A process for preparing low-carbon aluminum killed clean steel for slag blocking and feeding line
Through the slag-blocking wire feeding process and the use of limestone cored wire, the problems of pourability and molding performance of molten steel caused by the calcium treatment process have been solved, and the production of low-cost, low-inclusion low-carbon aluminum-killed steel has been achieved, significantly improving the product quality. Qualification rate and molding performance.
Patent Information
- Application Number
- CN202010132980.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2018-01-31
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2038-01-31
AI Technical Summary
In the existing low-carbon aluminum-killed steel production process, the calcium treatment step causes calcium residues that affect the castability and formability of the molten steel. The cost is high, and it is difficult to effectively control the number of inclusions.
The slag-blocking wire feeding process is adopted. Through molten iron pretreatment, oxygen top and bottom blowing converter, LF refining, argon soft blowing at the bottom of the ladle and continuous casting process, limestone cored wire is used instead of calcium treatment to control the composition of molten steel and slag, reducing High melting point calcium aluminate is mixed to improve the cleanliness and pourability of molten steel.
There is no need for calcium treatment, which significantly reduces the number of inclusions and the risk of cold bending cracking, reduces production costs, improves steel plate forming performance and product qualification rate, and meets the requirements for cleanliness and castability of molten steel.
Smart Images

Figure CN111218619B_ABST
Abstract
Description
Technical Field
[0001] The present invention is a divisional application of the invention patent application "A production process of clean steel without calcium treatment" (application number: 2018100948303). It specifically relates to the field of iron and steel metallurgy technology, and in particular to a production process of formable low-carbon aluminum-killed clean steel without calcium treatment in the field of thin slab continuous casting. Background Art
[0002] At present, calcium treatment is the core link in the production process of low-carbon (silicon-containing) aluminum-killed steel. The specific production process generally adopts the process flow of molten iron → oxygen top and bottom combined blowing converter → LF refining → argon soft blowing at the bottom of the ladle → calcium treatment → argon soft blowing at the bottom of the ladle → thin slab continuous casting → continuous rolling. The calcium treatment process is specifically: the molten steel is fed with a metal calcium solid core wire, the purpose of which is to control the appropriate calcium-aluminum ratio, generate low-melting-point liquid 12CaO·7Al2O3, 3CaO·Al2O3 aluminates, promote the floating of inclusions, and improve the castability of molten steel.
[0003] However, in actual production, the above-mentioned calcium treatment process is used, and the calcium recovery rate is usually around 20%. At the smelting temperature, most of the calcium remains in the metal melt in the following forms: (1) oxide inclusions, solid calcium aluminate (C.6A, C.2A, CA); (2) CaS inclusions in molten steel. These calcium inclusions can easily cause nozzle blockage, affecting and limiting the production efficiency of thin slab continuous casting; and, high-melting-point calcium aluminate inclusions in molten steel affect the formability of the steel plate, making cold bending cracking more likely to occur.
[0004] Therefore, different from the existing calcium treatment technology for producing low-carbon (silicon-containing) aluminum-killed steel, how to overcome the existing technical prejudices, get rid of the calcium treatment link, better control the number of inclusions, improve the castability of molten steel, and alleviate the flocculent problem has become the current technical difficulty in this field. Summary of the invention
[0005] The technical task of the present invention is to propose a slag-blocking and feeding line low-carbon aluminum-killed clean steel preparation process in view of the above shortcomings of the prior art. The present invention overcomes the prejudice of the prior art and gets rid of the calcium treatment process link, but can still fully meet the requirements of the castability of continuous casting molten steel, and because the number of high-melting point calcium aluminate inclusions is small, the steel plate forming performance is improved.
[0006] The technical solution of the present invention to solve the technical problem is: a slag-blocking and feeding line low-carbon aluminum killed clean steel preparation process, characterized in that the production process includes the following steps:
[0007] (1) Molten iron: Reduce the sulfur content of molten iron to below 0.02% by pretreatment of molten iron;
[0008] (2) Oxygen top and bottom combined blowing converter: adopt auxiliary lance technology and bottom argon blowing technology, slag blocking steel tapping, slag blocking process control 3-4 kg slag per ton of steel, control converter end point molten steel [O] < 550 ppm, reduce the amount of deoxidized aluminum added, and reduce the total amount of Al2O3 deoxidized inclusions;
[0009] (3) LF refining: adjust the [Al] of the incoming molten steel to 0.02-0.04%, and the temperature of the molten steel ≥ 1550°C; add lime at 6-7 kg / ton, and control the slag composition to be CaO 54-56%, Al2O3 25-30%, SiO2 6-7%, MgO 5-7%, and the basicity CaO / SiO2 value 8-9; refine and make white slag; adjust the aluminum content of the molten steel, add aluminum twice, and feed 400 meters of limestone cored wire; the silicon content of the molten steel is 0.15-0.25%; the mass percentage of the components of the refined outgoing molten steel is controlled to be: C: 0.038-0.045%, Si: 0.15-0.25%, Mn: 0.50-0.60%, P≤0.015%, S≤0.003%, Alt: 0.008-0.020%, and the balance is iron and trace amounts of unavoidable impurities;
[0010] (4) Argon soft blowing and calming at the bottom of the ladle: The ladle uses double permeable bricks, and the blowing intensity is based on not exposing the molten steel. The soft blowing calming time is 30 minutes; and the bottom blowing after refining is not allowed to stir and cool down; so that Al2O3 inclusions can fully float up and purify the molten steel;
[0011] (5) Continuous casting: adopt integral submerged nozzle, argon gas purging during tundish pouring, double-layer covering agent with alkaline at the bottom and acidic at the top, long nozzle protection pouring of the ladle, integral submerged nozzle with zirconia lining, high-purity magnesium stopper rod, automatic control of the crystallizer liquid level, electromagnetic brake, and ladle slag detection; continuous casting of molten steel is protected by argon gas, and the ladle slag is automatically detected; the difference between acid-soluble aluminum and total aluminum is controlled to ≤0.002%, and the casting speed is 3-6m / min;
[0012] (6) Steel rolling.
[0013] Wherein: in step (3), the limestone cored wire is a limestone cored wire in an iron sheet, and the cored wire material is low-sulfur limestone.
[0014] Compared with the prior art, the present invention has the following outstanding beneficial effects:
[0015] 1. The present invention overcomes the prejudice of the prior art, gets rid of the calcium treatment process, avoids the problem of flocculence of high-melting-point aluminates, improves the forming performance of steel plates, and reduces the probability of cold bending cracking;
[0016] 2. The use of the technology of the present invention can avoid the nitrogen increase problem caused by the calcium treatment process;
[0017] 3. The technology of the present invention reduces the process steps, simplifies the process flow, can completely control and reduce the number of inclusions, meet the requirements of continuous casting molten steel cleanliness and castability, and has obvious inclusion floating and adsorption effects, and the qualified rate of product composition reaches 99.3%;
[0018] 4. The use of the technology of the present invention saves the cost of calcium treatment, saving about 4.1 yuan per ton of steel, thereby increasing the profit margin for the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a scanning electron microscope picture of the inclusions in Comparative Example 3.
[0020] Figure 2 This is a scanning electron microscope image of the inclusions in Example 1.
[0021] Figure 3 This is a scanning electron microscope image of inclusions in Example 3.
[0022] Figure 4 This is a scanning electron microscope image of inclusions in Example 4.
[0023] Figure 5 This is the rod plug erosion diagram of Comparative Example 3.
[0024] Figure 6 This is the rod plug erosion diagram of Example 3. DETAILED DESCRIPTION
[0025] The thin slab continuous casting low-carbon aluminum killed clean steel production technology of the present invention is further described in detail below in conjunction with comparative examples and specific embodiments.
[0026] The following is the production process of steel grade H01301. Low carbon (silicon controlled) aluminum killed steel.
[0027] Comparative Example 1: It is an existing calcium treatment process, and the technical route is: molten iron → oxygen top and bottom combined blowing converter → LF refining → argon soft blowing at the bottom of the ladle → calcium treatment → argon soft blowing at the bottom of the ladle → continuous casting → steel rolling.
[0028] (1) Molten iron: Reduce the sulfur content of molten iron to below 0.02% by molten iron pretreatment or other methods;
[0029] (2) Converter smelting: The molten iron is initially smelted in the converter, and oxygen is blown from the top and bottom of the converter. The auxiliary lance technology and bottom argon blowing technology are used to control the final molten steel [O] of the converter to be less than 600ppm, and the slag is blocked for tapping.
[0030] (3) LF refining: After steel is tapped, ladle refining is performed, and aluminum deoxidizer, alloy, and quicklime are added to adjust the composition of the molten steel. Then, argon is blown at the argon station for deoxidation refining. After deoxidation is completed, the argon is adjusted to a soft blowing state, and the argon flow rate is 30m 3 / h, soft blowing time 8min. The mass percentage of molten steel components is controlled as follows: C: 0.038-0.045%, Si: 0.025-0.035%, Mn: 0.08-0.20%, P≤0.015%, S≤0.003%, Alt: 0.015-0.040%, the remainder is iron and trace amounts of unavoidable impurities. The amount of aluminum deoxidizer, alloy, and quicklime added shall be in accordance with the steel grade manufacturing standards.
[0031] (4) Calcium treatment: adjust the bottom blowing argon flow rate to 30m 3 / h, use a wire feeder at a speed of 2-2.5m / s to feed 400-600m / furnace of seamless metal calcium wire to achieve Ca: 0.0010-0.0040% in the molten steel;
[0032] (5) Argon soft blowing calming at the bottom of the ladle: After the calcium treatment, adjust the argon to the soft blowing state, the soft blowing time is 8 minutes, and the argon flow rate is 30m 3 / h.
[0033] (6) Continuous casting: Aluminum-carbon integral stopper rod is used to control the steel flow, long nozzle protection casting is adopted from ladle to tundish, aluminum-carbon external immersion nozzle, and casting speed is 3-6m / min.
[0034] (7) Steel rolling.
[0035] The above process is the existing thin slab continuous casting production technology, and its specific steps will not be repeated.
[0036] Comparative Example 2: The calcium treatment step in Comparative Example 1 is removed, and the pre-designed process technology route is: molten iron→oxygen top and bottom combined blowing converter→LF refining→argon soft blowing at the bottom of the ladle→thin slab continuous casting→continuous rolling.
[0037] Except for the calcium treatment step, the other process steps and parameters are the same as those in Comparative Example 1.
[0038] Example 1
[0039] (1) Molten iron: Reduce the sulfur content of molten iron to below 0.02% by molten iron pretreatment or other methods;
[0040] (2) Oxygen top and bottom blown converter: Use auxiliary gun technology and bottom blowing argon technology to control the converter end point molten steel [O] < 600ppm, stop slag and tap steel, control the converter end point molten steel [O] < 600ppm, reduce the amount of deoxidized aluminum added, and reduce the total amount of Al2O3 deoxidized inclusions.
[0041] (3) LF refining: adjust the [Al] of the incoming molten steel to 0.030-0.060% and the temperature of the molten steel to ≥1550°C; add lime at 8-12 kg / ton and control the slag composition to 55-60% CaO, 35-40% Al2O3, 3-4% SiO2, and MgO 5~7%, basicity CaO / SiO2 value 20~26; refining to make white slag; adjusting the aluminum composition of molten steel, the number of aluminum additions is less than 3 times, specifically twice in this embodiment; feeding 500 meters of limestone cored wire; the silicon content of molten steel is 0.025~0.035%; the mass percentage of the refined molten steel composition is controlled as follows: C: 0.038~0.045%, Si: 0.025~0.035%, Mn: 0.08~0.20%, P≤0.015%, S≤0.003%, Alt: 0.015~0.040%, and the remainder is iron and trace amounts of inevitable impurities. Control the aluminum content and temperature of the incoming molten steel to facilitate refining and making white slag and stabilize the production rhythm; the slag-making agent controls the basicity within the range of 20-26 so that the slag has good deoxidation and desulfurization capabilities and the ability to adsorb aluminum oxide inclusions. The number of aluminum additions is less than 3, and concentrated deoxidation is conducive to the aggregation and floating of inclusions. The more aluminum additions are made, the lower the oxygen concentration in the molten steel is in the later stage, and the more dispersed the aluminum oxide inclusions are, which is not conducive to the floating of inclusions. The protective pouring from the continuous casting ladle to the tundish and the protective pouring from the tundish to the crystallizer are important links in nitrogen control.
[0042] (4) Argon soft blowing and calming at the bottom of the ladle: The ladle uses double air-permeable bricks, and the blowing intensity is based on not exposing the molten steel. The soft blowing and calming time is 24 minutes; and the bottom blowing after refining is not allowed to stir and cool down. This allows the aluminum oxide inclusions to fully float up and purify the molten steel.
[0043] (5) Continuous casting: adopt integral submerged nozzle, automatic detection of ladle slag. Argon gas purging when the tundish is opened, double-layer covering agent (lower alkaline, upper acidic), protective pouring of ladle long nozzle, integral submerged nozzle (zirconia lining), high-purity magnesium stopper rod, automatic control of crystallizer liquid level, electromagnetic brake, ladle slag detection; continuous casting molten steel is poured with argon protection, the difference between acid-soluble aluminum and total aluminum is controlled to ≤0.002%, and the casting speed is 3-6m / min; protective pouring from the continuous casting ladle to the tundish and from the tundish to the crystallizer are important links in nitrogen control.
[0044] (6) Steel rolling.
[0045] The present invention focuses on the clean production technology of molten steel. The steel rolling process is the same and does not involve changes in the steel rolling process. Therefore, the parts not described in the embodiments are prior art and can be operated according to the processes and parameters of the prior art.
[0046] The principle of the limestone cored wire is as follows: the limestone cored wire is fed into the ladle, and the main component of the limestone, calcium carbonate, is heated and decomposed in the molten steel to generate calcium oxide and carbon dioxide. The reaction formula is:
[0047] CaCO3=(CaO)+CO2↑
[0048] The newly generated calcium oxide helps further desulfurization, reaction formula:
[0049] [FeS] + (CaO) = (CaS) + [FeO]
[0050] The generated CaO combines and aggregates with inclusions such as Al2O3 in molten steel at high temperature, and the reaction formula is:
[0051] (CaO)+(Al2O3)=Ca(AlO2)2
[0052] The original inclusions in the molten steel and the newly formed inclusions collide and gather together and float to the surface of the molten steel together with the CO2 bubbles generated by the reaction, thereby absorbing the inclusions and floating to purify the molten steel. Preventing floccules at the continuous casting nozzle helps to produce economical clean steel at low cost.
[0053] The specific specifications of the limestone cored wire may be: wire diameter: 10mm+0.5mm; iron sheet thickness: 1.5mm+ / -0.2mm; powder weight: 80g / m+ / -5%; iron sheet weight: 360g / m+ / -5%.
[0054] The physical and chemical indicators of the limestone cored wire are:
[0055]
[0056] The cost of calcium treatment is 8.7 yuan / ton, and the cost of limestone cored wire is 70% lower than that. Calculated based on an annual output of 5 million tons of steel: annual cost savings = 500×8.7×70% = 30.45 million yuan.
[0057] Example 2
[0058] (1) Molten iron: Reduce the sulfur content of molten iron to below 0.02% by molten iron pretreatment or other methods;
[0059] (2) Oxygen top and bottom blown converter: Use auxiliary lance technology and bottom blowing argon technology to control the final converter molten steel [O] < 550ppm, stop slag for steel tapping, and control the slag volume per ton of steel to 3-4 kg during the slag stopping process. The final converter molten steel [O] < 550ppm, reduce the amount of deoxidized aluminum added, and reduce the total amount of Al2O3 deoxidized inclusions.
[0060] (3) LF refining: adjust the [Al] of the incoming molten steel to 0.04-0.06%, and the temperature of the molten steel ≥1550°C; add lime at 9 kg / ton to control the slag composition to 57-60% CaO, 35-40% Al2O3, 2-3.5% SiO2, 5-7% MgO, and a basicity CaO / SiO2 value of 22-25; refine and make white slag; adjust the aluminum composition of the molten steel, and add aluminum twice; the silicon content of the molten steel is 0.025-0.035%; the mass percentage of the composition of the outgoing molten steel is controlled to be: C: 0.038-0.045%, Si: 0.025-0.035%, Mn: 0.08-0.20%, P≤0.015%, S≤0.003%, Alt: 0.015-0.040%, and the remainder is iron and trace amounts of unavoidable impurities. Adjusting the acid-soluble aluminum content of the incoming molten steel to make it have strong deoxidation and nitrogen fixation capabilities can reduce the number of aluminum additions during LF refining and improve the refining and desulfurization efficiency; controlling the incoming molten steel temperature to facilitate refining and white slag production and stabilize the production rhythm.
[0061] (4) Argon soft blowing and calming at the bottom of the ladle: The ladle uses double air-permeable bricks, and the blowing intensity is based on not exposing the molten steel. The soft blowing and calming time is 28 minutes; and after the refining station, the bottom blowing should not be stirred and cooled. The aluminum oxide inclusions can fully float up and purify the molten steel.
[0062] (5) Continuous casting: adopt integral immersion nozzle, automatic detection of ladle slag. Argon gas purging during tundish pouring, double-layer covering agent (lower alkaline, upper acidic), ladle long nozzle protection pouring, integral immersion nozzle (zirconia lining), high-purity magnesium stopper rod, automatic control of crystallizer liquid level, electromagnetic brake, ladle slag detection; continuous casting of molten steel is protected by argon gas, the difference between acid-soluble aluminum and total aluminum is controlled to ≤0.002%, and the casting speed is 3-6m / min;
[0063] (6) Steel rolling.
[0064] Examples 1 and 2 are preparations of low carbon (silicon-controlled) aluminum killed steel (H01301). The method of the present invention is also applicable to the preparation of low carbon (silicon-containing) aluminum killed steel, and the following is low carbon (silicon-controlled) aluminum killed steel (H06201).
[0065] Comparative Example 3: It is an existing calcium treatment process, and the technical route is: molten iron → oxygen top and bottom combined blowing converter → LF refining → argon soft blowing at the bottom of the ladle → calcium treatment → argon soft blowing at the bottom of the ladle → continuous casting → steel rolling.
[0066] (1) Molten iron: Reduce the sulfur content of molten iron to below 0.02% by molten iron pretreatment or other methods;
[0067] (2) Converter smelting: The molten iron is initially smelted in the converter, and oxygen is blown from the top and bottom of the converter. The auxiliary lance technology and bottom argon blowing technology are used to control the final molten steel [O] of the converter to less than 700ppm, and the slag is blocked for tapping.
[0068] (3) LF refining: After steel is tapped, ladle refining is performed, and aluminum deoxidizer, alloy, and quicklime are added to adjust the composition of the molten steel. Then, argon is blown at the argon station for deoxidation refining. After deoxidation is completed, the argon is adjusted to a soft blowing state, and the argon flow rate is 30m 3 / h, soft blowing time 8min. The mass percentage of molten steel composition is controlled as follows: C: 0.038-0.045%, Si: 0.15-0.25%, Mn: 0.50-0.60%, P≤0.018%, S≤0.003%, Alt: 0.008-0.020%, and the balance is iron and trace amounts of unavoidable impurities.
[0069] (4) Calcium treatment: adjust the bottom blowing argon flow rate to 30m 3 / h, use a wire feeder at a speed of 2-2.5m / s to feed 400-600m / furnace of seamless metal calcium wire to achieve Ca: 0.0010-0.0040% in the molten steel;
[0070] (5) Argon soft blowing calming at the bottom of the ladle: After the calcium treatment, adjust the argon to the soft blowing state, the soft blowing time is 8 minutes, and the argon flow rate is 30m 3 / h.
[0071] (6) Continuous casting: Aluminum-carbon integral stopper rod is used to control the steel flow, long nozzle protection casting is adopted from ladle to tundish, aluminum-carbon external immersion nozzle, and casting speed is 3-6m / min.
[0072] (7) Steel rolling.
[0073] Example 3
[0074] (1) Molten iron: Reduce the sulfur content of molten iron to below 0.02% by molten iron pretreatment or other methods;
[0075] (2) Oxygen top and bottom combined blowing converter: adopt auxiliary gun technology and bottom blowing argon technology to control the converter end point molten steel [O] < 600ppm, and block slag for steel tapping; control the converter end point molten steel [O] < 600ppm, reduce the amount of deoxidized aluminum added, and reduce the total amount of Al2O3 deoxidized inclusions. The converter end point and steel tapping operations are important links in nitrogen control in the present invention.
[0076] (3) LF refining: refining incoming molten steel [Al] 0.020-0.030%, molten steel temperature ≥1550°C; adding lime at 6-7 kg / ton, controlling the slag composition to be CaO 55-60%, Al2O3 25-30%, SiO2 7-8%, MgO 5-7%, and the basicity CaO / SiO2 value to be 7-8; refining to make white slag; adjusting the aluminum composition of the molten steel, strictly controlling the number of aluminum additions to be less than 3 times, specifically twice in this embodiment; the mass percentage of the molten steel components is controlled to be: C: 0.038-0.045%, Si: 0.15-0.25%, Mn: 0.50-0.60%, P≤0.015%, S≤0.003%, Alt: 0.008-0.020%, and the remainder is iron and trace amounts of unavoidable impurities.
[0077] (4) Argon soft blowing and calming at the bottom of the ladle: The ladle uses double air-permeable bricks, and the blowing intensity is based on not exposing the molten steel. The soft blowing and calming time is 22 minutes; and the bottom blowing after refining station should not be stirred and cooled. The aluminum oxide inclusions can fully float up and purify the molten steel.
[0078] (5) Continuous casting: adopt integral submerged nozzle, automatic detection of ladle slag. Argon gas purging during tundish pouring, double-layer covering agent (lower alkaline, upper acidic), ladle long nozzle protection pouring, integral submerged nozzle (zirconia lining), high-purity magnesium stopper rod, automatic control of crystallizer liquid level, electromagnetic brake, ladle slag detection; continuous casting of molten steel is protected by argon gas, the difference between acid-soluble aluminum and total aluminum is controlled to ≤0.002%, and the casting speed is 3-6m / min.
[0079] (6) Steel rolling.
[0080] Example 4
[0081] (1) Molten iron: Reduce the sulfur content of molten iron to below 0.02% by molten iron pretreatment or other methods;
[0082] (2) Oxygen top and bottom blown converter: Auxiliary lance technology and bottom argon blowing technology are used to control the final molten steel [O] of the converter to be less than 600ppm, and slag blocking is used for tapping and pre-deoxidation. Slag blocking makes the total content of FeO and MnO entering the ladle 5-7% (by weight) of the amount of molten steel entering the ladle. An aluminum-iron-magnesium composite deoxidizer is added to the molten steel for pre-deoxidation, and aluminum is fed to the molten steel in the ladle once after tapping, so that the argon station molten steel [O] is less than 200ppm, thereby reducing the amount of refined deoxidized aluminum added and reducing the total amount of Al2O3 deoxidation inclusions.
[0083] (3) LF refining: Refining the incoming molten steel [Al] 0.035-0.050%, molten steel temperature 1550-1650°C; adding lime at 6-7 kg / ton, controlling the slag composition to be CaO 54-58%, Al2O3 26-28%, SiO2 7-8%, MgO 5-6%, basicity CaO / SiO2 value 6-8; refining to make white slag; adjusting the aluminum content of the molten steel, feeding aluminum three times, feeding aluminum-iron-rare earth cored wire; making the silicon content of the molten steel 0.15-0.25%; the mass percentage of the refined outgoing molten steel composition is controlled to be: C: 0.038-0.045%, Si: 0.15-0.25%, Mn: 0.50-0.60%, P≤0.015%, S≤0.003%, Alt: 0.008-0.020%, and the remainder is iron and trace amounts of unavoidable impurities. This embodiment carries out pre-deoxidation design, and the aluminum content of the incoming molten steel is higher than that of Embodiment 1. During the refining process, the slag basicity is adjusted accordingly.
[0084] (4) Argon soft blowing and calming at the bottom of the ladle: The ladle uses double air-permeable bricks, and the blowing intensity is based on not exposing the molten steel. The soft blowing and calming time is 20 minutes; and after the refining station, the bottom blowing should not be stirred and cooled. The aluminum oxide inclusions can fully float up and purify the molten steel.
[0085] (5) Continuous casting: adopt integral submerged nozzle, automatic detection of ladle slag. Argon gas purging during tundish pouring, double-layer covering agent (lower alkaline, upper acidic), ladle long nozzle protection pouring, integral submerged nozzle (zirconia lining), high-purity magnesium stopper rod, automatic control of crystallizer liquid level, electromagnetic brake, ladle slag detection; continuous casting of molten steel is protected by argon gas, the difference between acid-soluble aluminum and total aluminum is controlled to ≤0.002%, and the casting speed is 3-6m / min.
[0086] (6) Steel rolling.
[0087] Example 5
[0088] (1) Molten iron: Reduce the sulfur content of molten iron to below 0.02% by molten iron pretreatment or other methods;
[0089] (2) Oxygen top and bottom blown converter: Use auxiliary lance technology and bottom blowing argon technology to control the final converter molten steel [O] < 550ppm, stop slag for steel tapping, and control the slag volume per ton of steel to 3-4 kg during the slag stopping process. The final converter molten steel [O] < 550ppm, reduce the amount of deoxidized aluminum added, and reduce the total amount of Al2O3 deoxidized inclusions.
[0090] (3) LF refining: adjusting the refining incoming molten steel [Al] 0.02-0.04%, molten steel temperature ≥ 1550°C; adding lime at 6-7 kg / ton, controlling the slag composition to be CaO 54-56%, Al2O3 25-30%, SiO2 6-7%, MgO 5-7%, basicity CaO / SiO2 value 8-9; refining and making white slag; adjusting the aluminum composition of the molten steel, adding aluminum twice, feeding 400 meters of limestone cored wire (specifications are the same as in Example 1); the silicon content of the molten steel is 0.15-0.25%; the mass percentage of the refining outgoing molten steel composition is controlled to be: C: 0.038-0.045%, Si: 0.15-0.25%, Mn: 0.50-0.60%, P≤0.015%, S≤0.003%, Alt: 0.008-0.020%, and the remainder is iron and trace amounts of inevitable impurities. Adjusting the acid-soluble aluminum content of the incoming molten steel to make it have strong deoxidation and nitrogen fixation capabilities can reduce the number of aluminum additions during LF refining and improve the refining and desulfurization efficiency; controlling the incoming molten steel temperature to facilitate refining and white slag production and stabilize the production rhythm.
[0091] (4) Argon soft blowing and calming at the bottom of the ladle: The ladle uses double air-permeable bricks, and the blowing intensity is based on not exposing the molten steel. The soft blowing and calming time is 30 minutes; and after the refining station, the bottom blowing should not be stirred and cooled. This allows the aluminum oxide inclusions to fully float up and purify the molten steel.
[0092] (5) Continuous casting: adopt integral immersion nozzle, automatic detection of ladle slag. Argon gas purging during tundish pouring, double-layer covering agent (lower alkaline, upper acidic), ladle long nozzle protection pouring, integral immersion nozzle (zirconia lining), high-purity magnesium stopper rod, automatic control of crystallizer liquid level, electromagnetic brake, ladle slag detection; continuous casting of molten steel is protected by argon gas, the difference between acid-soluble aluminum and total aluminum is controlled to ≤0.002%, and the casting speed is 3-6m / min;
[0093] (6) Steel rolling.
[0094] The present invention achieves the goal of clean steel production by optimizing the process flow, and no flocculent flow or water blocking occurs during the molten steel casting process, and the rod position is stable. The comparative examples and specific embodiments are compared, and the results are as follows:
[0095] 1. Comparison of flocculation occurrence
[0096] Whether molten steel will flocculate depends on whether the key inclusions can actually float. Comparative Example 1 is a prior art calcium-treated molten steel. The original technical purpose of calcium treatment is to control the appropriate calcium-aluminum ratio to generate low-melting-point liquid 12CaO·7Al2O3, 3CaO·Al2O3 aluminates to promote the floating of inclusions. But in fact, since calcium is very active and easy to oxidize, if the calcium component is not properly controlled, too much or too little, solid calcium oxide or solid calcium aluminate will be generated, which will not achieve the purpose of generating low-melting-point calcium aluminate; resulting in insufficient floating inclusions, which not only wastes the cost of calcium treatment, but also cannot avoid the occurrence of flocculations.
[0097] The technology of the present invention achieves effective inclusion floating by: ① controlling the oxygen content at the converter end, the aluminum composition and temperature at the refining station, the slag composition and basicity; ② controlling the bottom blowing agitation; ③ controlling the number of aluminum additions; ④ increasing the bottom blowing permeability by improving the air-permeable bricks, and replacing the more expensive solid calcium cored wire with an economical and cheap limestone cored wire to achieve effective inclusion floating, thus overcoming the technical prejudice in the prior art that inclusion floating must rely on calcium treatment.
[0098] The flocculation incidence rate of each group: Comparative Example 1 is 0.96%; Comparative Example 2 has serious flocculation, the water outlet is blocked, and the process fails; Comparative Example 3 is 1.05%; Example 1 is 0.07%; Example 2 is 0.08%; Example 3 is 0.08%; Example 4 is 0.09%; Example 5 is 0.07%.
[0099] The results show that the difference in flocculation incidence between the technical process of the present invention and the comparative example 1 treated with calcium in the prior art is not statistically significant (P>0.05), and from the data alone, the flocculation incidence of Examples 1 and 5 (fed limestone cored wire) of the technical process of the present invention is significantly lower than that of the comparative examples 1 to 3 treated with calcium in the prior art. By comparing the results of the technical process of the present invention and the comparative examples, it can be seen that the technical effectiveness of the technical process of the present invention lies in the combination of improvements in each link in the process steps and the invention and innovation of the economical and cheap limestone cored wire, rather than simply removing the calcium treatment step.
[0100] 2. The final product steel composition is compared as shown in the following table: The preparation process of comparative example 2 failed due to severe flocculation and nozzle blockage, which made its preparation impossible, so the final product data is missing.
[0101] Low carbon (silicon controlled) aluminum killed steel (H01301)
[0102]
[0103]
[0104] Low carbon (silicon containing) aluminum killed steel (H06201)
[0105] element% C Si Mn P S Alt Ca Comparative Example 3 0.04424 0.19344 0.52386 0.0136 0.00077 0.01329 0.00145 Example 3 0.04357 0.18208 0.53512 0.01761 0.00105 0.01461 — Example 4 0.04229 0.18776 0.53521 0.01751 0.00051 0.01289 — Example 5 0.0416 0.18239 0.53709 0.01736 0.00181 0.01553 —
[0106] By comparing the components in the above table, it can be found that the low-carbon (silicon-controlled) aluminum-killed steels of Examples 1 and 2 and the low-carbon (silicon-containing) aluminum-killed steels of Examples 3 to 5, which adopt the non-calcium treatment process, have stable compositions.
[0107] 3. Comparison of physical and chemical properties of final product materials: The preparation process of comparative example 2 failed. Due to severe flocculation and nozzle blockage, its preparation could not be carried out, so the final product data was missing.
[0108] Low carbon (silicon controlled) aluminum killed steel (H01301)
[0109] Example comparison Specifications (mm) Yield Strength MPA Tensile strength MPA Elongation % r-value Inspection Standards ≤330 270-420 ≥32.0 Comparative Example 1 2.00×1500 295 375 39.5 0.79 Example 2 2.00×1500 291 371 42.1 0.78 Example 3 2.00×1500 298 371 41.0 0.80
[0110] Low carbon (silicon containing) aluminum killed steel (H06201)
[0111]
[0112]
[0113] The mechanical properties of the calcium-treated steels of Comparative Examples 1 and 3 and the non-calcium-treated steels of Examples 1 to 5 all meet the steel grade inspection standards. The non-calcium-treated steels obtained by Examples 1 to 5 have a higher elongation than the steel processed by the process of Comparative Example 1, and a lower r value than that of Comparative Example 1. The elongation and r value (ratio of yield strength / tensile strength) reflect the formability of steel. In theory, the smaller the r value, the better the plastic deformation and the better the processing and forming performance. The technical solution of the present invention is explained. The hot-rolled plate made by the non-calcium treatment process has better processing and forming performance than the calcium-treated process steel. This is because the high-melting-point calcium aluminate inclusions in the molten steel of this treatment process affect the formability of the steel plate, making cold bending cracking prone to occur.
[0114] 4. The electron microscope scanning results of hot rolled plate sampling inclusions are as follows:
[0115] (1) Comparison of inclusion composition
[0116]
[0117] By comparing the inclusion compositions in the above table, it can be found that the inclusion composition under the non-calcium treatment process is mainly alumina inclusions, while the inclusion composition of the product under the calcium treatment process is complex, mainly high-melting point calcium aluminates. This type of inclusion is easy to gather over a large area, causing flocculation in the continuous casting machine, affecting production and increasing production costs.
[0118] (2) Scanning electron microscope images:
[0119] Figures 1 to 4They are respectively: scanning electron microscope pictures of inclusions in comparative example 3 and examples 1, 3 and 4. By comparison, it can be found that the inclusions in examples 1, 3 and 4 are similar in size to those in comparative example 3. In terms of shape, comparative example 3 is mainly nearly spherical, while examples 1, 3 and 4 are irregular. Since comparative example 3 is subjected to a calcium treatment process, the high-melting-point calcium aluminates in the inclusions are easily aggregated into large-sized inclusions, affecting the quality of the ingot and ultimately affecting the quality of the steel, resulting in a decrease in the qualified rate of the steel.
[0120] 5. Comparison of stopper rod erosion
[0121] Figure 5 This is the rod plug erosion diagram of comparative example 3. It can be seen that calcium treats the molten steel, and calcium reacts with Al2O3 in the stopper rod refractory to generate low-melting-point aluminate, causing obvious erosion grooves on the head of the stopper rod. This is because the following reactions occur in the molten steel: [Ca]+[O]=CaO, 12CaO+7Al2O3=12CaO7Al2O3, [Ca] in the molten steel reacts with [O] to generate CaO, and CaO reacts with Al2O3 in the stopper rod refractory to generate low-melting-point 12CaO7Al2O3, causing the solid stopper rod to continuously dissolve and erode. When the stopper rod erosion is severe, it will cause unstable molten steel injection and unstable crystallizer liquid level, resulting in flocculent flow, slag rolls, and even steel leakage and other production, quality and safety accidents.
[0122] Figure 6 This is the rod plug erosion diagram of Example 3. The corrosion morphology of the non-calcium treated steel plug rod is that the plug rod head is relatively smooth and the degree of corrosion is relatively reduced. Because it does not contain calcium and cannot generate low melting point aluminates, the degree of corrosion is light. The pouring is stable, avoiding production and quality safety accidents such as flocculent flow, slag roll, and steel leakage.
[0123] 6. Cost comparison
[0124] Compared with the calcium treatment process of the prior art comparative example, the various embodiment groups (including silicon / silicon controlled) adopting the technical solution of the present invention simplify the steps, save the calcium treatment cost, and the castability, composition and performance of the molten steel meet the standard requirements. The cost is reduced by 4.1 yuan / ton compared with the same grade of steel.
[0125] The use of low-cost limestone cored wire instead of the more expensive calcium solid cored wire reduces production costs. The castability, composition and performance of the molten steel all meet the standard requirements, and the cost is reduced by 8.7×70%=6.09 yuan / ton compared with the same grade of steel.
[0126] It should be noted that the specific embodiments of the present invention have been described in detail. For those skilled in the art, various obvious changes to the present invention without departing from the spirit and scope of the present invention are within the protection scope of the present invention.
Claims
1. A process for preparing low-carbon aluminum killed clean steel with slag blocking and feeding line, characterized in that: The production process includes the following steps: (1) Molten iron: Reduce the sulfur content of molten iron to below 0.02% through molten iron pretreatment; (2) Oxygen top and bottom combined blowing converter: adopt auxiliary lance technology and bottom argon blowing technology, slag blocking steel tapping, control the slag amount per ton of steel to 3-4 kg during the slag blocking process, control the converter end point molten steel [O] < 550 ppm, reduce the amount of deoxidized aluminum added, and reduce the total amount of Al2O3 deoxidized inclusions; (3) LF refining: adjust the [Al] content of the incoming molten steel to 0.02-0.04% and the temperature of the molten steel to ≥1550°C; add lime at 6-7 kg / ton and control the slag composition to be CaO 54-56%, Al2O3 25-30%; SiO2 6-7%; MgO 5-7% and the basicity CaO / SiO2 value to 8-9; refine and produce white slag; adjust the aluminum content of the molten steel, add aluminum twice and feed 400 meters of limestone cored wire; the specific specifications of the limestone cored wire are: wire diameter: 10 mm ± 0.5 mm; iron sheet thickness: 1.5 mm ± 0.2 mm; powder weight: 80 g / m ± 5%; iron sheet weight: 360 g / m±5%; the material name of the limestone cored wire is low-sulfur limestone, and its chemical composition includes CaO≥52%, S≤0.030%, SiO2≤1.5%, and MgO≤1.5%; the particle size is 3mm; the silicon content of molten steel is 0.15-0.25%; the mass percentage of the refined molten steel composition is controlled as follows: C: 0.038-0.045%, Si: 0.15-0.25%, Mn: 0.50-0.60%, P≤0.015%, S≤0.003%, Alt: 0.008-0.020%, and the balance is iron and trace amounts of unavoidable impurities; (4) Argon soft blowing calming at the bottom of the ladle: The ladle uses double air-permeable bricks, and the blowing intensity is based on not exposing the molten steel. The soft blowing calming time is 30 minutes; and the bottom blowing after refining is not allowed to stir and cool down; so that Al2O3 inclusions can fully float up and purify the molten steel; (5) Continuous casting: adopt integral submerged nozzle, argon gas purging for tundish pouring, double-layer covering agent with alkaline at the bottom and acidic at the top, long nozzle protection pouring for ladle, integral submerged nozzle with zirconia lining, high-purity magnesium stopper rod, automatic control of crystallizer liquid level, electromagnetic brake, and ladle slag detection; continuous casting of molten steel is protected by argon gas, and ladle slag is automatically detected; the difference between acid-soluble aluminum and total aluminum is controlled to ≤0.002%, and the casting speed is 3-6m / min; (6) Steel rolling.