Method for manufacturing semiconductor device
By ion implanting p-type and n-type impurities on the SOI substrate to form a ground plane region with high impurity concentration, the problem of reduced reliability of MISFET is solved, and the stability and performance of MISFET are improved.
Patent Information
- Application Number
- CN201811431496.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-11-27
- Filing Date
- 2018-11-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2038-11-26
AI Technical Summary
In MISFETs formed on SOI substrates, the performance of the semiconductor substrate deteriorates as the impurity concentration in the ground plane region decreases, especially when the impurity concentration at the interface between the ground plane region and the BOX layer decreases, the reliability of the MISFET Reduced sexuality.
The ground plane region of the n-channel MISFET is formed by ion implanting p-type impurities and nitrogen in the semiconductor substrate, and the ground plane region of the p-channel MISFET is formed by ion implanting n-type impurities and carbon or fluorine is formed by ion implanting n-type impurities and carbon or fluorine, thereby maintaining the insulating layer BX The impurity concentration in the ground plane area below is high, thereby improving the reliability of the MISFET.
The reliability of the MISFET is effectively improved, the change time constant of the source-drain current Ids is reduced, the inversion layer is formed under the insulating layer BX is prevented, and the stability of the MISFET is enhanced.
Smart Images

Figure CN109994419B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] The disclosure of Japanese Patent Application No. 2017-226708 filed on November 27, 2017 including the specification, drawings and abstract is incorporated herein by reference in its entirety. Technical Field
[0003] The present invention relates to a method of manufacturing a semiconductor device, and to a technique effective when applied to, for example, a method of manufacturing a semiconductor device using an SOI substrate. Background Art
[0004] There is a technology for forming a MISFET (metal insulator semiconductor field effect transistor) on an SOI (silicon on insulator) substrate as a semiconductor device for low power consumption applications. The MISFET is formed in a semiconductor layer provided on a semiconductor substrate via a BOX layer (insulating film). Further, a ground plane region (semiconductor region) corresponding to a back gate is provided in the semiconductor substrate. The threshold voltage of the MISFET is adjusted by applying a desired voltage to the ground plane region.
[0005] For example, Japanese Unexamined Patent Application Publication No. 2016-66678 discloses that diffusion of impurities forming a ground plane region is suppressed by forming the ground plane region in a silicon carbide thin film. Japanese Unexamined Patent Application Publication No. 2016-66678 also discloses an example of forming a ground plane region by ion implanting carbon and boron into a semiconductor substrate made of silicon.
[0006] Japanese Unexamined Patent Application Publication No. 2006-59843 discloses a technique of ion-implanting a diffusion suppressing element (fluorine, nitrogen, or carbon) to surround an extension region in a p-channel MISFET in order to suppress a short channel effect.
[0007] Japanese Unexamined Patent Application Publication No. 2011-9571 discloses a technique of ion-implanting nitrogen in a lower portion of an extension region in an n-channel MISFET in order to reduce local variations in threshold value. Summary of the invention
[0008] In a MISFET formed on an SOI substrate, as the impurity concentration of a ground plane region decreases, the performance of the semiconductor substrate deteriorates. The inventors of the present application have confirmed that the reliability of a MISFET decreases, particularly when the impurity concentration of the interface between the ground plane region and the BOX layer decreases.
[0009] Other objects and novel features will be apparent from the present specification and accompanying drawings.
[0010] According to one embodiment, a method of manufacturing a semiconductor device forms a ground plane region of an n-channel MISFET by ion implanting p-type impurities and nitrogen (N), and forms a ground plane region of a p-channel MISFET by ion implanting n-type impurities and carbon (C) or fluorine (F).
[0011] According to the embodiments, the reliability of a semiconductor device can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 is a cross-sectional view of a semiconductor device according to an embodiment.
[0013] Figure 2 are cross-sectional views illustrating manufacturing steps of the semiconductor device according to the embodiment.
[0014] Figure 3 It is a graphic representation of Figure 2 A cross-sectional view of subsequent manufacturing steps of a semiconductor device.
[0015] Figure 4 It is a graphic representation of Figure 3 A cross-sectional view of subsequent manufacturing steps of a semiconductor device.
[0016] Figure 5 It is a graphic representation of Figure 4 A cross-sectional view of subsequent manufacturing steps of a semiconductor device.
[0017] Figure 6 It is a graphic representation of Figure 5 A cross-sectional view of subsequent manufacturing steps of a semiconductor device.
[0018] Figure 7 It is a graphic representation of Figure 6 A cross-sectional view of subsequent manufacturing steps of a semiconductor device.
[0019] Figure 8 It is a graphic representation of Figure 7 A cross-sectional view of subsequent manufacturing steps of a semiconductor device.
[0020] Fig. 9 It is a graphic representation of Figure 8 A cross-sectional view of subsequent manufacturing steps of a semiconductor device.
[0021] Fig.10 It is a graphic representation of Fig. 9 A cross-sectional view of subsequent manufacturing steps of a semiconductor device.
[0022] Fig.11 It is a graphic representation of Fig.10 A cross-sectional view of subsequent manufacturing steps of a semiconductor device.
[0023] Fig.12FIG. 1 shows the impurity concentration distribution in the ground plane region of the n-channel MISFET.
[0024] Fig.13 The figure shows the impurity concentration distribution in the ground plane region of the p-channel MISFET.
[0025] Fig.14 is a cross-sectional view of a MISFET of a comparative example taken along the direction of the gate width.
[0026] Fig.15 The relationship between the gate width and the threshold value of the MISFET is shown in the figure.
[0027] Fig.16 The figure shows the source-drain current characteristics of MISFET.
[0028] Fig.17 are cross-sectional views illustrating manufacturing steps of a semiconductor device according to a modification.
[0029] Fig.18 It is a graphic representation of Fig.17 A cross-sectional view of subsequent manufacturing steps of a semiconductor device. DETAILED DESCRIPTION
[0030] The following embodiments will be described, and for convenience, if necessary, the following embodiments will be divided into multiple parts or embodiments. However, unless otherwise specified, these parts or embodiments are not independent of each other, but are in such a relationship that a part or embodiment is a part of another part or embodiment or a modification, details, supplementary explanation, etc. of the whole. In the following embodiments, unless otherwise specified, or except in principle the number is obviously limited to the specific number of cases, or except other cases, when the number of reference elements, etc. (including numerical value, quantity, range, etc.), the number of elements is not limited to the specific number, but can be a specific number or more or less. In addition, in the following embodiments, unless otherwise specified, or except in principle it is obviously considered to be necessary, or except other cases, otherwise constituent elements (including element steps, etc.) are not always necessary. Similarly, in the following embodiments, unless otherwise specified, or except in principle the situation that is obviously considered, or except other cases, when referring to the shape, positional relationship, etc. of constituent elements, it should be understood that they include shapes that are substantially similar or similar to shapes, etc. This also applies to the aforementioned numerical value and range.
[0031] The embodiments are described in detail below with reference to the accompanying drawings. In the accompanying drawings used to explain the embodiments, the same reference symbols are used to mark the components with the same functions, and repeated descriptions are omitted. In the following embodiments, the description of the same or similar parts is not repeated in principle unless it is particularly necessary.
[0032] Example
[0033] The MISFET according to the present embodiment has a configuration of fully depleted silicon on insulator (FD-SOI). The semiconductor layer located below the gate electrode is a channel with a sufficiently low impurity concentration or a channel into which no impurities are introduced (i.e., a so-called undoped channel). The threshold (threshold voltage) of the MISFET is adjusted by providing a ground plane region corresponding to the back gate in the semiconductor substrate under the BOX layer (hereinafter, also referred to as the insulating layer BX) and applying a required voltage to the ground plane region.
[0034] The inventors' research has revealed that a decrease in the impurity concentration at the interface between the ground plane region and the BOX layer will lead to a decrease in the reliability of the MISFET. In an n-channel MISFET having a fully depleted SOI configuration, the threshold can be lowered by applying a negative voltage to the ground plane region. However, when the impurity concentration of the ground plane region is reduced, the MISFET has a characteristic of having a time constant, such as Fig.16 As shown. That is, it has been confirmed that it takes a long time for the source-drain current Ids of the MISFET to become stable. In the case where the MISFET operation is caused by applying a negative voltage to the ground plane region, when the impurity concentration of the ground plane region has been reduced, a depletion layer is formed at the interface with the insulating layer BX in the first stage, and an inversion layer is formed at the interface with the insulating layer BX in the second stage. Because the parasitic capacitance between the gate electrode and the ground plane region in the first stage and the parasitic capacitance between the gate electrode and the ground plane region in the second stage are different from each other, the source-drain current Ids is varied.
[0035] The present embodiment provides a technique for maintaining high impurity concentration in the ground plane region directly below the insulating layer BX.
[0036] <Semiconductor Device of the Present Embodiment>
[0037] Figure 1 There is shown a cross-sectional structure of an n-channel MISFET 1Tr and a p-channel MISFET 2Tr forming the semiconductor device of the present embodiment.
[0038] The semiconductor device of the present embodiment includes a region An where an n-channel MISFET 1Tr is to be formed, a region TAn for supplying power to a well region PW of the region An, a region Ap where a p-channel MISFET 2Tr is to be formed, and a region TAp for supplying power to a well region NW of the region Ap.
[0039] The region An and the region TAn are separated from each other by an isolation portion STI formed in the semiconductor substrate SB. The well region PW is formed deeper than the isolation portion STI to extend over the region An and the region TAn. The region Ap and the region TAp are separated from each other by the isolation portion STI. The well region NW is formed deeper than the isolation portion STI to extend over the region Ap and the region TAp.
[0040] An insulating layer BX is formed on the semiconductor substrate SB, and a semiconductor layer SM is formed on the insulating layer BX. That is, the semiconductor layer SM and the semiconductor substrate SB are electrically isolated from each other by the insulating layer BX. The thickness of the insulating layer BX is about 10nm to 20nm, and the thickness of the semiconductor layer SM is about 10nm to 20nm. Further, in the region TAn and the region TAp as the power supply region, the insulating layer BX and the semiconductor layer SM are removed. Therefore, a voltage can be applied to the well region PW and the well region NW respectively via the epitaxial layer EP.
[0041] First, the structure of the MISFET 1Tr in the region An is described.
[0042] In the region An, an n-well region DNW is formed in the semiconductor substrate SB. In the well region DNW, a p-well region PW is formed. The well region PW is electrically isolated from the semiconductor substrate SB by the well region DNW. In the surface of the well region PW in contact with the insulating layer BX, a p-type ground plane region (impurity region) GP1 having an impurity concentration higher than that of the well region PW is formed. The ground plane region GP1 serves as a back gate of the MISFET 1Tr. The threshold of the MISFET 1Tr is adjusted by supplying a desired voltage to the ground plane region GP1.
[0043] The well region PW and the ground plane region GP1 are regions where p-type impurities (for example, boron (B)) are introduced. The impurity concentration of the well region PW is about 5×10 17 / cm 3 Up to 5×10 18 / cm 3 , and the impurity concentration of the ground plane region GP1 is about 1×10 18 / cm 3 Up to 1×10 19 / cm 3 In addition, in this embodiment, nitrogen is implanted into the ground plane region GP1, and the concentration thereof is 1×10 19 / cm 3 Up to 1×10 20 / cm 3 .
[0044] In the region An, a gate electrode G1 is formed on the semiconductor layer SM via a gate insulating film GF1. The gate insulating film GF1 is formed of, for example, a silicon oxide film or a silicon oxynitride film. The gate electrode G1 is formed of, for example, a polysilicon film.
[0045] A sidewall spacer SW is formed on the side surface of the gate electrode G1 via the offset spacer OS. An extension region EX1 as a low-concentration n-type impurity region is formed in the semiconductor layer SM below the offset spacer OS and below the sidewall spacer SW. An epitaxial layer EP is formed on a portion of the semiconductor layer SM. A diffusion region D1 is formed in the epitaxial layer EP. The diffusion region D1 is an n-type impurity region having a higher concentration than the extension region EX1. The extension region EX1 and the diffusion region D1 form a source region or a drain region of the MISFET1Tr.
[0046] In the region TAn, the well region DNW and the well region PW are formed as in the region An. Although the ground plane region GP1 is formed in the surface of the well region PW, the ground plane region GP1 in the region TAn may be omitted. Since the insulating layer BX and the semiconductor layer SM are removed in the region TAn as described above, the epitaxial layer EP is formed to be in direct contact with the well region PW including the ground plane region GP1. A diffusion region D2 is formed in the epitaxial layer EP as a p-type impurity region. Therefore, the voltage supplied to the plug PG in the region TAn is supplied to the ground plane voltage GP1 in the region An via the epitaxial layer EP and the well region PW.
[0047] Next, the structure of the MISFET 2Tr in the region Ap is described.
[0048] In the region Ap, an n-well region NW is formed in the semiconductor substrate SB. In the surface of the well region NW in contact with the insulating layer BX, an n-type ground plane region GP2 having a higher impurity concentration than the well region NW is formed. The ground plane region GP2 serves as a back gate of the MISFET 2Tr. The threshold of the MISFET 2Tr is adjusted by supplying a desired voltage to the ground plane region GP2.
[0049] The well region NW and the ground plane region GP2 are regions where n-type impurities (for example, phosphorus (P) or arsenic (As)) are introduced. The impurity concentration of the well region NW is about 5×10 16 / cm 3 Up to 5×10 17 / cm 3 , and the impurity concentration of the ground plane region GP2 is about 4×10 17 / cm 3 Up to 4×10 18 / cm 3In addition, in this embodiment, carbon (C) or fluorine (F) is implanted into the ground plane region GP2, and the concentration thereof is 1×10 19 / cm 3 Up to 1×10 20 / cm 3 .
[0050] In the region Ap, a gate electrode G2 is formed on the semiconductor layer SM via a gate insulating film GF2. The gate insulating film GF2 is formed of, for example, a silicon oxide film or a silicon oxynitride film. That is, in this embodiment, the gate insulating film GF1 and the gate insulating film GF2 are formed of the same film.
[0051] A sidewall spacer SW is formed on the side surface of the gate electrode G2 via the offset spacer OS. An extension region EX2 is formed as a low-concentration p-type impurity region in the semiconductor layer SM below the offset spacer OS and in the direction of the sidewall spacer SW. An epitaxial layer EP is formed on a portion of the semiconductor layer SM. A diffusion region D2 is formed in the epitaxial layer EP. The diffusion region D2 is a p-type impurity region having a higher concentration than the extension region EX2. The extension region EX2 and the diffusion region D2 form a source region or a drain region of the MISFET2Tr.
[0052] In the region TAp, the well region NW is formed as in the region Ap. Although the ground plane region GP2 is formed in the surface of the well region NW, the ground plane region GP2 in the region TAp may be omitted. Since the insulating layer BX and the semiconductor layer SM are removed in the region TAp as described above, the epitaxial layer EP is formed to be in direct contact with the well region NW including the ground plane region GP2. A diffusion region D1 is formed in the epitaxial layer EP as an n-type impurity region. Therefore, the voltage supplied to the plug PG in the region TAp is supplied to the ground plane voltage GP2 in the region Ap via the epitaxial layer EP and the well region NW.
[0053] Further, the diffusion region D1 formed in the region An and the diffusion region D1 formed in the region TAp are n-type impurity regions formed by the same process, as will be described later. Similarly, the diffusion region D2 formed in the region Ap and the diffusion region D2 formed in the region TAn are p-type impurity regions formed by the same process.
[0054] A silicide layer made of, for example, nickel silicide (NiSi) or cobalt silicide (COSi2) is formed on the gate electrode G1, the gate electrode G2, and the epitaxial layer EP in order to reduce the contact resistance with the plug PG.
[0055] An interlayer insulating film IL1 is formed in the region An, the region Ap, the region TAn, and the region TAp to cover the MISFET1Tr and the MISFET 2Tr. As the interlayer insulating film IL1, for example, a single-layer film of a silicon oxide film or a multilayer film of a silicon nitride film and a thick silicon oxide film formed thereon can be used. A contact hole is formed in the interlayer insulating film IL1. A plurality of plugs PG are formed in the interlayer insulating film IL1 by embedding a conductive film mainly made of tungsten (W) or the like into the contact hole. Each plug PG is coupled to the gate electrode G1, the gate electrode G2, and the epitaxial layer EP via the silicide layer SI.
[0056] An interlayer insulating film IL2 is formed on the interlayer insulating film IL1 in which the plug PG is embedded. In the interlayer insulating film IL2, a groove for a wire is formed. By embedding a conductive film made of copper as a main component in the groove for the wire, a wire M1 to be coupled to the plug PG is formed in the interlayer insulating film IL2.
[0057] <Method of Manufacturing the Semiconductor Device of the Present Embodiment>
[0058] Refer to the following Figures 2 to 11 A method of manufacturing the semiconductor device of the present embodiment is described.
[0059] Figure 2 A so-called SOI substrate is shown, which includes a semiconductor substrate SB as a supporting substrate, an insulating layer BX formed on the semiconductor substrate SB, and a semiconductor layer SM formed on the insulating layer BX.
[0060] The semiconductor substrate SB is made of single crystal silicon (e.g., p-type single crystal silicon) preferably having a resistivity of about 1 Ωcm to 10 Ωcm. The insulating layer BX is made of, for example, silicon oxide. The thickness of the insulating layer BX is, for example, about 10 nm to 20 nm. The semiconductor layer SM is made of single crystal silicon preferably having a resistivity of about 1 Ωcm to 10 Ωcm. The thickness of the semiconductor layer SM is, for example, about 10 nm to 20 nm. The semiconductor layer SM is an intrinsic semiconductor layer into which no n-type or p-type impurities are introduced by ion implantation or the like. Alternatively, even if the semiconductor layer SM contains p-type impurities introduced therein, the impurity concentration thereof is 1×10 13 / cm 3 Or less.
[0061] Further, Figure 2 An isolation portion STI is also illustrated. The isolation portion STI is formed by forming a trench extending through the semiconductor layer SM and the insulating layer BX and reaching the semiconductor substrate SB and embedding an insulating film in the trench. The region An, the region Ap, the region TAn, and the region TAp are isolated from each other by the isolation portion STI.
[0062] Subsequently, an n well region DNW is formed in the semiconductor substrate SB in the region An and the region TAn by photolithography and ion implantation.
[0063] Next, if Figure 3 As shown in , the region TAn and the region TAP are selectively removed by photolithography and dry etching to expose the insulating layer BX in the region TAn and the region TAP. Subsequently, in the region An and the region TAn, a p-well region PW is formed in the well region DNW. The impurity concentration of the well region PW is about 5×10 17 / cm 3 Up to 5×10 18 / cm 3 For example, the well region PW is formed by ion implanting boron (B) or boron difluoride (BF 2 ).
[0064] Then, a ground plane region GP1 is formed in the well region PW in the region An and the region TAn by photolithography and dry etching, as shown in FIG. Figure 4 As shown in . For example, in the formation of the ground plane region GP1, ion implantation of boron (B) or boron difluoride (BF2) as a p-type impurity is performed, and thereafter ion implantation of nitrogen (N) as an inert dopant is performed. However, ion implantation of boron (B) or boron difluoride (BF2) may be performed after ion implantation of nitrogen (N). For example, the dose of boron (B) is 5×10 13 / cm 2 , and the implantation energy is 40KeV, and the nitrogen (N) dose is 5×10 14 / cm 2 , and the implantation energy is 40KeV.
[0065] Then, in the region Ap and the region TAp, an n well region NW is formed in the semiconductor substrate SB, as shown in FIG. Figure 5 The impurity concentration of the well region NW is about 5×10 16 / cm 3 Up to 5×10 17 / cm 3 For example, the well region NW is formed by ion implantation of phosphorus (P) or arsenic (As).
[0066] Then, if Figure 6As shown in FIG. 1 , in the region Ap and the region TAp, an n-type ground plane region GP2 is formed in the well region NW by photolithography and dry etching. For example, in the formation of the ground plane region GP2, ion implantation of phosphorus (P), arsenic (As), or antimony (Sb) as an n-type impurity is performed, and thereafter ion implantation of carbon (C) or fluorine (F) as an inert dopant is performed. However, ion implantation of phosphorus (P), arsenic (As), or antimony (Sb) may be performed after ion implantation of carbon (C) or fluorine (F). For example, the dose of phosphorus (P) is 5×10 13 / cm 2 , and the implantation energy is 90KeV, and the carbon (C) dose is 5×10 14 / cm 2 , and the implantation energy is 50KeV.
[0067] Then, if Figure 7 As shown in FIG. 1 , gate insulating films GF1 and GF2 formed of, for example, a silicon oxide film are formed on the semiconductor layer SM in the region An and the region Ap by, for example, thermal oxidation. The thickness of the gate insulating films GF1 and GF2 is about 2 nm to 3 nm. The thermal oxidation is performed at a temperature of 800° C. to 1100° C.
[0068] Then, gate electrodes G1 and G2 are formed on the gate insulating film GF1 of the region An and the gate insulating film GF2 of the region Ap, respectively. Further, a cap film CP is formed on each gate electrode. The gate electrodes G1 and G2 are formed by, for example, polysilicon. The cap film CP is formed by, for example, a silicon oxide film. Specifically, an insulating film for forming the gate insulating films GF1 and GF2, a conductive film for forming the gate electrodes G1 and G2, and an insulating film for forming the cap film CP are sequentially formed, and thereafter these films are processed by photolithography and dry etching (or wet etching). In this way, a multilayer structure of the gate insulating film GF1, the gate electrode G1, and the cap film CP is formed in the region An, and a multilayer structure of the gate insulating film GF2, the gate electrode G2, and the cap film CP is formed in the region Ap. When processing the gate insulating films GF1 and GF2, the insulating layer BX in the region TAn and the region TAp is also removed, so that the ground plane regions GP1 and GP2 are exposed.
[0069] Figure 8 The steps of forming the offset spacer OS, the dummy sidewall spacer DSW, and the epitaxial layer EP are illustrated.
[0070] First, an insulating film, for example, formed of a silicon oxide film, is formed by, for example, CVD to cover the region An, the region Ap, the region TAn, and the region TAp. Subsequently, anisotropic etching is performed on the insulating film so that an offset spacer OS is formed on the side surface of each of the gate electrode G1 and the gate electrode G2. In this process, in the region TAn and the region TAp, the insulating film of the offset spacer OS is removed by anisotropic etching, and the semiconductor substrate SB is exposed.
[0071] Subsequently, an insulating film formed of, for example, a silicon nitride film is formed by, for example, CVD to cover the region An, the region Ap, the region TAn, and the region TAp. Then, anisotropic etching is performed on the insulating film so that a dummy sidewall spacer DSW is formed on the side surface of each of the gate electrodes G1 and G2 via the offset spacer OS. In this process, in the region TAn and the region TAp, the insulating film of the dummy sidewall spacer DSW is removed by anisotropic etching, and the semiconductor substrate SB is exposed.
[0072] Subsequently, an epitaxial layer EP (semiconductor layer EP) made of, for example, single crystal silicon is formed on the semiconductor layer SM in the region An and the region Ap and over the semiconductor substrate SB in the region TAn and the region TAp by epitaxial growth. The thickness of the semiconductor layer EP is about 20 nm to 40 nm. In this process, since the gate electrode G1 and the gate electrode G2 are covered by the cap film CP, the epitaxial layer EP is not formed on the gate electrode G1 and the gate electrode G2.
[0073] Since the epitaxial layer EP is made of the same material as the semiconductor layer SM, they are integrated with each other. However, in the present embodiment, the epitaxial layer EP is illustrated with arrows and the boundary between the epitaxial layer EP and the semiconductor layer SM is illustrated with dotted lines to provide a simple understanding of the present invention.
[0074] Fig. 9 The steps of removing the dummy sidewall spacers DSW and the cap film CP and forming the extension region EX1 are shown.
[0075] First, etching is performed under the condition that the offset spacer OS is hardly etched, thereby removing the dummy sidewall spacer DSW and the cap film CP in the region An and the region Ap. Since the dummy sidewall spacer DSW and the cap film CP are formed of the same material, they can be removed at the same time. Therefore, an additional mask is not required, which leads to simplification of the manufacturing process.
[0076] Subsequently, an n-type extension region (impurity region) EX1 is formed in the semiconductor layer SM and the epitaxial layer EP on both sides of the gate electrode G1 in the region An by photolithography and ion implantation. For example, in the region An and the region TAp, the extension region EX1 is formed by ion implantation of phosphorus (P) or arsenic (As). The extension region EX1 forms a part of the source region or a part of the drain region of the MISFET 1Tr. Although the extension region EX1 is also formed in the surface of the epitaxial layer EP in the region TAp, it is not necessary to form the extension region EX1 in the region TAp.
[0077] Then, if Fig.10 As shown, an extension region EX2 is formed. By photolithography and ion implantation, a p-type extension region (impurity region) EX2 is formed in the semiconductor layer SM and the epitaxial layer EP on both sides of the gate electrode G2 in the region Ap. For example, in the region Ap and the region TAn, the extension region EX2 is formed by ion implantation of boron (B) or boron difluoride (BF2). The extension region EX2 forms a part of the source region or a part of the drain region of the MISFET 2Tr. Although the extension region EX2 is also formed in the surface of the epitaxial layer EP in the region TAn, it is not necessary to form the extension region EX2 in the region TAn.
[0078] Fig.11 The steps of forming the sidewall spacers SW, the diffusion region D1, the diffusion region D2, and the silicide layer SI are shown.
[0079] First, an insulating film formed of, for example, a silicon nitride film is formed by, for example, CVD to cover the regions An, Ap, TAn, and TAp. Subsequently, anisotropic etching is performed on the insulating film to form side wall spacers SW on the side surfaces of each of the gate electrodes G1 and G2 via the offset spacers OS.
[0080] Next, by photolithography and ion implantation, an n-type diffusion region (impurity region) D1 is formed in the epitaxial layer EP and the semiconductor layer SM in the region An and the epitaxial layer EP in the region TAp, and a p-type diffusion region (impurity region) D2 is formed in the epitaxial layer EP and the semiconductor layer SM in the region Ap and the epitaxial layer EP in the region TAn. In the region An and the region TAp, the n-type diffusion region D1 is formed by ion implantation of phosphorus (P) or arsenic (As). In the region Ap and the region TAn, the p-type diffusion region D2 is formed by ion implantation of boron (B) or boron difluoride (BF2).
[0081] In the region An, the n-type diffusion region D1 has a higher impurity concentration than the extension region EX1, is coupled to the extension region EX1, and forms a part of the source region or a part of the drain region of the MISFET 1Tr.
[0082] In the region Ap, the p-type diffusion region D2 has a higher impurity concentration than the extension region EX2, is coupled to the extension region EX2, and forms a part of the source region or a part of the drain region of the MISFET 2Tr.
[0083] Subsequently, heat treatment is performed on the semiconductor substrate SB at a temperature of about 1050° C. so as to activate the impurities contained in the extension regions EX1 and EX2 and the diffusion regions D1 and D2.
[0084] Then, a low-resistance silicide layer SI is formed on the top surface of each of the diffusion region D1, the diffusion region D2, the gate electrode G1, and the gate electrode G2 by a silicide (self-aligned silicide) technique.
[0085] Specifically, the silicide layer SI can be formed in the following manner. First, a metal film for forming the silicide layer SI is formed to cover the region An, the region Ap, the region TAn, and the region TAP. The metal film is made of, for example, cobalt, nickel, or a nickel-platinum alloy. Then, the semiconductor substrate SB is heat-treated at a temperature of about 600° C. to 700° C. so that the diffusion region D1, the diffusion region D2, the gate electrode G1, and the gate electrode G2 react with the metal film. In this way, a silicide film SI is formed on the top surface of each of the diffusion region D1, the diffusion region D2, the gate electrode G1, and the gate electrode G2. Thereafter, the unreacted metal film is removed.
[0086] Through the above steps, the MISFET 1Tr is formed in the region An, and the MISFET 2Tr is formed in the region Ap.
[0087] exist Fig.11 After the manufacturing steps, interlayer insulating films IL1 and IL2, plug connector PG, and wire M1 are formed.
[0088] First, an interlayer insulating film IL1 is formed to cover the region An, the region Ap, the region TAn, and the region TAp. As the interlayer insulating film IL1, for example, a single-layer film of a silicon oxide film or a multilayer film of a silicon nitride film and a thick silicon oxide film formed thereon can be used. After the interlayer insulating film IL1 is formed, the top surface of the interlayer insulating film IL1 can be polished by CMP (chemical mechanical polishing) if necessary.
[0089] Subsequently, a contact hole is formed in the interlayer insulating film IL1 by, for example, photolithography and dry etching, and a conductive film mainly made of tungsten (W) or the like is embedded in the contact hole. In this way, a plurality of plugs PG are formed in the interlayer insulating film IL1. The plug PG formed in each region is coupled to the diffusion region D1 or D2 via the silicide layer SI. Although each of the gate electrodes G1 and G2 is also coupled to the plug PG, illustration is omitted in the present embodiment.
[0090] Subsequently, an interlayer insulating film IL2 is formed on the interlayer insulating film IL1 in which the plug PG is embedded. Thereafter, a groove for a wire is formed in the interlayer insulating film IL2, and a conductive film made of, for example, copper as a main component is embedded in the groove for the wire, so that a wire M1 coupled to the plug PG is formed in the interlayer insulating film IL2. The structure of this wire M1 is a so-called damascene wire structure.
[0091] Thereafter, the wires in the subsequent layers including the second layer are formed by, for example, dual damascene technology. However, description and illustration are omitted here. The wire M1 and the wires above the wire M1 are not limited to the damascene wire structure. Those wires can be formed by patterning conductive films and can be, for example, tungsten wires or aluminum wires.
[0092] As described above, the semiconductor device according to the present embodiment is manufactured.
[0093] <Features of the Method of Manufacturing the Semiconductor Device of the Present Embodiment>
[0094] One of the characteristics of the method for manufacturing a semiconductor device according to the present embodiment is that the ground plane region GP1 is formed by ion implantation of boron (B) or boron difluoride (BF2) as a p-type impurity and nitrogen (N) as an inert dopant, and the ground plane region GP2 is formed by ion implantation of phosphorus (P), arsenic (As) or antimony (Sb) as an n-type impurity and carbon (C) or fluorine (F) as an inert dopant.
[0095] Fig.12 and Fig.13 The impurity concentration distribution in the ground plane regions GP1 and GP2 in the depth direction is shown. Fig.12 and Fig.13 The diagram shows a state after completion of heat treatment for activating impurities contained in the extension regions EX1 and EX2 and the diffusion regions D1 and D2.
[0096] exist Fig.12In the figure, (a) represents the concentration distribution corresponding to the present embodiment in the case where boron (B) and nitrogen (N) are ion-implanted, and (b) represents the concentration distribution corresponding to a comparative example in the case where boron (B) is ion-implanted. In (b) of the comparative example, the impurity concentration directly below the insulating layer BX is low. This is because the boron (B) that has been ion-implanted is segregated into the insulating layer BX when the gate insulating film GF1 is formed. At the same time, accumulation of the boron (B) that has been ion-implanted occurs directly below the insulating layer BX. Accumulation is a phenomenon in which, when interstitial defects associated with the ion implantation of boron (B) are introduced into the silicon substrate interface (the interface between the insulating layer BX and the ground plane region GP1) in a later heat treatment, boron (B) follows the interstitial defects and accumulates near the silicon substrate interface. Accumulation is a phenomenon that occurs for all ion-implanted impurities. However, in the case of boron (B), the amount of segregation is greater than the amount of accumulation, and thus the impurity concentration directly below the insulating layer BX becomes low, as shown in FIG. Fig.12 When the impurity concentration directly under the insulating layer BX is reduced, an inversion layer is formed directly under the insulating layer BX during the operation of the MISFET 1Tr, so that the MISFET 1Tr is characterized by a time constant, as described above.
[0097] On the other hand, in (a) of the present embodiment, the impurity concentration directly below the insulating layer BX can be made higher than in the comparative example. In the present embodiment, boron (B) and nitrogen (N) as inert elements are ion-implanted in the step of forming the ground plane region GP1, thereby promoting accumulation. That is, by ion implanting a high dose of nitrogen (N), excessive gap defects are introduced into the silicon substrate, accumulation in heat treatment is promoted, and the impurity concentration directly below the insulating layer BX is increased. In this way, the formation of an inversion layer can be prevented. As inert elements, carbon (C), fluorine (F), etc. are also considered in addition to nitrogen (N). However, the use of nitrogen (N) is preferred. This is because nitrogen (N) has the characteristic of being more difficult to trap excessive gap defects than carbon (C) or fluorine (F).
[0098] exist Fig.13In the figure, (c) represents the concentration distribution in the case where phosphorus (P) and carbon (C) are ion-implanted corresponding to the present embodiment, and (d) represents the concentration distribution in the case where phosphorus (P) is ion-implanted corresponding to a comparative example. In the present embodiment, phosphorus (P) and carbon (C) as inert elements are ion-implanted in the step of forming the ground plane region GP2. Thus, the diffusion of phosphorus (P) in the depth direction can be suppressed by transient enhanced diffusion, so that the average impurity concentration directly below the insulating layer BX (for example, within a range of approximately 0.1 μm from the insulating layer BX) can be improved compared to the average impurity concentration in the comparative example. Therefore, the inversion layer can be prevented from being formed directly below the insulating layer BX. Further, as an inert element, it is more preferable to use carbon (C) or fluorine (F) than nitrogen (N). This is because carbon (C) or fluorine (F) can react with a lower dose of interstitial defects to form clusters or trap phosphorus (P) compared to nitrogen (N). Therefore, transient enhanced diffusion of phosphorus (P) caused by the introduction of excessive interstitial defects generated in the case of ion implantation with a high dose of an inert element can be prevented.
[0099] Further, according to the present embodiment, the threshold value can be reduced by the reduction in the channel width (the so-called "narrow channel effect") in the n-channel MISFET 1Tr. Fig.14 is a cross-sectional view of a MISFET of a comparative example taken along the direction of the gate width, and Fig.15 The relationship between the gate width and threshold value of MISFET is shown in the figure. Fig.15 In FIG. 1 , (e) represents the characteristics of the MISFET 1Tr of this embodiment, and (f) represents Figure 4 Characteristics of MISFET of comparative example.
[0100] As described above, boron (B) that has been ion-implanted to form the ground plane region is segregated into the insulating layer BX by undergoing heat treatment, and thus the impurity concentration is reduced. Fig.14 As described above, the impurity concentration at both ends (marked as GP1L) of the ground plane region is further reduced compared to the central portion (marked as GP1). This is because the segregation of boron (B) occurs not only in the insulating layer BX but also in the isolation portions STI at both ends of the ground plane region. Therefore, in the comparative example MISFET, the thresholds at both ends in the gate width direction are lowered compared to the thresholds at the central portion, so that the threshold of the MISFET is lowered, as shown in FIG. Fig.15 As shown in (f) in .
[0101] On the other hand, according to an embodiment of the present invention, ion implantation of boron (B) and nitrogen (N) as inert elements can promote the accumulation and can also increase the impurity concentration at both ends in the gate width direction as described above. Therefore, the above-mentioned narrow channel effect can be reduced, so that the gate width can be obtained. Figure 5 That is, it is possible to prevent the threshold value of the MISFET1Tr from being lowered.
[0102] <Edit>
[0103] Fig.17 and Fig.18 is a cross-sectional view illustrating the manufacturing steps of a semiconductor device according to a modification. The modification is different from the above embodiment in the process of forming the ground plane regions GP1 and GP2. In the above embodiment, the p-well region PW, the ground plane region GP1, the n-well region NW and the ground plane region GP2 are formed in the above order. In this modification, the step of forming the ground plane region GP1 is performed after forming the extension region EX1, and the step of forming the ground plane region GP2 is performed after forming the extension region EX2. For the formation of the ground plane regions GP1 and GP2, the modification is the same as the above embodiment. However, the energy of the ion implantation is set to be higher than that in the above embodiment so that the ions pass through the gate electrodes G1 and G2, the epitaxial layer EP, etc. Although an example is described in which the ground plane region GP2 is formed after the ground plane region GP1 is formed, the order of formation can be reversed.
[0104] In the above, the invention made by the inventors of the present application has been specifically described by way of embodiment. However, it is naturally understood that the present invention is not limited to the aforementioned embodiment and can be changed in various ways within the scope not departing from the gist thereof.
Claims
1. A method for manufacturing a semiconductor device, comprising the following steps: (a) providing an SOI substrate, the SOI substrate having: A semiconductor substrate comprising a first region and a second region, wherein an n-type first MISFET is to be formed in the first region and a p-type second MISFET is to be formed in the second region; an insulating layer formed on the semiconductor substrate; as well as a semiconductor layer formed on the insulating layer; (b) forming a first semiconductor region by ion implanting p-type impurities and nitrogen into the semiconductor substrate in the first region; (c) forming a second semiconductor region by ion implanting one of carbon and fluorine and an n-type impurity into the semiconductor substrate in the second region; (d) forming the first MISFET in the first region; and (e) Forming the second MISFET in the second region.
2. The method according to claim 1, Each of the first semiconductor region and the second semiconductor region is in contact with the insulating layer.
3. The method according to claim 1, The impurity concentration of the semiconductor layer is 1×10 13 cm -3 Or less. The method according to claim 1 , wherein the semiconductor layer has a thickness of 10 nm to 20 nm.
5. The method according to claim 1, The thickness of the insulating layer is 10 nm to 20 nm.
6. The method according to claim 1, wherein said step (d) comprises: (d-1) forming a first gate electrode on the semiconductor layer via a first gate insulating film; as well as (d-2) forming an n-type third semiconductor region in the semiconductor layer at both sides of the first gate electrode; as well as Wherein said step (e) comprises: (e-1) forming a second gate electrode on the semiconductor layer via a second gate insulating film, and (e-2) Forming a p-type fourth semiconductor region in the semiconductor layer at both sides of the second gate electrode.
7. The method according to claim 1, in, forming the first semiconductor region by ion implanting p-type impurities and nitrogen into the semiconductor substrate in the first region without ion implanting carbon into the semiconductor substrate in the first region, and The second semiconductor region is formed by ion implanting one of carbon and fluorine and n-type impurities into the semiconductor substrate in the second region without ion implanting nitrogen into the semiconductor substrate in the second region.
Citation Information
Patent Citations
Semiconductor device and its manufacturing method
JP2006059843A
Semiconductor device and manufacturing method of the same
JP2016066678A
Semiconductor structure and manufacture method thereof
CN101252146A
Method for making semiconductor device
CN1581442A
Semiconductor device and its manufacturing method
CN1643690A