A method for determining FLD0 of steel plate

By calculating FLD0 in the simulation test of the steel plate forming limit curve, the problem of cumbersome steps and unsuitability for ultra-low carbon steel in the existing technology is solved, and fast and accurate FLD0 calculation is achieved, which is suitable for a variety of steel plate thicknesses and reduces the cost. Cost and time expenditure.

CN110851964BActive Publication Date: 2024-10-29TIANLAN NEW ENERGY VEHICLE (HAINAN) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN201911032896.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-10-28
Publication Date
2024-10-29
Estimated Expiration
2039-10-28

AI Technical Summary

Technical Problem

The existing technology is cumbersome and time-consuming to determine the forming limit curve (FLC) of steel plates, is not suitable for ultra-low carbon steel, and the empirical formulas are insufficient in accuracy and universality.

Method used

By establishing a cupping mold sample model, use simulation software to set the blank holder force, draw bead strength, friction coefficient and stamping speed to conduct a rigid die bulging simulation test, set observation points to detect the mesh thinning rate, and calculate the main plane strain Strain FLD0 value, suitable for ultra-low carbon steel and simplifying the operation process.

Benefits of technology

It achieves fast calculation of FLD0, reduces cost and time expenditure, improves measurement accuracy and applicability, is suitable for a variety of steel plate thicknesses, and the calculation results are close to the empirical formula with small errors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110851964B_ABST
    Figure CN110851964B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for determining FLD0 of a steel plate, comprising the following steps: step S1: establishing a sample model of a cupping die, setting the blank holder force, drawbead strength, friction coefficient and punching speed through simulation software, and performing a rigid die bulging simulation test; step S2: setting a first observation point and a second observation point on the sample model, the first observation point and the second observation point are both located at the middle position of the wide side of the sample model, the first observation point is located at 3 / 8 of the long side of the sample model, and the second observation point is located at 5 / 8 of the long side of the sample model; step S3: the first observation point and the second observation point detect whether the grid thinning rate reaches a set threshold, and if so, record the current principal strain value and secondary strain value; step S4: substituting the principal strain value and the secondary strain value into the strain value formula, and calculating the value of the principal strain FLD0 at the plane strain. Compared with the prior art, the present invention has the advantages of being applicable to ultra-low carbon steel, reducing costs, and saving time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a determination method, and in particular to a method for determining FLD0 of a steel plate. Background Art

[0002] Since Keeler and Goodwin established the metal sheet forming limit curve FLC by experimental methods in the 1860s, FLC has been widely used in sheet metal forming analysis and is a key indicator for forming material selection.

[0003] The FLC obtained by experiment is generally based on GB / T 15825.8 "Metal Sheet Formability and Test Methods - Guide for Determination of Forming Limit Diagram FLD", but it is easily affected by test conditions and human factors, and the FLC of different grades of steel plates or even different batches of the same grade of steel plates are different. Since the test method is expensive and time-consuming to obtain FLC, people often use empirical formulas or prediction models to replace the test method to obtain FLC, so as to achieve twice the result with half the effort.

[0004] In the 1980s, North American steel mills studied the FLC of different steel plates and believed that the shapes of the FLC of steel plates were basically similar, and the main difference was the value of the principal strain FLD0 at the plane strain.

[0005] The Keeler formula is a widely known and used empirical formula, which is mainly related to the thickness and n value of the steel plate, but is limited to low carbon steel and low alloy steel, and is not applicable to ultra-low carbon steel; the Arcelor V9 empirical formula is mainly related to the thickness of the steel plate and the mechanical properties in the vertical rolling direction, including uniform elongation, tensile strength and r value. The empirical formula has strict requirements on the performance of the steel plate: tensile strength is 260-1500MPa, thickness is 0.5-3.5mm, and r value is between 0.6-3.

[0006] Chinese patent CN103424318A discloses a method of determining FLD0 through CAE simulation and experiment, and then fitting the Keeler empirical formula to obtain FLC. However, this method still requires experimental steps and is overall cumbersome and time-consuming. Summary of the invention

[0007] The purpose of the present invention is to provide a method for determining FLD0 of a steel plate in order to overcome the defects of the above-mentioned prior art in that the steps are complicated and time-consuming and not applicable to ultra-low carbon steel.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] A method for determining FLD0 of a steel plate comprises the following steps:

[0010] Step S1: Establish a sample model of the cupping die, set the blank holder force, drawbead strength, friction coefficient and punching speed through simulation software, and conduct a rigid die bulging simulation test;

[0011] Step S2: setting a first observation point and a second observation point on the sample model, wherein the first observation point and the second observation point are both located at the middle of the wide side of the sample model, the first observation point is located at 3 / 8 of the long side of the sample model, and the second observation point is located at 5 / 8 of the long side of the sample model;

[0012] Step S3: any one of the first observation point and the second observation point detects whether the grid thinning rate reaches a set threshold, and if so, records the current principal strain value and secondary strain value;

[0013] Step S4: Substitute the principal strain value and the secondary strain value into the strain value formula to calculate the value of the principal strain FLD0 at the plane strain.

[0014] The strain value formula is specifically:

[0015]

[0016] Among them, y is the principal strain value, x is the secondary strain value, is the weighted mean of the plastic strain ratio, and k is the proportional coefficient.

[0017] The proportionality coefficient k takes a value of 0.9 when the plastic strain ratio anisotropy Δr is less than 0.3, and takes a value of 1 when the plastic strain ratio anisotropy Δr is greater than or equal to 0.3.

[0018] The threshold value of the grid thinning rate is set to 0.2.

[0019] The friction coefficient has a value interval of 0.1-0.13, and the drawbead strength has a value interval of 0.5-0.9.

[0020] The punching speed is set at 2 mm / s to 50 mm / s.

[0021] The punch of the cupping mold is a cylindrical ball head with a diameter of 100 mm.

[0022] The thickness of the steel plate is less than 3 mm. When the thickness of the steel plate is less than 1 mm, the inner hole diameter of the concave die of the cupping mold is 102 mm. When the thickness of the steel plate is between 1-3 mm, the inner hole diameter of the concave die of the cupping mold is 106 mm.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention can calculate FLD0 by only recording the principal strain value and the secondary strain value in the simulation process, and the operation steps are simple and applicable to ultra-low carbon steel.

[0025] 2. The present invention only needs to conduct one test after the simulation parameters are set, and only sets observation points at the 3 / 8 and 5 / 8 positions. Compared with the method in the prior art that requires multiple measurements, it reduces costs and saves a lot of time.

[0026] 3. The inner hole diameter of the concave die of the sample model of the present invention is set according to the thickness of the steel plate, and is applicable to steel plates of various thicknesses. The threshold value is set to 0.2 to make the calculation result closer to the result of the empirical formula, thereby improving the measurement accuracy and reducing the error. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of the process of the present invention;

[0028] Figure 2 A schematic diagram of observation points on the sample model of the present invention;

[0029] Figure 3 A schematic diagram of the dimensions of a sample model of an embodiment of the present invention;

[0030] Figure 4 Schematic diagram of FLD0 calculation results of various steel materials according to an embodiment of the present invention.

[0031] Reference numerals:

[0032] 1-first observation point; 2-second observation point. DETAILED DESCRIPTION

[0033] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0034] like Figure 1 As shown, a method for determining FLD0 of a steel plate comprises the following steps:

[0035] Step S1: Establish a sample model of the cupping die, set the blank holder force, drawbead strength, friction coefficient and punching speed through simulation software, and conduct a rigid die bulging simulation test;

[0036] Step S2: Figure 2 As shown, a first observation point and a second observation point are set on the sample model, and the first observation point and the second observation point are both located in the middle of the wide side of the sample model, the first observation point is located at 3 / 8 of the long side of the sample model, and the second observation point is located at 5 / 8 of the long side of the sample model;

[0037] Step S3: any one of the first observation point and the second observation point detects whether the grid thinning rate reaches a set threshold, and if so, records the current principal strain value and secondary strain value;

[0038] Step S4: Substitute the principal strain value and the secondary strain value into the strain value formula to calculate the value of the principal strain FLD0 at the plane strain.

[0039] The strain value formula is as follows:

[0040]

[0041] Among them, y is the principal strain value, x is the secondary strain value, is the weighted mean of the plastic strain ratio, and k is the proportional coefficient.

[0042] The proportionality coefficient k is 0.9 when the plastic strain ratio anisotropy Δr is less than 0.3, and is 1 when the plastic strain ratio anisotropy Δr is greater than or equal to 0.3.

[0043] The threshold value of the mesh thinning ratio is set to 0.2.

[0044] The value range of the friction coefficient is 0.1-0.13, and the value range of the drawbead strength is 0.5-0.9.

[0045] The punching speed is set between 2 mm / s and 50 mm / s.

[0046] Other types of ultra-low temperature steels include deep drawing steel, extra deep drawing steel, ultra deep drawing steel, high strength IF steel and bake hardening steel. Figure 4 ,When the threshold of the mesh thinning rate is set to 0.2, it is close to the result of the Arcelor V9 empirical formula and has the lowest error rate.

[0047] Embodiment 1

[0048] HC220BD+Z steel with a thickness of 1.2 mm is used as the test steel. The specific material performance parameters are shown in Table 2:

[0049] Table 2 HC220BD+Z material performance parameters

[0050]

[0051] like Figure 3 As shown, the punch of the cupping die is set to a cylindrical ball head with a diameter of 100 mm, the inner diameter of the die is 106 mm, the blank holding force is set to 200 KN, the drawbead strength is set between 0.5-0.9, the friction coefficient is set between 0.1-0.13, and the stamping speed is set at 2-50 mm / s.

[0052] The simulation parameters of Autoform are shown in Table 1:

[0053] Table 1 Autoform simulation parameters

[0054] parameter Settings Maximum refinement level 10 Main element size 20.00mm Initial subdivision level 1 / 4 Drawing component type EPS-11

[0055] When the grid thinning rate is detected to be 0.2 at the observation point, the principal strain value y=0.208 and the secondary strain value x=0.017 are recorded. Substituting into the strain value formula, FLD0=0.319 is obtained. The comparison results with the Keeler formula and Arcelor V9 empirical formula are shown in Table 3:

[0056] Table 3 FLD0 result comparison table

[0057]

[0058] The error rate with Keeler's formula is 8%, and the error rate with Arcelor V9 empirical formula is 1%, both of which are within the acceptable range.

[0059] In addition, it should be noted that the specific embodiments described in this specification may be named differently, and the above contents described in this specification are merely examples of the structure of the present invention. Any small or simple changes made based on the structure, features and principles of the present invention are included in the protection scope of the present invention. Those skilled in the art of the present invention may make various modifications or supplements to the specific examples described or adopt similar methods, as long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for determining FLD0 of a steel plate, It is characterized in that The following steps are involved: Step S1: Establish a sample model of the cupping die, set the blank holder force, drawbead strength, friction coefficient and punching speed through simulation software, and conduct a rigid die bulging simulation test; Step S2: setting a first observation point and a second observation point on the sample model, wherein the first observation point and the second observation point are both located at the middle of the wide side of the sample model, the first observation point is located at 3 / 8 of the long side of the sample model, and the second observation point is located at 5 / 8 of the long side of the sample model; Step S3: any one of the first observation point and the second observation point detects whether the grid thinning rate reaches a set threshold, and if so, records the current principal strain value and secondary strain value; Step S4: Substituting the principal strain value and the secondary strain value into the strain value formula, the value of the principal strain FLD0 at the plane strain is calculated; The strain value formula is specifically: Among them, y is the principal strain value, x is the secondary strain value, is the weighted mean of the plastic strain ratio, and k is the proportional coefficient.

2. A method for determining FLD0 of a steel plate according to claim 1, It is characterized in that The proportionality coefficient k takes a value of 0.9 when the ratio of the anisotropy plastic strain to the anisotropy Δr is less than 0.3, and takes a value of 1 when the ratio of the anisotropy plastic strain to the anisotropy Δr is greater than or equal to 0.

3.

3. A method for determining FLD0 of a steel plate according to claim 1, It is characterized in that The threshold value of the grid thinning rate is set to 0.

2.

4. A method for determining FLD0 of a steel plate according to claim 1, It is characterized in that The friction coefficient has a value interval of 0.1-0.13, and the drawbead strength has a value interval of 0.5-0.

9.

5. A method for determining FLD0 of a steel plate according to claim 1, It is characterized in that The punching speed is set at 2 mm / s to 50 mm / s.

6. A method for determining FLD0 of a steel plate according to claim 1, It is characterized in that The punch of the cupping mold is a cylindrical ball head with a diameter of 100 mm.

7. A method for determining FLD0 of a steel plate according to claim 1, It is characterized in that The thickness of the steel plate is less than 3 mm. When the thickness of the steel plate is less than 1 mm, the inner hole diameter of the concave die of the cupping mold is 102 mm. When the thickness of the steel plate is between 1-3 mm, the inner hole diameter of the concave die of the cupping mold is 106 mm.

Citation Information

Patent Citations

  • Method for determination of forming limit curve of sheet metal

    CN103424318A

  • Apparatus for separating trim from a fluid conveying medium

    EP0110055A2

  • Method for evaluating stiffness performance of automotive stamping part

    CN107796604A

  • Method and device for evaluating quality of steel

    JP2019098394A

  • Hot rolled steel sheet and method for producing same

    WO2012121219A1