Magnetic storage device

By using ferromagnetic Hasler material and topological insulator material to construct SOT structures in magnetic memory devices, the problem of insufficient fast switching and low current operation efficiency in the prior art is solved, and a high-performance magnetic memory cell is realized.

CN111312745BActive Publication Date: 2024-11-29SAMSUNG ELECTRONICS CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201911232220.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-12-05
Publication Date
2024-11-29
Estimated Expiration
2039-12-05

AI Technical Summary

Technical Problem

The existing magnetic memory devices are inefficient in fast switching and low current operation, especially in the design of spin-orbit torque (SOT) structures, which are difficult to achieve good crystal quality and high perpendicular magnetic anisotropy, resulting in memory cells. performance limitations.

Method used

Using fixed layer and free layer structures including ferromagnetic Hasler materials, and constructing SOT structures through topological insulator materials, using spin Hall effect to achieve fast switching and low current operation, ensuring good crystal quality of free layer and fixed layer and high perpendicular magnetic anisotropy.

Benefits of technology

Fast switching and low current operation of the magnetic memory device are realized, the performance of the memory cell is improved, the damage to the SOT structure in the patterning process is avoided, and the crystallinity and current transfer efficiency of the free layer are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111312745B_ABST
    Figure CN111312745B_ABST
Patent Text Reader

Abstract

A magnetic memory device comprises: a buffer layer on a substrate; a magnetic tunnel junction structure, which comprises a fixed layer structure, a tunnel barrier and a free layer stacked in sequence on the buffer layer; and a spin-orbit torque (SOT) structure, which is located on the magnetic tunnel junction structure and comprises a topological insulator material, wherein the free layer comprises a Hassler material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of Korean Patent Application No. 10-2018-0159037, filed on December 11, 2018, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field

[0003] The inventive concept relates to a magnetic memory device, and more particularly, to a magnetic memory device including a magnetic tunnel junction (MTJ). Background Art

[0004] Electronic devices that utilize the magnetoresistive properties of MTJs have been studied. Specifically, as MTJ cells of highly integrated magnetic random access memory (MRAM) devices are miniaturized, MRAM devices that store information by programming MTJ cells using spin-orbit torque have been proposed. Such MRAM devices may require fast switching and low current operation. Summary of the invention

[0005] The inventive concept provides a magnetic memory device capable of fast switching and low current operation.

[0006] According to one aspect of the present invention, a magnetic memory device is provided, comprising: a buffer layer on a substrate; a magnetic tunnel junction structure comprising a fixed layer structure, a tunnel barrier and a free layer stacked in sequence on the buffer layer; and a spin-orbit torque (SOT) structure located on the magnetic tunnel junction structure and comprising a topological insulator material, wherein the free layer comprises a Heusler material.

[0007] According to another aspect of the inventive concept, a magnetic memory device is provided, the magnetic memory device comprising: a buffer layer on a substrate; a magnetic tunnel junction structure arranged on the buffer layer, the magnetic tunnel junction comprising a fixed layer structure, a tunnel barrier and a free layer sequentially stacked on the buffer layer;

[0008] And a spin-orbit torque (SOT) structure arranged on a magnetic tunnel junction structure, the SOT structure comprising: a first electrode layer, which is located on the magnetic tunnel junction structure and comprises a ferrimagnetic Hassler material; and a second electrode layer, which is located on the first electrode layer and comprises a topological insulator material.

[0009] According to another aspect of the inventive concept, a magnetic memory device is provided, comprising: a buffer layer on a substrate; a fixed layer structure, which is located on the buffer layer and includes a ferrimagnetic Heusler material; a tunnel barrier, which is located on the fixed layer structure; a free layer, which is located on the tunnel barrier and includes a ferrimagnetic Heusler material; and a spin-orbit torque (SOT) structure, which is located on the free layer and includes a topological insulator material. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Embodiments of the inventive concept will be more clearly understood from the following detailed description taken in conjunction with the accompanying drawings, in which:

[0011] Figure 1 is a layout diagram showing a magnetic memory device according to an example embodiment;

[0012] Figure 2A It is along Figure 1 A sectional view taken along line IIA-IIA' in FIG. Figure 2B It is along Figure 1 A sectional view taken along line IIB-IIB';

[0013] Figure 3 yes Figure 2A A magnified view of area CX in FIG.

[0014] FIG. 4A to FIG. 4C are schematic diagrams of a method of driving a magnetic memory device according to example embodiments;

[0015] Figure 5 is a cross-sectional view illustrating a magnetic memory device according to an example embodiment;

[0016] Figure 6 is a cross-sectional view illustrating a magnetic memory device according to an example embodiment;

[0017] Figure 7 is a cross-sectional view illustrating a magnetic memory device according to example embodiments; and

[0018] Figures 8 to 13 are cross-sectional views illustrating a method of manufacturing a magnetic memory device according to example embodiments, respectively. DETAILED DESCRIPTION

[0019] Hereinafter, embodiments of the inventive concept will be described in detail with reference to the accompanying drawings.

[0020] Figure 1 is a layout diagram illustrating a magnetic memory device 100 according to example embodiments. Figure 2A It is along Figure 1 A cross-sectional view taken along line IIA-IIA' in FIG. Figure 2B It is along Figure 1A cross-sectional view taken along line IIB-IIB'. Figure 3 yes Figure 2A Magnified view of area CX.

[0021] Reference Figures 1 to 3 , the magnetic memory device 100 may include word lines WL, memory cells MC, and spin-orbit torque (SOT) lines SL and bit lines BL located on / over a substrate 110. The word lines WL and the bit lines BL may be arranged to cross each other, and a plurality of memory cells MC may be located between the word lines WL and the bit lines BL (or may be located at the intersection of the word lines WL and the bit lines BL in a plan view). Figure 1 As shown, the magnetic memory device 100 may have a cross-point array structure.

[0022] For example, the word line WL may extend in a first direction (X direction) on the substrate 110, and the bit line BL may extend in a second direction (Y direction) at a higher level than the word line WL. The SOT line SL may be located between the bit line BL and the memory cell MC, and may extend in the first direction (X direction), for example. The terms first, second, etc. may be used herein to distinguish one element from another element.

[0023] The SOT line SL may include a non-magnetic material having a high spin-orbit coupling characteristic and may be used as a source line of the SOT in the SOT-type MRAM device. In the SOT-type MRAM device, when current flows through the SOT line SL, the free layer 170 may be switched by the spin Hall effect (i.e., a phenomenon in which spin polarization occurs perpendicular to the current direction, wherein the current direction interacts with spins in the SOT line SL lattice contacting the SOT line SL).

[0024] like Figure 2A As shown, the first conductive line 120 may be located on the substrate 110, and the plurality of switching elements 130 may be located on the first conductive line 120. An intermediate layer such as an interlayer insulating layer may also be disposed on the substrate 110, and the interlayer insulating layer may be located between the substrate 110 and the first conductive line 120.

[0025] The first conductive line 120 may be Figure 1 The first conductive line 120 may include a conductive material such as doped polysilicon, titanium, titanium nitride, tantalum, tantalum nitride, titanium tungsten, tungsten, aluminum, cobalt, and / or nickel.

[0026] The plurality of switch elements 130 may be configured to selectively control the current passing through the memory cell MC. In example embodiments, the plurality of switch elements 130 may include a PMOS transistor or an NMOS transistor. In this case, some of the plurality of switch elements 130 may be located within the substrate 110 (e.g., may include a region located on or in the substrate 110), and a wiring structure for electrically connecting the first conductive line 120 to the plurality of switch elements 130 may also be formed. In other embodiments, the plurality of switch elements 130 may include a diode or a bidirectional threshold switch (OTS) device.

[0027] A plurality of bottom electrodes 132 may be respectively located on the plurality of switching elements 130. The plurality of bottom electrodes 132 may electrically connect the plurality of switching elements 130 to the plurality of memory cells MC. For example, the plurality of bottom electrodes 132 may include at least one of TiN, Ti, TaN, Ta, Ru, and W. Elements listed using the terms “at least one of” and “or” include any and all combinations of one or more of the associated listed elements, and may also be indicated herein by the term “and / or”.

[0028] A first interlayer insulating layer 136 covering the first conductive line 120, the plurality of switching elements 130, and the plurality of bottom electrodes 132 may be located on the substrate 110. A top surface of the first interlayer insulating layer 136 may be located at the same level as top surfaces of the plurality of bottom electrodes 132, and the first interlayer insulating layer 136 may cover sidewalls of the plurality of bottom electrodes 132. The first interlayer insulating layer 136 may have a stacked structure including a plurality of insulating layers.

[0029] Each of the plurality of memory cells MC may include a buffer layer 140 and an MTJ structure (MTJS) sequentially arranged on each of the plurality of bottom electrodes 132. The plurality of memory cells MC may be located between a word line WL and a bit line BL. Figure 1 As shown, the horizontal cross-section of the plurality of memory cells MC may be circular, but the embodiment is not limited thereto, and the horizontal cross-section of the plurality of memory cells MC may have various shapes such as rectangle, triangle, trapezoid or other polygons. The width of each of the plurality of memory cells MC in the first direction (X direction) may be greater than the width of each of the plurality of bottom electrodes 132 in the first direction (X direction), but the embodiment is not limited thereto. Figure 2A and Figure 2B Unlike shown, the width of each of the plurality of memory cells MC in the first direction (X direction) may be the same as the width of each of the plurality of bottom electrodes 132 in the first direction (X direction).

[0030] The buffer layer 140 may be located on each of the plurality of bottom electrodes 132. The buffer layer 140 may be used as a growth template in the process of forming the MTJ structure MTJS to obtain excellent crystal quality. The buffer layer 140 may include a non-magnetic metal material (such as chromium (Cr), ruthenium (Ru) and / or tantalum (Ta)), a non-magnetic compound (such as cobalt gallium (CoGa) and / or manganese gallium nitride (MnGaN)) and / or a non-magnetic alloy (such as nickel aluminum alloy (NiAl)).

[0031] The MTJ structure may include a fixed layer structure 150 , a tunnel barrier 160 , and a free layer 170 sequentially disposed on a buffer layer 140 .

[0032] The fixed layer structure 150 may include a fixed easy magnetization axis and have a fixed magnetization direction. For example, the fixed layer structure 150 may have an easy magnetization axis in a third direction (Z direction) and may include a perpendicular magnetic anisotropy (PMA) material. The free layer 170 may have a magnetization direction that changes according to conditions. For example, the free layer 170 may have an easy magnetization axis that changes in the third direction (Z direction). In this case, a vertical magnetic memory device may be implemented. In other embodiments, the fixed layer structure 150 may have an easy magnetization axis in a first direction (X direction), and the free layer 170 may have a variable easy magnetization axis in the first direction (X direction). In this case, a horizontal magnetic memory device may be implemented.

[0033] The resistance value of the MTJ structure may depend on the magnetization direction of the free layer 170. When the magnetization direction of the free layer 170 is parallel to the magnetization direction of the fixed layer structure 150, the MTJ structure may have a low resistance value and store data "0". When the magnetization direction of the free layer 170 is anti-parallel to the magnetization direction of the fixed layer structure 150, the MTJ structure may have a high resistance value and store data "1".

[0034] In example embodiments, the fixed layer structure 150 may have a stacked structure including a bottom fixed layer 152 and a top fixed layer 154. Both the bottom fixed layer 152 and the top fixed layer 154 may include a ferrimagnetic Heusler material. The ferrimagnetic Heusler material may refer to a manganese-based alloy having a tetragonal phase, and may include a manganese-based alloy including, for example, D0 22 Crystal structure. Here, the term 'alloy' may refer not only to a substance in which different kinds of metal elements are mixed to have a regular crystal structure but also to a material in which at least one metal element and at least one non-metal element are mixed to have a regular crystal structure.

[0035] The bottom pinned layer 152 may contact the buffer layer 140 and include a binary ferrimagnetic Heusler material. The bottom pinned layer 152 may include a material having a chemical formula of Mn a X bAnd a binary ferrimagnetic Heusler material having high perpendicular magnetic anisotropy and / or low damping characteristics (e.g., low Gilbert damping characteristics). In the above chemical formula, the atomic contents a and b of Mn and X may have various values, respectively. For example, the bottom fixed layer 152 may include at least one of manganese gallium (MnGa) and manganese germanium (MnGe).

[0036] The top pinned layer 154 may be located on the bottom pinned layer 152 and include a ternary ferrimagnetic Heusler material. The top pinned layer 154 may include a material having a chemical formula of Mn a X b Y c And a ternary ferrimagnetic Heusler material with high perpendicular magnetic anisotropy and / or low damping characteristics. The letter Y may refer to a magnetic metal element such as cobalt, nickel or iron. In the above chemical formula, the atomic contents a, b and c of Mn, X and Y may have various values, respectively. For example, the top fixed layer 154 may include at least one of MnGaNi, MnGeNi, MnGaCo, MnGeCo, MnGaFe and MnGeFe.

[0037] Since both the bottom pinned layer 152 and the top pinned layer 154 include a ferrimagnetic Heusler material, both the bottom pinned layer 152 and the top pinned layer 154 formed on the buffer layer 140 may have excellent crystal quality. In addition, the stacked structure of the bottom pinned layer 152 and the top pinned layer 154 may have high perpendicular magnetic anisotropy due to relatively high exchange coupling, and thus, the pinned layer structure 150 may have high tunnel magnetoresistance (TMR).

[0038] The tunnel barrier 160 may be located on the fixed layer structure 150. The tunnel barrier 160 may have a thickness less than the spin diffusion length. For example, the tunnel barrier 160 may have a thickness of about 1 to about 20 nm in a third direction (Z direction) perpendicular to the top surface of the substrate 110.

[0039] The tunnel barrier 160 may include a non-magnetic material. In example embodiments, the tunnel barrier 160 may include at least one of an oxide such as an oxide of magnesium (Mg), titanium (Ti), aluminum (Al), magnesium zinc (MgZn), and / or magnesium boron (B) and a nitride such as a nitride of titanium (Ti) and / or vanadium (V). For example, the tunnel barrier 160 may include a magnesium oxide (MgO) layer or a magnesium aluminum oxide (MgAlO) layer. Alternatively, the tunnel barrier 160 may include a plurality of layers. For example, the tunnel barrier 160 may have a stacked structure including Mg / MgO, MgO / Mg, MgO / MgAlO, MgAlO / MgO, Mg / MgAlO / Mg, MgO / MgAlO / MgO, MgAlO / MgO / MgAlO, and the like. The tunnel barrier 160 may have a NaCl crystal structure (face-centered cubic lattice structure).

[0040] In some embodiments, the tunnel barrier 160 may include magnesium aluminum oxide (MgAlO), in which case the lattice mismatch between the top pinned layer 154 including a ferrimagnetic Heusler material and the tunnel barrier 160 may be relatively small.

[0041] The free layer 170 may be located on the tunnel barrier 160. The free layer 170 may include a ferrimagnetic Heusler material. The free layer 170 may include a manganese-based alloy having a tetragonal phase and may include a D0 22 The free layer 170 may include a manganese-based alloy having a chemical formula of Mn a X b And a binary ferrimagnetic Heusler material having high perpendicular magnetic anisotropy and / or low damping characteristics. In the above chemical formula, the atomic contents a and b of Mn and X may have various values, respectively. For example, the free layer 170 may include at least one of MnGa or MnGe.

[0042] In example embodiments, since the lattice mismatch between the free layer 170 and the tunnel barrier 160 is relatively small and the tunnel barrier 160 has a relatively small thickness, the free layer 170 may be formed by using the fixed layer structure 150 on the bottom surface of the tunnel barrier 160 as a growth template. 22 The ferrimagnetic Heusler material of the crystal structure, so the free layer 170 can also have a D0 of good crystal quality. 22 Crystal structure. In addition, the interface quality between the free layer 170 and the tunnel barrier 160 may also be good. In addition, the free layer 170 may include a binary ferrimagnetic Heusler material exhibiting high perpendicular magnetic anisotropy and low damping characteristics, and thus, a low current switching operation may be achieved by using an MTJ structure including the free layer 170.

[0043] like Figure 3 As shown, the sidewalls of the buffer layer 140, the sidewalls of the fixed layer structure 150, the sidewalls of the tunnel barrier 160, and the sidewalls of the free layer 170 may be aligned relative to each other along a straight line. Fig. 9 ), initial bottom fixing layer 152P (refer to Fig. 9 ), initial top fixing layer 154P (refer to Fig. 9 ), initial tunnel barrier 160P (refer to Fig. 9 ) and the initial free layer 170P (refer to Fig. 9 ) are sequentially formed and then patterned to form the plurality of memory cells MC including the buffer layer 140, the fixed layer structure 150, the tunnel barrier 160 and the free layer 170, so such alignment is possible.

[0044] The insulating pattern 146 may be located on the first interlayer insulating layer 136 to surround the sidewalls of the plurality of memory cells MC. The insulating pattern 146 may surround the sidewalls of the buffer layer 140 and the sidewalls of the MTJ structure, and the top surface of the insulating pattern 146 may be located at the same level as the top surface of the free layer 170. As used herein, an element surrounding or covering another element may partially or completely surround or cover the other element.

[0045] The SOT structure 180 extending in the second direction (Y direction) may be located on the MTJ structure and the insulating pattern 146. The SOT structure 180 may include a first electrode layer 182 and a second electrode layer 184 stacked in sequence, and both the first electrode layer 182 and the second electrode layer 184 may extend in the second direction. Figure 1 Corresponding to the SOT line SL in.

[0046] The second electrode layer 184 may include a non-magnetic material having spin-orbit coupling properties, and may include, for example, a topological insulator material. The topological insulator material may have insulating properties therein due to a specific crystallization order, while portions adjacent to its surface generally include a conductive material. For example, portions adjacent to the top and bottom surfaces of the second electrode layer 184 may exhibit conductivity, while other portions of the second electrode layer 184 may exhibit insulating properties. In an example embodiment, the second electrode layer 184 may include bismuth antimony (Bi 1-x Sb x , wherein x is from about 0.05 to about 0.25) or bismuth selenide (Bi 1-y Se y , where y is at least one of about 0.05 to about 0.25). The second electrode layer 184 may have a relatively high spin Hall angle value. The second electrode layer 184 may have a high spin Hall angle value of about 0.5 or more (e.g., about 2 or more, or about 5 or more), but the embodiment is not limited thereto.

[0047] The first electrode layer 182 may be used as a buffer layer to improve the interface characteristics between the second electrode layer 184 and the MTJ structure (or the free layer 170). In example embodiments, the first electrode layer 182 may include a binary ferrimagnetic Heusler material such as MnGe and / or MnGa. In other embodiments, the first electrode layer 182 may include a ternary ferrimagnetic Heusler material such as MnGaNi, MnGeNi, MnGaCo, MnGeCo, MnGaFe, and / or MnGeFe.

[0048] The second electrode layer 184 can transfer the spin current to the free layer 170 by using the spin Hall effect. The second electrode layer 184 may include a topological insulator material, and the topological insulator material as a source of spin-orbit torque may exhibit a higher spin-orbit coupling characteristic than a commonly used metal material (such as tantalum, tungsten and / or platinum) with a spin Hall effect. For example, the second electrode layer 184 may have a relatively higher spin Hall angle value than a commonly used metal material (such as tantalum, tungsten and / or platinum) with a spin Hall effect. Since the second electrode layer 184 uses a topological insulating material with good spin-orbit coupling characteristics, the magnetic memory device 100 can be driven at low current or low power.

[0049] like Figure 3 As shown, the first electrode layer 182 may have a first thickness t11 in a third direction (Z direction) perpendicular to the top surface of the substrate 110, and the second electrode layer 184 may have a second thickness t12 in the direction (Z direction) greater than the first thickness t11. The first thickness t11 may be about 1 to about 10 nm, but is not limited thereto.

[0050] The SOT structure 180 may include a first bottom surface 180L1 on the free layer 170 and a second bottom surface 180L2 on the insulating pattern 146. The entire top surface of the free layer 170 may contact the bottom surface of the SOT structure 180, that is, the first bottom surface 180L1. The entire bottom surface of the second electrode layer 184 may be located on the first electrode layer 182, the second electrode layer 184 may not contact the insulating pattern 146, and the first electrode layer 182 may be located on the top surface of the insulating pattern 146 and the free layer 170. Since the first electrode layer 182 includes a manganese-based alloy having a tetragonal crystal phase and has the same crystal structure as the material included in the free layer 170, the flatness and crystal quality of the second electrode layer 184 may be good, and the interface characteristics between the first electrode layer 182 and the second electrode layer 184 may be good.

[0051] The second interlayer insulating layer 186 may be located on the SOT structure 180 and higher than the insulating pattern 146 .

[0052] A second conductive line 190 extending in the second direction (Y direction) may be located on the second interlayer insulating layer 186, and a plurality of contacts 188 penetrating the second interlayer insulating layer 186 may connect the SOT structure 180 to the second conductive line 190. The second conductive line 190 may be connected to the second interlayer insulating layer 186. Figure 1 Each of the plurality of contacts 188 may be arranged at a position vertically overlapping with each of the plurality of MTJ structures MTJS.

[0053] The plurality of contacts 188 and the second wire 190 may include conductive materials such as doped polysilicon, titanium, titanium nitride, tantalum, tantalum nitride, titanium tungsten, tungsten, aluminum, cobalt and / or nickel. In example embodiments, the SOT structure 180 including the topological insulator material may have a relatively low resistivity and be separated from the second wire 190, and the amount of current flowing in the SOT structure 180 may be increased compared to, for example, the second wire 190 and the SOT structure 180 are formed in a stacked manner or the second wire 190 and the SOT structure 180 are formed in contact with each other. However, the inventive concept is not limited thereto.

[0054] like Figure 3 As shown, with respect to the top surface level LV0 of the substrate 110, the top surface level LV3 of the free layer 170 may be higher than the top surface level LV1 of the fixed layer structure 150, and the bottom surface level (that is, the top surface level LV3) of the SOT structure 180 may be higher than the top surface level LV2 of the tunnel barrier 160. According to example embodiments, the SOT structure 180 may be arranged at a higher level than the MTJ structure, and thus, the SOT structure 180 may not be damaged in the patterning process of the MTJ structure.

[0055] Typically, in a SOT type MRAM device, a SOT line may be located on a switching element, and an MTJ structure including a free layer, a tunnel barrier, and a fixed layer in order may be arranged on the SOT line. In the etching process of patterning the MTJ structure, etching residues that typically include heavy metal materials may be redeposited on the patterned sidewalls, causing a short circuit between the free layer and the fixed layer, and the top surface of the SOT line exposed to the etching environment may be damaged by etching gas or etchant. However, according to example embodiments, the SOT structure 180 may be arranged at a higher level than the MTJ structure MTJS, and therefore, damage to the SOT structure 180 during the patterning process of the MTJ structure MTJS may be prevented.

[0056] In addition, generally, in an MRAM device of the SOT type, the SOT line may be located on the switching element, and the MTJ structure including the free layer, the tunnel barrier and the fixed layer in order may be arranged on the SOT line. Specifically, since the SOT line and the free layer need to contact each other without an additional material layer between them, it may be difficult to arrange a buffer layer for improving the crystallinity of the free layer, and therefore, the crystal quality of the free layer may be relatively low, and there may be limitations in selecting the material to be used for the free layer. Specifically, although the ferrimagnetic Hasler material has low damping characteristics and high perpendicular magnetic anisotropy, it may be difficult to form a ferrimagnetic Hasler material with good crystal characteristics without a buffer layer. However, according to example embodiments, since the fixed layer structure 150 and the free layer 170 are formed on the buffer layer 140, and both the fixed layer structure 150 and the free layer 170 include ferrimagnetic Hasler materials, the buffer layer 140 and the fixed layer structure 150 can be used as a growth template in the epitaxial growth process of the free layer 170, so the free layer 170 can have good crystal quality.

[0057] In addition, since the SOT structure 180 is a stacked structure of the second electrode layer 184 including a topological insulator material and the first electrode layer 182 for improving the interface characteristics between the second electrode layer 184 and the free layer 170, a relatively high spin-orbit coupling characteristic can be obtained through the SOT structure 180. Therefore, the magnetic memory device 100 according to the example embodiment is capable of fast switching and low current operation.

[0058] In the following, refer to FIG. 4A to FIG. 4C A driving method of the magnetic memory device 100 according to example embodiments is schematically described.

[0059] Figure 4A Schematic illustration of the spin current generated by the current in the junction structure of non-magnetic material and magnetic material.

[0060] Reference Figure 4A After forming a layered structure including a non-magnetic material layer NM and a magnetic metal layer FM, a current may flow in a longitudinal direction of the non-magnetic material layer NM of the layered structure (eg, a longitudinal direction of the layered structure or Figure 4A For example, the non-magnetic material layer NM may include a topological insulator material, and the magnetic metal layer FM may include a ferrimagnetic Heusler material. Here, the current caused by the charge transfer may be represented as J C Due to the strong spin-orbit coupling property of the non-magnetic material layer NM, electrons with one spin can be in the lateral direction of the non-magnetic material layer NM (for example, the direction perpendicular to the longitudinal direction of the layered structure, or Figure 4A The electrons with opposite spin can be turned in the +Z direction (for example, Figure 4A For example, when the current flows in the X direction, the upward spins may be accumulated in the +Z direction, and the downward spins may be accumulated in the -Z direction. In short, a spin current is generated in the -Z direction (or the +Z direction). This spin current can be expressed as Figure 4A J in S In other words, when current flows through the non-magnetic material layer NM, the C The spin current J is induced in the direction of S , and the spin torque can be transferred to the ferrimagnetic metal layer FM in contact with the nonmagnetic material layer NM.

[0061] Figure 4B and Figure 4C A write operation and a read operation of the magnetic memory device 100 according to example embodiments are schematically illustrated, respectively.

[0062] Reference Figure 4B , a voltage may be applied to the first conductive line 120 to turn on the switch element 130, and the write current I write is applied to the SOT structure 180. At this time, a spin current I can be generated by the spin Hall effect of the SOT structure 180 (specifically, the second electrode layer 184). spin , and the generated spin current I spin Applied to the free layer 170. The write current I write The spin current I is generated in the direction of spin Therefore, the spin current I spin Data is written to the memory cell MC.

[0063] Reference Figure 4C , a potential difference may be generated between the first conductive line 120 and the second conductive line 190 (that is, between the word line WL and the bit line BL). Due to this potential difference, the read current I read The read current I may flow through the second conductive line 190, the MTJ structure MTJS and the first conductive line 120. read The measured value of may vary according to the resistance state of the MTJ structure MTJS (ie, the magnetization direction of the free layer 170 and the magnetization direction of the fixed layer structure 150). read By comparing the measured value with the comparison value, it is possible to determine whether the MTJ structure MTJS is in a low resistance state (that is, the data is 0 or 1) or a high resistance state (that is, the data is 1 or 0). Therefore, the data stored in the MTJ structure MTJS can be determined.

[0064] Figure 5 is a cross-sectional view illustrating a magnetic memory device 100A according to example embodiments. Figure 5 is with Figure 2A The area CX in FIG. 1 corresponds to an enlarged cross-sectional view of the area. Figure 5 In, with Figures 1 to 4C The same reference numerals as in the drawings may indicate the same components.

[0065] Reference Figure 5 , the memory cell MCA may include a buffer layer 140, a fixed layer structure 150A, a tunnel barrier 160, and a free layer 170A.

[0066] The free layer 170A may include a bottom free layer 172 on the tunnel barrier 160 and a top free layer 174 located on the bottom free layer 172 and in contact with the bottom surface of the SOT structure 180. The top free layer 174 may have the same Figures 1 to 3 The free layer 170 described above has similar technical features. The top free layer 174 may include a binary ferrimagnetic Heusler material. The top free layer 174 may have a chemical formula of Mn a X b , and may include, for example, at least one of MnGa and MnGe.

[0067] The bottom free layer 172 may include a ternary ferrimagnetic Heusler material. The bottom free layer 172 may have a chemical formula of Mn a X b Y c , and may include, for example, at least one of MnGaNi, MnGeNi, MnGaCo, MnGeCo, MnGaFe, and MnGeFe. The bottom free layer 172 may have a lattice constant having a value between the lattice constant of the tunnel barrier 160 and the lattice constant of the top free layer 174. The bottom free layer 172 may be used as an intermediate layer to offset the lattice mismatch between the tunnel barrier 160 and the top free layer 174, and thus, the free layer 170A may have relatively good crystal quality.

[0068] The fixed layer structure 150A may include a plurality of fixed layer stacks 150UA. Each of the plurality of fixed layer stacks 150UA may include a bottom fixed layer 152A and a top fixed layer 154A. The bottom fixed layer 152A and the top fixed layer 154A may have the same Figures 1 to 3 The bottom pinned layer 152 and the top pinned layer 154 may have similar technical features. For example, the bottom pinned layer 152A may include a binary ferrimagnetic Heusler material having a chemical formula of Mn a X b , and may include, for example, at least one of MnGa and MnGe. The top pinned layer 154A may include a ternary ferrimagnetic Heusler material, which may have a chemical formula of Mn a X b Y c, and may include, for example, at least one of MnGaNi, MnGeNi, MnGaCo, MnGeCo, MnGaFe or MnGeFe. Figure 5 , two fixed layer stacks 150UA are shown stacked in the third direction (Z direction), but the number of fixed layer stacks 150UA is not limited thereto. Since the fixed layer structure 150A is formed as a stacked structure including the plurality of fixed layer stacks 150UA, the fixed layer structure 150A may have a relatively high exchange coupling force, and therefore, the fixed layer structure 150A may exhibit high perpendicular magnetic anisotropy.

[0069] In addition, the top fixed layer 154A may have a lattice constant having a value between the lattice constant of the tunnel barrier 160 and the lattice constant of the bottom fixed layer 152A. The top fixed layer 154A may be used as an intermediate layer to offset the lattice mismatch between the tunnel barrier 160 and the bottom fixed layer 152A, and thus, the top fixed layer 154A may have relatively good crystal quality.

[0070] Although the case where the bottom fixed layer 152A includes a binary ferrimagnetic Heusler material and the top fixed layer 154A includes a ternary ferrimagnetic Heusler material in one fixed layer stack 150UA is described above, the materials of the bottom fixed layer 152A and the top fixed layer 154A may be interchanged with each other in one fixed layer stack 150UA. For example, the bottom fixed layer 152A including the ternary ferrimagnetic Heusler material and arranged at the lowermost portion of the fixed layer stack 150UA may be directly arranged on the buffer layer 140, and the top fixed layer 154A including the binary ferrimagnetic Heusler material and arranged at the uppermost portion of the fixed layer stack 150UA may be directly arranged under the tunnel barrier 160. When one element is referred to as being arranged "directly" "on" another element, "directly" "under" another element, or "directly adjacent" another element, there is no intermediate element.

[0071] According to example embodiments, the free layer 170A may have good crystal quality, and in addition, the fixed layer structure 150A may have high perpendicular magnetic anisotropy. Therefore, the magnetic memory device 100 is capable of fast switching and low current operation.

[0072] Figure 6 is a cross-sectional view illustrating a magnetic memory device 100B according to example embodiments. Figure 6 is with Figure 2A The area CX in FIG. 1 corresponds to an enlarged cross-sectional view of the area. Figure 6 In, with Figures 1 to 5 The same reference numerals as in the drawings may indicate the same components.

[0073] Reference Figure 6, the memory cell MCB may include a buffer layer 140 , a fixed layer structure 150B, a tunnel barrier 160 , and a free layer 170B.

[0074] The free layer 170B may include a bottom free layer 172B located on the tunnel barrier 160 and a top free layer 174 located on the bottom free layer 172B and contacting the bottom surface of the SOT structure 180. The top free layer 174 may have a Figures 1 to 3 The free layer 170 described above has similar technical features. The top free layer 174 may include a binary ferrimagnetic Heusler material, which may have a chemical formula of Mn a X b , and may include, for example, at least one of MnGa and MnGe.

[0075] The bottom free layer 172B may include a ferrimagnetic Heusler material. The bottom free layer 172B may have a chemical formula X 2 YZ, and may include, for example, Co 2 MnSi、Co 2 MnAl、Co 2 MnGa、Co 2 MnGe、Co 2 NiGa、Co 2 FeSi、Co 2 FeAl, Fe 2 MnSi、Fe 2 VSi、Ni 2 MnAl、Ni 2 MnIn and Ni 2 The bottom free layer 172B may have a lattice constant having a value between the lattice constant of the tunnel barrier 160 and the lattice constant of the top free layer 174. The bottom free layer 172B may be used as an intermediate layer to offset the lattice mismatch between the tunnel barrier 160 and the top free layer 174, so that the free layer 172B may have relatively good crystal quality.

[0076] The fixed layer structure 150B may include a plurality of fixed layer stacks 150UB. Each of the plurality of fixed layer stacks 150UB may include a bottom fixed layer 152A and a top fixed layer 154B. The bottom fixed layer 152A may have a similar structure to the reference layer 154B. Figures 1 to 3 The bottom fixed layer 152A may have similar technical features as described above. For example, the bottom fixed layer 152A may include a binary ferrimagnetic Heusler material having a chemical formula of Mn a X b , and may include, for example, at least one of MnGa or MnGe.

[0077] The top pinned layer 154B may include a ferrimagnetic Heusler material. The top pinned layer 154B may have a chemical formula X2 YZ, and may include, for example, Co 2 MnSi、Co 2 MnAl、Co 2 MnGa、Co 2 MnGe、Co 2 NiGa、Co 2 FeSi、Co 2 FeAl, Fe 2 MnSi、Fe 2 VSi、Ni 2 MnAl、Ni 2 MnIn and Ni 2 At least one of MnGa.

[0078] The top fixed layer 154B may have a lattice constant having a value between the lattice constant of the tunnel barrier 160 and the lattice constant of the bottom fixed layer 152A. The top fixed layer 154B may be used as an intermediate layer to offset the lattice mismatch between the tunnel barrier 160 and the bottom fixed layer 152A, and thus, the top fixed layer 154B may have relatively good crystal quality. Since the fixed layer structure 150B has a stacked structure including a plurality of fixed layer stacks 150UB, the fixed layer structure 150B may have a relatively high exchange coupling force, and thus, the fixed layer structure 150B may exhibit high perpendicular magnetic anisotropy.

[0079] According to example embodiments, the free layer 170B may have good crystal quality, and in addition, the fixed layer structure 150B may have high perpendicular magnetic anisotropy. Therefore, the magnetic memory device 100B is capable of fast switching and low current operation.

[0080] Figure 7 is a cross-sectional view illustrating a magnetic memory device 100C according to example embodiments. Figure 7 is with Figure 1 A cross-sectional view of the area corresponding to the line IIA-IIA' in FIG. Figure 7 In, with Figures 1 to 6 The same reference numerals in the drawings may denote the same components.

[0081] Reference Figure 7 , the SOT structure 180C may extend in a second direction (Y direction) parallel to the top surface of the substrate 110, and the second conductive line 190 may extend in the second direction (Y direction) at a higher level than the SOT structure 180C. A plurality of contacts 188 for electrically connecting the second conductive line 190 to the SOT structure 180C may be arranged to pass through the second interlayer insulating layer 186.

[0082] According to example embodiments, the SOT structure 180C including the topological insulator material may have a relatively low resistivity and be spaced apart from the second conductive line 190, and the amount of current flowing in the SOT structure 180C may be increased compared to, for example, a case where the second conductive line 190 and the SOT structure 180C are formed in a stacked manner or are formed in contact with each other. Therefore, the magnetic memory device 100C is capable of fast switching and low current operation.

[0083] Figures 8 to 13 are cross-sectional views illustrating a method of manufacturing the magnetic memory device 100 according to example embodiments. Figures 8 to 13 In the figure, the process sequence is shown in Figure 1 The cross section of the area corresponding to the line IIA-IIA' in Figures 8 to 13 In, with Figures 1 to 7 The same reference numerals as in the drawings may indicate the same components.

[0084] Reference Figure 8 , the first conductive line 120 and the switching element 130 may be formed on the substrate 110 .

[0085] The substrate 110 may include a semiconductor substrate such as a silicon (Si) substrate, a germanium (Ge) substrate, a silicon carbide (SiC) substrate, a gallium arsenide (GaAs) substrate, and / or an indium arsenide (InAs) substrate. An intermediate layer such as an interlayer insulating film may also be disposed on the substrate 110.

[0086] A conductive layer may be formed on the substrate 110 by using doped polysilicon, metal, or metal nitride, and the first conductive line 120 may be formed by patterning the conductive layer. The switching element 130 may be formed on the first conductive line 120.

[0087] In example embodiments, the switch element 130 may include a PMOS transistor or an NMOS transistor. The substrate 110 may include a conductive region, or, for example, a doped well or a doped structure, an insulating layer of a shallow trench isolation (STI) structure may be formed, and a bottom insulating layer may be formed on the substrate 110. The conductive region may constitute or define a portion of the switch element 130.

[0088] In other embodiments, the switch element 130 may include a diode. In this case, the switch element 130 may be formed by sequentially epitaxially growing a p-type semiconductor layer and an n-type semiconductor layer on the first conductive line 120, or by sequentially epitaxially growing an n-type semiconductor layer and a p-type semiconductor layer on the first conductive line 120.

[0089] A first interlayer insulating layer 136 may be formed covering the first conductive line 120 and the switching element 130. After removing a portion of the first interlayer insulating layer 136 to form a bottom electrode opening exposing the top surface of the switching element 130, a bottom electrode 132 may be formed by filling a metal material or metal nitride in the bottom electrode opening.

[0090] By selectively performing a planarization process on the first interlayer insulating layer 136 and the bottom electrode 132 , an upper surface of the first interlayer insulating layer 136 may be coplanar with an upper surface of the bottom electrode 132 .

[0091] like Fig. 9 As shown, an initial buffer layer 140P, an initial bottom pinned layer 152P, an initial top pinned layer 154P, an initial tunnel barrier 160P, and an initial free layer 170P may be sequentially formed on the first interlayer insulating layer 136 and the bottom electrode 132 .

[0092] The initial buffer layer 140P, the initial bottom fixed layer 152P, the initial top fixed layer 154P, the initial tunnel barrier 160P and the initial free layer 170P may be formed by a sputtering process, a chemical vapor deposition (CVD) process, a metal organic CVD process, an atomic layer deposition (ALD) process, a molecular beam epitaxy process, or the like.

[0093] The initial buffer layer 140P may be formed by using a non-magnetic metal material such as chromium (Cr), ruthenium (Ru) and / or tantalum (Ta), a non-magnetic compound such as cobalt gallium (CoGa) and / or manganese gallium nitride (MnGaN) and / or a non-magnetic alloy such as nickel aluminum alloy (NiAl). The initial buffer layer 140P may be used as a template for epitaxial growth on which the initial bottom fixed layer 152P is formed. The thickness and lattice constant of the initial buffer layer 140P in the third direction (Z direction) may be appropriately selected to reduce the mismatch in lattice constant between the initial bottom fixed layer 152P and the initial top fixed layer 154P.

[0094] The initial bottom fixed layer 152P may be formed by at least one of MnGa and MnGe. The initial top fixed layer 154P may be formed by using at least one of MnGaNi, MnGeNi, MnGaCo, MnGeCo, MnGaFe, or MnGeFe.

[0095] The initial tunnel barrier 160P and the initial free layer 170P may be sequentially formed on the initial top fixed layer 154P. In the process of forming the initial tunnel barrier 160P, the initial top fixed layer 154P exposed at the bottom of the initial tunnel barrier 160P may include a material having a relatively small lattice mismatch with the initial tunnel barrier 160P, and thus, the crystal quality of the initial tunnel barrier 160P and / or the interface quality between the initial top fixed layer 154P and the initial tunnel barrier 160P may be good.

[0096] The initial free layer 170P may be formed by using at least one of MnGa or MnGe, may have a tetragonal phase, and may be formed to have, for example, D0 22 Crystal structure. In the process of forming the initial free layer 170P on the initial tunnel barrier 160P, because of the relatively small thickness of the initial tunnel barrier 160P, the initial top fixed layer 154P below the initial tunnel barrier 160P can be used as a template for the epitaxial growth of the initial free layer 170P. Therefore, the crystal quality of the initial free layer 170P and / or the interface quality between the initial tunnel barrier 160P and the initial free layer 170P can be good.

[0097] Reference Fig.10 as well as Fig. 9 , a mask pattern may be formed on the initial buffer layer 140P, the initial bottom fixed layer 152P, the initial top fixed layer 154P, the initial tunnel barrier 160P, and the initial free layer 170P. By using the mask pattern as an etching mask to pattern the initial free layer 170P, the initial tunnel barrier 160P, the initial top fixed layer 154P, the initial bottom fixed layer 152P, and the initial buffer layer 140P in sequence, a memory cell MC including the buffer layer 140 and the MTJ structure MTJS may be formed. The MTJ structure MTJS may include a fixed layer structure 150, a tunnel barrier 160, and a free layer 170 formed on the buffer layer 140, and the fixed layer structure 150 may include a bottom fixed layer 152 and a top fixed layer 154.

[0098] Through the patterning, an opening 146H may be formed in a space between one memory cell MC and another memory cell MC adjacent thereto. The sidewalls of the buffer layer 140, the fixed layer structure 150, the tunnel barrier 160, and the free layer 170 may be aligned with each other along a straight line. The top surface of the first interlayer insulating layer 136 may be exposed at the bottom of the opening 146H.

[0099] In addition, an over-etching process may be performed in the patterning to appropriately electrically and physically separate one memory cell MC from another memory cell MC adjacent thereto. As a result of the over-etching process, a groove may also be formed on the first interlayer insulating layer 136, and the top surface of the first interlayer insulating layer 136 may be locally located at a lower level than the top surface of the bottom electrode 132.

[0100] According to a general SOT-type MRAM device, a SOT line SL may be formed under the MTJ structure MTJS, and in this case, etching damage of the top surface of the SOT line SL may occur in the patterning for forming the MTJ structure MTJS. However, according to the present invention, the SOT structure 180 may not be damaged by etching in the patterning for forming the MTJ structure MTJS.

[0101] Reference Fig.11 , an insulating layer may be formed on the first interlayer insulating layer 136 and the memory cells MC to fill the openings 146H, and then an insulating pattern 146 may be formed by planarizing the insulating layer so that the top surface of the free layer 170 is exposed. The insulating pattern 146 may surround the sidewalls of the buffer layer 140 and the sidewalls of the MTJ structure MTJS.

[0102] exist Figures 9 to 11 , an example embodiment of forming a memory cell MC and an insulating pattern 146 by performing one patterning process and one insulating layer forming process is described. However, according to other embodiments, the memory cell MC and the insulating pattern 146 may be formed by performing two or more patterning processes and two or more insulating layer forming processes. For example, after first forming an initial buffer layer 140P, an initial bottom fixed layer 152P, and an initial top fixed layer 154P, a bottom stack may be formed by patterning the initial buffer layer 140P, the initial bottom fixed layer 152P, and the initial top fixed layer 154P, and a bottom insulating pattern surrounding the bottom stack may be formed. An initial tunnel barrier 160P and an initial free layer 170P may be formed on the bottom stack and the bottom insulating pattern, a top stack may be formed by patterning the initial tunnel barrier 160P and the initial free layer 170, and a top insulating pattern surrounding the top stack (or the patterned initial tunnel barrier 160P and the patterned initial free layer 170) may be formed.

[0103] Reference Fig.12 The initial first electrode layer 182P may be formed on the top surface of the MTJ structure MTJS and the insulating pattern 146. The first electrode layer 182P may be formed by using at least one of MnGe or MnGa to have a thickness t11 of about 1 to about 10 nm (refer to Figure 3The initial first electrode layer 182p may be formed by an epitaxial growth process using the top surface of the free layer 170 below the initial first electrode layer 182p as a template.

[0104] Reference Fig.13 The initial second electrode layer may be formed on the initial first electrode layer 182P (refer to Fig.12 ). A mask pattern may be formed on the initial second electrode layer, and by using the mask pattern as an etching mask to pattern the initial second electrode layer and the initial first electrode layer 182P in sequence, a SOT structure 180 including a second electrode layer 184 and a first electrode layer 182 may be formed. The mask pattern may have a linear shape or a straight line shape extending in the second direction (Y direction).

[0105] This can be achieved by using topological insulator materials (e.g., bismuth antimony (Bi 1-x Sb x , wherein x is from about 0.05 to about 0.25) or bismuth selenide (Bi 1-y Se y , wherein y is at least one of about 0.05 to about 0.25) to form an initial second electrode layer. The initial second electrode layer may have a hexagonal phase. The initial second electrode layer may be formed on the initial first electrode layer 182P having a tetragonal phase to have a relatively high crystal quality and a relatively high flatness. In addition, since the initial second electrode layer is not directly arranged on the top surface of the insulating pattern 146, but is formed on the initial first electrode layer 182P, the interface quality between the free layer 170 and the SOT structure 180 (for example, the interface quality between the free layer 170 and the initial first electrode layer 182P, and / or the interface quality between the initial first electrode layer 182P and the initial second electrode) may be better.

[0106] Refer to Figure 2A By forming an insulating layer covering the SOT structure 180 on the insulating pattern 146 and planarizing the top surface of the insulating layer so that the top surface of the SOT structure 180 is exposed, a second interlayer insulating layer 186 may be formed. By removing a portion of the second interlayer insulating layer 186 to form the plurality of openings, and by using a metal or a metal nitride, the plurality of contacts 188 may be formed in the plurality of openings 146H. By using the plurality of contacts 188 and the metal or the metal nitride on the second interlayer insulating layer 186 to form a conductive layer, and by patterning the conductive layer, a second conductive line 190 may be formed.

[0107] The magnetic memory device 100 may be completed by performing the above-mentioned processes.

[0108] Typically, in a SOT-type MRAM device, a SOT line may be located on a switching element, and an MTJ structure may be located on the SOT line. However, in an etching process for patterning the MTJ structure MTJS, etching residues that typically include heavy metal materials may be redeposited on the patterned sidewalls to cause a short circuit between the free layer and the fixed layer, and the top surface of the SOT line exposed to the etching environment may be damaged by etching gas or etchant. However, according to example embodiments, since the SOT structure 180 is arranged on the MTJ structure MTJS, the SOT structure 180 may be prevented from being damaged during the patterning process of the MTJ structure MTJS.

[0109] In addition, in a general SOT-type MRAM device, since the SOT line and the free layer need to contact each other without an additional material layer between them, the free layer, the tunnel barrier and the fixed layer may be located on the SOT line. In this case, it is difficult to arrange a buffer layer for improving the crystallinity of the free layer, and therefore, the quality of the free layer is poor, or the selection of materials included in the free layer is limited. However, according to example embodiments, an initial bottom fixed layer 152P and an initial top fixed layer 154P including a ferrimagnetic Hasler material may be formed on the initial buffer layer 140P, and an initial free layer 170P may be formed on the initial tunnel barrier 160P. Therefore, since the initial buffer layer 140P, the initial bottom fixed layer 152P and the initial top fixed layer 154P are all used as growth templates in the epitaxial growth process of the initial free layer 170P, the free layer 170 may have good crystal quality.

[0110] In addition, since the SOT structure 180 is formed in a stacked structure including the second electrode layer 184 and the first electrode layer 182, wherein the second electrode layer 184 and the first electrode layer 182 include a topological insulator, the second electrode layer 184 can have good crystal quality and interface quality. Therefore, the magnetic memory device 100 formed by the above method can perform fast switching and low current operation.

[0111] In reference Fig. 9 In the described process, the initial bottom pinned layer 152A and the initial top pinned layer 154A may be formed multiple times on the initial buffer layer 140P in an alternating manner. In addition, the bottom free layer 172 may be formed by using a ternary ferrimagnetic Heusler material on the initial tunnel barrier 160P, and then the top free layer 174 may be formed. In this case, reference Figure 5 A magnetic memory device 100A is described.

[0112] In addition, in reference Fig. 9 In the process described, the initial bottom fixed layer 152B and the bottom free layer 172B can be formed by using a ferrimagnetic Heusler material. In this case, reference Figure 6A magnetic memory device 100B is described.

[0113] As described above, embodiments are disclosed in the drawings and the specification. Although embodiments have been described herein with reference to specific terms, it should be understood that they are only used for the purpose of describing the technical ideas of the inventive concept and are not used to limit the scope of the inventive concept as defined in the claims. Therefore, it should be understood by those skilled in the art that various modifications and equivalent embodiments are possible without departing from the scope of the inventive concept, and the scope of protection of the inventive concept is described by the claims.

Claims

1. A magnetic memory device, include: a buffer layer on the substrate; A magnetic tunnel junction structure on the buffer layer, wherein the magnetic tunnel junction structure comprises a fixed layer structure, a tunnel barrier and a free layer stacked in sequence on the buffer layer; as well as A spin-orbit torque structure on the magnetic tunnel junction structure, wherein the spin-orbit torque structure comprises a topological insulator material, wherein the free layer comprises a Hassler material, Wherein, the spin-orbit torque structure comprises: a first electrode layer, which is located on the magnetic tunnel junction structure and includes a ferrimagnetic Heusler material, the first electrode layer is in contact with the free layer, and the first electrode layer and the free layer have the same crystal structure; and The second electrode layer is located on the first electrode layer and comprises the topological insulator material.

2. The magnetic memory device according to claim 1, in, The Heusler material includes a ferrimagnetic Heusler material, and the ferrimagnetic Heusler material includes at least one of MnGa or MnGe.

3. The magnetic memory device according to claim 1, in, The Heusler material includes a Mn-based alloy, the Mn-based alloy includes a tetragonal phase, and the Mn-based alloy including the tetragonal phase has a D0 22 Crystal structure.

4. The magnetic memory device according to claim 1, in, The topological insulator material includes Bi 1-x Sb x and Bi 1- y Se y At least one of , wherein x is from 0.05 to 0.25, and y is from 0.05 to 0.

25.

5. The magnetic memory device according to claim 1, in, The entire top surface of the free layer contacts the bottom surface of the spin-orbit torque structure.

6. The magnetic memory device according to claim 1, in, The fixed layer structure comprises: a bottom pinned layer located on the buffer layer and comprising a binary ferrimagnetic Heusler material; and a top pinned layer located on the bottom pinned layer and comprising at least one of a ternary ferrimagnetic Heusler material and a ferrimagnetic Heusler material, The binary ferrimagnetic Heusler material includes at least one of MnGa and MnGe, the ternary ferrimagnetic Heusler material includes at least one of MnGaNi, MnGeNi, MnGaCo, MnGeCo, MnGaFe and MnGeFe, and the ferrimagnetic Heusler material includes Co 2 MnSi、Co 2 MnAl、Co 2 MnGa、Co 2 MnGe、Co 2 NiGa、Co 2 FeSi、Co 2 FeAl, Fe 2 MnSi、Fe 2 VSi、Ni 2 MnAl、Ni 2 MnIn and Ni 2 At least one of MnGa.

7. The magnetic memory device according to claim 1, in, The fixed layer structure includes a plurality of fixed layer stacks, and each of the plurality of fixed layer stacks includes: a bottom pinned layer comprising a binary ferrimagnetic Heusler material; and A top pinned layer is located on the bottom pinned layer and includes at least one of a ternary ferrimagnetic Heusler material and a ferrimagnetic Heusler material, wherein the at least one of the ternary ferrimagnetic Heusler material and the ferrimagnetic Heusler material has a lattice constant between the lattice constant of the tunnel barrier and the lattice constant of the bottom pinned layer.

8. The magnetic memory device according to claim 1, in, The free layer includes: a bottom free layer located on the tunnel barrier; and a top free layer located on the bottom free layer and contacting a bottom surface of the spin-orbit torque structure, Wherein, the bottom free layer includes at least one of a ternary ferrimagnetic Halles material and a ferrimagnetic Halles material, at least one of the ternary ferrimagnetic Heusler material and the ferrimagnetic Heusler material has a lattice constant between the lattice constant of the tunnel barrier and the lattice constant of the top free layer, and the top free layer includes a binary ferrimagnetic Heusler material.

9. The magnetic memory device according to claim 1, further comprising: include: a plurality of first conductive lines located between the substrate and the buffer layer and extending in a first direction parallel to a top surface of the substrate; a plurality of second conductive lines located on the plurality of first conductive lines and extending in a second direction parallel to the top surface of the substrate and perpendicular to the first direction; as well as A plurality of memory cells are respectively arranged between intersections of the plurality of first conductive lines and the plurality of second conductive lines, wherein each of the plurality of memory cells includes the buffer layer and the magnetic tunnel junction structure.

10. The magnetic memory device according to claim 1, further comprising: include: An insulating pattern is located on the substrate and extends on a sidewall of the buffer layer and a sidewall of the magnetic tunnel junction structure, wherein a bottom surface of the spin-orbit torque structure contacts a top surface of the insulating pattern.

11. The magnetic memory device according to claim 1, in, Relative to a top surface of the substrate, a bottom surface of the spin-orbit torque structure is located at a higher level than a top surface of the tunnel barrier, and a top surface of the free layer is located at a higher level than a top surface of the pinned layer structure.

12. A magnetic memory device, include: a buffer layer on the substrate; A magnetic tunnel junction structure on the buffer layer, wherein the magnetic tunnel junction structure comprises a fixed layer structure, a tunnel barrier and a free layer stacked in sequence on the buffer layer; as well as A spin-orbit torque structure on the magnetic tunnel junction structure, wherein the spin-orbit torque structure comprises: A first electrode layer, which is located on the magnetic tunnel junction structure and includes a ferrimagnetic Heusler material, the first electrode layer is in contact with the free layer, and the first electrode layer and the free layer have the same crystal structure; as well as The second electrode layer is located on the first electrode layer and comprises a topological insulator material.

13. The magnetic memory device according to claim 12, in, Relative to a top surface of the substrate, a bottom surface of the spin-orbit torque structure is located at a higher level than a top surface of the tunnel barrier, and a top surface of the free layer is located at a higher level than a top surface of the pinned layer structure.

14. The magnetic memory device according to claim 12, in, The first electrode layer has a first thickness in a direction perpendicular to a top surface of the substrate, and the second electrode layer has a second thickness in the direction perpendicular to the top surface of the substrate that is greater than the first thickness.

15. The magnetic memory device according to claim 12, further comprising: include: An insulating pattern is arranged on the substrate and extends on sidewalls of the buffer layer and the magnetic tunnel junction structure, wherein a bottom surface of the first electrode layer contacts top surfaces of the insulating pattern and the free layer.

16. The magnetic memory device according to claim 15, in, The entire bottom surface of the second electrode layer contacts the first electrode layer, and the second electrode layer does not contact the insulating pattern.

17. A magnetic memory device, include: a buffer layer on the substrate; a fixed layer structure located on the buffer layer and comprising a first ferrimagnetic Heusler material; a tunnel barrier located on the fixed layer structure; a free layer located on the tunnel barrier and comprising a second ferrimagnetic Heusler material; as well as a spin-orbit torque structure located on the free layer opposite to the substrate and comprising a topological insulator material, Wherein, the spin-orbit torque structure comprises: a first electrode layer, which is located on the free layer and includes a ferrimagnetic Heusler material, the first electrode layer is in contact with the free layer, and the first electrode layer and the free layer have the same crystal structure, and The second electrode layer is located on the first electrode layer and comprises the topological insulator material.

18. The magnetic memory device according to claim 17, further comprising: include: An insulating pattern is located on the substrate and extends on sidewalls of the buffer layer, sidewalls of the fixed layer structure, sidewalls of the tunnel barrier and sidewalls of the free layer, wherein a bottom surface of the spin-orbit torque structure contacts a top surface of the insulating pattern and a top surface of the free layer.

19. The magnetic memory device according to claim 17, further comprising: include: a plurality of first conductive lines located between the substrate and the buffer layer and extending in a first direction parallel to a top surface of the substrate; a plurality of second conductive lines located on the plurality of first conductive lines and extending in a second direction parallel to the top surface of the substrate and perpendicular to the first direction; as well as A plurality of memory cells are respectively arranged between intersections of the plurality of first conductive lines and the plurality of second conductive lines, wherein each of the plurality of memory cells includes the buffer layer, the fixed layer structure, the tunnel barrier and the free layer.

20. The magnetic memory device according to claim 19, in, The spin-orbit torque structure extends in the first direction and is connected to the plurality of second conductive lines via contacts.

21. The magnetic memory device according to claim 17, further comprising: include: A switch element is located between the substrate and the buffer layer, wherein the switch element includes at least one of a diode, a transistor and a bidirectional threshold switch device.

Citation Information

Patent Citations

  • Magnetoresistive element and magnetic memory

    JP2018049880A

  • Magnetoresistive effect element, magnetic memory, magnetization reversal method, and spin current magnetization reversal element

    WO2017090733A1

  • Exchange bias utilization-type magnetization reversal element, exchange bias utilization-type magnetoresistance effect element, exchange bias utilization-type magnetic memory, nonvolatile logic circuit and magnetic neuron element

    WO2017213261A1