Preparation method of cellulose acetate based hybrid membrane
A technology of cellulose acetate and silver nitrate, applied in chemical instruments and methods, special treatment targets, water/sludge/sewage treatment, etc., can solve the problem of poor mechanical properties, lack of practical value, and poor mechanical properties of pure silk fibroin solution and other problems, to achieve the effect of excellent antibacterial effect, low equipment requirements and good stability
Patent Information
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Publication Date
- 2019-01-04
Smart Images

Figure 1 
Figure 2
Abstract
Description
technical field
[0001] The invention belongs to the technical field of nanomaterial synthesis, and in particular relates to a preparation method of a cellulose acetate-based hybrid membrane. Background technique
[0002] Since the 1970s, continuous environmental pollution and energy shortages have aroused people's concerns about global crises, especially the increasingly prominent problem of water pollution, which has seriously affected the sustainable development of human society and caused various health and Safety issues, sewage treatment is imminent. At present, the commonly used methods for removing harmful substances from sewage include coagulation method, acid analysis method, biochemical method, liquid membrane separation method, granular activated carbon method, etc., but the effect is not satisfactory and it is difficult to apply it alone. Therefore, it is very necessary to develop new and practical environmental protection treatment technology.
[0003] In recen...
Examples
Embodiment 1
[0044] One of the embodiments of the preparation method of a cellulose acetate-based hybrid membrane of the present invention comprises the following steps:
[0045] (1) Preparation of cellulose acetate solution: Weigh 9g of cellulose acetate particles and 90g of N,N-dimethylformamide in the ratio of 1:10 to add cellulose acetate and N,N-dimethylformamide to the reaction In the container, stir at a constant temperature at 25°C for 8 hours, and after the cellulose acetate particles are completely dissolved, a cellulose acetate solution with a mass fraction of 9.1% is obtained;
[0046] (2) Prepare the mixed solution: add silk fibroin powder with a particle size of 5 μm and a solid content of 62% to the above cellulose acetate solution, stir with a high-speed stirrer for 30 minutes, and then let it stand for 30 minutes to defoam, to obtain mixed solution;
[0047] (3) Preparation of cellulose acetate / silk fibroin hybrid film: Coat the mixed solution on a release paper with a th...
Embodiment 2
[0052] One of the embodiments of the preparation method of a cellulose acetate-based hybrid membrane of the present invention comprises the following steps:
[0053] (1) Preparation of cellulose acetate solution: Weigh 8g of cellulose acetate particles and 80g of N,N-dimethylacetamide into the reaction according to the ratio of 1:8 of cellulose acetate and N,N-dimethylacetamide In the container, heat and stir at 40°C for 8 hours. After the cellulose acetate particles are completely dissolved, a cellulose acetate solution with a mass fraction of 11.1% is obtained;
[0054] (2) Prepare the mixed solution: add silk fibroin powder with a particle size of 5 μm and a solid content of 65% to the above cellulose acetate solution, and then use a high-speed stirrer to stir for 30 minutes to obtain a well-mixed organic-inorganic mixture solution, left to defoam for 30 minutes to obtain a mixed solution;
[0055] (3) Preparation of cellulose acetate / silk fibroin hybrid film: Coat the mix...
Embodiment 3
[0060] One of the embodiments of the preparation method of a cellulose acetate-based hybrid membrane of the present invention comprises the following steps:
[0061] (1) Preparation of cellulose acetate solution: Weigh 10g of cellulose acetate particles and 65g of N,N-dimethylformamide into the reaction In the container, heat and stir at 45°C for 8 hours. After the cellulose acetate particles are completely dissolved, a cellulose acetate solution with a mass fraction of 13.3% is obtained;
[0062] (2) Prepare the mixed solution: add silk fibroin powder with a particle size of 5 μm and a solid content of 70% to the above cellulose acetate solution, and then use a high-speed stirrer to stir for 30 minutes to obtain a well-mixed organic-inorganic mixture solution, left to defoam for 30 minutes to obtain a mixed solution;
[0063] (3) Preparation of cellulose acetate / silk fibroin hybrid film: Coat the mixed solution on a release paper with a thickness of 0.05 mm, and quickly imme...