Photosensitive resin composition, photosensitive resin laminate and pattern forming method

By adding primary alcoholic hydroxyl groups, cross-linking agents and multifunctional epoxy compounds to polyimide silicone resin, and using fillers and colorants during exposure, the problem of high-temperature curing and light transmittance reduction of polyimide resin is solved. problem, a photosensitive resin composition with high modulus and heat resistance was achieved.

CN110297398BActive Publication Date: 2024-10-08SHIN ETSU CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910220518.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-03-23
Filing Date
2019-03-22
Publication Date
2024-10-08
Estimated Expiration
2039-03-22

AI Technical Summary

Technical Problem

Polyimide resin has the problem of thermal deterioration caused by high-temperature curing during processing, and the addition of fillers and colorants will reduce the light transmittance, making it difficult to improve the modulus and reliability of the resin at the same time.

Method used

A photosensitive resin composition containing polyimide silicone containing primary alcoholic hydroxyl groups, a cross-linking agent, a photoacid generator and a multifunctional epoxy compound is used, and fillers and colorants of specific particle sizes are added during exposure. The reaction forms cross-linking points to increase the resin's modulus and heat resistance.

Benefits of technology

The polyimide silicone resin that is cured at low temperature and in a short time has been realized with high modulus, good heat resistance, mechanical strength and adhesion to the substrate, while maintaining the light transmittance of the resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004858668680000011
    Figure FDA0004858668680000011
  • Figure FDA0004858668680000012
    Figure FDA0004858668680000012
  • Figure FDA0004858668680000021
    Figure FDA0004858668680000021
Patent Text Reader

Abstract

The present invention is a photosensitive resin composition, a photosensitive resin laminate and a pattern forming method. A photosensitive resin composition is provided, which comprises 100 pbw of a polyimide silicone containing a primary alcohol hydroxyl group, a crosslinking agent, a photoacid generator, a multifunctional epoxy compound, 1-70 pbw of a filler having an average particle size of 0.01-20.0 μm and 0.01-30 pbw of a colorant. The resin composition is colored and photosensitive and is cured into a product with an improved modulus.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This nonprovisional application claims priority under 35 U.S.C. § 119(a) to patent application No. 2018-056546, filed in Japan on March 23, 2018, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to a photosensitive resin composition, a photosensitive resin laminate and a pattern forming method. Background Art

[0004] Due to excellent heat resistance and electrical insulation properties, polyimide resin is widely used as printed circuit board, heat-resistant adhesive tape, electrical components, semiconductor material protective film and interlayer insulation film etc. However, polyimide resin encounters processing problems because they can only be dissolved in limited solvents. Common practice then is to coat substrates with a solution of polyamic acid relatively soluble in various organic solvents, and to process polyamic acid at high temperatures to form polyimide resin by dehydration cyclization. However, this method requires long-term heating at high temperatures, which causes thermal degradation of substrate. On the other hand, insufficient heating may leave residual polyamic acid in the resin structure, causing moisture resistance and corrosion resistance to reduce.

[0005] In order to solve this problem, patent documentation 1 proposes to replace the polyamic acid coating substrate with the solution of the polyimide resin soluble in an organic solvent, and heat the coating to evaporate the solvent and form a method for polyimide resin film. However, the solvent resistance of the resin film obtained by the organic solvent soluble polyimide resin is poor. Then patent documentation 2 and 3 disclose the organosilicon-modified polyimide (also referred to as polyimide silicone) of heat-curing type, which has a polymerizable side chain and is soluble in an organic solvent. The resin of patent documentation 2 is said to be solidified by heat or light means. The resin of patent documentation 3 is solidified by the hydrosilylation reaction with organohydrogensiloxane, but solidification is carried out for 5 hours.

[0006] Reference List

[0007] Patent Document 1: JP-A H02-036232

[0008] Patent Document 2: JP-A H02-147630

[0009] Patent Document 3: JP-A H07-268098 Summary of the Invention

[0010] In this context, polyimide silicone resin compositions are currently used, which cure at relatively low temperatures and in relatively short periods of time. Compared to conventional polyimide resins, these silicone-modified polyimide resins are softer and have a high coefficient of linear expansion that is difficult to reduce. This makes it difficult to formulate resin compositions with high modulus and reliability. Typically, these high modulus and reliability are achieved by incorporating fillers.

[0011] However, the use of fillers in photosensitive resin compositions is disadvantageous because the light transmittance of the filled composition decreases. Similarly, when colorants are added to photosensitive resin compositions, the light transmittance of the composition decreases. It is very difficult to use fillers and colorants at the same time.

[0012] An object of the present invention is to provide a photosensitive resin composition containing a filler and a colorant, a photosensitive resin laminate, and a pattern forming method using the same.

[0013] The inventors have attempted to add fillers and colorants to a photosensitive resin composition containing a polyimide silicone containing primary hydroxyl groups, a crosslinker, and a photoacid generator. When the photosensitive resin composition is exposed to light, the photoacid generator generates acid, which reacts with the crosslinker and the hydroxyl groups in the resin to form crosslinking sites. This requires irradiating light to each area to be cured. The presence of fillers and colorants scatters or absorbs light, hindering the crosslinking reaction.

[0014] The inventors have continued their research and found that when a predetermined amount of a filler having a specific particle size and a predetermined amount of a colorant are added to a photosensitive resin composition containing a polyimide silicone containing primary hydroxyl groups, a crosslinking agent, a photoacid generator, and a multifunctional epoxy compound, a resin composition is obtained that is colored and photosensitive and cures to a product having an improved modulus.

[0015] In one aspect, the present invention provides a photosensitive resin composition comprising:

[0016] (A) contains 1.0×10 -7 to 8.0×10 -3 Equivalent weight / gram (eq / g) of primary alcohol hydroxyl polyimide silicone,

[0017] (B) a cross-linking agent,

[0018] (C) a photoacid generator,

[0019] (D) a polyfunctional epoxy compound,

[0020] (E) a filler having an average particle size of 0.01 to 20.0 μm in an amount of 1 to 70 parts by weight per 100 parts by weight of the polyimide silicone (A), and

[0021] (F) A colorant in an amount of 0.01 to 30 parts by weight per 100 parts by weight of the polyimide silicone (A).

[0022] The composition may further comprise (G) an organic solvent. Preferably, the organic solvent is selected from propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, cyclohexanone, cyclopentanone, methyl isobutyl ketone and γ-butyrolactone.

[0023] In a preferred embodiment, the polyimide silicone (A) comprises a repeating unit having formula (1-1) and a repeating unit having formula (1-2):

[0024]

[0025] where X 1 is a tetravalent group having formula (2):

[0026]

[0027] where R 1 to R 6 Each independently represents a C1-C8 monovalent hydrocarbon group, R 7 and R 8 Each independently is a single bond or C1-C 12 Divalent hydrocarbon group, R 9 and R 10 Each is independently a trivalent organic group, m is an integer from 0 to 120, and the dotted line represents a valence bond,

[0028] Y 1 is a group having formula (3):

[0029]

[0030] Among them A 1 To A 3 Each is independently a single bond, a methylene group, an ether bond, a sulfonyl group, an amide bond, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group, R 11 and R 12 Each independently represents a hydroxyl group or an organic group containing an alcoholic hydroxyl group, R 11 and R 12 At least one of the organic groups is a primary hydroxyl group, R 13 to R 16 are each independently a C1-C4 alkyl group, a is an integer from 0 to 10, b and c are each independently 0 or 1, d to g are each independently 0, 1 or 2,

[0031] X 2 is a tetravalent organic group different from the group of formula (2),

[0032] p and q are positive integers satisfying 0.01≤p / (p+q)<1, and the dotted lines represent valence bonds.

[0033] Preferably, X 2 is a group selected from the following:

[0034]

[0035] The dotted lines represent valence bonds.

[0036] Typically, the colorant (F) is carbon black.

[0037] Preferably, component (D) comprises at least one compound selected from the group consisting of a polyfunctional epoxy compound having a bisphenol skeleton, a phenol novolac polyfunctional epoxy compound, and a polyfunctional epoxy silicone.

[0038] In another aspect, the present invention provides a photosensitive resin laminate comprising a supporting film layer, a photosensitive resin layer composed of the photosensitive resin composition defined above, and a cover film layer.

[0039] In another aspect, the present invention provides a pattern forming method comprising the steps of:

[0040] (i) forming a photosensitive resin film on a substrate using the photosensitive resin composition defined above, (ii) exposing the resin film to radiation, and (iii) developing the resin film in a developer, or

[0041] (i) forming a photosensitive resin film on a substrate using the photosensitive resin laminate defined above, (ii) exposing the resin film to radiation, and (iii) developing the resin film in a developer.

[0042] Beneficial effects of the present invention

[0043] The photosensitive resin composition cures to a product with high modulus and a relatively low coefficient of linear expansion, while remaining highly reliable. The cured product also exhibits excellent heat resistance, mechanical strength, solvent resistance, and adhesion to various substrates. Because the photosensitive resin composition maintains flexibility even in the B-stage, it can be processed into films. The inclusion of a colorant allows the cured product to be laser-marked. DETAILED DESCRIPTION

[0044] As used herein, the notation (Cn-Cm) indicates a group containing n to m carbon atoms per group. In chemical formulae, dashed lines represent valence bonds.

[0045] The present invention provides a photosensitive resin composition, which comprises (A) polyimide silicone, (B) a crosslinking agent, (C) a photoacid generator, (D) a multifunctional epoxy compound, (E) a filler and (F) a colorant.

[0046] (A) Polyimide silicone

[0047] Component (A) contains 1.0×10 -7 to 8.0×10 -3 The polyimide silicone (A) is preferably a polyimide silicone having a primary alcohol hydroxyl group content of 1 eq / g. If the content of primary alcohol hydroxyl groups is outside the above range, the resin film may peel from the substrate and the resin film in the unexposed area may be difficult to dissolve during development. As used herein, "primary alcohol hydroxyl group" refers to a hydroxyl group bonded to a primary carbon atom. That is, the polyimide silicone (A) has a primary alcohol structure.

[0048] Preferably, the polyimide silicone comprises a repeating unit having formula (1-1) and a repeating unit having formula (1-2).

[0049]

[0050] In formula (1-1), X 1 is a tetravalent group having the formula (2). The introduction of the repeating unit having the formula (1-1) makes the polymer main chain skeleton flexible and imparts flexibility to the resin itself.

[0051]

[0052] In formula (2), R 1 to R 6 Each independently represents a C1-C8 monovalent hydrocarbon group. The monovalent hydrocarbon group may be linear, branched, or cyclic. Examples include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, and hexyl, cycloalkyl groups such as cyclopentyl and cyclohexyl, aryl groups such as phenyl, aralkyl groups such as benzyl and phenethyl, and alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, and butenyl. In particular, methyl, ethyl, phenyl, and vinyl groups are preferred due to the availability of reactants.

[0053] In formula (2), R 7 and R 8 Each independently is a single bond or C1-C 12 Divalent hydrocarbon group. The divalent hydrocarbon group may be linear, branched or cyclic. Examples include methylene, ethane-1,1-diyl, ethane-1,2-diyl, propane-1,3-diyl, butane-1,4-diyl, benzene-1,4-diyl and biphenyl-4,4'-diyl. Preferably, R 7 and R 8 is a single bond, a methylene group, an ethane-1,2-diyl group, a propane-1,3-diyl group, or a benzene-1,4-diyl group.

[0054] In formula (2), R 9 and R 10Each is independently a trivalent organic group, preferably having 2 to 10 carbon atoms. Preferred examples of the trivalent organic group are shown below, but are not limited thereto.

[0055]

[0056] In formula (2), m is an integer from 0 to 120, preferably an integer from 3 to 80, and more preferably an integer from 5 to 50. When m ≥ 2, that is, when two or more siloxane units are included, the siloxane units may all be the same or have two or more different types. When two or more different types of siloxane units are included, they may be arranged randomly or alternately, or may include multiple blocks of the same type of siloxane units.

[0057] X 1 Typical groups of are shown below, but are not limited thereto.

[0058]

[0059] Among them, m 1 and m 2 are each independently 0 or an integer of at least 1, m 1 +m 2 =m;m 3 and m 4 are each independently 0 or an integer of at least 1, m 3 +m 4 =m;m 5 and m 6 are each independently 0 or an integer of at least 1, m 5 +m 6 =m, where m is an integer from 0 to 120 as defined above.

[0060] Preferably, the unit having a vinyl group and an aromatic group is included in an amount of 3 to 60% by weight of the total units. Within this range, the organic silicon portion becomes more compatible and the fracture strength of the cured product is improved.

[0061] X 1 Preferred groups are shown below.

[0062]

[0063] In formula (1-2), X 2 is a tetravalent organic group different from the group of formula (2). 2 Preferred groups are shown below, but are not limited thereto.

[0064]

[0065] In formulas (1-1) and (1-2), Y 1is a group having the formula (3).

[0066]

[0067] In formula (3), A 1 To A 3 Each is independently a single bond, a methylene group, an ether bond, a sulfonyl group, an amide bond, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group.

[0068] In formula (3), a is an integer of 0 to 10, preferably an integer of 1 to 10, b is 0 or 1, and c is 0 or 1.

[0069] In formula (3), R 11 and R 12 Each independently represents a hydroxyl group or an organic group containing an alcoholic hydroxyl group, R 11 and R 12 At least one of the organic groups is a primary hydroxyl group. Suitable organic groups containing a primary hydroxyl group include -OCH2CH(OH)CH2OH and -OCH(CH2OH)CH2OH.

[0070] In formula (3), R 13 to R 16 Each is independently a C1-C4 alkyl group. Suitable alkyl groups include methyl, ethyl, propyl and butyl, with methyl being preferred.

[0071] In formula (3), d to g are each independently 0, 1 or 2, preferably 0 or 1.

[0072] Examples of the group having the formula (3) are shown below, but are not limited thereto.

[0073]

[0074] In formulas (1-1) and (1-2), p and q are each independently a positive integer, preferably 1 ≤ p ≤ 500 and 1 ≤ q ≤ 500, more preferably 3 ≤ p ≤ 300 and 3 ≤ q ≤ 300, and satisfy 0.01 ≤ p / (p + q) < 1, preferably 0.1 ≤ p / (p + q) < 1, more preferably 0.2 ≤ p / (p + q) ≤ 0.95, and even more preferably 0.5 ≤ p / (p + q) ≤ 0.9. If p / (p + q) is less than 0.01, sufficient flexibility cannot be obtained.

[0075] The polyimide silicone may further comprise a repeating unit having the formula (1-3) and a repeating unit having the formula (1-4).

[0076]

[0077] In formulas (1-3) and (1-4), X 1 and X 2 As defined above. 2 is a divalent organic group different from the group having formula (3); r and s are each independently 0 or a positive integer, preferably 0≤r≤500 and 0≤s≤500, more preferably 0≤r≤300 and 0≤s≤300. When the polyimide silicone contains a repeating unit having formula (1-3) and a repeating unit having formula (1-4), the following relationship is satisfied: 0.01≤(p+r) / (p+q+r+s)<1.

[0078] Y 2 It is a divalent organic group different from the group of formula (3), that is, a divalent organic group not containing a primary hydroxyl group. Among such divalent organic groups, the divalent group of formula (4) is preferred.

[0079]

[0080] In formula (4), B 1 To B 3 Each is independently a single bond, a methylene group, an ether bond, a sulfonyl group, an amide bond, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group, and j and k are each independently 0 or 1.

[0081] Examples of the group having formula (4) are given below, but are not limited thereto.

[0082]

[0083] Also preferably, Y 2 is a divalent group having the formula (5).

[0084]

[0085] In formula (5), R 21 to R 24 Each independently represents a C1-C8 monovalent hydrocarbon group. The monovalent hydrocarbon group may be linear, branched, or cyclic. Examples include alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, and hexyl, cycloalkyl groups such as cyclopentyl and cyclohexyl, and aryl groups such as phenyl. In particular, methyl and phenyl groups are preferred due to the availability of reactants.

[0086] In formula (5), n is an integer of 1 to 80, preferably an integer of 1 to 20.

[0087] The polyimide silicone (A) may be a random or block copolymer. It should preferably have a weight average molecular weight (Mw) of 2,000 to 200,000, more preferably 4,000 to 100,000. Polymers with Mw within this range are easy to handle and cure to products with sufficient strength.

[0088] The polyimide silicone (A) can be prepared by first reacting a diamine having phenolic hydroxyl groups with an anhydride-modified silicone, an acid anhydride, and optionally a diamine free of phenolic hydroxyl groups and carboxyl groups to form a polyamic acid.

[0089] Examples of the diamine having a phenolic hydroxyl group include phenol-containing diamines such as

[0090] 3,3'-diamino-4,4'-dihydroxybiphenyl,

[0091] 2,2'-diamino-4,4'-dihydroxybiphenyl, 2,2-bis(4-amino-3-hydroxyphenyl)propane,

[0092] 2,2-bis(3-amino-4-hydroxyphenyl)propane, 9,9-bis(3-amino-4-hydroxyphenyl)fluorene,

[0093] 2,2'-methylenebis[6-(4-amino-3,5-dimethylbenzyl)-4-methyl]phenol,

[0094] 3,3'-diamino-4,4'-dihydroxydiphenyl ether, and

[0095] 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane.

[0096] Examples of the anhydride-modified silicone are shown below, but are not limited thereto.

[0097]

[0098] Among them, m and m 1 to m 6 As defined above.

[0099] An anhydride-modified organosilicon is obtained by reacting an acid anhydride having an unsaturated group, such as succinic anhydride, norbornene dicarboxylic anhydride, propyl nadic anhydride, or phthalic anhydride, with an organohydrogen polysiloxane. The number of siloxane units in the anhydride-modified polysiloxane corresponds to the number of siloxane units in the organohydrogen polysiloxane, and therefore, m in formula (2) represents the average number of siloxane units.

[0100] Examples of acid anhydrides include

[0101] 3,3',4,4'-diphenylsulfone tetracarboxylic dianhydride,

[0102] 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3',3,4'-biphenyltetracarboxylic dianhydride,

[0103] 5-(2,5-dioxotetrahydro-3-furyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride,

[0104] 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride,

[0105] 1,2,3,4-Butanetetracarboxylic dianhydride,

[0106] 3,3',4,4'-Benzophenonetetracarboxylic dianhydride,

[0107] 4,4'-Hexafluoropropylidene diphthalic dianhydride, 2,2-bis(trimellitoxyphenyl)propane,

[0108] 1,3-Tetramethyldisiloxane diphthalic dianhydride and 4,4'-oxydiphthalic dianhydride.

[0109] Examples of diamines containing no phenolic hydroxyl group and no carboxyl group include

[0110] 4,4'-diaminobenzanilide, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 3,3'-dimethyl-4,4'-diaminobiphenyl,

[0111] 4,4'-(p-phenylenediisopropylidene)diphenylamine, 4,4'-(m-phenylenediisopropylidene)diphenylamine,

[0112] 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenoxy)benzene,

[0113] 1,3-bis(3-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane,

[0114] 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane,

[0115] Bis[4-(4-aminophenoxy)phenyl]sulfone, Bis[4-(3-aminophenoxy)phenyl]sulfone,

[0116] 4,4'-bis(4-aminophenoxy)biphenyl and 9,9-bis(4-aminophenyl)fluorene.

[0117] In the synthesis of polyamic acid, the ratio of diamine to dianhydride can be appropriately determined depending on the desired molecular weight of the polyamide and is typically about 0.95 to 1.05, preferably 0.98 to 1.02, in terms of molar ratio. In order to introduce reactive functional groups at the ends of the polyimide silicone, an anhydride or amine compound having functional groups such as amino alcohol, aminothiol, or trimellitic anhydride can be added after the reaction and further reacted with the reaction product. The amount of the anhydride or amine compound having functional groups added at this time is preferably no more than 0.2 moles per mole of the anhydride or diamine component.

[0118] The reaction of diamine and dianhydride is typically carried out in a solvent. The solvent used herein is not particularly limited as long as the polyimide is soluble therein. Examples of solvents include ethers such as tetrahydrofuran and anisole; ketones such as cyclohexanone, 2-butanone, methyl isobutyl ketone, 2-heptanone, 2-octanone and acetophenone; esters such as butyl acetate, methyl benzoate and γ-butyrolactone; cellosolves such as butyl cellosolve acetate and propylene glycol monomethyl ether acetate; amides such as N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone; and aromatic hydrocarbons such as toluene and xylene. Among these, ketones, esters and cellosolves are preferred. In particular, γ-butyrolactone, propylene glycol monomethyl ether acetate, N,N-dimethylacetamide and N-methyl-2-pyrrolidone are most preferred. The solvents can be used alone or in combination. The amount of the solvent used is typically adjusted in consideration of the yield per batch and the viscosity of the solution, so that the concentration of the polyamic acid may be 10 to 40% by weight.

[0119] The resulting polyamic acid is then converted into a polyimide having a phenolic hydroxyl group through a dehydration cyclization reaction. The dehydration cyclization reaction can be carried out by heating a polyamic acid solution at a temperature of 80 to 250° C., preferably 150 to 220° C., or by adding an acetic anhydride / pyridine mixture to a polyamic acid solution and heating the resulting solution at about 50° C. The dehydration cyclization reaction then occurs on the acid amide portion of the polyamic acid to induce polyimidization.

[0120] Thereafter, the desired polyimide silicone can be obtained by reacting the reaction product with a primary alcohol having an epoxy group as shown below.

[0121]

[0122] The amount of epoxy-containing primary alcohol charged can be appropriately set depending on the desired content of primary alcohol hydroxyl groups to be introduced. Typically, the epoxy-containing primary alcohol is preferably used in an amount of 0.3 to 3 moles per mole of phenolic hydroxyl groups. The reaction temperature is typically about 40 to 180°C, preferably 60 to 160°C. The reaction time is preferably from several minutes to about 15 hours. A catalyst such as triethylamine may be added to accelerate the reaction.

[0123] After reacting the epoxy-containing primary alcohol, an acid anhydride may be reacted, if desired. Suitable anhydrides include phthalic anhydride, norbornene dicarboxylic anhydride, cyclohexyl dicarboxylic anhydride, methylcyclohexyl dicarboxylic anhydride, and succinic anhydride. By adding the necessary equivalent amount of anhydride and heating the mixture, a polyimide silicone having carboxyl groups and primary alcohol hydroxyl groups is obtained. The reaction temperature is typically about 10 to 120°C, preferably 20 to 90°C. The reaction time is preferably about 1 to 15 hours. A catalyst may be added to accelerate the reaction.

[0124] (B) Cross-linking agent

[0125] Component (B) is a cross-linking agent that initiates a cross-linking reaction with component (A) to promote pattern formation and enhance film strength.

[0126] Examples of the crosslinking agent include nitrogen-containing compounds containing an average of at least two methylol and / or alkoxymethyl groups per molecule, such as melamine compounds, guanamine compounds, glycoluril compounds and urea compounds, and condensates thereof, and phenol compounds containing an average of at least two methylol or alkoxymethyl groups per molecule.

[0127] Suitable melamine compounds include those having formula (6).

[0128]

[0129] Among them, R 31 to R 36 Each independently represents a hydroxymethyl group, a C2-C5 alkoxymethyl group or hydrogen, R 31 to R 36 At least two of the methyl groups are hydroxymethyl or alkoxymethyl. Typical alkoxymethyl groups are methoxymethyl and ethoxymethyl.

[0130] Examples of the melamine compound include trimethoxymethylmonomethylolmelamine, dimethoxymethylmonomethylolmelamine, trimethylolmelamine, hexamethylolmelamine, hexamethoxymethylmelamine, and hexaethoxymethylmelamine.

[0131] Examples of guanamine compounds include tetramethylolguanamine, tetramethoxymethylguanamine, and tetramethoxyethylguanamine. Examples of glycoluril compounds include tetramethylol glycoluril and tetra(methoxymethyl) glycoluril. Examples of urea compounds include tetramethylolurea, tetramethoxymethylurea, tetramethoxyethylurea, tetraethoxymethylurea, and tetrapropoxymethylurea.

[0132] Examples of the condensate of the nitrogen-containing compound include condensates of the nitrogen-containing compound and formaldehyde. Condensates of melamine compounds and condensates of urea compounds are preferred. The condensate of the nitrogen-containing compound can be prepared by any method known in the art.

[0133] Examples of the phenol compound containing an average of at least two hydroxymethyl or alkoxymethyl groups per molecule include (2-hydroxy-5-methyl)-1,3-benzenedimethanol and 2,2′,6,6′-tetramethoxymethylbisphenol A.

[0134] The appropriate amount of component (B) used is 0.5 to 50 parts by weight, more preferably 1 to 30 parts by weight per 100 parts by weight of component (A). As long as the amount of component (B) is within the above range, the composition is fully photocurable and can be used as a resist material. The aforementioned compounds as component (B) can be used alone or in combination.

[0135] (C) Photoacid generator

[0136] Component (C) is a photoacid generator (PAG), which is not particularly limited as long as it decomposes to produce acid when exposed to light. Preferred PAGs are compounds that decompose and produce acid when exposed to light of a wavelength of 240 to 500 nm. PAGs act as curing catalysts. Suitable examples of PAGs include onium salts, diazomethane derivatives, glyoxime derivatives, β-ketosulfone derivatives, disulfone derivatives, nitrobenzenemethylsulfonate derivatives, sulfonate derivatives, imidosulfonate derivatives, sulfonic acid oxime ester derivatives, imidosulfonate derivatives, and triazine derivatives.

[0137] Examples of the onium salt include sulfonium salts having the formula (7) and iodonium salts having the formula (8).

[0138]

[0139] Among them, R 41 to R 45 Each is independently an optionally substituted C1-C 12 Alkyl, optionally substituted C6-C 12 Aryl or optionally substituted C7-C 12 Aralkyl. A - It is a non-nucleophilic counterion.

[0140] Alkyl groups may be linear, branched or cyclic, and examples include methyl, ethyl, n-propyl, isopropyl, cyclopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, cyclobutyl, n-pentyl, cyclopentyl, cyclohexyl, norbornyl and adamantyl. Suitable aryl groups include phenyl, naphthyl and biphenyl. Suitable aralkyl groups include benzyl and phenethyl. Suitable substituents include oxo, linear, branched or cyclic C1-C 12 Alkoxy, linear, branched or cyclic C1-C 12 Alkyl, C6-C 24 Aryl, C7-C 25 Arylalkyl, C6-C24 Aryloxy and C6-C 24 Arylthio.

[0141] R 41 to R 45 Preferably, the group is selected from optionally substituted alkyl groups such as methyl, ethyl, propyl, butyl, cyclohexyl, norbornyl, adamantyl, and 2-oxocyclohexyl; optionally substituted aryl groups such as phenyl, naphthyl, biphenyl, 2-, 3-, or 4-methoxyphenyl, ethoxyphenyl, 3- or 4-tert-butoxyphenyl, 2-, 3-, or 4-methylphenyl, ethylphenyl, 4-tert-butylphenyl, 4-butylphenyl, dimethylphenyl, terphenyl, biphenyloxyphenyl, and biphenylthiophenyl; and optionally substituted aralkyl groups such as benzyl and phenethyl. In particular, optionally substituted aryl groups and optionally substituted aralkyl groups are preferred.

[0142] Examples of non-nucleophilic counterions include halides such as chloride and bromide; fluoroalkanesulfonate ions such as trifluoromethanesulfonate, 1,1,1-trifluoroethanesulfonate, and nonafluorobutanesulfonate; arylsulfonate ions such as toluenesulfonate, benzenesulfonate, 4-fluorobenzenesulfonate, and 1,2,3,4,5-pentafluorobenzenesulfonate; alkanesulfonate ions such as methanesulfonate and butanesulfonate; and hexafluorophosphate and fluorinated alkylfluorophosphate ions.

[0143] Diazomethane derivatives include compounds having the formula (9).

[0144]

[0145] Among them, R 51 and R 52 Each independently is C1-C 12 Alkyl or haloalkyl, optionally substituted C6-C 12 Aryl or optionally substituted C7-C 12 Aralkyl.

[0146] Examples of alkyl groups are as described above for R 41 to R 45 Examples of the haloalkyl group include a trifluoromethyl group, a 1,1,1-trifluoroethyl group, a 1,1,1-trichloroethyl group, and a nonafluorobutyl group.

[0147] Examples of optionally substituted aryl groups include phenyl, alkoxyphenyl such as 2-, 3- or 4-methoxyphenyl, 2-, 3- or 4-ethoxyphenyl, 3- or 4-tert-butoxyphenyl, alkylphenyl such as 2-, 3- or 4-methylphenyl, ethylphenyl, 4-tert-butylphenyl, 4-butylphenyl, dimethylphenyl, and halogenated aryl such as fluorophenyl, chlorophenyl and 1,2,3,4,5-pentafluorophenyl. Examples of optionally substituted aralkyl groups include benzyl and phenethyl.

[0148] Glyoxime derivatives include compounds having the formula (10).

[0149]

[0150] Among them, R 61 to R 64 Each independently is C1-C 12 Alkyl or haloalkyl, optionally substituted C6-C 12 Aryl or optionally substituted C7-C 12 Aralkyl. R 63 and R 64 may be bonded together with the carbon atoms to which they are attached to form a ring, and in the case of a ring, R 63 and R 64 The combination is a straight chain or branched C1-C 12 Alkanediyl.

[0151] Examples of alkyl, haloalkyl, optionally substituted aryl and optionally substituted aralkyl are as described above for R 51 and R 52 Examples of the linear or branched alkanediyl group include methylene, ethanediyl, propanediyl, butanediyl, and hexanediyl.

[0152] Suitable onium salts include

[0153] Diphenyliodonium trifluoromethanesulfonate,

[0154] (p-tert-Butoxyphenyl)phenyliodonium trifluoromethanesulfonate,

[0155] Diphenyliodonium p-toluenesulfonate,

[0156] (p-tert-Butoxyphenyl)phenyliodonium p-toluenesulfonate,

[0157] Triphenylsulfonium trifluoromethanesulfonate,

[0158] (p-tert-Butoxyphenyl)diphenylsulfonium trifluoromethanesulfonate,

[0159] Bis(p-tert-butoxyphenyl)phenylsulfonium trifluoromethanesulfonate,

[0160] Tris(p-tert-butoxyphenyl)sulfonium trifluoromethanesulfonate,

[0161] Triphenylsulfonium p-toluenesulfonate,

[0162] (p-tert-Butoxyphenyl)diphenylsulfonium p-toluenesulfonate,

[0163] Bis(p-tert-butoxyphenyl)phenylsulfonium p-toluenesulfonate,

[0164] Tris(p-tert-butoxyphenyl)sulfonium p-toluenesulfonate,

[0165] Triphenylsulfonium nonafluorobutanesulfonate, triphenylsulfonium butanesulfonate,

[0166] Trimethylsulfonium trifluoromethanesulfonate, trimethylsulfonium p-toluenesulfonate,

[0167] Cyclohexylmethyl (2-oxocyclohexyl) sulfonium trifluoromethanesulfonate,

[0168] Cyclohexylmethyl (2-oxocyclohexyl) sulfonium p-toluenesulfonate,

[0169] Dimethylphenylsulfonium trifluoromethanesulfonate,

[0170] Dimethylphenylsulfonium p-toluenesulfonate,

[0171] Dicyclohexylphenylsulfonium trifluoromethanesulfonate,

[0172] Dicyclohexylphenylsulfonium p-toluenesulfonate,

[0173] Bis(4-tert-butylphenyl)iodonium hexafluorophosphate,

[0174] Diphenyl (4-thiophenoxyphenyl) sulfonium hexafluoroantimonate,

[0175] [4-(4-biphenylthio)phenyl]-4-biphenylphenylsulfonium tris(trifluoromethanesulfonyl)methide,

[0176] Triphenylsulfonium tetrakis(fluorophenyl)borate,

[0177] Tris[4-(4-acetylphenyl)thiophenyl]sulfonium tetrakis(fluorophenyl)borate,

[0178] triphenylsulfonium tetrakis(pentafluorophenyl)borate, and

[0179] Tris[4-(4-acetylphenyl)thiophenyl]sulfonium tetrakis(pentafluorophenyl)borate.

[0180] Suitable diazomethane derivatives include

[0181] Bis(phenylsulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane,

[0182] Bis(xylenesulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane,

[0183] Bis(cyclopentylsulfonyl)diazomethane, bis(n-butylsulfonyl)diazomethane,

[0184] Bis(isobutylsulfonyl)diazomethane, Bis(sec-butylsulfonyl)diazomethane,

[0185] Bis(n-propylsulfonyl)diazomethane, Bis(isopropylsulfonyl)diazomethane,

[0186] Bis(tert-butylsulfonyl)diazomethane, Bis(n-pentylsulfonyl)diazomethane,

[0187] Bis(isopentylsulfonyl)diazomethane, bis(sec-pentylsulfonyl)diazomethane,

[0188] Bis(tert-amylsulfonyl)diazomethane,

[0189] 1-cyclohexylsulfonyl-1-(tert-butylsulfonyl)diazomethane,

[0190] 1-cyclohexylsulfonyl-1-(tert-amylsulfonyl)diazomethane, and

[0191] 1-tert-Amylsulfonyl-1-(tert-butylsulfonyl)diazomethane.

[0192] Suitable glyoxime derivatives include

[0193] Bis-O-(p-toluenesulfonyl)-α-dimethylglyoxime,

[0194] Bis-O-(p-toluenesulfonyl)-α-diphenylglyoxime,

[0195] Bis-O-(p-toluenesulfonyl)-α-dicyclohexylglyoxime,

[0196] Bis-O-(p-toluenesulfonyl)-2,3-pentanedione glyoxime,

[0197] Bis-O-(p-toluenesulfonyl)-2-methyl-3,4-pentanedione glyoxime,

[0198] Bis-O-(n-butanesulfonyl)-α-dimethylglyoxime,

[0199] Bis-O-(n-butanesulfonyl)-α-diphenylglyoxime,

[0200] Bis-O-(n-butanesulfonyl)-α-dicyclohexylglyoxime,

[0201] Bis-O-(n-butanesulfonyl)-2,3-pentanedione glyoxime,

[0202] Bis-O-(n-butanesulfonyl)-2-methyl-3,4-pentanedione glyoxime,

[0203] Bis-O-(methylsulfonyl)-α-dimethylglyoxime,

[0204] Bis-O-(trifluoromethanesulfonyl)-α-dimethylglyoxime,

[0205] Bis-O-(1,1,1-trifluoroethanesulfonyl)-α-dimethylglyoxime,

[0206] Bis-O-(tert-butanesulfonyl)-α-dimethylglyoxime,

[0207] Bis-O-(perfluorooctanesulfonyl)-α-dimethylglyoxime,

[0208] Bis-O-(cyclohexanesulfonyl)-α-dimethylglyoxime,

[0209] Bis-O-(phenylsulfonyl)-α-dimethylglyoxime,

[0210] Bis-O-(p-fluorophenylsulfonyl)-α-dimethylglyoxime,

[0211] Bis-O-(p-tert-butylbenzenesulfonyl)-α-dimethylglyoxime,

[0212] Bis-O-(ditoluenesulfonyl)-α-dimethylglyoxime, and

[0213] Bis-O-(camphorsulfonyl)-α-dimethylglyoxime;

[0214] Suitable β-ketosulfone derivatives include

[0215] 2-cyclohexylcarbonyl-2-(p-toluenesulfonyl)propane, and

[0216] 2-Isopropylcarbonyl-2-(p-toluenesulfonyl)propane.

[0217] Suitable disulfone derivatives include diphenyl disulfone and dicyclohexyl disulfone.

[0218] Suitable nitrobenzenemethylsulfonate derivatives include

[0219] 2,6-Dinitrobenzyl p-toluenesulfonate and 2,4-Dinitrobenzyl p-toluenesulfonate.

[0220] Suitable sulfonate derivatives include

[0221] 1,2,3-Tris(methanesulfonyloxy)benzene, 1,2,3-tris(trifluoromethanesulfonyloxy)benzene and 1,2,3-tris(p-toluenesulfonyloxy)benzene.

[0222] Suitable imide sulfonate derivatives include phthalimidoyl triflate, phthalimidoyl tosylate, 5-norbornene-2,3-dicarboxyimidotriflate, 5-norbornene-2,3-dicarboxyimidotosylate, 5-norbornene-2,3-dicarboxyimidon-butylsulfonate, and N-trifluoromethylsulfonyloxynaphthyl imide.

[0223] A typical sulfonic acid oxime ester derivative is α-(phenylsulfonyloxyimino)-4-methylphenylacetonitrile.

[0224] Suitable imidosulfonate derivatives include (5-(4-methylphenyl)sulfonyloxyimino-5H-thiophen-2-ylidene)-(2-methylphenyl)acetonitrile and [5-(4-(4-methylphenylsulfonyloxy)phenylsulfonyloxyimino)-5H-thiophen-2-ylidene]-(2-methylphenyl)acetonitrile.

[0225] Suitable triazine derivatives include

[0226] 2-(Methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine,

[0227] 2-[2-(3,4-dimethoxyphenyl)vinyl]-4,6-bis(trichloromethyl)-s-triazine,

[0228] 2-[2-(Furan-2-yl)vinyl]-4,6-bis(trichloromethyl)-s-triazine, and

[0229] 2-[2-(5-methylfuran-2-yl)vinyl]-4,6-bis(trichloromethyl)-s-triazine.

[0230] Among PAG (C), onium salts are preferred, and sulfonium salts are more preferred.

[0231] The appropriate amount of component (C) used is 0.05 to 20 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of component (A). As long as the amount of component (C) is within the above range, the composition is fully photocurable and can be effectively cured in the form of a thick film. The aforementioned compounds as component (C) can be used alone or in combination.

[0232] (D) Multifunctional epoxy compounds

[0233] Component (D) is a multifunctional epoxy compound that undergoes a crosslinking reaction with the base polymer (i.e., component (A)) upon thermal curing of the patterned resin film, contributing to the reliability of the film and the adhesion of the film to the substrate (hereinafter referred to as "substrate adhesion").

[0234] Examples of the polyfunctional epoxy compound include glycidyl ether forms of phenol, alicyclic epoxy compounds having a cyclohexene oxide group, and those obtained by introducing an epoxy compound having an unsaturated bond into an organosiloxane having a hydrosilyl group by a hydrosilylation reaction.

[0235] In the glycidyl ether form of phenol, the phenol structure can be a novolac, bisphenol, biphenyl, phenol aralkyl, dicyclopentadiene, naphthalene or amino-containing type. Suitable glycidyl ether forms of phenol include glycidyl ethers of bisphenol A, bisphenol AD, bisphenol S and bisphenol F types, glycidyl ethers of hydrogenated bisphenol A, glycidyl ethers of ethylene oxide adducted bisphenol A, glycidyl ethers of propylene oxide adducted bisphenol A, glycidyl ethers of phenol novolac resins, glycidyl ethers of cresol novolac resins, glycidyl ethers of naphthalene resins, glycidyl ethers of dicyclopentadiene phenol novolac resins and trifunctional epoxy forms of aminophenols.

[0236] Alicyclic epoxy compounds having a cyclohexene oxide group include tetrakis(3,4-epoxycyclohexylmethyl)-modified ε-caprolactone butane tetracarboxylate and compounds shown below.

[0237]

[0238] Compounds obtained by introducing an epoxy compound having an unsaturated bond into an organosiloxane having a hydrosilyl group through a hydrosilylation reaction include reaction products obtained by reacting an epoxy compound having an unsaturated bond such as allyl glycidyl ether or vinylcyclohexyl epoxide with an organosiloxane having a hydrosilyl group.

[0239] Illustrative examples of such compounds include epoxy-containing organopolysiloxanes having formula (11), epoxy-containing cyclosiloxanes having formula (12), and bis-silyl-substituted compounds having formula (13).

[0240]

[0241]

[0242] In formulas (11) to (13), R A to R DEach independently is an organic group containing an epoxy group. Preferred examples of organic groups containing an epoxy group include, but are not limited to, alkyl groups containing an epoxy group, such as glycidyloxypropyl and cyclohexylepoxyethyl. Among these, glycidyloxypropyl is most preferred as R A to R D .

[0243] In formulas (11) to (13), R 61 to R 70 、R 81 to R 83 、R 92 and R 93 Each independently represents a C1-C8 monovalent hydrocarbon group. Suitable monovalent hydrocarbon groups are as described above for R in formula (2). 1 to R 6 The example given.

[0244] In formula (11), R 71 is hydrogen or C1-C8 alkyl. Suitable alkyl groups include methyl, ethyl, propyl, butyl, pentyl, hexyl and octyl.

[0245] In formula (11), z 1 to z 6 is an integer in the following range: 0≤z 1 ≤10, 0≤z 2 ≤10, 0≤z 3 ≤30, 0≤z 4 ≤100, 0≤z 5 ≤10, 0≤z 6 ≤20, z 1 +z 3 ≥2,0.1≤(z 1 +z 3 ) / (z 1 +z 2 +z 3 +z 4 )≤1 and 0≤(z 5 +z 6 ) / (z 1 +z 2 +z 3 +z 4 +z 5 +z 6 )≤0.05.

[0246] In formula (12), z 11 and z 12 is an integer in the following range: 2≤z 11 ≤10, 0≤z 12 ≤20 and 0.2≤z 11 / (z 11 +z12 )≤1.

[0247] In formula (13), R 91 C2-C 24 Divalent organic groups. Divalent organic groups can be linear, branched, or cyclic. Examples include alkanediyl groups such as ethanediyl, propanediyl, and hexanediyl, cycloalkanediyl groups such as cyclopentanediyl and cyclohexanediyl, divalent aromatic groups such as phenylene and biphenyldiyl, and groups obtained by combining a plurality of such groups.

[0248] In formula (13), z 21 and z 22 are each independently an integer from 1 to 3.

[0249] Examples of the epoxy-containing organopolysiloxane having the formula (11) are shown below, but are not limited thereto.

[0250]

[0251] Here, x is preferably an integer of 1 to 10, and y is preferably an integer of 1 to 5.

[0252] Examples of the epoxy-containing cyclosiloxane having the formula (12) are shown below, but are not limited thereto.

[0253]

[0254] Examples of the bis-silyl-substituted compound having the formula (13) are shown below, but are not limited thereto.

[0255]

[0256] The amount of component (D) used is preferably 0.05 to 100 parts by weight, more preferably 0.1 to 50 parts by weight, and even more preferably 1 to 30 parts by weight per 100 parts by weight of component (A). As long as the amount of component (D) is within the above range, the composition cures into a film having improved toughness and substrate adhesion. The aforementioned compounds as component (D) can be used alone or in combination.

[0257] (E) Filler

[0258] Component (E) is a filler, which is typically selected from silicon dioxide, aluminum oxide, silicon nitride and titanium dioxide, but is not limited thereto. The filler surface may or may not be modified before use. Modified fillers are preferred because better transparency can be expected. For example, silane coupling agents, titanate coupling agents and organosilyl chlorides can be used for surface modification of the filler.

[0259] The filler should have an average particle size of 0.01 to 20.0 μm, preferably 0.05 to 3.0 μm. An average particle size of less than 0.01 μm leads to increased costs, while a size exceeding 20.0 μm results in a loss of transparency. The average particle size is measured as a volume average, i.e., a 50% cumulative particle diameter (D 50 ) or median diameter.

[0260] The amount of component (E) used is 1 to 70 parts by weight, preferably 10 to 40 parts by weight, per 100 parts by weight of component (A). If the amount is less than the above range, the filling effect is less likely to be exerted. Excessive filler reduces the transparency of the film and prevents the film from receiving a sufficient dose of light during the exposure step. The aforementioned compounds as component (E) can be used alone or in combination.

[0261] (F) Colorant

[0262] Component (F) is a colorant, which is typically selected from pigments and dyes. In particular, carbon black is preferred from the viewpoint of laser marking. The amount of component (F) used is 0.01 to 30 parts by weight, preferably 0.1 to 10 parts by weight, and more preferably 0.8 to 5 parts by weight per 100 parts by weight of component (A). Component (F) less than 0.01 parts by weight achieves very little coloring effect. Component (F) greater than 30 parts by weight causes a significant drop in transmittance, resulting in problems of insufficient curing during exposure and side reactions that interfere with the cross-linking reaction. The aforementioned compounds as component (F) can be used alone or in combination.

[0263] (G) Organic solvents

[0264] If necessary, the photosensitive resin composition may further contain (G) an organic solvent. Preferred are solvents in which components (A), (B), (C) and (D) are soluble and components (E) and (F) are dispersible.

[0265] Examples of the organic solvent include ketones such as cyclohexanone, cyclopentanone, and methyl-2-n-pentyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, t-butyl acetate, t-butyl propionate, propylene glycol mono-t-butyl ether acetate, and γ-butyrolactone; and amides such as N-methyl-2-pyrrolidone and N,N-dimethylacetamide.

[0266] Among the above organic solvents, preferred are propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, cyclohexanone, cyclopentanone, methyl isobutyl ketone, γ-butyrolactone and mixtures thereof, in which PAG is most soluble.

[0267] The organic solvent as component (G) is preferably used in an amount of 20 to 90 wt %, more preferably 30 to 65 wt % of the resin composition. As long as the amount of component (G) is within the range, components (A) to (D) remain fully compatible and effectively coat the composition. The aforementioned solvents as component (G) can be used alone or in combination.

[0268] Other components

[0269] In addition to the aforementioned components, the photosensitive resin composition may further contain any other components. Surfactants and adhesion promoters are exemplary.

[0270] Surfactants are effective in improving the properties of coatings. Preferred surfactants are nonionic surfactants, such as fluorochemical surfactants, such as perfluoroalkyl polyoxyethylene ethanols, fluorinated alkyl esters, perfluoroalkyl amine oxides, and fluorinated organosiloxane compounds. These surfactants are commercially available. Illustrative examples include 3M's FC-4430 from AGC Seimi Chemical Co., Ltd. S-141 and S-145 from Daikin Industries Ltd. DS-401, DS-4031, and DS-451 from DIC Corp. F-8151, and X-70-093 from Shin-Etsu Chemical Co., Ltd. Preferred surfactants are Fluorad FC-4430 and X-70-093. The amount of surfactant is preferably 0.03 to 5 parts by weight, more preferably 0.1 to 3 parts by weight, based on 100 parts by weight of component (A). The aforementioned surfactants can be used alone or in combination.

[0271] Adhesion promoters are effective in improving adhesion properties. Suitable adhesion promoters include silane coupling agents and hydrolysis condensates (or oligomers) thereof, and commercially available adhesion promoters. Suitable epoxy silane coupling agents can be obtained under the trade names of KBM-403, KBM-402, KBE-403 and KBE-402, and suitable amine silane coupling agents can be obtained under the trade names of KBM-903, KBM-603 and KBM-573, all of which are from Shin-Etsu Chemical Co., Ltd. The amount of adhesion promoter is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of component (A). The aforementioned adhesion promoters can be used alone or in combination.

[0272] In addition, a light absorber may be added to improve the light absorption efficiency of the PAG, etc. Suitable light absorbers include diaryl sulfoxides, diaryl sulfones, 9,10-dimethylanthracene, and 9-fluorenone. A basic compound may be added for sensitivity adjustment. Suitable basic compounds include tertiary amine compounds such as triethanolamine, and nitrogen-containing compounds such as benzotriazole and pyridine. The amount of these additives is not particularly limited, as long as it does not impair the benefits of the present invention.

[0273] In one embodiment, the photosensitive resin composition is used as a resist material. In this embodiment, any other optional components commonly used in resist materials can be added. The amount of the optional components is not particularly limited as long as the benefits of the present invention are not impaired.

[0274] The photosensitive resin composition of the present invention can be prepared by any conventional method. For example, it can be prepared by stirring and mixing the aforementioned components and optional organic solvents and additives, and optionally passing the mixture through a filter.

[0275] Photosensitive resin laminate

[0276] The photosensitive resin composition of the present invention can be processed into a film before use. When the photosensitive resin composition is processed into a film, another embodiment of the present invention is a photosensitive resin laminate comprising a support film layer, a photosensitive resin layer formed from the photosensitive resin composition on the support film layer, and a coating layer disposed on the photosensitive resin layer.

[0277] The support film will support the photosensitive resin layer and is preferably selected from polyester, polyimide, polyamide, polyamideimide, polyetherimide, cellulose triacetate, polyethersulfone and polyphenylene sulfide resins. The support film may be a multilayer film.

[0278] Suitable polyesters include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polyethylene naphthalate (PEN).

[0279] The thickness of the support film is not particularly limited, but is preferably 10 to 500 μm, more preferably 35 to 200 μm. A thickness within the range ensures that the support film has sufficient flexibility to handle the photosensitive resin laminate and provide efficient processing, with minimum necessary rigidity.

[0280] Regarding the thickness of the photosensitive resin laminate, the total thickness of the resin film layer and the support film layer is preferably 15 to 700 μm, more preferably 25 to 300 μm, and even more preferably 30 to 200 μm. A total thickness of at least 15 μm ensures easy handling of the laminate. A total thickness of at most 700 μm ensures good thermal conductivity, making it easy to attach the laminate to a substrate.

[0281] The photosensitive resin layer can be formed by coating a photosensitive resin composition onto a support film and heating the coating to remove the solvent.

[0282] When the photosensitive resin laminate is applied or applied to the substrate, any suitable device can be used, such as a vacuum laminator, a pressure vacuum laminator, a belt laminator, or a vacuum belt laminator. The receiving substrate is preferably heated so that the photosensitive resin layer of the photosensitive resin laminate softens and is tightly bonded to the substrate.

[0283] The photosensitive resin composition is also used as a protective film for semiconductor devices, a protective film for cables, a cover film, a solder resist, and a micromachining photoresist material.

[0284] Pattern formation method

[0285] Another embodiment of the present invention is a method for forming a pattern on a substrate using a photosensitive resin composition. The method comprises the following steps: (i) forming a photosensitive resin film on a substrate using the photosensitive resin composition or a photosensitive resin laminate, (ii) exposing a resist film to radiation, and (iii) developing the resist film with a developer.

[0286] Step (i) is to form a photosensitive resin film on a substrate using a photosensitive resin composition or a photosensitive resin laminate. Examples of substrates include silicon, glass, quartz wafers, silicon nitride substrates, silicon dioxide substrates, plastic substrates such as phenolic paper, glass epoxy resin and polyimide, ceramic circuit boards, and substrates having a resin coating on their surfaces.

[0287] The photosensitive resin film can be formed on the substrate by any well-known method. For example, the photosensitive resin composition is applied to the substrate by dip coating, spin coating or roller coating. The thickness of the photosensitive resin film can be appropriately selected according to the desired application and situation, for example, in the range of 0.1 to 300 μm. Alternatively, the photosensitive resin film can be formed on the substrate by using a photosensitive resin laminate, peeling off the coating layer and laminating the photosensitive resin layer of the laminate to the substrate, thereby transferring the photosensitive resin layer to the substrate.

[0288] For efficient photocuring reaction, the photosensitive resin composition may be preheated to evaporate the solvent, etc. The preheating may be performed, for example, at 40 to 140° C. for about 1 minute to 1 hour.

[0289] In step (ii), the photosensitive resin film is exposed to radiation, preferably radiation having a wavelength of 240 to 500 nm. The photosensitive resin film is cured during exposure. The exposure can be performed through a photomask. The photomask can be a mask perforated with a desired pattern. The photomask is preferably capable of shielding radiation having a wavelength of 240 to 500 nm. In this sense, the photomask is preferably, for example, a photomask having a chromium light-shielding film, but is not limited thereto.

[0290] The radiation having a wavelength of 240 to 500 nm may be radiation emitted by a radiation generator, for example, UV radiation such as g-line or i-line or deep-UV (248 nm). The exposure dose is preferably, for example, 10 to 5,000 mJ / cm 2 If necessary, the exposure step may be followed by a post-exposure bake (PEB) to further increase the development sensitivity. PEB may be performed, for example, at 40 to 140° C. for about 0.5 to 10 minutes.

[0291] Following the exposure or PEB step, step (iii) is performed: developing the exposed resin film with a developer. The developer used herein is preferably selected from organic solvent developers, such as dimethylacetamide and cyclohexanone, and alkaline aqueous solutions, such as aqueous solutions of tetramethylammonium hydroxide (TMAH) and sodium carbonate. Development can typically be performed by immersing the pattern-wise exposed film in the developer. If necessary, development is followed by washing, rinsing, and drying. The desired pattern of the photosensitive resin film is obtained.

[0292] The patterned film can be further heated in an oven or on a hot plate at 70 to 300°C, preferably 120 to 300°C, for about 10 minutes to 10 hours to increase the crosslinking density and remove any remaining volatile components. This results in a cured resin film with tight substrate adhesion and satisfactory heat resistance, strength, and electrical properties.

[0293] When it is desired to form a uniform or flat film, the above-described method for forming a pattern may be followed without using a photomask.

[0294] The cured film obtained by the photosensitive resin composition has satisfactory substrate adhesion, heat resistance and electrical insulation properties, and is advantageously used as a protective film for electrical or electronic components and semiconductor components. A pattern of finer size can be formed. The cured film with satisfactory substrate adhesion, electrical and mechanical properties can also be used as a protective film for semiconductor components, a protective film for cables, a coating film, a solder resist, etc.

[0295] Example

[0296] Examples of the present invention are given below by way of illustration and not by way of limitation.In the examples, the weight average molecular weight (Mw) is measured by GPC relative to polystyrene standards using tetrahydrofuran (THF) solvent.

[0297] The anhydride-modified silicones (S-1), (S-2), and (S-3) used in the examples were identified as follows.

[0298]

[0299] [1] Synthesis of polyimide silicone

[0300] Synthesis example 1

[0301] A flask equipped with a stirrer, a thermometer, and a nitrogen purge line was charged with 62.0 g (0.2 mol) of 4,4'-oxydiphthalic dianhydride, 302.3 g (0.3 mol) of anhydride-modified silicone (S-1), and 800 g of N-methyl-2-pyrrolidone. 183.1 g (0.5 mol) of 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane was added to the flask in a controlled manner so that the temperature of the reaction solution did not exceed 50°C. Stirring was continued at room temperature for 10 hours. After a reflux condenser with a water trap was connected to the flask, 120 g of xylene was added to the flask, which was heated at 170°C and maintained at that temperature for 6 hours, at which point the solution turned brown. The brown solution was cooled to room temperature (25°C), which was a solution of polyimide silicone with phenolic hydroxyl groups.

[0302] 25.0 g of glycidol was added to the polyimide silicone solution, which was heated at 120° C. for 3 hours. At the end of the reaction, the reaction solution was cooled to room temperature and poured into methanol for precipitation. The precipitate was filtered and dried to obtain the desired polyimide silicone (A-1) having primary alcohol hydroxyl groups. 1 Analysis of polyimide silicone (A-1) by H-NMR spectroscopy revealed a decrease in the 10 ppm peak attributable to phenolic hydroxyl groups, while peaks at 4.6 ppm and 4.8 ppm attributable to primary and secondary hydroxyl groups were observed. These data indicate that polyimide silicone (A-1) is a polymer of the formula shown below. GPC analysis revealed that polyimide silicone (A-1) had an Mw of 19,000. The primary hydroxyl group content was 0.00046 eq / g.

[0303]

[0304] Synthesis example 2

[0305] A flask equipped with a stirrer, thermometer, and nitrogen purge line was charged with 111.1 g (0.25 mol) of 4,4'-hexafluoropropylidene diphthalic dianhydride, 264.0 g (0.25 mol) of anhydride-modified silicone (S-2), and 800 g of γ-butyrolactone. 183.1 g (0.5 mol) of 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane was added to the flask in a controlled manner so that the temperature of the reaction solution did not exceed 50°C. Stirring was continued at room temperature for 10 hours. After connecting a reflux condenser with a water trap to the flask, 120 g of xylene was added to the flask, which was heated at 170°C and maintained at that temperature for 6 hours, at which point the solution turned brown. The brown solution was cooled to room temperature (25°C), which was a solution of polyimide silicone with phenolic hydroxyl groups.

[0306] 26.2 g of glycidol was added to the polyimide silicone solution, which was heated at 120°C for 3 hours. At the end of the reaction, the reaction solution was cooled to room temperature and poured into methanol for precipitation. The precipitate was filtered and dried to obtain the desired polyimide silicone (A-2) having primary alcohol hydroxyl groups. 1 Analysis of polyimide silicone (A-2) by H-NMR spectroscopy revealed a decrease in the 10 ppm peak attributable to phenolic hydroxyl groups, while peaks at 4.6 ppm and 4.8 ppm attributable to primary and secondary hydroxyl groups were observed. These data indicate that polyimide silicone (A-2) is a polymer of the formula shown below. GPC analysis revealed that polyimide silicone (A-2) had an Mw of 18,100. The primary hydroxyl group content was 0.00056 eq / g.

[0307]

[0308] Synthesis example 3

[0309] A flask equipped with a stirrer, a thermometer, and a nitrogen purge line was charged with 62.0 g (0.2 mol) of 4,4'-oxydiphthalic dianhydride, 325.0 g (0.2 mol) of anhydride-modified organosilicon (S-3), and 800 g of γ-butyrolactone. 73.3 g (0.2 mol) of 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane and 58.5 g (0.2 mol) of 1,3-bis(3-aminophenoxy)benzene were added to the flask in a controlled manner so that the temperature of the reaction solution did not exceed 50°C. 1.1 g (0.01 mol) of p-aminophenol was then added. Stirring was continued at room temperature for 10 hours. After a reflux condenser with a water trap was connected to the flask, 250 g of xylene was added to the flask, which was heated at 170°C and maintained at that temperature for 6 hours, at which point the solution turned brown. The brown solution was cooled to room temperature (25° C.), which was a solution of polyimide silicone having phenolic hydroxyl groups.

[0310] 22.4 g of glycidol was added to the polyimide silicone solution, which was heated at 120° C. for 3 hours. At the end of the reaction, the reaction solution was cooled to room temperature and poured into methanol for precipitation. The precipitate was filtered and dried to obtain the desired polyimide silicone (A-3) having primary hydroxyl groups. 1 Analysis of polyimide silicone (A-3) by H-NMR spectroscopy revealed a decrease in the 10 ppm peak attributable to phenolic hydroxyl groups, while peaks at 4.6 ppm and 4.8 ppm attributable to primary and secondary hydroxyl groups were observed. These data indicate that polyimide silicone (A-3) is a polymer of the formula shown below. GPC analysis revealed that polyimide silicone (A-3) had an Mw of 19,700.

[0311] The content of primary hydroxyl groups was 0.00029 eq / g.

[0312]

[0313] Synthesis example 4

[0314] A flask equipped with a stirrer, thermometer, and nitrogen purge line was charged with 91.6 g (0.25 mol) of 4,4'-oxydiphthalic dianhydride, 406.2 g (0.25 mol) of anhydride-modified organosilicon (S-3), and 1,000 g of γ-butyrolactone. 146.5 g (0.40 mol) of 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane and 29.2 g (0.10 mol) of 1,3-bis(3-aminophenoxy)benzene were added to the flask in a controlled manner, so that the temperature of the reaction solution did not exceed 50°C. 2.7 g (0.025 mol) of p-aminophenol was then added. Stirring was continued at room temperature for 10 hours. After connecting a reflux condenser with a water trap to the flask, 300 g of xylene was added to the flask, which was heated at 170°C and maintained at that temperature for 6 hours, at which point the solution turned brown. The brown solution was cooled to room temperature (25° C.), which was a solution of polyimide silicone having phenolic hydroxyl groups.

[0315] 30.1 g of glycidol was added to the polyimide silicone solution, which was heated at 120°C for 3 hours. At the end of the reaction, the reaction solution was cooled to room temperature and poured into methanol for precipitation. The precipitate was filtered and dried to obtain the desired polyimide silicone (A-4) having primary alcohol hydroxyl groups. 1 Analysis of polyimide silicone (A-4) by H-NMR spectroscopy revealed a decrease in the 10 ppm peak attributable to phenolic hydroxyl groups, while peaks at 4.6 ppm and 4.8 ppm attributable to primary and secondary hydroxyl groups were observed. These data indicate that polyimide silicone (A-4) is a polymer of the formula shown below. GPC analysis revealed that polyimide silicone (A-4) had an Mw of 18,400. The primary hydroxyl group content was 0.00039 eq / g.

[0316]

[0317] Comparative Synthesis Example 1

[0318] A flask equipped with a stirrer, a thermometer, and a nitrogen purge line was charged with 62.0 g (0.2 mol) of 4,4'-oxydiphthalic dianhydride, 302.3 g (0.3 mol) of anhydride-modified silicone (S-1), and 800 g of N-methyl-2-pyrrolidone. 183.1 g (0.5 mol) of 2,2-bis(4-amino-3-hydroxyphenyl)hexafluoropropane was added to the flask in a controlled manner so that the temperature of the reaction solution did not exceed 50°C. Stirring was continued at room temperature for 10 hours. After a reflux condenser with a water trap was connected to the flask, 120 g of xylene was added to the flask, which was heated at 170°C and maintained at that temperature for 6 hours, at which point the solution turned brown. The brown solution was cooled to room temperature (25°C) and poured into methanol for precipitation. The precipitate was filtered and dried to obtain a polyimide silicone (A'-1) having phenolic hydroxyl groups. Upon GPC analysis, the polyimide silicone (A'-1) had an Mw of 17,800.

[0319] [2] Preparation and evaluation of photosensitive resin compositions

[0320] Examples 1 to 16 and Comparative Examples 1 to 8

[0321] The photosensitive resin composition was prepared by combining components (A) to (G), stirring and mixing them according to the formulations shown in Tables 1 and 2. The components were identified as follows.

[0322] (A) Polyimide silicone:

[0323] Polyimide silicones A-1 to A-4 and A'-1

[0324] (B) Cross-linking agents: B-1 and B-2

[0325]

[0326] (C)PAG: C-1 and C-2

[0327]

[0328] (D) Multifunctional epoxy compounds:

[0329] D-1: Epikote 828, difunctional epoxy resin, Mitsubishi Chemical Corp.

[0330] D-2: 2021P, difunctional epoxy resin, Daicel Corp.

[0331] (E) Filling:

[0332] E-1: Silicon dioxide, average particle size 0.5 μm, Admatechs

[0333] E-2: Silica, average particle size 8.0 μm, Admatechs

[0334] E-3: Silica, average particle size 20.0 μm, Admatechs

[0335] (F) Colorant:

[0336] F-1: Carbon black, pigment, Mitsubishi Chemical Corp.

[0337] F-2: 1821, dye, Orient Chemical Industries Co.,Ltd.

[0338] (G) Solvent:

[0339] G-1: Cyclopentanone

[0340] G-2: Propylene glycol monomethyl ether

[0341] Table 1

[0342]

[0343] Table 2

[0344]

[0345] [Preparation of Photosensitive Resin Laminate]

[0346] Each of the photosensitive resin compositions in Tables 1 and 2 was applied to a 100 μm thick PET support film using a doctor blade. The coating was dried in a dryer at 100°C for 10 minutes to form a 50 μm thick photosensitive resin layer on the PET film. A polyethylene coating was placed on the photosensitive resin layer to complete the photosensitive resin laminate. Evaluation was performed using the following test. The thickness of the resin layer was measured using a contact thickness gauge.

[0347] Patterning test

[0348] The covering film was peeled off from the laminate to expose the photosensitive resin layer. The photosensitive resin layer was bonded to an 8-inch silicon wafer with the aid of a film laminator, after which the PET support film was peeled off. The photosensitive resin layer was transferred onto the silicon wafer. The resin layer was dried by heating at 90° C. for 2 minutes on a hot plate. The photosensitive resin layer was exposed to 2,000 mJ / cm using a Mask Aligner MA8 (SUSS MicroTec AG, light source wavelength: broadband) through a quartz mask with equally spaced holes of 200 μm in diameter. 2 A broad spectrum of UV radiation with a dose of 100 nm was applied. After exposure, the resin layer was heated on a hot plate at 90°C for 2 minutes, cooled, and immersed in a 2.38 wt% TMAH aqueous solution for 5 minutes to dissolve the unexposed areas, forming a pattern. Samples were rated "OK" when the pattern was formed and the holes reached the bottom, and "NG" when the holes did not reach the bottom. The results are shown in Tables 3 and 4.

[0349] Laser marking test

[0350] The cover film was peeled off from the laminate to expose the photosensitive resin layer. The photosensitive resin layer was bonded to an 8-inch silicon wafer with the aid of a film laminator, after which the PET support film was peeled off. The photosensitive resin layer was transferred onto the silicon wafer. The resin layer was dried by heating at 90°C for 2 minutes on a hot plate. The entire surface of the resin layer was irradiated with 800 mJ / cm without using a mask. 2 The resin layer was exposed to radiation of a wavelength of 365 nm at a dose of 100 nm. After exposure, the resin layer was heated at 90° C. for 2 minutes, cooled, and heated at 200° C. for 2 hours to cure. The resin layer was laser marked under the following irradiation conditions using a laser marking machine MD-V9900 (Keyence Corp.): 1,064 nm, 5 W, and 0.6 seconds. When the laser mark could be visually read, the sample was rated as "OK", and when the laser mark was not read or the imprinted mark was too thin to be read, the sample was rated as "NG". The results are shown in Tables 3 and 4.

[0351] Flexibility test

[0352] The photosensitive resin laminate was wound around a plastic cylinder with a diameter of 8.5 cm, held for 10 seconds, and unwound. The laminate was observed for abnormalities. When there was no change, the sample was rated as "OK", and when cracked or broken, the sample was rated as "NG". The results are shown in Tables 3 and 4.

[0353] Transmittance measurement

[0354] The transmittance of light of wavelength 365 nm of the photosensitive resin layer (in the photosensitive resin laminate) was measured using a spectrophotometer U-3900H (Hitachi High-Tech Science Corp.).

[0355] Physical properties

[0356] The photosensitive resin layer was exposed as is, heated in an oven at 90°C for 2 minutes, and then heated again in an oven at 200°C for 2 hours to cure. The modulus of the cured film was measured using a viscoelasticity meter DMA7100 (Hitachi High-Tech Science Corp.) while heating from -10°C to 320°C. The modulus was read at 25°C. The results are shown in Tables 3 and 4.

[0357] Table 3

[0358]

[0359] Table 4

[0360]

[0361] As can be seen from the data, the compositions of Examples 1 to 16 exhibited improved resolution and satisfactory properties as photosensitive materials. The cured films had sufficient modulus.

[0362] Japanese Patent Application No. 2018-056546 is incorporated herein by reference.

[0363] While certain preferred embodiments have been described, numerous modifications and variations are possible in light of the above teachings. It will therefore be understood that the present invention may be practiced otherwise than as specifically described without departing from the scope of the appended claims.

Claims

1. A photosensitive resin composition comprising: (A) contains 1.0×10 -7 Up to 8.0×10 -3 eq / g of primary alcohol hydroxyl polyimide silicone, (B) a cross-linking agent, (C) a photoacid generator, (D) a polyfunctional epoxy compound, (E) a filler having an average particle size of 0.01 to 20.0 μm in an amount of 1 to 70 parts by weight per 100 parts by weight of the polyimide silicone (A), and (F) a colorant in an amount of 0.01 to 30 parts by weight per 100 parts by weight of the polyimide silicone (A), wherein the colorant (F) is carbon black. 2 . The composition according to claim 1 , further comprising (G) an organic solvent.

3. The composition according to claim 2, wherein the organic solvent is at least one solvent selected from propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, cyclohexanone, cyclopentanone, methyl isobutyl ketone and γ-butyrolactone.

4. The composition according to claim 1, wherein the polyimide silicone (A) comprises a repeating unit having the formula (1-1) and a repeating unit having the formula (1-2): Where X 1 is a tetravalent group having formula (2): Where R 1 To R 6 Each independently is C 1 -C 8 Monovalent hydrocarbon group, R 7 and R 8 Each independently is a single bond or C 1 -C 12 Divalent hydrocarbon group, R 9 and R 10 Each is independently a trivalent organic group, m is an integer from 0 to 120, and the dotted line represents a valence bond, Y 1 is a group having formula (3): Among them A 1 To A 3 Each is independently a single bond, a methylene group, an ether bond, a sulfonyl group, an amide bond, a propane-2,2-diyl group, a 1,1,1,3,3,3-hexafluoropropane-2,2-diyl group or a fluorene-9,9-diyl group, R 11 and R 12 Each independently represents a hydroxyl group or an organic group containing an alcoholic hydroxyl group, R 11 and R 12 At least one of them is an organic group containing a primary alcohol hydroxyl group, R 13 To R 16 Each independently is C 1 -C 4 alkyl, a is an integer from 0 to 10, b and c are each independently 0 or 1, d to g are each independently 0, 1 or 2, X 2 is a tetravalent organic group different from the group of formula (2), p and q are positive integers satisfying 0.01≤p / (p+q)<1, and the dotted lines represent valence bonds.

5. The composition according to claim 4, wherein X 2 is a group selected from the following: The dotted lines represent valence bonds.

6. The composition according to claim 1, wherein component (D) comprises at least one compound selected from the group consisting of a polyfunctional epoxy compound having a bisphenol skeleton, a phenol novolac polyfunctional epoxy compound, and a polyfunctional epoxy silicone. 7 . A photosensitive resin laminate comprising a support film layer, a photosensitive resin layer composed of the photosensitive resin composition according to claim 1 , and a coating layer.

8. A pattern forming method, wherein The following steps are involved: (i) forming a photosensitive resin film on a substrate using the photosensitive resin composition according to claim 1, (ii) exposing the resin film to radiation, and (iii) developing the resin film with a developer.

9. A method for forming a pattern, wherein The following steps are involved: (i) forming a photosensitive resin film on a substrate using the photosensitive resin laminate according to claim 7, (ii) exposing the resin film to radiation, and (iii) developing the resin film with a developer.