispersants and other additives mainly play the role of bridge and catalyst. After dyeing is completed, they continue to remain on the treated object, which will cause defects such as poor consumption and unsafe use. Therefore, the main purpose of multiple cleaning in post-treatment is to clean and remove the above-mentioned components that play the role of catalyst and bridge. Therefore, the traditional process not only has many processes and long cycles, but also produces a large amount of cleaning wastewater; at the same time, the presence of the above-mentioned catalytic components will also play a certain barrier role between the fabric structure and the dye, and specifically manifested as floating color. Therefore, the cleaning water will contain a certain proportion of dyes, which will not only cause turbidity in the cleaning water, but also continue to act with the components that play the role of catalyst and bridge, resulting in a high COD value of the cleaning water.
[0003] The above problems are the main reasons why the traditional printing and dyeing industry has been criticized in terms of environmental protection and energy saving. How to achieve low or even zero pollution, energy saving and environmental protection in printing and dyeing is an urgent problem to be solved in this field.
[0004] Based on this, this application is made. Summary of the invention
[0005] In view of the above-mentioned defects existing in the use of existing dyes, the present application first provides a printing paste which is water-free, has high dyeing efficiency and can effectively shorten the dyeing cycle.
[0006] To achieve the above objectives, the technical solutions adopted by this application are as follows:
[0007] A color paste, the color paste particle size is less than 200nm (preferably 50-200nm), comprising a dye, a dispersant, water and a comprehensive auxiliary agent for adjusting level dyeing and dyeing fastness, the dispersant contains S less than 5% (preferably 2-3), and its content is 3-10%; the dye content is 10-40%, the comprehensive auxiliary agent is 0-10%, and the rest is water.
[0008] The present application uses dye, dispersant and comprehensive auxiliary agent as raw materials to form color paste. The particle size of the color paste is less than 200nm, which can be directly combined with the fiber during the dyeing process, reducing the addition of dyeing auxiliary agents, etc., avoiding floating color, effectively reducing the cleaning process and the residual amount of dye in the cleaning water, and realizing the self-circulation process of water, saving water and time; the S content in the dispersant is controlled to effectively reduce the COD of the treatment liquid.
[0009] The applicant has also conducted further research on dyes to improve the amount of impurities contained in the color paste. Specifically, the dye is a disperse dye, and more preferably, the dye comes from a filter cake. When the filter cake is used as a raw material, the filter cake is mixed with a dispersant for coarse grinding and a certain degree of fine grinding, and then a comprehensive auxiliary agent is added for the final few fine grindings. The finished product is a color paste with pure ingredients. The color paste does not contain any other impurities or catalytic components except the added dispersant and comprehensive auxiliary agent.
[0010] The applicant has conducted further research on the dyeing of comprehensive additives with ink-like dyes, and achieved good results in terms of color paste stability, color paste safety and environmental protection: the comprehensive additive is compounded from N-methyl-2-pyrrolidone, urea, sodium dodecylbenzene sulfate and deionized water, and the mass percentages of each component are: N-methyl-2-pyrrolidone 10-30%, urea 5-10%, sodium dodecylbenzene sulfate 2-3% and deionized water 60-77%. More preferably, the ratio of the comprehensive auxiliary agent is: 22% N-methyl-2-pyrrolidone, 8% urea, 3% sodium dodecylbenzene sulfate and 67% deionized water; or, the ratio of the comprehensive auxiliary agent is: 30% N-methyl-2-pyrrolidone, 5% urea, 2% sodium dodecylbenzene sulfate and 63% deionized water; or, the ratio of the comprehensive auxiliary agent is: 10% N-methyl-2-pyrrolidone, 10% urea, 3% sodium dodecylbenzene sulfate and 77% deionized water. Among them, the molecular formula of N-methyl-2-pyrrolidone is C5H9NO, the molecular weight is 99.134, the boiling point is 202°C, and the flash point is 95°C; the deionized water is the water after the anion and cation exchange column, and the impurities have been removed. The comprehensive auxiliary agent, in combination with dyes and dispersants, can effectively improve the stability of the color paste at high and normal temperatures, and effectively avoid high-temperature steaming, boiling and cleaning of the treated objects such as fibers, fabrics or fabrics, and prevent the overflow and diffusion of dyes when they are sprayed onto fibers, fabrics or fabrics. In addition, during the production and processing, there is no pollution to the atmosphere and water quality, and no odor or harmful substances are emitted, and the energy-saving and environmental protection efficiency is high.
[0011] The applicant has conducted further research on the dyeing of the comprehensive auxiliary agent with the rotary screen or digital printing, and achieved good results in the stability, safety and environmental protection of the color paste: the comprehensive auxiliary agent is composed of urea, acetic acid, sodium bicarbonate, sodium sulfate, OP-10, and deionized water, and the mass percentages of each component are: urea 4-15%, acetic acid 0.5-2%, sodium bicarbonate 1.5-3%, sodium sulfate 0.5-2%, OP-100.5-2%, deionized water 82-87.5%. More preferably, the ratio of the comprehensive auxiliary agent is: urea 10%, acetic acid 1%, sodium bicarbonate 1.5%, sodium sulfate 1%, OP-10 1.5%, deionized water 85%; or, the ratio of the comprehensive auxiliary agent is: urea 4%, acetic acid 2%, sodium bicarbonate 3%, sodium sulfate 2%, OP-10 2%, deionized water 87%. Among them, the component of OP-10 is alkylphenol polyoxyethylene ether. This comprehensive auxiliary agent, combined with dyes and dispersants, has excellent leveling, wetting, emulsifying, diffusing and antistatic properties, which can effectively improve the stability of color paste at high and normal temperatures, and effectively avoid high-temperature steaming, boiling and cleaning of fibers, fabrics or fabrics, and prevent the overflow and diffusion of dyes when they are sprayed onto fibers, fabrics or fabrics. In addition, there is no pollution to the atmosphere and water quality during production and processing, and no odor or harmful substances are emitted, with high energy-saving and environmental protection efficiency.
[0012] On the basis of the above research, the applicant also studied the preparation method of the color paste and the equipment used in the preparation, and formed a set of color paste processing technology that matches it, which can be described as follows:
[0013] A color paste processing technology, after the dye and dispersant are mixed in a mixing area, they are sent to a coarse grinding area for coarse grinding, the coarse grinding area is equipped with a separator and grinding beads, the separator gap is 0.5-1.5mm, the rotation speed is 1200-2000r / min, the linear speed is 10-15m / s, the grinding bead diameter is 0.8-2mm, the particles are ground to a particle size of less than 10μm, and then transferred to a fine grinding area for fine grinding; the fine grinding area is equipped with a rotor, a separator and grinding beads, the separator The gap is less than 0.8mm (more preferably, the separator gap is 0.05-0.6mm), the grinding beads are PU beads or 95 and above zirconia beads, the diameter of the grinding beads is less than 0.4mm, and when the comprehensive additives are added to complete the fine grinding, the temperature of the fine grinding zone is 0-40°C, the processing time is 5-20h, and the line speed is 5-20m / s; comprehensive additives are added as needed before fine grinding and discharging, and then transferred to the storage area, and the finished color paste is obtained after passing through the inspection area and the packaging area.
[0014] The raw and auxiliary materials used in this application mainly include three kinds: dye, dispersant and comprehensive additives that may be added subsequently. The dye and dispersant in powder form are coarsely ground and finely ground to reduce the particle size step by step to ensure that the particle size of the formed color paste is below 200nm, and comprehensive additives are added as needed before fine grinding to meet the special requirements of different usage environments.
[0015] The applicant has conducted further research on fine grinding on the basis of the above scheme to improve the quality of the color paste in terms of grinding fineness. The fine grinding area includes a fine grinder, a cylinder A and a cylinder B. The separator and grinding beads are all arranged in the fine grinder. The cylinder A is provided with two inlets and one opening, one of which is connected to the coarse grinding area, and the other is connected to the comprehensive additive area; the opening is connected to the fine grinder, and the cylinder B is provided with two openings, one of which is connected to the fine grinder, and the other is connected to the storage area; the material discharged from the coarse grinding area enters the cylinder A, and is sent to the fine grinder through the cylinder A. After the grinding is completed in the fine grinder, it is sent to the cylinder B. After standing in the cylinder B, it is rotated back to the fine grinder, and then transferred to the cylinder B. This reciprocating process is repeated until the penultimate grinding, and then it is transferred to the cylinder A through the fine grinder, the comprehensive additive area is opened, and the comprehensive additive is added as needed, and then it is transferred to the fine grinder for the last grinding, and then sent to the storage area through the cylinder B. Dye and dispersant are the main active ingredients in dyeing. In the present application, the two are first mixed and subjected to coarse grinding and (N-1) fine grinding, and then the entrance of cylinder A and the comprehensive auxiliary agent area are opened, and the required amount of comprehensive auxiliary agent is added to the dye and dispersant that have been finely ground (N-1) times, and then transferred to the fine grinder. After the last fine grinding (i.e., the Nth fine grinding) is completed, the material is sent to the storage area by cylinder B. The above-mentioned materials are reciprocated in cylinder A, fine grinder and cylinder B to form internal circulation fine grinding, and different cycles are realized for different materials, which not only makes full use of the grinding process, but also avoids excessive grinding of other materials that do not need too much grinding, thereby improving the grinding fineness.
[0016] The present application has also done further work on the cooling in the above scheme to avoid high-temperature polymerization caused by grinding: a cooling water pipe is set on the outer wall of the fine grinder, and the cooling water pipe uses 0-30°C cooling water or (-25-15°C) cooling liquid as a cooling medium to cool and insulate the fine grinder. As the grinding proceeds, high-speed grinding friction will generate a certain amount of heat, which will gradually accumulate in a fixed space, causing the temperature of the entire grinding chamber and the material in the grinding chamber to increase, and the dye and dispersant will produce high-temperature polymerization under high temperature conditions, which will not only affect the utilization rate of the raw materials (referring to dyes, dispersants and necessary amounts of comprehensive additives, the same below), but also form raw material impurities, affecting the molding effect of the color paste. The present application controls the temperature of the fine grinding zone, and preferably uses cooling water or cooling liquid to control the temperature of the fine grinding zone, especially the fine grinder, at 0-40°C, which will not affect the normal function of the raw materials and avoid excessive energy consumption.
[0017] This application has done further work on the rotor in the above scheme to ensure the rapid flow of materials: the rotor includes a body, a rotating shaft, rotating teeth and rotating grooves. The rotating shaft is driven to rotate by a power source. The rotating shaft is fixedly connected to the body. The outer wall of the body is provided with rotating teeth. The cross section of the rotating teeth is trapezoidal. The grooves between adjacent rotating teeth and the outer wall of the body form a rotating groove. When the rotating shaft drives the body to rotate, the rotating teeth rotate accordingly. The trapezoidal cross-sectional shape of the rotating teeth, which is large outside and small inside, effectively drives the material to rotate accordingly, and forms a vortex shape between the rotating grooves, thereby effectively improving the grinding efficiency.
[0018] In order to ensure sufficient grinding, the present application also improves the mixing zone to improve the mixing uniformity of the dye and dispersant: the mixing zone includes a stirring barrel, a stirring shaft and a stirring disk, the stirring shaft is driven by a motor, the lower end of the stirring shaft extends into the stirring barrel, and a stirring disk is arranged on the stirring shaft located in the stirring barrel. When the material enters the stirring barrel, the stirring shaft starts to rotate driven by the motor, and this rotation itself will drive the material to rotate and mix, and the setting of the stirring disk effectively stirs the material rotating with the rotating shaft, intensifies the mixing of the dye and dispersant, and provides a prerequisite for subsequent uniform grinding. More preferably, the stirring disk is provided with multiple layers.
[0019] The present application is applied to the processing of color paste, the filter cake and the dispersant are first mixed evenly, and these mixtures are then used together to complete the entire coarse grinding and most of the fine grinding. In the material formed at this time, the dye is wrapped by the dispersant; when the comprehensive auxiliary agent is added for the remaining fine grinding, the dye is wrapped by the dispersant and the comprehensive auxiliary agent. The final color paste has a lower particle size and can be directly combined with the fiber during the dyeing process. It only contains the dispersant and the necessary amount of comprehensive auxiliary agents, has few impurities, and does not require water washing. Compared with the traditional process, at least two cleaning steps are saved, water and time are saved, water consumption is reduced by about 75%, and the dyeing time is reduced from 3 hours to half the time; when washing is used after dyeing, due to the high bonding strength between the dye and the fiber, the washing water can be self-circulated, and high COD and high-chroma printing and dyeing wastewater will not be generated. The repeated addition of auxiliary agents is also reduced in the recycling of washing water, the auxiliary agents are reduced, and the cost can be effectively controlled. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a flowchart of the application;
[0021] Figure 2 This is a diagram illustrating the principles of this application;
[0022] Figure 3 This is a diagram of one implementation device of the processing process of this application;
[0023] Figure 4 for Figure 3 Schematic diagram of the structure of the middle mixing zone;
[0024] Figure 5 for Figure 3 Schematic diagram of the structure of the medium and coarse grinding area;
[0025] Figure 6 A cross-sectional view of the present application;
[0026] Figure 7 It is a schematic diagram of the cross-sectional structure of the rotor in this application.
[0027] Numbers in the figure: 1. Mixing area; 11. Motor; 12. Drive belt; 13. Pulley; 14. Stirring shaft; 15. Stirring barrel; 16. Dispersing disc; 17. Ball valve; 18. Column; 2. Coarse grinding area; 21. Feed pipe; 211. Pressure gauge; 22. Water inlet pipe; 23. Water outlet pipe; 24. Funnel; 241. Seal; 25. Pneumatic diaphragm pump; 251. Oil-water separator; 26. Discharge valve; 27 .Discharge pipe; 271.Discharge base; 272.Thermometer; 28.Main base; 281.Operation panel; 29.Frame; 3.Fine grinding area; 31.Cylinder A; 32.Fine grinder; 33.Cylinder B; 3a.Main body; 3b.Gear; 3c.Groove; 3d.Shaft; 3e.Bead receiving bucket; 3f.Separator; 4.Storage area; 5.Inspection area; 6.Packing area; 7.Pump 1; 8.Comprehensive additive area; 9.Pump 2. DETAILED DESCRIPTION
[0028] Example 1
[0029] The present embodiment provides a color paste, the color paste particle size is less than 200nm, and includes a dye, a dispersant, water, and a comprehensive auxiliary agent for adjusting level dyeing and dyeing fastness. The dispersant contains less than 5% S, and its content is 3-10%; the dye content is 10-40%, the comprehensive auxiliary agent is 0-10%, and the rest is water.
[0030] As a typical example, the above color paste can adopt the following formula:
[0031] Formula 1: The color paste particle size is 150-200nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 3% and the dispersant content is 10%; the dye is Yabang 60 blue, the content of which is 40%, and the rest is water.
[0032] Formula 2: The color paste particle size is 150-200nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 2% and the dispersant content is 8%; the dye is Yabang 60 blue, the content of which is 33%, and the rest is water.
[0033] Formula 3: The color paste particle size is 150-200nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 3% and the dispersant content is 6.2%; the dye is Yabang 60 blue, the content of which is 28%, and the rest is water.
[0034] Formula 4: Color paste particle size 150-200nm; dispersant uses sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 3% and the dispersant content is 6.2%; dye uses Yabang 60 blue, its content is 30%, comprehensive auxiliary agent for adjusting level dyeing is 10%, and the rest is water.
[0035] Formula 5: The color paste particle size is 150-200nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 3% and the dispersant content is 6.2%; the dye is Yabang 60 blue, the content of which is 35%, the comprehensive auxiliary agent for adjusting the level dyeing is 13%, and the rest is water.
[0036] Formula 6: The color paste particle size is 100-150nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 2% and the dispersant content is 4.8%; the dye is Yabang 60 blue, the content of which is 25%, and the rest is water.
[0037] Formula seven: The color paste particle size is 100-150nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 2% and the dispersant content is 4%; the dye is Yabang 60 blue, the content of which is 22%, and the rest is water.
[0038] Formula 8: The color paste particle size is 100-150nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 2% and the dispersant content is 4%; the dye is Yabang 60 blue, the content of which is 22%, and the rest is water.
[0039] Formula nine: The color paste particle size is 100-150nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 3% and the dispersant content is 5%; the dye is Yabang 60 blue, the content of which is 34%, the comprehensive auxiliary agent for adjusting the dyeing fastness is 10%, and the rest is water.
[0040] Formula 10: Color paste particle size is 100-150nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 3% and the dispersant content is 6%; the dye is Yabang 60 blue, and its content is 37%, and the comprehensive auxiliary agent for adjusting both level dyeing and dyeing fastness is 15%, and the rest is water.
[0041] Formula 11: The color paste particle size is 50-100nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 3% and the dispersant content is 10%; the dye is Yabang 60 blue, the content of which is 40%, and the rest is water.
[0042] Formula 12: The color paste particle size is 50-100nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 2% and the dispersant content is 8%; the dye is Yabang 60 blue, the content of which is 38%, the comprehensive auxiliary agent for adjusting the dyeing fastness is 13%, and the rest is water.
[0043] Formula 13: The color paste particle size is 100-150nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 3% and the dispersant content is 3%; the dye is Yabang 60 blue, and its content is 10%, the comprehensive auxiliary agent for adjusting the levelness is 5%, and the rest is water.
[0044] Formula 14: Color paste particle size is 100-150nm; the dispersant is sodium lignin benzene sulfonate (Zhe Chuang, MF1#), in which the S content is 3% and the dispersant content is 5%; the dye is Yabang 60 blue, its content is 20%, the comprehensive auxiliary agent for adjusting the levelness and dyeing fastness is 10%, and the rest is water.
[0045] The present application uses dye, dispersant and comprehensive auxiliary agent as raw materials to form color paste. The particle size of the color paste is less than 200nm, which can be directly combined with the fiber during the dyeing process, reducing the addition of dyeing auxiliary agents, etc., avoiding floating color, effectively reducing the cleaning process and the residual amount of dye in the cleaning water, and realizing the self-circulation process of water, saving water and time; the S content in the dispersant is controlled to effectively reduce the COD of the treatment liquid.
[0046] In order to improve the problem of impurity content in the color paste, the above scheme can preferably adopt the following scheme for supplementary improvement: the dye is 60#, 72#, 30#, 288#, 56#, 93#, 79#, 167#, 153#, 114#, 291:1#, etc. in the disperse dye, and the dye comes from the filter cake (Longsheng, Yabang, Jihua, Runtu, Shanyu, Shengji, etc.). When the filter cake is used as the raw material, the filter cake is mixed with the dispersant for coarse grinding and a certain degree of fine grinding, and then the comprehensive additive is added for the last few fine grindings. The finished product is a pure color paste, which no longer contains any other impurities or catalytic components except the added dispersant and comprehensive additives.
[0047] When the above raw materials are processed into color paste, Figure 1, after mixing the dye and dispersant, coarsely grind and grind to a particle size of less than 10μm, and then transfer to fine grinding. The fine grinding temperature is 0-40℃ (preferably 11-17℃; for the convenience of control, the discharge temperature shall prevail), the processing time is 5-20h, and the line speed is 5-20m / s; before fine grinding and discharging, comprehensive additives are added as needed, and then transferred to storage, inspection, and packaging to obtain the finished color paste.
[0048] The raw and auxiliary materials used in this application mainly include three kinds: dye, dispersant and comprehensive additives that may be added later (non-essential ingredients, can be added as needed). The dye and dispersant in powder form are coarsely ground and finely ground to reduce the particle size step by step to ensure that the particle size of the formed color paste is below 200nm, and comprehensive additives are added as needed before fine grinding to meet the special requirements of different usage environments.
[0049] For full description, the forming process of the above color paste can be described as Figure 2 Form: The filter cake and the dispersant are first mixed evenly, and these mixtures are then used together to complete the entire coarse grinding and most of the fine grinding. In the material formed at this time, the dye is wrapped by the dispersant; when the comprehensive additives are added for the remaining fine grinding, the dye is wrapped by the dispersant and the comprehensive additives. The final color paste has a lower particle size and can be directly combined with the fiber during the dyeing process. It only contains dispersants and a necessary amount of comprehensive additives, has few impurities, and does not require water washing. Compared with the traditional process, at least two cleaning steps are saved, saving water and time, reducing water consumption by about 75%, and reducing the dyeing time from 3 hours to half the time; when washing after dyeing, due to the high bonding strength between the dye and the fiber, the washing water can be self-circulated, and no high COD and high-chroma printing and dyeing wastewater will be generated. The repeated addition of additives is also reduced in the recycling of washing water, the additives are reduced, and the cost can be effectively controlled.
[0050] The applicant has conducted further research on the dyeing of comprehensive additives with ink-like dyes, and achieved good results in terms of color paste stability, color paste safety and environmental protection: the comprehensive additive is compounded from N-methyl-2-pyrrolidone, urea, sodium dodecylbenzene sulfate and deionized water, and the mass percentages of each component are: N-methyl-2-pyrrolidone 10-30%, urea 5-10%, sodium dodecylbenzene sulfate 2-3% and deionized water 60-77%. When dyeing with this type of dye, the following formula of comprehensive auxiliary agent is particularly preferred: 22% N-methyl-2-pyrrolidone, 8% urea, 3% sodium dodecylbenzene sulfate and 67% deionized water; or, the ratio of the comprehensive auxiliary agent is: 30% N-methyl-2-pyrrolidone, 5% urea, 2% sodium dodecylbenzene sulfate and 63% deionized water; or, the ratio of the comprehensive auxiliary agent is: 10% N-methyl-2-pyrrolidone, 10% urea, 3% sodium dodecylbenzene sulfate and 77% deionized water. Among them, the molecular formula of N-methyl-2-pyrrolidone is C5H9NO, the molecular weight is 99.134, the boiling point is 202°C, and the flash point is 95°C; the deionized water is the water after the anion and cation exchange column, and the impurities have been removed. The comprehensive auxiliary agent, in combination with dyes and dispersants, can effectively improve the stability of the color paste at high and normal temperatures, and effectively avoid high-temperature steaming, boiling and cleaning of the treated objects such as fibers, fabrics or fabrics, and prevent the overflow and diffusion of dyes when they are sprayed onto fibers, fabrics or fabrics. In addition, during the production and processing, there is no pollution to the atmosphere and water quality, and no odor or harmful substances are emitted, and the energy-saving and environmental protection efficiency is high.
[0051] The applicant has conducted further research on the dyeing of the comprehensive auxiliary agent with the rotary screen or digital printing, and achieved good results in the stability, safety and environmental protection of the color paste: the comprehensive auxiliary agent is composed of urea, acetic acid, sodium bicarbonate, sodium sulfate, OP-10, and deionized water, and the mass percentages of each component are: urea 4-15%, acetic acid 0.5-2%, sodium bicarbonate 1.5-3%, sodium sulfate 0.5-2%, OP-100.5-2%, deionized water 82-87.5%. More preferably, the ratio of the comprehensive auxiliary agent is: urea 10%, acetic acid 1%, sodium bicarbonate 1.5%, sodium sulfate 1%, OP-10 1.5%, deionized water 85%; or, the ratio of the comprehensive auxiliary agent is: urea 4%, acetic acid 2%, sodium bicarbonate 3%, sodium sulfate 2%, OP-10 2%, deionized water 87%. Among them, the component of OP-10 is alkylphenol polyoxyethylene ether. This comprehensive auxiliary agent, combined with dyes and dispersants, has excellent leveling, wetting, emulsifying, diffusing and antistatic properties, which can effectively improve the stability of color paste at high and normal temperatures, and effectively avoid high-temperature steaming, boiling and cleaning of fibers, fabrics or fabrics, and prevent the overflow and diffusion of dyes when they are sprayed onto fibers, fabrics or fabrics. In addition, there is no pollution to the atmosphere and water quality during production and processing, and no odor or harmful substances are emitted, with high energy-saving and environmental protection efficiency.
[0052] On the basis of the above research, the applicant also studied the equipment used in the preparation of the color paste, and formed a set of color paste processing technology that matches it, which can be combined with Figure 3 The statement is as follows:
[0053] A color paste processing technology, after the dye and dispersant are mixed in the mixing area 1, they are sent to the coarse grinding area 2 by a pump 7 for coarse grinding, combined with Figure 5 , Figure 6 and Figure 7The coarse grinding zone 2 is provided with a rotor, a separator 3f, and grinding beads (which fall into the rotating groove 3c of the rotor), the gap of the separator 3f (the separator 3f can adopt a screen structure, in which case the gap refers to the aperture of the screen or the gap between adjacent screens) is 0.6-1.0mm, the rotation speed is 1500r / min, the linear speed is 11.5m / s, the diameter of the grinding beads is 1.5mm, and the particles are ground to a particle size of less than 10μm, and then transferred to the fine grinding zone 3 for fine grinding; the fine grinding zone 3 is provided with a rotor, a separator (the separator can adopt a screen structure, in which case the gap refers to the aperture of the screen or the gap between adjacent screens) or the gap between adjacent sieves) and grinding beads, the separator gap is less than 0.59mm (as a preferred case, the separator gap is 0.05-0.15mm), the grinding beads are PU beads or 95 and above zirconia beads, the diameter of the grinding beads is less than 0.4mm, and the comprehensive additives in the comprehensive additive area 8 are added through pump 29 to complete the fine grinding process. Ensure that the temperature of the fine grinding area 3 is 0-40℃, the processing time is 6-20h, and the line speed is 5-18m / s; the fine grinding output is transferred to the storage area 4, and the finished color paste is obtained after passing through the inspection area 5 and the packaging area 6.
[0054] The applicant has further studied the fine grinding on the basis of the above scheme to improve the quality of the color paste in terms of grinding fineness. Figure 3 The fine grinding area 3 includes a fine grinder 32, an A cylinder 31 and a B cylinder 33. The separator and the grinding beads are arranged in the fine grinder 32. The A cylinder 31 is provided with two inlets and one opening. One inlet is connected to the coarse grinding area 2, and the other inlet is connected to the comprehensive auxiliary agent area 8 through a pump 9; the opening is connected to the fine grinder 32, and the B cylinder 33 is provided with two openings, one opening is connected to the fine grinder 32, and the other opening is connected to the material storage area 4; the material discharged from the coarse grinding area 2 enters the A cylinder 31, and ... Figure 1, it is sent to the fine grinder 32 along the direction of the arrow through the A cylinder 31, and after grinding in the fine grinder 32, it is sent to the B cylinder 33 along the direction of the arrow, and after standing in the B cylinder 33, it is rotated back to the fine grinder 32 along the direction of the arrow, and then transferred to the B cylinder 33 along the direction of the arrow, and this reciprocating process is repeated until the penultimate grinding, and then it is transferred to the A cylinder 31 along the direction of the arrow through the fine grinder 32, and the pump 2 9 and the comprehensive auxiliary agent area 8 are turned on, and the comprehensive auxiliary agent is added as needed, and then it is transferred to the fine grinder 32 along the direction of the arrow for the last grinding, and sent to the storage area 4 through the B cylinder 33. Dye and dispersant are the main active ingredients in dyeing. In the present application, the two are first mixed and subjected to coarse grinding and (N-1) fine grinding, and then the entrance of cylinder A 31 and the comprehensive auxiliary agent area 8 are opened, and the necessary amount of comprehensive auxiliary agent is added to the dye and dispersant that have been finely ground (N-1) times, and then transferred to the fine grinder 32. After the last fine grinding (i.e., the Nth fine grinding) is completed, the material is sent to the storage area 4 by cylinder B 33. The above-mentioned materials are reciprocated in cylinder A 31, fine grinder 32 and cylinder B 33 to form an internal circulation fine grinding, and different cycles are realized for different materials, which not only makes full use of the grinding process, but also avoids excessive grinding of other materials that do not need too much grinding, thereby improving the grinding fineness.
[0055] For ease of use, the fine grinder 32 and the coarse grinding zone 2 can be set to have the same structure. Considering the different functions of the two, the specifications of the specific rotor, grinding beads, and separator are specifically set; taking the coarse grinding zone 2 as an example, combined with Figure 5 The coarse grinding area 2 mainly includes a main base 28 and a frame 29. The main base 28 is located on the frame 29, and an operation panel 281 is arranged on the main base 28; the coarse grinding chamber is arranged in the main base 28, and the rotor, the separator 3f and the grinding beads are arranged in the main base 28. One end of the feed pipe 21 is connected to the pneumatic diaphragm pump 25, and the pneumatic diaphragm pump 25 is connected to the pump 7 (if it is a fine grinder, it is connected to the A cylinder through the pneumatic diaphragm pump), and the other end is connected to the grinding chamber in the main base 28; a funnel 24 is arranged on the top of the main base 28, and the funnel 24 provides lubricating oil to the rotor and forms a lubricating oil at the end of the rotor. A seal 241 is connected to the grinding chamber with a temperature gauge 272 and a pressure gauge 211, which are respectively connected to an operating panel 281. The temperature and pressure in the grinding chamber are monitored through the operating panel 281 to ensure that grinding is carried out under appropriate conditions. A discharge valve 26 and a discharge pipe 27 are set at the bottom of the main frame 28. When used as a coarse grinding area 2, the discharge valve 26 and the discharge pipe 27 are connected to the fine grinding area 3 (the A cylinder 31 in the middle) by selecting one (preferably the discharge pipe 27); when used as a fine grinder, the discharge valve 26 is connected to the A cylinder 31, and the discharge pipe 27 is connected to the B cylinder.
[0056] The present application has also done further work on the cooling in the above scheme to avoid high temperature polymerization caused by grinding: a cooling water pipe is set on the outer wall of the fine grinder 32, and the cooling water pipe uses 0-30°C cooling water or (-25-15°C) cooling liquid as a cooling medium to cool and keep the fine grinder warm; Figure 5 For example, the outer wall of the main base 28 is equipped with an inlet pipe 22 and an outlet pipe 23 as cooling water pipes, and cooling water or coolant passes through the inlet pipe 22 and the outlet pipe 23 to cool the grinding chamber. As the grinding proceeds, high-speed grinding friction will generate a certain amount of heat, which gradually accumulates in a fixed space, causing the temperature of the entire grinding chamber and the material in the grinding chamber to rise, and dyes and dispersants will produce high-temperature polymerization under high temperature conditions, which not only affects the utilization rate of raw materials (referring to dyes, dispersants and necessary amounts of comprehensive additives, the same below), but also forms raw material impurities, affecting the molding effect of the color paste. The present application controls the temperature of the fine grinding zone, and preferably uses cooling water or coolant to control the temperature of the fine grinding zone, especially the fine grinder, at 0-40°C, which will not affect the normal function of the raw materials and avoid excessive energy consumption.
[0057] This application has done further work on the rotor in the above scheme to ensure fast material flow: combined with Figure 6 The rotor includes a body 3a, a rotating shaft 3d, rotating teeth 3b and a rotating groove 3c. The rotating shaft 3d is driven to rotate by a power source (not shown in the figure, a motor or the like can be used as a power source). The rotating shaft 3d is fixedly connected to the body 3a. The outer wall of the body 3a is provided with rotating teeth 3b. The cross section of the rotating teeth 3b is trapezoidal. The grooves between adjacent rotating teeth 3b and the outer wall of the body 3a form a rotating groove 3c. The grinding beads fall into the rotating groove 3c and cooperate with it to complete the grinding. When the rotating shaft 3d drives the body 3a to rotate, the rotating teeth 3b rotate accordingly. The trapezoidal cross-sectional shape of the rotating teeth 3b, which is large on the outside (referring to the side away from the body 3a) and small on the inside (referring to the side close to the body 3a), effectively drives the material to rotate accordingly, and makes the material form a vortex between the rotating grooves 3c, thereby effectively improving the grinding efficiency.
[0058] To ensure sufficient grinding, the present application also improves the mixing zone to improve the mixing uniformity of the dye and dispersant: Figure 4, the mixing zone 1 includes a mixing barrel 15, a mixing shaft 14 and a mixing disk 16. The motor 11 is located on the column 18. The output end of the motor 11 is connected to the pulley 13 of the rotating shaft 14 by a transmission belt 12. The motor 11 rotates, and the power is transmitted to the mixing shaft 14 through the transmission belt 12, and the mixing shaft 14 is driven to rotate. The lower end of the mixing shaft 14 extends into the mixing barrel 15, and a mixing disk 16 is set on the mixing shaft 14 located in the mixing barrel 15 (the mixing disk 16 can be set in one layer or multiple layers). When the material enters the mixing barrel 15, the mixing shaft 14 starts to rotate under the drive of the motor 11 (which is different from the coarse grinding zone and the fine grinding zone). This rotation itself will drive the material to rotate and mix, and the setting of the mixing disk 16 effectively stirs the material rotating with the rotating shaft, intensifies the mixing of the dye and the dispersant, and provides a prerequisite for subsequent uniform grinding. After the grinding is completed, the ball valve 17 is opened, and the mixed material can be transferred to the coarse grinding zone 2.
[0059] The above color paste was tested, and the solid content of the color paste was 13.25% (no-wash sample, 180kg). The particle fineness of the color paste has reached the nanometer level, and there is no need to add too much dispersing and dissolving auxiliaries such as diffusers and abrasives, so its dyeing rate is much higher than that of conventional dyes (such as commercially available disperse orange S-4RL, disperse red GS, disperse dark blue H-GL, disperse black ECT, etc.); the "foot water" after dyeing is relatively clear, without too much residue, except for the special dark color, basically no reduction cleaning is required, which can save reduction cleaning and post-washing process, which has a very significant effect on reducing the water consumption of dyeing, saving 3 water steps, saving the use of insurance powder, alkali or reduction cleaning agent 80℃×30 minutes reduction cleaning and post-acid neutralization and washing process.
[0060] During the stability test, the suspension system is stable and will not form film or agglomerate during long-term storage. This can prevent quality problems such as color spots and color spots caused by poor material cutting of powder dyes. It can be directly poured into the yarn dyeing tank and dyed with water, which can reduce the material cutting time and effectively improve production efficiency.
[0061] The fabric dyed with the color paste in this case was tested (testing standards: GB / T 21295-2014 "Technical requirements for physical and chemical properties of clothing", GB 18401-2010 "National Basic Safety Technical Specifications for Textile Products" B-type textile products in direct contact with the skin), and the color fastness to washing, color fastness to rubbing, color fastness to perspiration, and color fastness to light all met the requirements of the corresponding standards (report number GZHT02021837). Specific test results are shown in Tables 1 to 4.
[0062] Table 1 Summary of product washing color fastness test results
[0063]
[0064] Table 2 Summary of product abrasion fastness test results
[0065]
[0066] Table 3 Summary of product perspiration fastness test results
[0067]
[0068]
[0069] Table 4 Summary of product light fastness test results
[0070]
Claims
1. A color paste, characterized in that: The color paste has a particle size of less than 200 nm and includes a dye, a dispersant, water, and a comprehensive auxiliary agent for adjusting level dyeing and dyeing fastness. The dispersant contains less than 5% S, and its content is 3-10%; the dye content is 10-40%, the comprehensive auxiliary agent is 0-10%, and the rest is water. The dye is a disperse dye, The ratio of the comprehensive auxiliary agent is: 22% N-methyl-2-pyrrolidone, 8% urea, 3% sodium dodecylbenzene sulfate and 67% deionized water; or, the ratio of the comprehensive auxiliary agent is: 30% N-methyl-2-pyrrolidone, 5% urea, 2% sodium dodecylbenzene sulfate and 63% deionized water; or, the ratio of the comprehensive auxiliary agent is: 10% N-methyl-2-pyrrolidone, 10% urea, 3% sodium dodecylbenzene sulfate and 77% deionized water, The filter cake is used as the dye, and the dye and dispersant are mixed in the mixing area and then sent to the coarse grinding area for coarse grinding. The coarse grinding area is equipped with a separator and grinding beads. The separator gap is 0.5-1.5mm, the linear speed is 10-15m / s, and the diameter of the grinding beads is 0.8-2mm. The particles are ground to a particle size of less than 10μm and then transferred to the fine grinding area for fine grinding. The fine grinding area is equipped with a rotor, a separator and grinding beads. The separator gap is less than 0.59mm. The grinding beads are PU beads or 95 and above zirconium oxide beads, and the diameter of the grinding beads is less than 0.4mm. When the comprehensive additives are added to complete the fine grinding, the temperature of the fine grinding area is 0-40℃, the processing time is 5-20h, and the linear speed is 5-20m / s. The comprehensive additives are added as needed before the fine grinding is discharged, and then the material is transferred to the storage area. After passing through the inspection area and the packaging area, it is the finished color paste. The fine grinding area includes a fine grinder, an A cylinder and a B cylinder. The separator and the grinding beads are arranged in the fine grinder. The A cylinder is provided with two inlets and one opening, one of which is connected to the coarse grinding area, and the other is connected to the comprehensive additive area; the opening is connected to the fine grinder, and the B cylinder is provided with two openings, one of which is connected to the fine grinder, and the other is connected to the storage area; the material discharged from the coarse grinding area enters the A cylinder, is sent to the fine grinder through the A cylinder, and after the grinding is completed in the fine grinder, it is sent to the B cylinder. After standing in the B cylinder, it is rotated to the fine grinder, and then transferred to the B cylinder. This reciprocating process is repeated until the penultimate grinding, and then it is transferred to the A cylinder through the fine grinder, the comprehensive additive area is opened, and the comprehensive additive is added as needed, and then it is transferred to the fine grinder for the last grinding, and then it is sent to the storage area through the B cylinder. A cooling water pipe is arranged on the outer wall of the fine grinder, and the cooling water pipe uses cooling water at 0-30°C or cooling liquid at -25-15°C as a cooling medium.
2. A color paste according to claim 1, characterized in that: The ratio of the comprehensive additive is: urea 10%, acetic acid 1%, sodium bicarbonate 1.5%, sodium sulfate 1%, OP-10 1.5%, and deionized water 85%; or, the ratio of the comprehensive additive is: urea 4%, acetic acid 2%, sodium bicarbonate 3%, sodium sulfate 2%, OP-10 2%, and deionized water 87%.
Citation Information
Patent Citations
Efficient energy-saving reactive printing process
CN105088822A
Preparation method and dyeing method of liquid disperse dye composition
CN106380893A
Ultrafine disperse dye black color paste and preparation method thereof
CN106752392A