Coating composition

By using polymer dispersants with anti-agglomeration functional groups to disperse inorganic particles in water-based coating compositions, the colloidal stability problem caused by the reaction between conventional acrylic polymers and epoxy resins is solved, and the stability and mixing difficulty of the coatings are improved. Improvement ensures the viscosity stability of the coating under thermal aging conditions.

CN109983090BActive Publication Date: 2024-10-18DOW GLOBAL TECHNOLOGIES LLC +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201680090213.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2016-11-02
Publication Date
2024-10-18
Estimated Expiration
2036-11-02

AI Technical Summary

Technical Problem

In water-based coating compositions, conventional acrylic polymer dispersants react with epoxy resins causing colloidal stability issues, increasing the difficulty of mixing the two parts and the risk of condensation of the coating.

Method used

The inorganic particles are dispersed in the water-based epoxy resin dispersion using a polymer dispersant containing anti-agglomeration functional groups to avoid reaction with the epoxy resin and added separately from the hardener to stabilize the components.

Benefits of technology

The stability of the inorganic particles in the water-based coating composition is improved, the risk of coating condensation is reduced, the mixing process is simplified, and good viscosity stability is maintained under thermal aging conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002032151090000041
    Figure BDA0002032151090000041
  • Figure BDA0002032151090000081
    Figure BDA0002032151090000081
  • Figure BDA0002032151090000111
    Figure BDA0002032151090000111
Patent Text Reader

Abstract

A water-based coating composition comprises two parts (Part A and Part B), (A) a binder component comprising an aqueous epoxy resin dispersion and dispersed inorganic particles with a polymer dispersant, and (B) a hardener component. The polymer dispersant contains an anti-agglomeration functional group that does not react with the oxirane group of the epoxy resin dispersion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to a water-based coating composition with improved storage stability. In particular, the present invention relates to a water-based coating composition consisting of two parts (Part A and Part B). Part A comprises an aqueous epoxy resin dispersion having dispersed inorganic particles containing a polymeric dispersant, while Part B comprises a hardener. The polymeric dispersant comprises an anti-agglomeration functional group that does not react with the oxirane groups of the epoxy resin dispersion. Background Art

[0002] Water-based coating compositions are used to form coatings for buildings or structures because they reduce the impact on the environment. Aqueous epoxy adhesive systems are referred to as water-based coating compositions, which form coatings with good properties (such as excellent chemical resistance and corrosion resistance). In the first generation of such aqueous epoxy adhesive systems, liquid epoxy resins were used as epoxy adhesives. The coating compositions of the first generation aqueous epoxy adhesive systems typically contain external emulsifiers to help the epoxy adhesive to be dispersed in the coating composition.

[0003] In the second generation of waterborne epoxy adhesive systems, solid epoxy resins are used instead of liquid epoxy resins. In a further innovation, a coating composition comprising an aqueous dispersion of acrylic polymer particles imbibed with a waterborne epoxy resin (acrylic / epoxy hybrid dispersion) was developed and disclosed in US2012 / 0301621A. In the acrylic / epoxy hybrid dispersion, the waterborne epoxy resin is absorbed in an acrylic polymer having anti-agglomeration functional groups. US2012 / 0301621A discloses that the concentration of anti-agglomeration functional groups in the acrylic polymer is sufficient to stabilize the epoxy resin under heat aging conditions.

[0004] Typically, epoxy coating compositions are formed from two different components (parts). The two components are mixed just before applying the coating composition to prevent the coating composition from coagulating (two-component system). Typically, the first component (Part A) includes most of the ingredients of the coating composition, while the second component (Part B) includes a hardener. Part B is added to Part A and mixed thoroughly with Part A just before applying the coating composition on the material.

[0005] When inorganic particles (such as pigments) are added to the coating composition, the inorganic particles are dispersed (grinded) in the coating composition using a dispersant. However, when the inorganic particles are ground using a conventional acrylic polymer dispersant in Part A, there is a colloidal stability problem in Part A because the acrylic acid carboxylate group of the acrylic polymer dispersant reacts with the oxirane group of the epoxy resin. Therefore, an inorganic material and a dispersant must be added to Part B, but since the amount of Part B is increased by adding the inorganic material and the dispersant, the difficulty of mixing the two parts is increased. Summary of the invention

[0006] The present invention successfully solves the stability problem when an inorganic material is added to part A. In one embodiment of the present invention, the present invention relates to a coating composition comprising components (A) and (B); wherein component (A) comprises (a) an aqueous epoxy resin dispersion, (b) a polymer dispersant and (c) inorganic particles, and component (B) comprises a curing agent, wherein the polymer dispersant is a polymer comprising an anti-agglomeration functional group. DETAILED DESCRIPTION

[0007] The water-based coating composition of the present invention is formed of two parts - Part A and Part B. Part A is a binder phase and comprises (a) an aqueous epoxy resin dispersion, (b) a polymer dispersant and (c) inorganic particles, wherein the inorganic particles are dispersed in Part A through a polymer dispersant, the polymer dispersant comprising an anti-agglomeration functional group that does not react with the oxirane group of the epoxy resin dispersion. Part B is a hardener phase and comprises a hardener (curing agent).

[0008] (A)-(a) Waterborne epoxy resin dispersion

[0009] Aqueous epoxy resins are water-based epoxy resins and are dispersed / emulsified in water. In this application, aqueous epoxy resin dispersions are also referred to as aqueous epoxy resins. Examples of aqueous epoxy resins include, but are not limited to, diglycidyl ether of bisphenol A, diglycidyl ether of bisphenol F, 1,4-butanediol diglycidyl ether, 1,6-hexanediol diglycidyl ether, diglycidyl ester of phthalic acid, 1,4-cyclohexane methanol diglycidyl ether, 1,3-cyclohexane methanol diglycidyl ether, hexahydrophthalic acid diglycidyl ester, and novolac resins. Two or more aqueous epoxy resins in the form of a mixture may be used. Such aqueous epoxy resins are mixed in water and form a dispersion. Commercially available aqueous epoxy resin dispersions are OUDRASPERSE provided by Olin Corporation TM WB-6001.

[0010] Waterborne epoxy resins can also be absorbed into acrylic polymer particles to form aqueous dispersions with multiphase polymer particles. US2012 / 0301621A describes absorbed waterborne epoxy resins. Commercially available waterborne epoxy resin dispersions absorbed with acrylic polymer particles are MAINCOTE® provided by DOW Chemical. TM AEH-20.

[0011] The amount of the aqueous epoxy resin dispersion is 10 wt % to 75 wt % based on the total dry weight of Part A. The amount of the aqueous epoxy resin dispersion is preferably 15 wt % or more, more preferably 20 wt % or more, based on the total dry weight of Part A. The amount of the aqueous dispersion is preferably 70 wt % or less, more preferably 60 wt % or less, based on the total dry weight of Part A.

[0012] (A)-(b) Polymer dispersants

[0013] Polymer dispersants are polymers having anti-agglomeration functional groups. Anti-agglomeration functional groups refer to hydrophilic groups that do not react sufficiently with ethylene oxide groups. Typically, such polymers are formed by polymerizing a monomer composition containing monomers having anti-agglomeration functional groups, although it is also possible to synthesize such polymers by graft polymerization.

[0014] In certain embodiments of the present invention, the polymer dispersant is formed by polymerizing a monomer composition comprising: i) a monomer having an anti-agglomeration functional group, ii) an α,β-ethylenically unsaturated carboxylic acid monomer, and iii) an α,β-ethylenically unsaturated nonionic monomer.

[0015] Examples of monomers having anti-agglomeration functional groups include, but are not limited to, acrylamide, methyl methacrylate phosphoethyl ester, sodium styrene sulfonate, and acrylamide-methyl propane sulfonate. The corresponding anti-agglomeration functional groups formed by these monomers are shown below:

[0016]

[0017] The dotted line refers to the connection point of the anti-agglomeration functional monomer to the polymer. The amount of the monomer containing the anti-agglomeration functional group is preferably 5% or more, more preferably 10% or more, and most preferably 15% or more, based on the dry weight of the polymer dispersant. The amount of the monomer containing the anti-agglomeration functional group is 80% or less, more preferably 75% or less, and most preferably 70% or less, based on the dry weight of the polymer dispersant.

[0018] Examples of suitable α,β-ethylenically unsaturated carboxylic acid monomers include, but are not limited to, monoacids (such as acrylic acid, methacrylic acid, crotonic acid, and acyloxypropionic acid); and diacid monomers (such as maleic acid, fumaric acid, and itaconic acid). The amount of the α,β-ethylenically unsaturated carboxylic acid monomer is preferably 0% or more, more preferably 0.1% or more, and most preferably 1% or more, based on the dry weight of the polymer dispersant. At the same time, the amount of the α,β-ethylenically unsaturated carboxylic acid monomer is preferably 10% or less, more preferably 8% or less, and most preferably 5% or less, based on the dry weight of the polymer dispersant.

[0019] Examples of suitable α,β-ethylenically unsaturated nonionic monomers include, but are not limited to, methyl acrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, decyl acrylate, lauryl acrylate, methyl methacrylate, butyl methacrylate, isodecyl methacrylate, lauryl methacrylate, hydroxyethyl (meth)acrylate, and hydroxypropyl (meth)acrylate; methacrylonitrile; ethacrylonitrile; styrene and substituted styrenes; butadiene; ethylene, propylene, α-olefins (such as 1-decene); vinyl acetate, vinyl butyrate, versatate and other vinyl esters; and vinyl monomers (such as vinyl chloride and vinylidene chloride). Preferred examples are butyl acrylate, butyl methacrylate, methyl methacrylate, 2-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl (meth)acrylate, styrene, and mixtures thereof. The amount of α,β-ethylenically unsaturated nonionic monomers is preferably 10% or more, more preferably 17% or more, and most preferably 30% or more, based on the dry weight of the polymer dispersant. The amount of α,β-ethylenically unsaturated nonionic monomer is preferably 95% or less, more preferably 90% or less, and most preferably 85% or less, based on the dry weight of the polymeric dispersant.

[0020] The method of forming the polymeric dispersant depends on the type of monomer used to form the polymeric dispersant and is understood by those skilled in the art, but includes solution polymerization and emulsion polymerization.

[0021] Preferably, the polymeric dispersant has a weight average molecular weight of 300 to 50,000 Daltons. More preferably, the weight average molecular weight is 500 to 40,000 Daltons.

[0022] The amount of polymeric dispersant is 0.01% to 5% based on the total dry weight of Part A. The amount of polymeric dispersant is preferably 0.015% or more, more preferably 0.02% or more, based on the total dry weight of Part A. The amount of polymeric dispersant is preferably 4% or less, more preferably 3% or less, based on the total dry weight of Part A.

[0023] (A)-(c) Inorganic particles

[0024] Part A comprises inorganic particles dispersed in Part A by the polymer dispersant disclosed above.

[0025] These inorganic particles may contain pigments, extenders and fillers. Examples of inorganic particles include, but are not limited to, metal oxides (such as titanium oxide, aluminum oxide, zinc oxide, silicon oxide and iron oxide), metal phosphates (such as zinc phosphate and aluminum phosphate, barium sulfate), metal carbonates (such as calcium carbonate, carbon black, talc, clay, feldspar and lime).

[0026] Extenders are particulate inorganic materials with a refractive index (RI) less than or equal to 1.8 and greater than 1.3. Examples of extenders include, but are not limited to, calcium carbonate, clay, calcium sulfate, aluminosilicates, silicates, zeolites, mica, diatomaceous earth, solid or hollow glass, and ceramic beads.

[0027] The amount of inorganic particles is 20% to 85% based on the total dry weight of Part A. The amount of inorganic particles is preferably 25% or more, more preferably 30% or more, based on the total dry weight of Part A. The amount of inorganic particles is preferably 80% or less, more preferably 75% or less.

[0028] (A)-(d) Other ingredients

[0029] Part A may optionally include other ingredients such as water, wetting agents, defoamers, adhesion promoters, solvents, and thickeners. Examples of wetting agents include, but are not limited to, Tego Twin 4100 wetting agent, TRITON TM CF-10 surfactant and ECOSURF TM LF-45 surfactant.

[0030] Examples of defoamers include, but are not limited to, Tego 902W defoamer, Tego 1488 texturizing agent, BYK-024 texturizing agent, and BYK-019 texturizing agent. Examples of adhesion promoters include, but are not limited to, DOW CORNING TM Z-6040 Silane and DOWCORNING TM Z-6011 silane. Examples of solvents include, but are not limited to, DOWANOL DPnB glycol ether, DOWANOL PM propylene glycol methyl ether, and Texanol ester alcohol. Examples of thickeners include, but are not limited to, PRIMAL TM RM-8W acrylic adhesive, PRIMAL TM RM-12W rheology modifier and Bentone LT additive.

[0031] Part A can be formulated using a bench top overhead mixer. Part A can be prepared by first grinding the pigment and extender with a polymer dispersant under high speed dispersion. During the decompression stage, the epoxy resin dispersion and other ingredients are added to the pigment grind under low speed agitation.

[0032] (B) Hardener phase

[0033] Part B is a hardener phase that is mixed with Part A prior to applying the coating composition. Part B includes a hardener (i.e., a curing agent) to cure the coating composition. Examples of such hardeners include, but are not limited to, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-methylhexamethylenediamine, 1,6-hexanediamine, 1-ethyl-1,3-propylenediamine, bis(3-aminopropyl)piperazine, N-aminoethylpiperazine, bis(3-aminopropyl)ethylenediamine, 2,4-toluenediamine, 2,6-toluenediamine, 1,2-diaminocyclohexane, 1,4-diamino-3,6-diethylcyclohexane, 1,2-diamino-4-ethylcyclohexane, 1,4-diamino-3,6-diethyl Cyclohexane, 1-cyclohexyl-3,4-diaminocyclohexane, isophorone-diamine, norbornyl diphenylamine, 4,4-diaminodicyclohexylmethane, 4,4-diaminodicyclohexylmethane, 4,4-diaminodicyclohexylpropane, 2,2-bis(4-aminocyclohexyl)propane, 3,3-dimethyl-4,4'-diaminodicyclohexylmethane, 3-amino-1-cyclohexane-amino-propane, 1,3- and 1,4-bis(aminomethyl)cyclohexane, m-phenylenediamine, p-phenylenediamine, polyoxypropylenediamine, polyamidoamines and aminoplast resins formed by reaction of ureas and melamines with aldehydes.

[0034] Commercially available hardeners include Epi-cure 8535, 8536, 8537, 8290 and 8292 curing agents provided by Hexion; Anquamine 401 and Epilink 381 curing agents provided by Air Products; Beckopox EH659W, EH623W and VEH2133W curing agents provided by Allnex; and Epotuf 37-680 and 37-681 curing agents provided by Reothold.

[0035] Part B may optionally include other ingredients (such as water, solvents, defoamers, and thickeners), which are also listed in Part A.

[0036] Part A and Part B are mixed together and the coating is ready for application. The ratio of Part A to Part B in the coating composition is 90:1 to 2:1, preferably 15:1 to 4:1 (by weight).

[0037] The solids content of the coating composition is preferably from 20 to 70% by weight, more preferably from 30 to 65% by weight, most preferably from 40 to 60% by weight.

[0038] Examples

[0039] 1. Raw materials

[0040] The raw materials used in the examples are listed in Table 1.

[0041] Table 1. Raw materials

[0042]

[0043] 2. Testing process

[0044] 1. Viscosity stability

[0045] The KU viscosity of the coating composition was analyzed using a Stormer viscometer according to the method of ASTM (American Society for Testing and Materials) D562. After forming the coating composition, the initial medium shear viscosity and initial KU of the coating composition were analyzed at room temperature, and then the coating composition was placed in an oven at 50°C for 7 days. The viscosity of the coating composition after storage was analyzed and recorded as the final KU. The difference between the initial KU and the final KU is defined as the heat aging viscosity change ΔKU. The smaller the ΔKU value, the better the viscosity stability.

[0046] 3. Experimental Examples

[0047] 1. Preparation of polymer dispersants (dispersants 1 to 4)

[0048] Dispersant 1 (Comparative Example):

[0049] 750g water and 6.35g Disponil Fes-32 surfactant provided by BASF were added to a 5-liter five-necked flask equipped with a mechanical stirrer, N2 purge, thermocouple and condenser. The solution was heated to 86°C. 2.10g sodium persulfate (SPS) dissolved in 30g water was added to the solution. Two minutes later, a monomer emulsion containing 419.36g deionized water, 60.87g Disponil Fes-32 surfactant, 50.00g ethyl acrylate, 600.00g 2-ethylhexyl acrylate, 350.00g methacrylic acid (MAA) and 19.40g 3-mercaptopropionic acid methyl ester (MMP) was added to the solution. At the same time, an initiator solution containing 1.75g ​​SPS and 90.8g water was added together within 90 minutes, while the temperature of the solution was maintained at about 86°C, and maintained for 5 minutes after the feeding was completed. After the solution was cooled to 60°C, the additive system included: 7.5g of ferrous sulfate solution (0.2%, aq) and 1.18g of tert-butyl hydroperoxide (t-BHP) solution in 20g of water, and 0.58g of isoascorbic acid (IAA) solution in 20g of water. After keeping for 15 minutes, the same additive system was filled again. The solution was cooled to 40°C and dilution water was added. Finally, the resultant was filtered through a 325 mesh screen to obtain a copolymer emulsion with a total solids content of 40%. The weight average molecular weight (Mw) of dispersant 1 is about 15,000 Daltons. Mw was measured by gel permeation chromatography.

[0050] Dispersant 2:

[0051] 420g water and 1.95g Disponil Fes-993 surfactant were added to a 3-liter five-necked flask equipped with a mechanical stirrer, N2 purge, thermocouple and condenser. The solution was heated to 86°C. An initiator of 0.65g sodium persulfate (SPS) dissolved in 5g water was added to the solution. Two minutes later, a monomer emulsion containing 130.00g deionized water, 18.30g Disponil Fes-993 surfactant, 210.00g butyl methacrylate (BMA), 15.00g methacrylic acid (MAA), 75.00g methacrylic acid ethyl phosphate (PEM), and 12.87g n-dodecyl mercaptan was added to the solution. At the same time, an initiator solution containing 0.53g SPS and 60g water was added together over a period of 90 minutes, while the temperature of the solution was maintained at about 86°C, and maintained for 5 minutes after the feeding was completed. After cooling to 60°C, a chaser system including 4g of ferrous sulfate solution (0.2%, aq) and 1.18g of tert-butyl hydroperoxide (t-BHP) solution in 5g of water, and 0.58g of isoascorbic acid (IAA) solution in 5g of water was added to the solution. After holding for 15 minutes, the same chaser system was filled again. The solution was cooled to 40°C and dilution water was added to the solution. Finally, the resultant was filtered through a 325 mesh screen to obtain a copolymer emulsion with a total solids content of 30%. The Mw of dispersant 2 was about 10,900 Daltons.

[0052] Dispersant 3:

[0053] 420g of water and 1.95g of Disponil Fes-993 surfactant were added to a 3-liter five-necked flask equipped with a mechanical stirrer, N2 purge, thermocouple and condenser. The solution was heated to 86°C. An initiator of 0.65g of sodium persulfate (SPS) dissolved in 5g of water was added to the solution. Two minutes later, a monomer emulsion containing 130.00g of deionized water, 18.30g of Disponil Fes-993 surfactant, 225.00g of butyl methacrylate (BMA), 75.00g of ethyl methacrylate (PEM) and 12.87g of n-dodecyl mercaptan was added to the solution. At the same time, an initiator solution containing 0.53g of SPS and 60g of water was added together over a period of 90 minutes, while the temperature of the solution was maintained at about 86°C, and maintained for 5 minutes after the feeding was completed. After cooling to 60°C, a chaser system comprising 4 g of ferrous sulfate solution (0.2%, aq) in 5 g of water and 1.18 g of tert-butyl hydroperoxide (t-BHP) solution and 0.58 g of isoascorbic acid (IAA) solution in 5 g of water was added to the solution. After holding for 15 minutes, the same chaser system was filled again. The solution was cooled to 40°C and dilution water was added. Finally, the resultant was filtered through a 325 mesh screen to obtain a copolymer emulsion with a total solids content of 30%.

[0054] Dispersant 2 and Dispersant 3 can also be synthesized by a solvent solution polymerization process. The process consists of solvent gradual addition thermal polymerization in propylene glycol in the presence of 2-mercaptoethanol and tert-butyl hydroperoxide. The Mw of Dispersant 3 is about 11,000 Daltons.

[0055] Dispersant 4

[0056] 600g of distilled water was added to a three-necked flask equipped with a condenser, a magnetic stirring bar and a thermocouple. 252g of 2-acrylamido-2-methylpropane sulfonic acid (AMPS), 142g of hydroxypropyl acrylate (HPA), 6g of acrylic acid (AA), 16g of mercaptoethanol and 4g of initiator were added to the flask and dissolved in water. The reaction mixture was heated to 65°C in an oil bath and the heating source was removed. The reaction was allowed to heat by exothermic heating. After the exothermic reaction, the reaction was heated to 80°C for 1.5 hours. Initiator was added and the reaction was heated to 85°C for 30 minutes. The reaction was then cooled to room temperature and the pH was adjusted to neutral by adding a NaOH solution. The Mw of dispersant 4 is about 6000 Daltons.

[0057] 2. Preparation of coating composition

[0058] The two-component (2k) formulation using the absorbed dispersion is listed in Table 2. Part A was formulated by grinding the pigment and extender with a polymeric dispersant at 1500 RPM. After 20-30 minutes, MAINCOTE TM AEH-20 and DOWCORNING TM Z6040, inhibitor solution, solvent, thickener and water to adjust the viscosity of the coating. Part B is a hardener. Part A and Part B are stored separately before the formulation is applied to the substrate. The Stormer viscosity of Part A is measured before and after heat aging storage.

[0059] A two-component (2k) formulation using an aqueous epoxy dispersion is listed in Table 3 and the process is similar to that described above.

[0060] Table 2. Formulating 2K waterborne acrylic / epoxy absorbent dispersions

[0061]

[0062] Table 3.2K waterborne epoxy resin dispersion formulation

[0063]

[0064] 3. Results

[0065] Table 4. Formulation and properties of Part A acrylic / epoxy hybrid dispersion

[0066]

[0067] For MAINCOTE TM AEH-20 coating, comparative example 1 is conventional acrylic copolymer dispersant OROTAN TM 731A. The ΔKU 24 hours after painting is very high (+13 units). AAfter 7 days of heat aging storage (HA), the coating solidified, indicating poor stability of the coating due to the epoxy / acrylic reaction. Comparative Example 2 is another acrylic copolymer dispersant containing 35% MAA in the composition. The ΔKU after 24 hours of painting is acceptable (4.5 units), but the ΔKU after 7 days HA is still too high to be acceptable (27.9 units). In contrast, the sulfonic acid-containing dispersants (Dispersant 4, Inventive Example 3) and the phosphate dispersants (Dispersants 2 and 3, Inventive Examples 1 and 2) both show very good stability even after 7 days HA.

[0068] Table 5. Configuration and properties of Part A epoxy dispersions

[0069]

[0070] For users with OUDRASPERSE TM WB-6001 coating, comparative example-3 is conventional acrylic copolymer dispersant OROTAN TM 731A. Using acrylic dispersant, coating stability was poor. After 7 days HA, the paint settled and the ΔKU was as high as 26 units. Inventive Example 4 was prepared using Dispersant 3. The coating stability was very good and the ΔKU after HA was very low (2 units).

Claims

1. A coating composition comprising components (A) and (B); (A) is based on the total dry weight of the component (A), (a) from 10% to 75% of an aqueous epoxy resin dispersion, the aqueous epoxy resin being selected from diglycidyl ether of bisphenol A, (b) from 0.01% to 5% of a polymeric dispersant and (c) from 20% to 85% inorganic particles, and (B) curing agent, The ratio of the component (A) to the component (B) is 90:1 to 2:1, and the polymer dispersant is a polymer containing an anti-agglomeration functional group; wherein the monomer containing the anti-agglomeration functional group is selected from the group consisting of sodium styrene sulfonate and acrylamide-methyl propane sulfonate.

2. The coating composition of claim 1, wherein the polymeric dispersant is formed from a monomer composition comprising: i) a monomer containing the anti-agglomeration functional group, ii) an optional a,b-ethylenically unsaturated carboxylic acid monomer, and iii) an a,b-ethylenically unsaturated nonionic monomer.

3. The coating composition of claim 2, wherein the monomer composition comprises, based on the dry weight of the polymer dispersant: i) from 5 to 80 wt% of a monomer containing an anti-agglomeration functional group, ii) from 0 to 10 wt% of an a,b-ethylenically unsaturated carboxylic acid monomer and iii) from 10 to 95 wt% of an a,b-ethylenically unsaturated nonionic monomer.

4. The coating composition of claim 1, wherein the polymer dispersant has a weight average molecular weight of 500 to 50,000 Daltons. 5 . The coating composition according to claim 1 , wherein the inorganic particles are dispersed in component (A).

6. The coating composition according to claim 1, wherein the monomer containing an anti-agglomeration functional group is selected from acrylamide-methyl propane sulfonate.

Citation Information

Patent Citations

  • Epoxy Resin Imbibed Polymer Particles

    US20120301621A1

  • Sulphonic acid monomer based composition

    CN103570869A

  • Water-thinned epoxy wood white primer and preparation method thereof

    CN105754452A

  • Stable coating composition

    WO2016004575A1