Composite positive electrode active material, positive electrode and lithium battery each comprising the same, and method for preparing the composite positive electrode active material
By using a composite material of a layered structure of lithium nickel transition metal oxide and lithium metal oxide in the positive electrode active material of lithium battery and forming a metal oxide coating film on the surface, the performance deterioration and thermal stability of nickel battery are solved. The problem of insufficient results enables higher cycle characteristics and battery life.
Patent Information
- Application Number
- CN201910603189.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-10-25
- Filing Date
- 2019-07-05
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-07-05
AI Technical Summary
The existing nickel-based positive electrode active materials have deteriorated battery performance due to side reactions caused by the mixing of lithium and cations, and lack thermal stability, which cannot meet the requirements of high energy density and long life.
Using composite positive electrode active materials, including secondary particles of lithium nickel transition metal oxides and lithium metal oxides with layered crystal structures, the surface is covered with metal oxides, such as cobalt and group 2 elements, to form stable through heat treatment The coating film inhibits the elution and side reaction of lithium and nickel ions.
It significantly improves the circulation characteristics and thermal stability of lithium batteries, extends battery life, and reduces battery performance deterioration and gas generation.
Smart Images

Figure CN111106328B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2018-0128324 filed in the Korean Intellectual Property Office on October 25, 2018, and all rights arising therefrom, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present disclosure relates to a composite positive electrode active material, a positive electrode and a lithium battery each including the same, and a method for preparing the composite positive electrode active material. Background Art
[0004] In order to improve the miniaturization and performance of various devices, high energy density is becoming important in addition to the miniaturization and lightness of lithium batteries. In order to implement lithium batteries that meet such importance, nickel-based positive electrode active materials with high capacity are being studied.
[0005] Existing nickel-based positive electrode active materials exhibit deteriorated life characteristics due to a large amount of lithium remaining on the surface of the active material and side reactions caused by cation mixing and fail to provide satisfactory thermal stability. Therefore, a nickel-based positive electrode active material that effectively prevents degradation of battery performance is required. Summary of the invention
[0006] Provided is a composite positive electrode active material capable of effectively preventing degradation of battery performance.
[0007] A positive electrode including the composite positive electrode active material is provided.
[0008] A lithium battery including the positive electrode is provided.
[0009] A method for preparing the composite positive electrode active material is provided.
[0010] Additional aspects will be set forth in part in the description which follows and, in part, will be apparent from the description, or may be learned by practice of the presented embodiments.
[0011] According to an aspect of an embodiment, a composite positive electrode active material includes: secondary particles; and a coating layer on the surface of the secondary particles, wherein the secondary particles include a plurality of primary particles, and wherein the plurality of primary particles include a lithium nickel transition metal oxide having a layered crystal structure; and a grain boundary between the primary particles of the plurality of primary particles, the grain boundary including a lithium metal oxide having a crystal structure different from that of the lithium nickel transition metal oxide having a layered crystal structure and represented by Formula 1, wherein the coating layer on the surface of the secondary particles includes a metal oxide, the metal oxide including cobalt, and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof,
[0012] Formula 1
[0013] Li a M1 b O c
[0014] Wherein, in Formula 1, M1 is zirconium, manganese, silicon, molybdenum, palladium, Co, nickel, titanium, tin, iridium, platinum, aluminum, ruthenium, or a combination thereof, and
[0015] Among them, 1.9≤a≤4, 0.9≤b≤1.1 and 2.9≤c≤4.
[0016] According to an aspect of an embodiment, a positive electrode includes the composite positive electrode active material.
[0017] According to an aspect of an embodiment, a lithium battery includes the positive electrode.
[0018] According to aspects of an embodiment, the method for preparing the composite positive electrode active material includes: mixing a lithium nickel transition metal oxide having a layered crystal structure and a precursor of a metal oxide to obtain a composite positive electrode active material composition; and heat treating the composite positive electrode active material composition at a temperature of about 400°C to about 1000°C in an oxidizing atmosphere to prepare a composite positive electrode active material.
[0019] The lithium nickel transition metal oxide having a layered crystal structure can be prepared using a method comprising: mixing a precursor of a lithium nickel transition metal oxide having a layered crystal structure with a precursor of a compound represented by Formula 1 to prepare a mixture; and heat treating the mixture at a temperature of about 400° C. to about 1000° C. in an oxidative atmosphere. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] These and / or other aspects will become apparent and more readily understood from the following description of the embodiments considered in conjunction with the accompanying drawings, in which:
[0021] Figure 1 is a schematic diagram illustrating an embodiment of the structure of a composite positive electrode active material;
[0022] Figure 2A and 2B is a scanning electron microscope image of the composite positive electrode active material of Example 1;
[0023] Figure 3 is a graph showing the results of X-ray diffraction ("XRD") analysis of the composite positive active material of Example 1, showing intensity (arbitrary unit (au)) versus diffraction angle (degrees, 2 theta, 2θ);
[0024] Figures 4A to 4Eare high-angle annular dark-field scanning transmission electron microscopy ("HAADF STEM") and energy-dispersive X-ray spectroscopy ("EDS") images showing a cross section of the composite positive active material of Example 1;
[0025] Figure 5 is a graph of voltage (volt (V)) versus capacity (milliampere-hour (mAh)) showing capacity change according to voltage of lithium batteries of Manufacturing Examples 9 and 11;
[0026] Figure 6 is a graph showing the capacity retention rate (percent (%)) versus the cycle number, showing the change in the capacity retention rate of each of the lithium batteries of Manufacturing Examples 9 and 11;
[0027] Figure 7 and 8 are scanning electron microscope images showing cross sections of positive electrodes of lithium batteries of Manufacturing Examples 9 and 11 after charge and discharge cycles, respectively; and
[0028] Fig. 9 is a diagram of an embodiment of a lithium battery. DETAILED DESCRIPTION
[0029] Embodiments will now be described in detail, examples of which are shown in the accompanying drawings, wherein the same reference numerals represent the same elements throughout. In this regard, the present embodiment may have different forms and should not be construed as being limited to the description set forth herein. Therefore, the following description of the embodiments is to explain various aspects only by reference to the accompanying drawings. As used herein, the term "and / or" includes any and all combinations of one or more of the related listed items. Statements such as "at least one (individual)" modify the entire list of elements without modifying the individual elements of the list when before or after the list of elements.
[0030] It will be understood that when an element is referred to as being “on” another element, it can be directly on the other element or intervening elements may be present therebetween. In contrast, when an element is referred to as being “directly on” another element, there are no intervening elements present.
[0031] It will be understood that although the terms "first", "second", "third", etc. may be used herein to describe various elements, components (parts), regions, layers and / or parts, these elements, components (parts), regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish an element, component (part), region, layer or part from another element, component (part), region, layer or part. Therefore, without departing from the teachings herein, the "first element", "component (part)", "region", "layer" or "part" discussed below may be referred to as a second element, component (part), region, layer or part.
[0032] It will be understood that when used in this specification, the terms "include" or "comprises" indicate the presence of the described features, regions, wholes, steps, operations, elements and / or components (parts), but do not exclude the presence or addition of one or more other features, regions, wholes, steps, operations, elements, components (parts) and / or collections thereof.
[0033] As used herein, "about" includes the stated value and means within an acceptable range of deviation for a particular value determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations of the stated value, or within ±30%, 20%, 10%, or 5%.
[0034] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those commonly understood by those of ordinary skill in the art to which the present disclosure belongs. It will be further understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the present disclosure and the relevant art, and will not be interpreted in an idealized or over-formal sense unless explicitly defined as such herein.
[0035] Exemplary embodiments are described herein with reference to cross-sectional views as schematic diagrams of idealized embodiments. Therefore, variations from the illustrated shapes due to, for example, manufacturing techniques and / or tolerances are expected. Therefore, the embodiments described herein should not be interpreted as being limited to the specific shapes of the regions as shown herein, but rather include deviations in shape, for example, caused by manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. Moreover, the sharp corners shown may be rounded. Therefore, the regions shown in the figures are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions and are not intended to limit the scope of the claims.
[0036] The C rate refers to the current that discharges the battery in one hour, for example, the C rate for a battery with a discharge capacity of 1.6 ampere-hours is 1.6 amperes.
[0037] Hereinafter, a composite cathode active material, a method of preparing the composite cathode active material, and a lithium battery including the composite cathode active material according to an embodiment will be described in more detail.
[0038] A composite positive electrode active material according to an embodiment of the present disclosure includes secondary particles including a plurality of primary particles and a coating film (e.g., a coating layer) on the surface of the secondary particles, wherein the plurality of primary particles include a lithium nickel transition metal oxide having a layered crystal structure, a grain boundary between the primary particles includes a lithium metal oxide having a crystal structure different from that of the lithium nickel transition metal oxide and represented by the following Formula 1, and the coating film on the surface of the secondary particles includes a metal oxide including cobalt (Co) and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof:
[0039] Formula 1
[0040] Li a M1 b O c
[0041] Wherein, in Formula 1, M1 is zirconium (Zr), manganese (Mn), silicon (Si), molybdenum (Mo), palladium (Pd), Co, nickel (Ni), titanium (Ti), tin (Sn), iridium (Ir), platinum (Pt), aluminum (Al), ruthenium (Ru), or a combination thereof,
[0042] 1.9≤a≤4, 0.9≤b≤1.1 and 2.9≤c≤4. The metal for M1 includes a semi-metal such as Si.
[0043] The lithium metal oxide represented by Formula 1 has a monoclinic crystal structure and may be, for example, Li 2 ZrO 3 , Li 2 TiO 3 , Li 4 SiO 4 , Li 2 SiO 3 , or a combination thereof.
[0044] In the metal oxide containing Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof included in the coating film disposed on the surface of the secondary particle, the Group 2 element may be, for example, magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), or a combination thereof. The Group 12 element may be, for example, zinc, and the Group 13 element may be, for example, aluminum, gallium, indium, thallium, or a combination thereof.
[0045] The metal oxide including Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof may be a compound represented by Formula 2:
[0046] Formula 2:
[0047] Li x Co a Me b Oc
[0048] Among them, in Formula 2, Me is a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof.
[0049] 0 ≤ x ≤ 1.1, 0 < a ≤ 3, 0 < b ≤ 3, and 1 ≤ c ≤ 4.1.
[0050] As can be seen in Formula 2, when x = 0, the cobalt composite oxide containing Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof does not contain lithium.
[0051] The above Formula 2 can be understood as including the compositional formula (empirical formula) of the elements shown in Formula 2.
[0052] According to an embodiment, the metal oxide may be Co 3 O 4 , MgO, Li x CoO 2 where 0 < x ≤ 1.5, or a combination thereof, and the metal oxide may be, for example, a mixture of Co 3 O 4 and MgO, a Co 3 O 4 ·MgO composite, a mixture of LiCoO 2 and MgO, a LiCoO 2 ·MgO composite, a mixture of LiCoO 2 and Co 3 O 4 , a LiCoO 2 ·Co 3 O 4 composite, a mixture of LiCoO 2 , Co 3 O 4 and MgO, or a LiCoO 2 ·Co 3 O 4 ·MgO composite.
[0053] In Formula 2, x is, for example, from 0 to 1.09, from 0.01 to 1.09, or from 0.1 to 1.05, a is from 1 to 3, b is from 1 to 3, and c is from 1 to 4 or from 1.9 to 4.1.
[0054] In Formula 2, Me is aluminum (Al), gallium (Ga), magnesium (Mg), calcium (Ca), barium (Ba), zinc (Zn), or a combination thereof.
[0055] The compound of Formula 2 is, for example, Li x Co a Al b O 4, Li x Co a Zn b O 4 , Li x Co a Mg b O 4 , Li x Co a Ga b O 4 , Li x Co a Ca b O 4 or Li x Co a Ba b O 4 , where 1 ≤ x ≤ 1.1, 0 < a < 2, 0 < b < 2 and 0 < a + b ≤ 2, for example 1 ≤ x ≤ 1.1, 0.2 < a < 1.9, 0.2 < b < 1.9 and 0 < a + b ≤ 2. In one embodiment, a is less than b, and in one embodiment, a is greater than b.
[0056] The compound of formula 2 is for example LiCo 1.5 Al 0.5 O 4 , LiCo 1.5 Ga 0.5 O 4 , LiCo 1.33 Ga 0.67 O 4 , LiCo 1.33 Ca 0.67 O 4 , LiCo 1.33 Ba 0.67 O 4 , LiCo 1.33 Zn 0.67 O 4 , LiCo 1.2 Mg 0.8 O 4 , LiCo 1.2 Ga 0.8 O 4 , LiCo 1.2 Ca 0.8 O 4 , LiCo 1.2 Ba 0.8 O 4 , LiCo 1.2 Zn 0.8 O 4 , LiCo 1.6 Mg 0.4 O 4 , LiCo1.6 Ga 0.4 O 4 , LiCo 1.6 Ca 0.4 O 4 , LiCo 1.6 Ba 0.4 O 4 , LiCo 1.6 Zinc 0.4 O 4 , LiCo 0.8 Mg 1.2 O 4 , LiCo 0.8 Ga 1.2 O 4 , LiCo 0.8 Ca 1.2 O 4 , LiCo 0.8 Ba 1.2 O 4 , LiCo 0.8 Zinc 1.2 O 4 , LiCo 0.4 Mg 1.6 O 4 , LiCo 0.4 Ga 1.6 O 4 , LiCo 0.4 Ca 1.6 O 4 , LiCo 0.4 Ba 1.6 O 4 , a LiCo 0.4 Zinc 1.6 O 4 .
[0057] Formula 2 compound example LiCo 1.5 Al 0.5 O 4 , LiCo 1.33 Zinc 0.67 O 4 , LiCo 1.2 Mg 0.8 O 4 , LiCo 1.6 Mg 0.4 O 4 , LiCo 0.8 Mg 1.2 O 4 , a LiCo 0.4 Mg 1.6 O 4 .
[0058] The lithium nickel transition metal oxide having a layered crystal structure has a rock salt layered crystal structure (e.g., having an R-3m space group), and a lithium cobalt composite oxide having a spinel crystal structure and including Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof may belong to the Fd-3m space group. A lithium battery including a composite positive electrode active material having a disclosed crystal structure may exhibit further enhanced cycle characteristics and thermal stability. Although not wishing to be bound by theory, it is understood that the cations in the rock salt layered crystal structure are disordered, resulting in improved charge and discharge stability.
[0059] The term "grain boundary" as used herein refers to an interface between adjacent (neighboring) primary particles. Grain boundaries, that is, interfaces between adjacent and neighboring primary particles, exist inside secondary particles.
[0060] The term "primary particle" refers to a single (individual) particle, which can aggregate with each other to form a secondary particle, and can have a variety of shapes such as rods and quadrilaterals, and the term "secondary particle" as used herein refers to a particle that includes multiple primary particles and is not an aggregate of other particles or is not further aggregated, and the secondary particle can have a spherical shape.
[0061] Figure 1 : is a conceptual cross-sectional view showing a detailed structure of the secondary particle 12 in the composite positive electrode active material according to the embodiment.
[0062] refer to Figure 1 The primary particles 11 are aggregated with each other to form secondary particles 12, the grain boundaries 14 between adjacent primary particles 11 include a lithium metal oxide 13 represented by the above formula 1, and a coating film 15 including a metal oxide containing Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof on the surface of the secondary particles 12.
[0063] Without wishing to be bound by theory, it is understood that since the grain boundaries between adjacent primary particles include the lithium metal oxide of Formula 1, the lithium ion conduction inside the secondary particles is improved. For example, the secondary particles have reduced concentration polarization, and elution of nickel ions from the primary particles in the secondary particles into the electrolyte solution penetrating into the secondary particles is suppressed. In addition, the side reaction between the primary particles in the secondary particles and the electrolyte solution is suppressed. Therefore, the cycle characteristics of the lithium battery including the composite cathode active material are enhanced. In addition, the amount of lithium remaining on the surfaces of the plurality of primary particles present in the secondary particles is reduced, and thus deterioration of the composite cathode active material is suppressed, and gas generation is reduced, resulting in improved thermal stability of the lithium battery. Without wishing to be bound by theory, it is understood that the components included in the grain boundaries between adjacent primary particles prevent damage to the surfaces of the primary particles (which is understood to occur during washing of the composite cathode active material), and thus prevent deterioration of the life characteristics of the lithium battery. The components included in the grain boundaries between adjacent primary particles accept (withstand) the volume change in the primary particles during charging and discharging, and thus suppress separation between the primary particles, and thereby suppress deterioration of the mechanical strength of the composite cathode active material, even after long-term charging and discharging, thereby preventing deterioration of the lithium battery. In addition, the metal of the metal oxide included in the grain boundary is included, for example, doped into the lithium nickel transition metal oxide included in the primary particles, and thus the crystal structure of the lithium nickel transition metal oxide is stabilized, and thereby, the cycle characteristics of the lithium battery including the composite cathode active material are further enhanced.
[0064] The lithium metal oxide of Formula 1 may have a monoclinic crystal structure, such as a monoclinic crystal structure. The lithium metal oxide of Formula 1 is, for example, Li 2 ZrO 3 、Li 2 TiO 3 、Li 4 SiO 4 、Li 2 SiO 3 or a combination thereof.
[0065] The metal oxide included in the surface of the secondary particles includes a spinel structure metal oxide or a combination of a spinel structure metal oxide and a layered crystal structure metal oxide. The metal oxide is, for example, a combination of the following: i) Co 3 O 4 and at least one of Li x CoO 2 where 0 < x ≤ 1.5, and ii) MgO. The metal oxide having such a composition can be represented by Formula 2. Li x CoO 2 where 0 < x ≤ 1.5 is, for example, LiCoO 2or Li x CoO 2 In an embodiment, x≤1, for example, x<1, for example, 0 <x≤1。
[0066] The metal oxide of formula 2 is Co 3 O 4 and MgO mixture, Co 3 O 4 MgO composite, LiCoO 2 and MgO mixture, LiCoO 2 MgO composite, LiCoO 2 、Co 3 O 4 A mixture of MgO or LiCoO 2 ·Co 3 O 4 MgO complex.
[0067] The concentration of Co and the Group 2 element, the Group 12 element, the Group 13 element, or a combination thereof may be greater in the coating film than in the secondary particles. In the coating film, the concentration of Co and the Group 2 element, the Group 12 element, the Group 13 element, or a combination thereof may increase with increasing distance from the surface of the secondary particles.
[0068] Hereinafter, a theoretical basis provided by a composite positive active material according to an embodiment will be described, but this is provided to help understand the present disclosure and is not intended to limit the scope of the present disclosure in any way.
[0069] In order to inhibit the elution of nickel ions from the secondary particles into the electrolyte solution, for example, a lithium metal oxide of Formula 1 is included in the grain boundaries between adjacent primary particles of the composite positive electrode active material. By heat treatment performed during the preparation of the lithium metal oxide, the metal contained in the secondary particles is mixed with the metal of the lithium metal oxide, and thereby the elution of nickel ions from the secondary particles into the electrolyte solution is inhibited. In addition, in the process of forming a coating film on the surface of the secondary particles, a precursor of a metal oxide containing Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof reacts with the residual lithium on the secondary particles, and thereby reduces the amount of residual lithium on the surface of the composite positive electrode active material. The coating film formed on the surface of the secondary particles acts as a protective film, and the Co-containing phase in the coating film, such as LiCoO 2It helps to increase the capacity of the battery and mixes or forms a complex with a stable phase such as MgO to form a coating. In the process of forming a MgO coating on the surface of the secondary particles, Mg is diffused and arranged at the grain boundaries of the primary particles, thereby contributing to the structural stabilization of the composite positive active material. Therefore, for example, and although it is not desired to be bound by theory, it is understood that the side reactions and gas generation between the composite positive active material and the electrolyte solution are effectively suppressed. Therefore, the cycle characteristics and thermal stability of the lithium battery including the composite positive active material are enhanced.
[0070] According to an embodiment, during a heat treatment of a nickel-based lithium nickel transition metal oxide having a layered crystal structure with a precursor of a metal oxide including Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof, such as cobalt hydroxide, magnesium (Mg) and aluminum (Al) may be diffused into particles of the nickel-based lithium nickel transition metal oxide having a layered crystal structure, thereby forming MgAl 2 O 4 Here, the particles may be secondary particles or primary particles.
[0071] MgAl 2 O 4 It can be obtained by reacting Mg of magnesium nitrate used to form a coating film on the surface of the secondary particles with Al of nickel-based lithium nickel transition metal oxide having a layered crystal structure. 2 O 4 In addition, for example, gallium aluminum oxide, barium aluminum oxide, zinc aluminum compound, or the like may be formed inside the particles of the nickel-based lithium nickel transition metal oxide having a layered crystal structure.
[0072] The metal oxide may be Li x Co a Mg b O 4 , Li x Co a Ca b O 4 , Li x Co a Ba b O 4 , Li x Co a Zn b O 4 , Li x Co a Al b O 4 or Li x Co a Ga b O 4, where 1 ≤ x ≤ 1.1, 0 < a < 2, 0 < b < 2 and 0 < a + b ≤ 2.
[0073] The nickel-based lithium nickel transition metal oxide having a layered crystal structure has a rock salt layered crystal structure, may belong to the R-3m space group, and the lithium cobalt composite oxide is a composite cathode active material and may belong to the Fd-3m space group.
[0074] The coating film has a thickness of 1 micrometer (μm) or less, such as from about 0.01 nanometer (nm) to about 900 nm; 500 nanometers (nm) or less, such as from about 0.1 nm to about 400 nm; 100 nm or less, such as from about 0.5 nm to about 90 nm; or 50 nm or less, such as from about 1 nm to about 40 nm.
[0075] The lithium nickel transition metal oxide having a layered crystal structure may be doped with Al, Zr, or a combination thereof.
[0076] The lithium nickel transition metal oxide having a layered crystal structure may be, for example, a compound represented by Formula 3:
[0077] Formula 3
[0078] Li a M2O 2-α X α
[0079] Wherein, in Formula 3, 0.9 ≤ a ≤ 1.1, 0 ≤ α < 2, and M2 is at least two elements of nickel (Ni) and elements of Groups 2 to 13 other than Ni, X is F, Cl, Br, S, or P, and the nickel content in M2 ranges from about 70 mole percent (mol%) to less than about 100 mol%, based on the total content of M2 in the compound of Formula 3.
[0080] The compound of Formula 3 may include metals of lithium metal oxides present at grain boundaries.
[0081] The lithium nickel transition metal oxide having a layered crystal structure may be a compound represented by the following Formula 4:
[0082] Formula 4
[0083] Li a Ni b M2 c M3 d M4 e O 2-α X α
[0084] Wherein, in Formula 4, 0.9 ≤ a ≤ 1.1, 0.7 < b < 1, 0 < c < 0.3, 0 < d < 0.3, 0 ≤ e < 0.1, b + c + d + e = 1, and 0 ≤ α < 2.
[0085] M2, M3, and M4 are different from each other and each independently is Co, Mn, Al, Zr, rhenium (Re), vanadium (V), chromium (Cr), iron (Fe), boron (B), ruthenium (Ru), titanium (Ti), niobium (Nb), molybdenum (Mo), Mg, Pt, or a combination thereof, and X is F, Cl, Br, S, or P.
[0086] The lithium nickel transition metal oxide having a layered crystal structure can be a compound represented by Formula 5, a compound represented by Formula 6, or a combination thereof:
[0087] Formula 5
[0088] Li a Ni b Co c Mn d M5 e O 2-α X α
[0089] Formula 6
[0090] Li a Ni b Co c Al d M5 e O 2-α X α
[0091] Wherein, in Formula 5 and Formula 6, a, b, c, d, e, and α each independently are 0.9 ≤ a ≤ 1.1, 0.7 < b < 1, 0 < c < 0.2, 0 < d < 0.2, 0 ≤ e < 0.01, b + c + d + e = 1, 0 ≤ α < 2, M5 is Zr, Al, V, Cr, Fe, Re, B, Ru, Ti, Nb, Mo, Mg, or Pt, and X is F, Cl, Br, S, or P.
[0092] The lithium nickel transition metal oxide having a layered crystal structure can include, for example, a second layered structure crystal phase having a composition represented by Formula 7a and belonging to the C2 / m space group, and a third phase having a layered structure crystal with a composition represented by Formula 7b and belonging to the R-3m space group.
[0093] Formula 7a
[0094] Li 2 MnO 3
[0095] Formula 7b
[0096] LiMO 2
[0097] Among them, in Formula 7b, M includes Ni and Co, Mn, V, Cr, Fe, Zr, Re, Al, B, Ru, Ti, Nb, Mo, Mg, Pt, or a combination thereof.
[0098] At least a part of M is Ni. The amount of Ni in M can be 70 mol% or more, such as 70 mol% to 99 mol%, or 75 mol% to 95 mol%, based on the total content of M in the compound of Formula 7b. The second-layered structure crystal phase represented by Formula 7b may include, for example, doped metals.
[0099] The lithium nickel transition metal oxide having a layered crystal structure can be a compound represented by Formula 7:
[0100] Formula 7
[0101] aLi 2 MnO 3 ·(1-a)LiM6O 2-α X α
[0102] Among them, in Formula 7, 0 < a < 1, 0 ≤ α < 2, M6 includes Ni and Co, Mn, Zr, Al, Re, V, Cr, Fe, B, Ru, Ti, Nb, Mo, Mg, Pt, or a combination thereof, and X is F, Cl, Br, S or P.
[0103] The secondary particles including the lithium nickel transition metal oxide having a layered crystal structure may have an average particle size of about 1 μm to about 40 μm, or about 10 μm to about 20 μm. The lithium nickel transition metal oxide having a layered crystal structure can be a compound represented by Formula 8 or 9:
[0104] Formula 8
[0105] Li x Ni 1-y-z Mn z Co y O 2
[0106] Among them, in Formula 8, 0.8 ≤ x ≤ 1.1, 0 ≤ y ≤ 0.2, 0 ≤ z ≤ 0.2 and 0.8 ≤ 1 - y - z ≤ 0.99,
[0107] Formula 9
[0108] Li x Ni 1-y-z Al z Co y O 2
[0109] Wherein, in Formula 9, 0.8≤x≤1.1, 0≤y≤0.2, 0≤z≤0.2 and 0.8≤1-yz≤0.99.
[0110] As used herein, the term "average particle size" refers to the particle diameter corresponding to 50% of the particles in the distribution curve in which the particles are accumulated in the order of particle size from the smallest particle to the largest particle. Here, the total number of accumulated particles is 100%. The average particle size can be measured by methods known to those of ordinary skill in the art. For example, the average particle size can be measured using a particle size analyzer (Beckman Coulter LS13 320) or by using a transmission electron microscope (TEM) or a scanning electron microscope (SEM) image measurement. As an example of other measurement methods, the average particle size can be measured using a measurement device using dynamic light scattering. According to this method, the number of particles within a predetermined size range can be counted, and the average particle size can be calculated therefrom.
[0111] Examples of lithium nickel transition metal oxides having a layered crystal structure include Li 1.03 (Ni 0.91 Co 0.06 Mn 0.03 ) 2 , Li 1.03 (Ni 0.88 Co 0.08 Mn 0.04 ) 2 , Li 1.03 (Ni 0.8 Co 0.15 Mn 0.05 ) 2 , Li 1.03 (Ni 0.85 Co 0.10 Mn 0.05 ) 2 , Li 1.03 (Ni 0.91 Co 0.05 Mn 0.04 ) 2 , Li 1.05 (Ni 0.91 Co 0.06 Mn 0.03 ) 2 , Li 1.06 (Ni 0.91 Co 0.06 Mn 0.03 ) 2 , Li 1.06 (Ni 0.88 Co 0.08 Mn 0.04 ) 2 , Li1.06 (Ni 0.8 Co 0.15 Mr 0.05 )O 2 、Li 1.06 (Ni 0.85 Co 0.10 Mr 0.05 )O 2 、Li 1.06 (Ni 0.91 Co 0.05 Mr 0.04 )O 2 、Li 1.09 (Ni 0.91 Co 0.06 Mr 0.03 )O 2 、Li 1.09 (Ni 0.88 Co 0.08 Mr 0.04 )O 2 、Li 1.09 (Ni 0.8 Co 0.15 Mr 0.05 )O 2 、Li 1.09 (Ni 0.85 Co 0.10 Mr 0.05 )O 2 、Li 1.09 (Ni 0.91 Co 0.05 Mr 0.04 )O 2 、LiNi 0.91 Co 0.06 Al 0.03 O 2 、LiNi 0.88 Co 0.08 Al 0.04 O 2 、LiNi 0.8 Co 0.15 Al 0.05 O 2 、LiNi 0.85 Co 0.10 Al 0.05 O 2 、LiNi 0.91 Co 0.05 Al 0.04 O 2 、Li 1.09 (Ni 0.88 Co 0.08 Mr 0.04 ) 0.9963 Al0.0012 Zr 0.0025 O 2 and Li 1.09 (Ni 0.91 Co 0.06 Mn 0.03 ) 0.9963 Al 0.0012 Zr 0.0025 O 2 .
[0112] The total amount of the metal oxide in the coating film ranges from about 0.01 parts by weight to about 20 parts by weight relative to 100 parts by weight of a nickel-based lithium nickel transition metal oxide having a layered crystal structure. In addition, in an embodiment, the amount of residual lithium in the composite positive active material is about 3,000 parts per million (ppm) or more by weight before washing, for example, about 4000 ppm to about 10,000 ppm, or about 5000 ppm to about 8,000 ppm, and about 2,000 ppm or less after washing, for example, about 10 ppm to about 1800 ppm, or about 100 ppm to about 1500 ppm. In addition, the amount of residual lithium in the composite positive active material is about 90 weight percent (%) or less of the amount of residual lithium in the secondary particles including the lithium nickel transition metal oxide having a layered crystal structure.
[0113] The coating film may cover 50% or more, for example, 50% to 99%, of the surface of the lithium nickel transition metal oxide having a layered crystal structure. With such a structure, the side reaction between the lithium nickel transition metal oxide and the electrolyte solution may be significantly reduced and / or effectively minimized or prevented.
[0114] According to an embodiment of the present disclosure, a positive electrode including the composite positive electrode active material according to the embodiment is provided.
[0115] The positive electrode may further include an olivine-based positive electrode active material having an olivine structure. The olivine-based positive electrode active material may be a compound represented by Formula 10:
[0116] Formula 10
[0117] Li x M y M' 1-y PO 4
[0118] Wherein, in Formula 10, 0.1≤x≤2, 0≤y≤1, and M and M′ are each independently Fe, Ti, V, Mn, Cr, Co, Ni, copper (Cu), or Zn.
[0119] The olivine-based positive active material may be represented by, for example, the following Formula 11:
[0120] Formula 11
[0121] Li x M8 y M9 z PO 4-α X α
[0122] Wherein, in Formula 11, 0.9≤x≤1.1, 0≤y≤0.9, 0≤z≤0.5, 1-yz≤0, 0≤α≤2, M8 is Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Al, Mg, Zr, B, or a combination thereof, M9 is Mg, Ca, Sr, Ba, Ti, Zr, Nb, Mo, tungsten (W), Zn, Al, Si, Ni, Mn, Cr, Fe, V, a rare earth element, or a combination thereof, and X is fluorine (F), chlorine (Cl), bromine (Br), sulfur (S), or phosphorus (P).
[0123] The olivine-based positive electrode active material may be, for example, LiFePO 4 、LiNiPO 4 、LiMnPO 4 , or LiCoPO 4 .
[0124] The amount of the olivine-based positive electrode active material contained in the positive electrode ranges from, for example, about 1 part by weight to about 10 parts by weight, such as about 1 part by weight to about 7 parts by weight, such as 1 part by weight to about 5 parts by weight, relative to 100 parts by weight of the total weight of the positive electrode active material. Since the positive electrode further includes the olivine-based positive electrode active material within the above amount range, the cycle characteristics and mass density of the lithium battery can be further improved.
[0125] A lithium battery according to an embodiment includes a positive electrode including the composite positive active material.
[0126] Since a lithium battery employs a positive electrode including the composite positive electrode active material, enhanced cycle characteristics and thermal stability are provided.
[0127] The lithium battery is manufactured using, for example, the following example method, but the present disclosure is not particularly limited thereto, and the method may be modified as necessary.
[0128] First, a positive electrode was manufactured according to the following method.
[0129] A positive electrode active material composition in which a positive electrode active material, a binder, and a solvent are mixed is prepared. The positive electrode active material composition may further include a conductive agent.
[0130] The positive electrode active material composition is directly coated on a current collector and dried, thereby manufacturing a positive electrode plate. In an embodiment, the positive electrode active material composition may be cast on a separate support, and a film separated from the support may be laminated on a current collector, thereby manufacturing a positive electrode plate.
[0131] As the positive electrode active material, the composite positive electrode active material according to the embodiment may be used. In addition to the composite positive electrode active material, the positive electrode active material composition may further include a first positive electrode active material, which is a positive electrode active material used in a lithium battery.
[0132] The first positive active material may include lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium manganese oxide, or a combination thereof, but the present disclosure is not limited thereto and any suitable positive active material may be used as the first positive active material.
[0133] For example, the first positive electrode active material may be a compound represented by any of the following formulas: Li a A 1-b B' b D 2 , where 0.90≤a≤1.8 and 0≤b≤0.5; Li a E 1-b B' b O 2-c D c , where 0.90≤a≤1.8, 0≤b≤0.5 and 0≤c≤0.05; LiE 2-b B' b O 4-c D c , where 0≤b≤0.5 and 0≤c≤0.05; Li a Ni 1-b-c Co b B' c D α , where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2; Li a Ni 1-b-c Co b B' c O 2-α F' α , where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2; Li a Ni 1-b-c Mn b B' c D α , where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α≤2; Li a Ni 1-b-c Mnb B' c O 2-α F' α , where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05 and 0<α<2; Li a Ni b E c G d O 2 , where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5 and 0.001≤d≤0.1; Li a Ni b Co c Mn d G e O 2 , where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5 and 0.001≤e≤0.1; Li a NeG b O 2 , where 0.90≤a≤1.8 and 0.001≤b≤0.1; Li a CoG b O 2 , where 0.90≤a≤1.8 and 0.001≤b≤0.1; Li a MnG b O 2 , where 0.90≤a≤1.8 and 0.001≤b≤0.1; Li a Mn 2 G b O 4 , where 0.90≤a≤1.8 and 0.001≤b≤0.1; QO 2 ;QS 2 ;LiQS 2 ; V 2 O 5 ;LiV 2 O 5 ;LiI'O 2 ;LiNiVO 4 ;Li (3-f) J 2 (PO 4 ) 3 , where 0≤f≤2; Li (3-f) Fe 2 (PO 4 ) 3 , where 0≤f≤2; and LiFePO 4 .
[0134] In the above formula, A is Ni, Co, Mn or a combination thereof; B' is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; E is Co, Mn, or a combination thereof; F' is F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, lanthanum (La), cerium (Ce), Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; I' is Cr, V, Fe, scandium (Sc), yttrium (Y), or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu, or a combination thereof.
[0135] Next, the negative electrode is manufactured as follows. For example, the negative electrode is manufactured using a method substantially the same as the method for manufacturing the positive electrode, except that the negative electrode active material is used instead of the composite positive electrode active material. In addition, in the negative electrode active material composition, a conductive agent, a binder, and a solvent substantially the same as those used for the positive electrode may be used.
[0136] For example, a negative electrode active material, a conductive agent, a binder, and a solvent are mixed to prepare a negative electrode active material composition, and the negative electrode active material composition is directly coated on a Cu current collector, thereby manufacturing a negative electrode plate. In an embodiment, the prepared negative electrode active material composition is cast on a separate carrier, and a negative electrode active material film separated from the carrier is stacked on a Cu current collector, thereby manufacturing a negative electrode plate.
[0137] As the negative electrode active material, any suitable negative electrode active material of a lithium battery can be used. For example, the negative electrode active material includes lithium metal, a metal capable of alloying with lithium, a transition metal oxide, a non-transition metal oxide, a carbonaceous material, or a combination thereof.
[0138] The metal that can be alloyed with lithium may be, for example, silicon (Si), tin (Sn), aluminum (Al), germanium (Ge), lead (Pb), bismuth (Bi), antimony (Sb) / Si-Y' alloy (wherein Y' is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, or a combination thereof, except Si), Sn-Y' alloy (wherein Y' is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a Group 15 element, a Group 16 element, a transition metal, a rare earth element, or a combination thereof, except Sn), etc. Examples of element Y' include magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), (Rf), vanadium (V), niobium (Nb), tantalum (Ta), (Db), chromium (Cr), molybdenum (Mo), tungsten (W), (Sg), technetium (Tc), rhenium (Re), (Bh), iron (Fe), lead (Pb), ruthenium (Ru), osmium (Os), (Hs), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), boron (B), aluminum (Al), gallium (Ga), tin (Sn), indium (In), thallium (Tl), germanium (Ge), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), polonium (Po), and combinations thereof.
[0139] The transition metal oxide can be, for example, lithium titanium oxide, vanadium oxide, lithium vanadium oxide, etc.
[0140] The non-transition metal oxide can be, for example, SnO 2 , SiO where 0 < x < 2 x etc.
[0141] The carbonaceous material can be, for example, crystalline carbon, amorphous carbon, or a mixture thereof. Examples of crystalline carbon include graphite, such as natural graphite and artificial graphite, which can be in the form of non-shaped, plate, sheet, spherical, or fibrous. Examples of amorphous carbon include soft carbon (carbon sintered at low temperature), hard carbon, mesophase pitch carbonization products, or sintered coke.
[0142] The amounts of the negative electrode active material, conductive agent, binder, and solvent are not particularly limited and can be determined by those skilled in the art without undue experimentation. Depending on the use and structure of the lithium battery, at least one of the conductive agent, binder, and solvent can be omitted.
[0143] Next, a separator to be inserted between the positive electrode and the negative electrode is prepared.
[0144] Any suitable separator can be used. The separator is, for example, a separator having low resistance to ion migration in the electrolyte and excellent electrolyte retention ability. The separator can include, for example, glass fiber, polyester, Teflon TM , polyethylene, polypropylene, polytetrafluoroethylene (“PTFE”), or combinations thereof, each of which is a non-woven fabric or a woven fabric. For example, a wound separator including polyethylene, polypropylene, etc. is used for lithium-ion batteries, and a separator having excellent impregnation ability for organic electrolyte solutions is used for lithium-ion polymer batteries.
[0145] The separator is manufactured using the following example method, but the present disclosure is not limited thereto, and the method can be adjusted if necessary.
[0146] First, a polymer resin, a filler, and a solvent are mixed together to prepare a separator composition. The separator composition can be directly coated on an electrode and then dried to manufacture a separator. In an embodiment, the separator composition can be cast on a support and then dried, after which a separator film separated from the support is laminated on the electrode, thereby completing the manufacture of the separator.
[0147] The polymer used to make the separator is not particularly limited, and any suitable polymer that can be used as a binder for an electrode plate can be used. Examples of polymer resins include vinylidene fluoride / hexafluoropropylene copolymers, polyvinylidene fluoride ("PVDF"), polyacrylonitrile, polymethyl methacrylate, and mixtures thereof.
[0148] Next, an electrolyte is prepared. The electrolyte may be, for example, an organic electrolyte solution. The organic electrolyte solution may be prepared by, for example, dissolving a lithium salt in an organic solvent.
[0149] The organic solvent may be any suitable organic solvent. Examples of organic solvents include propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dimethoxybenzene ... oxane, 1,2-dimethoxyethane, sulfolane, ethylene dichloride, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether, or a combination thereof.
[0150] The lithium salt may be any suitable lithium salt. Examples of lithium salts include LiPF 6 , LiBF 4 、LiSbF 6 、LiAsF 6 、LiClO 4 、LiCF 3 SO 3 、Li(CF 3 SO 2 )2N、LiC 4 F 9 SO 3 、LiAlO 2 、LiAlCl 4 , where x and y are natural numbers LiN(C x F 2x+1 SO2)(C y F 2y+1SO2), LiCl, Lil, or a combination thereof. In an embodiment, the electrolyte is a solid electrolyte. The solid electrolyte may be, for example, boron oxide, lithium oxynitride, etc., but the present disclosure is not limited thereto, and any suitable solid electrolyte may be used. The solid electrolyte may be formed on the negative electrode using a method such as sputtering, or a separate solid electrolyte sheet may be arranged on the negative electrode.
[0151] like Fig. 9 As shown in , the lithium battery 21 includes a positive electrode 23, a negative electrode 22 and a separator 24. The positive electrode 23, the negative electrode 22 and the separator 24 can be wound or folded and arranged in a battery case 25. The organic electrolyte solution can be arranged (e.g., injected) into the battery case 25 and the battery case 25 can be sealed with a cap assembly 26, thereby completing the manufacture of the lithium battery 21. The battery case 25 has a cylindrical shape, but the present disclosure is not limited thereto. For example, the battery case 25 may have a rectangular shape, a film shape, etc.
[0152] The pouch-type lithium battery includes at least one battery assembly. The separator is arranged between the positive electrode and the negative electrode to form a battery assembly. In an embodiment, the battery assembly is stacked in a double-cell structure, then immersed in an organic electrolyte solution, and the resulting structure is placed in a bag and hermetically sealed, thereby completing the manufacture of the pouch-type lithium battery. Multiple battery assemblies are stacked to form a battery pack, and such a battery pack can be used in all types of devices that require high capacity and high output. For example, the battery pack can be used in a laptop computer, a smart phone, or an electric car.
[0153] Lithium batteries have excellent life characteristics and excellent rate performance, and therefore are used, for example, in electric vehicles ("EV"). For example, lithium batteries are used in hybrid vehicles such as plug-in hybrid electric vehicles ("PHEV"), etc. In addition, lithium batteries are used in fields that store large amounts of electricity. For example, lithium batteries are used in electric bicycles, motor-driven tools, etc.
[0154] A lithium battery including the composite positive active material according to an embodiment has a capacity of 210 mAh / g or more, and life characteristics of the lithium battery remain good even after 50 or more charge and discharge cycles.
[0155] A method of manufacturing a composite positive electrode active material according to an embodiment is as follows.
[0156] First, a nickel-based lithium nickel transition metal oxide having a layered crystal structure and a precursor of a metal oxide are mixed to obtain a composite positive active material composition.
[0157] Subsequently, the composite positive active material composition is subjected to a first heat treatment at a temperature of about 400° C. to about 1000° C. in an oxidizing atmosphere. The oxidizing atmosphere is an atmosphere containing oxygen or air. The oxidizing atmosphere includes oxygen, air, or a combination thereof, and is, for example, air including oxygen.
[0158] The first heat treatment is performed at a temperature of, for example, about 400° C. to about 1,000° C., for example, about 500° C. to about 900° C., for example, about 600° C. to about 800° C., for example, about 700° C. to about 750° C. The heat treatment time ranges from, for example, about 3 hours to about 20 hours, for example, about 3 hours to about 15 hours, for example, about 3 hours to about 10 hours, for example, about 3 hours to about 7 hours, for example, about 4 hours to about 6 hours. The heating rate to reach the heat treatment temperature is, for example, about 1° C. / minute (° C. / min) to about 10° C. / minute.
[0159] The precursor of the metal oxide includes a Co precursor and a precursor of a Group 2 element, a Group 12 element or a Group 13 element. The Co precursor may be a chloride, sulfate, acetate, nitrate, oxychloride, oxynitrate or hydroxide containing Co. Examples of Co precursors include cobalt nitrate, cobalt sulfate, cobalt chloride, cobalt oxide and cobalt hydroxide. In addition, the precursor of a Group 2 element, a Group 12 element or a Group 13 element may be, for example, a chloride, sulfate, nitrate, oxide or hydroxide containing a Group 2 element, a Group 12 element or a Group 13 element, and examples thereof include magnesium nitrate, magnesium sulfate, magnesium chloride, magnesium oxide, magnesium hydroxide or a combination thereof.
[0160] The amount of the metal oxide precursor is about 30 parts by weight or less, such as about 1 to about 25 parts by weight; about 20 parts by weight or less, such as about 2 to about 15 parts by weight; or about 10 parts by weight or less, such as about 3 to about 9 parts by weight, relative to 100 parts by weight of the nickel-based lithium nickel transition metal oxide having a layered crystal structure. The amount of the solvent is about 300 parts by weight or less, such as about 1 to about 250 parts by weight; about 200 parts by weight or less, such as about 5 to about 150 parts by weight; or about 100 parts by weight or less, such as about 10 to about 75 parts by weight, relative to 100 parts by weight of the nickel-based lithium nickel transition metal oxide having a layered crystal structure.
[0161] The nickel-based lithium nickel transition metal oxide having a layered crystal structure may be prepared by mixing a precursor of a lithium nickel transition metal hydroxide with a precursor of a compound represented by the following Formula 1 to obtain a mixture and subjecting the mixture to a second heat treatment at a temperature of about 400° C. to about 1000° C. in an oxidative atmosphere.
[0162] Formula 1
[0163] Li a M1 b Oc
[0164] Wherein, in Formula 1, M1 is Zr, Mn, Si, Mo, Pd, Co, Ni, Ti, Sn, Ir, Pt, Al, Ru, or a combination thereof, and
[0165] 1.9≤a≤4, 0.9≤b≤1.1 and 2.9≤c≤4.
[0166] The second heat treatment is carried out at a temperature of, for example, about 400°C to about 1,000°C, for example, about 500°C to about 900°C, for example, about 700°C to about 800°C, for example, about 700°C to about 750°C. The heat treatment time ranges from, for example, about 3 hours to about 20 hours, about 3 hours to about 15 hours, about 3 hours to about 10 hours, about 3 hours to about 7 hours, or about 4 hours to about 6 hours. The heating rate to reach the heat treatment temperature ranges from, for example, about 1°C / minute to about 10°C / minute. As in the first heat treatment, the oxidizing atmosphere is an atmosphere containing oxygen or air, and the oxidizing atmosphere includes oxygen, air, or a combination thereof, and is, for example, air including oxygen.
[0167] The preparation of the nickel-based lithium nickel transition metal oxide having a layered crystal structure can be carried out by, for example, a wet process including a solvent. The solvent is not particularly limited, and any suitable solvent can be used. The solvent is, for example, distilled water.
[0168] In the preparation of a composite positive electrode active material, the preparation of a lithium nickel transition metal oxide having a layered crystal structure includes: mixing a precursor of the lithium nickel transition metal oxide with a metal precursor to prepare a mixture; and heat treating the mixture at a temperature of 400°C to 1000°C in an oxidative atmosphere to prepare the lithium nickel transition metal oxide.
[0169] The mixture is prepared by, for example, a dry method without using a solvent. The mixture is, for example, a dry powder mixture of a lithium nickel transition metal oxide precursor powder and a metal precursor powder. In an embodiment, the mixture is prepared by, for example, a wet method including a solvent. The mixture includes a solvent capable of dissolving a precursor of the lithium nickel transition metal oxide and a metal precursor, and the type of solvent is not particularly limited, and any suitable solvent can be used. The solvent may be, for example, water, such as distilled water. By the wet method, a higher concentration of lithium metal oxide may be included in the grain boundaries between the primary particles.
[0170] An oxidizing atmosphere is an atmosphere containing oxygen or air. An oxidizing atmosphere includes oxygen, air, or a combination thereof, and is, for example, air with an increased amount of oxygen.
[0171] The precursor of the lithium nickel transition metal oxide may be an oxide or hydroxide of a metal, etc., but the present disclosure is not limited thereto, and any suitable second metal-containing material may be used. The precursor of the lithium nickel transition metal oxide may be, for example, LiOH, Li 2 CO 3 、ZrO 2 、ZrO(NO 3 ) 2 、ZrO(NO 3 ) 2 ·H 2 O、Zr(NO 3 ) 2 、ZrOCl 2 、ZrOCl 2 ·H 2 O, or Al 2 O 3 , or a combination thereof.
[0172] The amount of lithium metal precursor in the mixture is about 30 parts by weight or less, such as about 1 to about 25 parts by weight; about 20 parts by weight or less, such as 2 to 15 parts by weight; or about 10 parts by weight or less, about 3 to about 9 parts by weight, relative to 100 parts by weight of the lithium nickel transition metal oxide precursor.
[0173] The precursor of the lithium nickel transition metal oxide may include, for example, lithium nickel transition metal hydroxide.
[0174] The temperature of the heat treatment process may be, for example, a temperature of about 400°C to about 1,000°C, about 500°C to about 900°C, about 600°C to about 800°C, or about 700°C to about 750°C. The heat treatment time may be, for example, about 3 hours to about 20 hours, about 3 hours to about 15 hours, about 3 hours to about 10 hours, about 3 hours to about 7 hours, or about 4 hours to about 6 hours. The heating rate to reach the heat treatment temperature may be, for example, about 1°C / minute to about 10°C / minute. Since the heat treatment temperature, heat treatment time, and heating rate are within the above ranges, the lithium metal oxide may be contained in the grain boundaries between the primary particles, and the lithium nickel transition metal oxide may be doped with metals such as aluminum, zirconium, and the like.
[0175] The present disclosure will now be described in further detail with reference to the following examples and comparative examples. However, these examples are provided for illustrative purposes only and are not intended to limit the scope of the present disclosure.
[0176] Example
[0177] Example 1: Preparation of composite positive electrode active material
[0178] Zirconia (ZrO 2 ), aluminum oxide (Al 2 O3 )、Ni 0.88 Co 0.08 Mn 0.04 (OH) 2 (Reshine New Material Co., Ltd., China) and LiOH·H as a lithium precursor 2 O to obtain a first mixture. Zirconium oxide (ZrO 2 ), aluminum oxide (Al 2 O 3 )、Ni 0.88 Co 0.08 Mn 0.04 (OH) 2 and LiOH·H as lithium precursor 2 O to obtain Li 1.09375 (Ni 0.88 Co 0.08 Mn 0.04 )Al 0.00125 Zr 0.0025 O 2 . Added Ni 0.88 Co 0.08 Mn 0.04 (OH) 2 The powder includes secondary particles which are aggregates of needle-shaped primary particles.
[0179] The first mixture was put into a furnace and subjected to a first heat treatment at 760° C. for 12 hours while oxygen was flowing therein.
[0180] Through the first heat treatment process, Li 1.09375 (Ni 0.88 Co 0.08 Mn 0.04 )Al 0.00125 Zr 0.0025 O 2 , which is a lithium nickel transition metal oxide with a layered crystal structure. Li with a monoclinic crystal structure is formed on the grain boundaries between multiple primary particles. 2 ZrO 3 .
[0181] Preparation of Co(NO 3 ) 2 6H 2 O and Mg(NO 3 ) 2 6H 2 O precursor, Co(NO 3 ) 2 6H 2 O and Mg(NO 3 )2 6H 2 O are mixed in a weight ratio of 1.5:1, so that the total amount of Co and Mg in the coating film formed on the surface of the secondary particles of the composite positive electrode active material is 0.25 parts by weight relative to 100 parts by weight of lithium nickel transition metal oxide (Li 1.09375 (Ni 0.88 Co 0.08 Mn 0.04 )Al 0.00125 Zr 0.0025 O 2 ), and then added to 10 parts by weight of distilled water, followed by stirring at room temperature (25° C.) for 1 minute, thereby preparing a first composition.
[0182] 100 parts by weight of Li 1.09375 (Ni 0.88 Co 0.08 Mn 0.04 )Al 0.00125 Zr 0.0025 O 2 The powder was added to 90 parts by weight of distilled water to prepare a second composition, and while the second composition was stirred at room temperature for 20 minutes, the first composition obtained according to the above process was added thereto, thereby preparing a second mixture.
[0183] The second mixture was dried in an oven at 150°C for 15 hours.
[0184] The dried resultant was put into a furnace and subjected to heat treatment at 720° C. for 5 hours while allowing oxygen to flow therein, thereby completing the preparation of a composite positive electrode active material.
[0185] In Li 1.09375 (Ni 0.88 Co 0.08 Mn 0.04 )Al 0.00125 Zr 0.0025 O 2 The secondary particles formed on the surface include LiCoO 2 、Co 3 O 4 The total amount of Co and Mg in the coating is 0.25 parts by weight, relative to 100 parts by weight of lithium nickel transition metal oxide (Li 1.09375 (Ni 0.88 Co 0.08 Mn 0.04 )Al 0.00125 Zr 0.0025 O 2 ).
[0186] Figure 2A and2B : is a scanning electron microscope image of the composite positive electrode active material of Example 1.
[0187] Example 2: Preparation of composite positive electrode active material
[0188] The composite positive electrode active material was prepared in the same manner as in Example 1, except that the Co(NO 3 ) 2 6H 2 O and Mg(NO 3 ) 2 6H 2 The amount of the precursor of O was such that the total amount of Co and Mg in the coating film formed on the secondary particles of the composite positive electrode active material was 0.75 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide having a layered crystal structure.
[0189] The total amount of Co and Mg in the coating film was 0.75 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide having a layered crystal structure.
[0190] Examples 2-1 to 2-7
[0191] A composite positive active material was prepared in the same manner as in Example 2, except that heat treatment of the second mixture was performed under the conditions shown in Table 1 below.
[0192] Table 1
[0193] category Heat treatment conditions for the second mixture Example 2-1 600℃, 5 hours Example 2-2 700℃, 5 hours Example 2-3 740℃, 5 hours Embodiment 2-4 800℃, 5 hours Embodiment 2-5 720℃, 0.5 hours Embodiment 2-6 720℃, 10 hours Embodiment 2-7 720℃, 20 hours
[0194] Example 3: Preparation of composite positive electrode active material
[0195] The composite positive electrode active material was prepared in the same manner as in Example 1, except that the Co(NO 3 ) 2 6H 2 O and Mg(NO 3 ) 2 6H 2 The amount of the O precursor was such that the total amount of Co and Mg in the coating film formed on the secondary particles of the composite positive electrode active material was 1.5 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide having a layered crystal structure.
[0196] The total amount of Co and Mg in the coating film was 1.5 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide having a layered crystal structure.
[0197] Example 4: Preparation of composite positive electrode active material
[0198] The composite positive electrode active material was prepared in the same manner as in Example 1, except that the Co(NO 3 ) 2 6H 2 O and Mg(NO 3 ) 2 6H 2 The amount of the O precursor was such that the total amount of Co and Mg in the coating film formed on the secondary particles of the composite positive electrode active material was 5 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide having a layered crystal structure.
[0199] The total amount of Co and Mg in the coating film was 5 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide having a layered crystal structure.
[0200] Example 5: Preparation of composite positive electrode active material
[0201] The composite positive electrode active material was prepared in the same manner as in Example 1, except that in the preparation of the lithium nickel transition metal compound having a layered crystal structure, zirconium oxide (ZrO 2 ) and aluminum oxide (Al 2 O 3 )、Ni 0.88 Co 0.08 Mn 0.04 (OH) 2 (Reshine New Material Co., Ltd., China), LiOH·H as a lithium precursor 2 O mixing ratio, thus obtaining Li 1.09625 (Ni 0.88 Co 0.08 Mn 0.04 )Al 0.00125 Zr 0.005 O 2 .
[0202] Example 6: Preparation of composite positive electrode active material
[0203] The composite positive electrode active material was prepared in the same manner as in Example 5, except that: Co(NO 3 ) 2 6H 2 O and Mg(NO 3 ) 2 6H 2O was so total that the total amount of Co and Mg in the coating film formed on the secondary particles of the composite positive electrode active material was 0.75 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide having a layered crystal structure.
[0204] The total amount of Co and Mg in the coating film was 0.75 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide having a layered crystal structure.
[0205] Comparative Example 1: Composite positive electrode active material
[0206] Ni 0.88 Co 0.08 Mn 0.04 (OH) 2 (Reshine New Material Co., Ltd., China) and LiOH·H as a lithium precursor 2 O were mixed in a molar ratio of 1:1.09 to obtain a mixture. The mixture was put into a furnace and subjected to a first heat treatment at 760° C. for 12 hours while oxygen was flowing therein.
[0207] Through the first heat treatment process, Li 1.09 Ni 0.88 Co 0.08 Mn 0.04 O 2 , which is a lithium nickel transition metal oxide with a layered crystal structure.
[0208] Comparative Example 2: Composite positive electrode active material
[0209] A composite positive active material was prepared in the same manner as in Example 1, except that zirconium oxide was not added in the preparation of the first mixture.
[0210] Comparative Example 3: Composite positive electrode active material
[0211] 100 parts by weight of Li prepared by the first heat treatment process of Example 1 1.09375 (Ni 0.88 Co 0.08 Mn 0.04 )Al 0.00125 Zr 0.0025 O 2 The powder was put into 90 parts by weight of distilled water and stirred, and then the precipitate was filtered and separated, and a water washing process for removing residual lithium was performed once.
[0212] The separated precipitate was dried in an oven at 150° C. for 15 hours to prepare a dried product.
[0213] The dried product was put into a furnace and subjected to heat treatment at 720° C. for 5 hours while oxygen was allowed to flow therein, thereby completing the preparation of a composite positive electrode active material.
[0214] Comparative Example 4: Composite positive electrode active material
[0215] A composite positive active material was prepared in the same manner as in Example 1, except that the first composition was prepared according to the following procedure.
[0216] Only prepare Co(NO 3 ) 2 6H 2 O precursor so that the amount of Co in the coating film formed on the surface of the secondary particles of the composite positive electrode active material is 0.75 parts by weight relative to 100 parts by weight of lithium nickel transition metal oxide, and then added to 10 parts by weight of distilled water, followed by stirring at room temperature (25°C) for 1 minute, thereby preparing a first composition.
[0217] Comparative Example 5: Composite positive electrode active material
[0218] A composite positive active material was prepared in the same manner as in Example 1, except that the first composition was prepared according to the following procedure.
[0219] Only prepare Co(NO 3 ) 2 6H 2 O precursor so that the amount of Co in the coating film formed on the surface of the secondary particles of the composite positive electrode active material is 5 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide, and then added to 10 parts by weight of distilled water, followed by stirring at room temperature (25°C) for 1 minute, thereby preparing a first composition.
[0220] Comparative Example 6: Composite positive electrode active material
[0221] A composite positive active material was prepared in the same manner as in Example 1, except that the first composition was prepared according to the following procedure.
[0222] Only Mg(NO 3 ) 2 6H 2 O precursor so that the amount of Mg in the coating film formed on the surface of the secondary particles of the composite positive electrode active material is 0.75 parts by weight relative to 100 parts by weight of lithium nickel transition metal oxide, and then added to 10 parts by weight of distilled water, followed by stirring at room temperature (25°C) for 1 minute, thereby preparing a first composition.
[0223] Comparative Example 7: Composite positive electrode active material
[0224] A composite positive active material was prepared in the same manner as in Example 1, except that the first composition was prepared according to the following procedure.
[0225] Only Mg(NO 3 ) 2 6H 2 O precursor so that the amount of Mg in the coating film formed on the surface of the secondary particles of the composite positive electrode active material is 5 parts by weight relative to 100 parts by weight of the lithium nickel transition metal oxide, and then added to 10 parts by weight of distilled water, followed by stirring at room temperature (25°C) for 1 minute, thereby preparing a first composition.
[0226] Manufacturing Example 1: Lithium Battery (Coin Half Cell)
[0227] A mixture prepared by mixing the composite positive electrode active material of Example 1, a carbon conductive agent (Denka Black) and polyvinylidene fluoride ("PVdF") at a weight ratio of 92:4:4 was mixed with N-methylpyrrolidone ("NMP") in an agate mortar to prepare a slurry. The slurry was bar-coated on an aluminum current collector having a thickness of 15 micrometers (μm), dried at room temperature, and then dried again in a vacuum at 120° C., and the resulting current collector was rolled and punched, thereby manufacturing a positive electrode having a thickness of 45 μm.
[0228] The prepared positive electrode plate, Li metal as a counter electrode, a PTFE separator, and a 1.15 molar concentration (M) LiPF 6 A coin half cell was fabricated using a solution prepared as an electrolyte dissolved in ethylene carbonate ("EC"), ethyl methyl carbonate ("EMC"), and dimethyl carbonate ("DMC") in a volume ratio of 3:4:3.
[0229] Manufacturing Examples 2 to 6: Lithium Batteries (Coin Half Cells)
[0230] Coin half-cells were manufactured in the same manner as in Manufacturing Example 1, except that the composite positive electrode active materials of Examples 2 to 6 were used instead of the composite positive electrode active material of Example 1, respectively.
[0231] Manufacturing Examples 2-1 to 2-7: Lithium Batteries (Coin Half Cells)
[0232] Coin half-cells were manufactured in the same manner as in Manufacturing Example 1, except that the composite positive electrode active materials of Examples 2-1 to 2-7 were used instead of the composite positive electrode active material of Example 1, respectively.
[0233] Manufacturing Example 7: Addition of Lithium Iron Phosphate
[0234] A coin half-unit cell was manufactured in the same manner as in Manufacturing Example 1, except that 5 parts by weight of LiFePO4 having an olivine structure was added. 4 Added to 100 parts by weight of the composite positive electrode active material of Example 1.
[0235] Manufacturing Comparative Examples 1 to 7
[0236] Coin half-cells were manufactured in the same manner as in Manufacturing Example 1, except that the composite positive active materials prepared according to Comparative Examples 1 to 7 were used instead of the composite positive active material of Example 1, respectively.
[0237] Manufacturing Example 8: Manufacturing of Lithium Battery (Full Cell)
[0238] A mixture prepared by mixing the composite positive active material of Example 1, a carbon conductive agent (Denka Black) and PVdF at a weight ratio of 92:4:4 was mixed with NMP in an agate mortar to prepare a positive active material slurry. The slurry was applied to an aluminum current collector having a thickness of 15 μm, dried at room temperature, and then dried again in a vacuum at 120° C., and the resulting current collector was rolled and punched, thereby manufacturing a positive electrode having a thickness of 45 μm.
[0239] Graphite particles having an average particle size of 25 μm, styrene-butadiene rubber ("SBR") binder (ZEON) and carboxymethyl cellulose ("CMC") (NIPPON A&L) were mixed in a weight ratio of 97:1.5:1.5, and the resulting mixture was added to distilled water and stirred with a mechanical stirrer for 60 minutes to prepare a negative electrode active material slurry. The slurry was coated on a copper (Cu) current collector having a thickness of 10 μm using a scraper, and the resulting current collector was dried in a hot air dryer at 100° C. for 0.5 hours, dried again in a vacuum at 120° C. for 4 hours, and rolled and punched, thereby manufacturing a negative electrode having a thickness of 65 μm.
[0240] The positive electrode, the negative electrode, the PTFE separator and the like were prepared by mixing 1.15M LiPF 6 A solution prepared as an electrolyte dissolved in EC, EMC, and DMC in a volume ratio of 3:4:3 was used to fabricate a full unit cell.
[0241] Manufacturing Examples 9 and 10: Manufacturing of Lithium Batteries (Full Cells)
[0242] A full-unit cell was manufactured in the same manner as in Manufacturing Example 8, except that the composite positive electrode active materials of Examples 2 and 3 were used instead of the composite positive electrode active material of Example 1, respectively.
[0243] Manufacturing Example 11: Manufacturing of Lithium Battery (Full Cell)
[0244] A full-cell battery was manufactured in the same manner as in Manufacturing Example 8, except that 5 parts by weight of LiFePO 4 Added into 100 parts by weight of the composite positive electrode active material of Example 1.
[0245] Manufacturing Comparative Examples 8 to 14
[0246] A full-unit cell was manufactured in the same manner as in Manufacturing Example 8, except that the composite positive electrode active materials prepared according to Comparative Examples 1 to 7 were used instead of the composite positive electrode active material of Example 1, respectively.
[0247] Evaluation Example 1: X-ray Diffraction ("XRD") Spectrum Evaluation
[0248] The XRD spectrum of the composite positive electrode active material of Example 1 was measured, and the results are shown in Figure 3 In. Cu Kα radiation was used in the XRD spectroscopic measurements.
[0249] like Figure 3 As shown in , in the XRD spectrum of the composite positive electrode active material of Example 1, only the peak of the phase having a layered crystal structure belonging to the R-3m space group appears.
[0250] Rietveld analysis confirmed that the coating layer included Co 3 O 4 phase and MgO phase.
[0251] Evaluation Example 2: Evaluation of the composition inside and on the surface of the core
[0252] Figures 4A to 4E are high-angle annular dark-field scanning transmission electron microscopy (“HAADF STEM”) and energy-dispersive X-ray spectroscopy (“EDS”) images showing a cross section of the composite positive active material of Example 1.
[0253] like Figures 4A to 4E As shown in , it was confirmed that a coating layer containing Co and Mo was formed on the core.
[0254] In addition, from Figure 4B and Figure 4C It was confirmed that the concentration of Co and / or Mg contained in the coating layer was greater than the concentration of Co and / or Mg contained in the primary particles. Figure 4B and Figure 4C , the higher the concentration of the metal, the brighter the color corresponding to the metal. That is, it was confirmed that a coating layer containing high concentrations of Co and Mg was formed on the primary particles included in the core.
[0255] like Figure 4Aand 4B As shown in , the capping layer has a thickness of about 10 nanometers (nm) to about 20 nm.
[0256] Although not shown in the figure, it was confirmed by additional high-resolution analysis that a separate phase containing Zr existed at the grain boundaries between the primary particles included in the core and on the surface of the core. The separate phase was Li+ with a monoclinic crystal structure belonging to the C2 / m space group. 2 ZrO 3 Mutually.
[0257] Evaluation Example 3: Evaluation of the amount of residual lithium
[0258] The amount of residual lithium on the surface of each of the composite cathode active materials of Examples 1 and 2 and Comparative Examples 1 and 2 was measured, and some results thereof are shown in Table 2 below.
[0259] The Li remaining on the surface of each composite positive electrode active material was measured by a wet method (or titration). 2 CO 3 The amount of residual lithium was evaluated by the Li content in LiOH.
[0260] For details of the measurement method, reference may be made to the method disclosed in, for example, paragraph
[0054] of JP 2016-081903A.
[0261] Table 2
[0262] Amount of residual lithium (ppm by weight) Comparative Example 1 1786 Comparative Example 2 1862 Example 1 518 Example 2 656
[0263] As shown in Table 2, it was confirmed that the amount of residual lithium on the surface of each composite positive active material of Examples 1 and 2 was reduced compared with the amount of residual lithium on the surface of each composite positive active material of Comparative Examples 1 and 2. Although not wishing to be bound by theory, it is understood that the content of residual lithium is reduced because the residual lithium on the surface of the lithium nickel transition metal oxide sequentially reacts with the precursor of the metal oxide to form a coating film on the surface of the secondary particles.
[0264] In addition, the lithium battery including the composite positive active materials of Examples 1 and 2 showed enhanced life characteristics. Although not wishing to be bound by theory, it is understood that the improved performance is due to the suppressed gas generation during charge and discharge and the suppressed side reaction with the electrolyte solution compared to the lithium battery including the composite positive active materials of Comparative Examples 1 and 2.
[0265] Evaluation Example 4: Evaluation of charge and discharge characteristics at room temperature
[0266] The lithium batteries of Manufacturing Examples 5 and 6 and Manufacturing Comparative Examples 1 and 2 were each charged at 25° C. at a constant current of 0.1 C rate until the voltage reached 4.35 volts (V) (relative to Li / Li+ ), and then each was discharged at a constant current of 0.1C until the voltage reached 2.8V (relative to Li / Li + )(1st cycle, transformed into cycle).
[0267] After the first cycle, each lithium battery was charged at 25°C at a constant current rate of 0.33C until the voltage reached 4.35V (relative to Li / Li + ), and then, while maintaining a constant voltage of 4.35 V, the battery was cut off at a current rate of 0.05C. Subsequently, each lithium battery was discharged at a constant current rate of 0.2C until the voltage reached 2.8 V (relative to Li / Li + )(2nd cycle).
[0268] After the second cycle, each lithium battery was charged at 25°C at a constant current rate of 1C until the voltage reached 4.35V (relative to Li / Li + ), and then discharged at a constant current of 1C until the voltage reached 2.8V (relative to Li / Li + ), and the charge and discharge cycle was repeated 50 times under the same conditions until the 52nd cycle.
[0269] In all charge and discharge cycles, there was a 20 minute rest time at the end of each charge / discharge cycle.
[0270] Some charge and discharge test results are shown in the following Table 3. The capacity retention rate at the 52nd cycle is defined using the following Equation 1:
[0271] Equation 1
[0272] Capacity retention rate = (discharge capacity at the 52nd cycle / discharge capacity at the 3rd cycle) × 100%
[0273] Table 3
[0274] Classification Discharge capacity at the second cycle (mAh / g) Capacity retention rate (%) Manufacturing Comparative Example 1 220 83.2 Manufacturing Comparative Example 2 220 84.6 Manufacturing Example 5 222 90.6 Manufacturing Example 6 223 88.0
[0275] As shown in Table 3, the lithium batteries of Manufacturing Examples 5 and 6 exhibited enhanced lifespan characteristics without substantial capacity reduction compared to the lithium batteries of Manufacturing Comparative Examples 1 and 2.
[0276] Although not wishing to be bound by theory, it is understood that the enhanced lifespan characteristics are due to the fact that the surface of the composite positive electrode active material contained in each of the lithium batteries of Manufacturing Examples 5 and 6 is stabilized by the coating film, and thus the side reaction with the electrolyte solution is suppressed. In addition, this is because, in the composite positive electrode active material contained in the lithium batteries of Manufacturing Examples 5 and 6, Li 2 ZrO 3The core is located at the grain boundary between the primary particles, thereby coating the primary particles, and thereby suppressing a side reaction between the primary particles contained in the core and the electrolyte solution, and suppressing elution of the transition metal from the primary particles.
[0277] Evaluation Example 5: Evaluation of charge and discharge characteristics at room temperature
[0278] The lithium batteries of Manufacturing Examples 1, 2, 2-1 to 2-7, 3 and 4 and Manufacturing Comparative Examples 3 to 5 were each charged at 25° C. at a constant current of 0.1 C rate until the voltage reached 4.35 volts (V) (relative to Li / Li + ), and then each was discharged at a constant current of 0.1C until the voltage reached 2.8V (relative to Li / Li + )(1st cycle, transformed into cycle).
[0279] After the first cycle, each lithium battery was charged at 25°C at a constant current rate of 0.33C until the voltage reached 4.35V (relative to Li / Li + ), and then, while maintaining a constant voltage of 4.35 V, the battery was cut off at a current rate of 0.05C. Subsequently, each lithium battery was discharged at a constant current rate of 0.2C until the voltage reached 2.8 V (relative to Li / Li + )(2nd cycle).
[0280] After the second cycle, each lithium battery was charged at 25°C at a constant current rate of 1C until the voltage reached 4.35V (relative to Li / Li + ), and then discharged at a constant current of 1C until the voltage reached 2.8V (relative to Li / Li + ) (3rd cycle), and the charge and discharge cycle was repeated 50 times under the same conditions until the 52nd cycle. In all charge and discharge cycles, there was a 20-minute rest time at the end of each charge / discharge cycle.
[0281] Some charge and discharge test results are shown in the following Table 4. The capacity retention rate at the 52nd cycle is defined using the following Equation 1:
[0282] Equation 1
[0283] Capacity retention rate = (discharge capacity at the 52nd cycle / discharge capacity at the 3rd cycle) × 100%
[0284] The evaluation results are shown in Tables 4 and 5 below.
[0285] Table 4
[0286] Classification Capacity retention rate (%) Comparative Manufacturing Example 3 (Water Washing) 94 Comparative Manufacturing Example 4 (Co 0.75 wt%) 93 Comparative Manufacturing Example 5 (Co 5 wt%) 91 Manufacturing Example 1 (Co 0.15 wt% / Mg 0.1 wt%) 95 Manufacturing Example 2 (Co 0.45 wt% / Mg 0.3 wt%) 94 Manufacturing Example 3 (Co 0.9 wt% / Mg 0.6 wt%) 94 Manufacturing Example 4 (Co 3 wt% / Mg 2 wt%) 93
[0287] Table 5
[0288]
[0289] As shown in Table 4, the lithium batteries of Manufacturing Examples 1 to 4 exhibited enhanced life characteristics compared to the lithium batteries of Manufacturing Comparative Examples 4 and 5. The enhanced life characteristics are caused by the fact that the surface of the composite positive electrode active material contained in each of the lithium batteries of Manufacturing Examples 1 to 4 is stabilized by the coating film, and thus the side reaction with the electrolyte solution is suppressed. In addition, the excellent life characteristics exhibited by the lithium batteries of Manufacturing Examples 1, 2, 2-1 to 2-7, 3 and 4 as shown in Tables 4 and 5 are caused by the fact that in the composite positive electrode active material, Li 2 ZrO 3 Located at the grain boundaries between the primary particles, thereby coating the primary particles, and thereby suppressing the side reaction between the primary particles included in the core and the electrolyte solution, and suppressing the elution of the transition metal from the primary particles. In addition, as can be seen in Table 5, the life characteristics of each lithium battery vary depending on the heat treatment conditions.
[0290] Furthermore, all of the lithium batteries of Manufacturing Examples 1, 2, 2-1 to 2-7, 3, and 4 exhibited a discharge capacity of about 210 mAh / g or more at the 2nd cycle, which confirmed that the lithium batteries had excellent capacity characteristics.
[0291] Evaluation Example 6: Evaluation of charging and discharging characteristics at high temperature
[0292] The lithium batteries of Manufacturing Examples 9 and 11 were each charged at 45° C. at a constant current of 0.1 C rate until the voltage reached 4.30 volts (V) (relative to Li / Li + ), and then each was discharged at a constant current of 0.1C until the voltage reached 2.8V (relative to Li / Li + )(1st cycle, transformed into cycle).
[0293] After the first cycle, each lithium battery was charged at 45°C at a constant current rate of 0.33C until the voltage reached 4.30V (relative to Li / Li + ), and then, while maintaining a constant voltage of 4.30 V, the battery was cut off at a current rate of 0.05C. Subsequently, each lithium battery was discharged at a constant current rate of 0.2C until the voltage reached 2.8 V (relative to Li / Li + )(2nd cycle).
[0294] After the second cycle, each lithium battery was charged at 45°C at a constant current rate of 1C until the voltage reached 4.30V (relative to Li / Li +), and then discharged at a constant current of 1C until the voltage reached 2.8V (relative to Li / Li + ) (3rd cycle), and the charge and discharge cycle was repeated 200 times under the same conditions until the 202nd cycle.
[0295] In all charge and discharge cycles, there was a 20 minute rest time at the end of each charge / discharge cycle.
[0296] Some charging and discharging test results are shown in Table 6 and Figure 5 and 6 middle.
[0297] Figure 7 and 8 The electron scanning microscope images of the cross-sections of the positive electrodes after the charge and discharge cycles of the lithium batteries of the manufacturing examples 9 and 11 are shown respectively. The capacity retention rate at the 202nd cycle and the initial charge and discharge efficiency at the 1st cycle are defined by the following equations 3 and 4. In addition, the discharge capacity at the 2nd cycle is determined as the standard capacity.
[0298] Equation 3
[0299] Capacity retention rate = (discharge capacity at the 202nd cycle / discharge capacity at the 3rd cycle) × 100%
[0300] Equation 4
[0301] Initial efficiency (%) = (discharge capacity at the first cycle / charge capacity at the first cycle) × 100%
[0302] Table 6
[0303]
[0304] As shown in Table 6, compared with those of the lithium battery of Manufacturing Example 9, the lithium ion battery further includes LiFePO 4 The lithium battery of Manufacturing Example 11 exhibited enhanced initial discharge capacity, enhanced initial charge and discharge efficiency, enhanced standard capacity, and enhanced capacity retention rate.
[0305] Evaluation Example 7: Evaluation of direct current resistance ("DC-IR") at room temperature (25°C) (Evaluation of the effect of adding 5% of LFP)
[0306] The initial DC-IR of each of the lithium batteries of Manufacturing Examples 9 and 11 was measured at room temperature (25° C.) using the following method.
[0307] In the first cycle, each lithium battery was charged at a current of 0.5C until the voltage reached a 50% state of charge ("SOC") and was cut off at 0.02C, and then each lithium battery was left to stand for 10 minutes. Subsequently, each lithium battery was subjected to the following process: discharging at a constant current of 0.5C for 30 seconds, then standing for 30 seconds, and charging at a constant current of 0.5C for 30 seconds, then standing for 10 minutes; discharging at a constant current of 1C for 30 seconds, then standing for 30 seconds, and charging at a constant current of 0.5C for 1 minute, then standing for 10 minutes; discharging at a constant current of 2C for 30 seconds, then standing for 30 seconds, and charging at a constant current of 0.5C for 2 minutes, then standing for 10 minutes; discharging at a constant current of 3C for 30 seconds, then standing for 30 seconds, and charging at a constant current of 0.5C for 3 minutes, then standing for 10 minutes.
[0308] The average voltage drop value for 30 seconds at each C rate is a DC voltage value. The DC resistance calculated from the measured DC voltage is shown in Table 7 below.
[0309] Table 7
[0310] Classification Initial DC resistance (mΩ) Manufacturing Example 9 126 Manufacturing Example 11 122
[0311] As shown in Table 7, compared with those of the lithium battery of Manufacturing Example 9, the lithium ion battery further includes LiFePO 4 The lithium battery of (LFP) Manufacturing Example 11 exhibited a reduced initial DC resistance.
[0312] As is clear from the foregoing description, the composite positive electrode active material according to the embodiment has grain boundaries between multiple primary particles (which include the lithium metal oxide of Formula 1 above), and includes a coating film containing Co oxide and Group 2 element oxide, Group 12 element oxide, Group 13 element oxide, or a combination thereof on the surface of the secondary particles, and a lithium battery including the composite positive electrode active material exhibits enhanced capacity and life characteristics.
[0313] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for limiting purposes. The description of features or aspects in each embodiment should be considered as applicable to other similar features or aspects in other embodiments.
[0314] Although embodiments have been described with reference to the accompanying drawings, it will be understood by those skilled in the art that various changes in form and details may be made without departing from the spirit and scope defined by the following claims.
Claims
1. Composite cathode active material, comprising: secondary particles; a coating layer on the surface of the secondary particles, wherein the secondary particles comprise a plurality of primary particles, and wherein the plurality of primary particles comprise a lithium nickel transition metal oxide having a layered crystal structure; and grain boundaries between the primary particles of the plurality of primary particles, the grain boundaries comprising a lithium metal oxide having a crystal structure different from that of the lithium nickel transition metal oxide having a layered crystal structure and represented by Formula 1, wherein the coating layer on the surface of the secondary particles comprises a metal oxide comprising cobalt and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof, the Group 2 element being magnesium, calcium, strontium, barium, or a combination thereof, the Group 12 element being zinc, and the Group 13 element being aluminum, gallium, indium, thallium, or a combination thereof, Formula 1 Li a M1 b O c wherein, in Formula 1, M1 is zirconium, silicon, titanium, or a combination thereof, and where 1.9 ≤ a ≤ 4, 0.9 ≤ b ≤ 1.1 and 2.9 ≤ c ≤ 4, wherein the lithium metal oxide represented by Formula 1 has a monoclinic crystal structure and includes Li 2 ZrO 3 , Li 2 TiO 3 , Li 4 SiO 4 , Li 2 SiO 3 , or a combination thereof.
2. The composite cathode active material according to claim 1, wherein the metal oxide of the coating layer comprises a first metal oxide having a spinel structure, a second metal oxide having a layered structure, or a combination thereof.
3. The composite cathode active material according to claim 1, wherein the metal oxide of the coating layer is a metal oxide represented by Formula 2: Formula 2 Li x Co a Along with b O c wherein, in Formula 2, Me is a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof, the Group 2 element being magnesium, calcium, strontium, barium, or a combination thereof, the Group 12 element being zinc, and the Group 13 element being aluminum, gallium, indium, thallium, or a combination thereof, and 0 ≤ x ≤ 1.1, 0 < a ≤ 3, 0 < b ≤ 3 and 1 ≤ c ≤ 4.
1.
4. The composite cathode active material according to claim 1, wherein the metal oxide of the coating layer comprises the following combinations: i) Co 3 O 4 and Li where 0 < x ≤ 1.5 x CoO 2 at least one of, and ii) MgO.
5. The composite positive electrode active material according to claim 1, wherein the metal oxide of the coating layer comprises Co 3 O 4 and MgO mixture, Co 3 O 4 MgO composite, LiCoO 2 Mixture of LiCoO and MgO 2 MgO composite, LiCoO 2 、Co 3 O 4 and MgO mixture, or LiCoO 2 ·Co 3 O 4 MgO complex.
6. The composite cathode active material according to claim 1, wherein the concentration of Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof in the coating layer is greater than the concentration of Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof in the secondary particles.
7. The composite cathode active material according to claim 1, wherein, in the coating layer, the concentration of Co and a Group 2 element, a Group 12 element, a Group 13 element, or a combination thereof increases in a direction away from the surface of the secondary particles.
8. The composite positive electrode active material according to claim 1, wherein the metal oxide comprises Li x Co a Mg b O 4 、Li x Co a Ga b O 4 、Li x Co a Ca b O 4 、Li x Co a Ba b O 4 、Li x Co a Al b O 4 or Li x Co a Zn b O 4 , where 1 ≤ x ≤ 1.1, 0 < a < 2, 0 < b < 2 and 0 < a + b ≤ 2.
9. The composite positive electrode active material according to claim 1, wherein the particles of the lithium nickel transition metal oxide having a layered crystal structure include MgAl 2 O 4 .
10. The composite cathode active material according to claim 1, wherein the lithium nickel transition metal oxide having a layered crystal structure has a rock salt layered crystal structure and belongs to the R-3m space group, and wherein the metal oxide of the coating layer is a lithium cobalt composite oxide, and the lithium cobalt composite oxide belongs to the Fd-3m space group.
11. The composite cathode active material according to claim 1, wherein the coating layer has a thickness of 1 micron or less.
12. The composite cathode active material according to claim 1, wherein the lithium nickel transition metal oxide having a layered crystal structure comprises Al, Zr, or a combination thereof.
13. The composite cathode active material according to claim 1, wherein the lithium nickel transition metal oxide having a layered crystal structure is represented by Formula 3: Formula 3 Li a M2O 2-α X α wherein, In Formula 3, 0.9 ≤ a ≤ 1.1, 0 ≤ α < 2, and M2 includes nickel and at least two elements of Groups 2 to 13 other than Ni, X is F, Cl, Br, S, or P, and the nickel content in M2 ranges from 70 mol% to less than 100 mol%, based on the total content of M2.
14. The composite cathode active material according to claim 1, wherein the lithium nickel transition metal oxide having a layered crystal structure is represented by Formula 4: Formula 4 The a Nor b M2 c M3 d M4 e O 2-α X α wherein, in Formula 4, 0.9 ≤ a ≤ 1.1, 0.7 < b < 1, 0 < c < 0.3, 0 < d < 0.3, 0 ≤ e < 0.1, b + c + d + e = 1, and 0 ≤ α < 2, M2, M3, and M4 are different from each other and are each independently Co, Mn, Al, Zr, Re, V, Cr, Fe, B, Ru, Ti, Nb, Mo, Mg, or Pt, and X is F, Cl, Br, S, or P.
15. The composite cathode active material according to claim 1, wherein the lithium nickel transition metal oxide having a layered crystal structure is a compound represented by Formula 5, a compound represented by Formula 6, or a combination thereof: Formula 5 Li a Ni b Co c Mr d M5 e O 2-α X α , Formula 6 Li a Ni b Co c Al d M5 e O 2-α X α wherein, in Formulas 5 and 6, a, b, c, d, and e are each independently 0.9 ≤ a ≤ 1.1, 0.7 < b < 1, 0 < c < 0.1, 0 < d < 0.1, 0 ≤ e < 0.01, b + c + d + e = 1, and 0 ≤ α < 2, M5 in Formulas 5 and 6 are each independently Zr, Al, V, Cr, Fe, Re, B, Ru, Ti, Nb, Mo, Mg, or Pt, and X is F, Cl, Br, S, or P.
16. The composite cathode active material according to claim 1, wherein the lithium nickel transition metal oxide having a layered crystal structure is represented by Formula 7: Formula 7 aLi 2 MnO 3 ·(1-a)LiM6O 2-α X α wherein, in Formula 7, 0 < a < 1 and 0 ≤ α < 2, M6 includes Ni and Co, Mn, Zr, Al, Re, V, Cr, Fe, B, Ru, Ti, Nb, Mo, Mg, Pt, or a combination thereof, and X is F, Cl, Br, S, or P.
17. The composite cathode active material according to claim 1, wherein the secondary particles including the lithium nickel transition metal oxide having a layered crystal structure have an average particle size of 10 μm to 20 μm.
18. The composite cathode active material according to claim 1, wherein the lithium nickel transition metal oxide having a layered crystal structure is a compound represented by Formula 8 or 9: Formula 8 Li x Ni 1-y-z Mr z Co y O 2 wherein, in Formula 8, 0.8 ≤ x ≤ 1.1, 0 ≤ y ≤ 0.2, 0 ≤ z ≤ 0.2 and 0.8 ≤ 1 - y - z ≤ 0.99, Formula 9 Li x Ni 1-y-z Al z Co y O 2 wherein, in Formula 9, 0.8 ≤ x ≤ 1.1, 0 ≤ y ≤ 0.2, 0 ≤ z ≤ 0.2 and 0.8 ≤ 1 - y - z ≤ 0.
99.
19. The composite cathode active material according to claim 1, wherein the total amount of the metal oxide in the coating layer ranges from 0.01 part by weight to 20 parts by weight, relative to 100 parts by weight of the lithium nickel transition metal oxide having a layered crystal structure.
20. The composite positive electrode active material according to claim 1, in: The amount of residual lithium in the composite cathode active material is 2,000 parts per million or less by weight based on the total weight of the composite cathode active material, and The residual lithium in the composite positive electrode active material is on the surface of the secondary particle and is not in the coating layer.
21. The composite positive electrode active material according to claim 1, in: the amount of residual lithium in the composite positive electrode active material is 90 wt % or less of the amount of residual lithium in the secondary particles including the lithium nickel transition metal oxide having a layered crystal structure, The residual lithium in the composite positive electrode active material is on the surface of the secondary particles and not in the coating layer, and The residual lithium in the secondary particles including the lithium nickel transition metal oxide having a layered crystal structure is not in the lithium metal oxide having a crystal structure different from that of the lithium nickel transition metal oxide having a layered crystal structure. 22 . The composite positive active material of claim 1 , wherein the coating layer covers 50% or more of the total surface of the lithium nickel transition metal oxide having a layered crystal structure.
23. A positive electrode comprising the composite positive electrode active material according to any one of claims 1 to 22. 24 . The positive electrode of claim 23 , wherein the positive electrode further comprises a positive electrode active material having an olivine type structure.
25. The positive electrode according to claim 24, wherein the positive electrode active material having an olivine structure is represented by Formula 10: Formula 10 Li x M y M' 1-y P.O. 4 in, In Formula 10, 0.1≤x≤2, 0≤y≤1, and M and M′ are each independently iron, titanium, vanadium, manganese, chromium, cobalt, nickel, copper, or zinc. 26 . The positive electrode of claim 24 , wherein the amount of the positive electrode active material having an olivine type structure is 10 parts by weight or less relative to 100 parts by weight of the total weight of the positive electrode active material.
27. Lithium battery, include: The positive electrode according to any one of claims 23 to 26; negative electrode; as well as An electrolyte is between the positive electrode and the negative electrode.
28. A method for preparing a composite positive electrode active material according to any one of claims 1 to 22, the method include: mixing a lithium nickel transition metal oxide having a layered crystal structure and a precursor of a metal oxide to obtain a composite positive electrode active material composition; and The composite cathode active material composition is heat-treated at a temperature of 400° C. to 1000° C. in an oxidative atmosphere to prepare a composite cathode active material.
29. The method of claim 28, wherein the lithium nickel transition metal oxide having a layered crystal structure is prepared using a method comprising: mixing a precursor of the lithium nickel transition metal oxide having a layered crystal structure with a precursor of the compound represented by Formula 1 to prepare a mixture; and heat treating the mixture at a temperature of 400°C to 1,000°C in an oxidative atmosphere: Formula 1 Li a M1 b O c in, In Formula 1, M1 is zirconium, silicon, titanium, or a combination thereof, and Where 1.9≤a≤4, 0.9≤b≤1.1 and 2.9≤c≤4, wherein the lithium metal oxide represented by Formula 1 has a monoclinic crystal structure and includes Li 2 ZrO 3 , Li 2 TiO 3 , Li 4 SiO 4 , Li 2 SiO 3 , or a combination thereof.
Citation Information
Patent Citations
Positive electrode active material for lithium ion secondary battery, method of producing the same, and lithium ion secondary battery
JP2016081903A
Blade of reaper
KR1020180128324A
Positive electrode material for lithium-ion secondary battery, lithium-ion secondary battery and secondary battery module using the same
CN102376948A
Cathode active material particles and secondary battery including same
CN107408679A
Nickel-based active material for lithium secondary battery, method of preparing the same, and lithium secondary battery including positive electrode including the nickel-based active material
CN107644981A