Thermoelectric conversion device
Through the multi-layer structure and chemical bonding of the thermoelectric conversion device, hollow fillers and thermally expandable liquid hydrocarbons are used to solve the problems of reduced thermal insulation efficiency and uneven heat conduction when the thermoelectric conversion device in the existing technology is pressed and bent, achieving high efficiency, Uniform thermoelectric conversion and durability.
Patent Information
- Application Number
- CN201780096772.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2017-11-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2037-11-13
AI Technical Summary
Existing thermoelectric conversion devices are prone to uneven deformation when pressed or bent, resulting in reduced thermal insulation efficiency of thermoelectric conversion elements and damage to semiconductor elements, and uneven heat conduction, affecting the user experience.
A thermoelectric conversion device with a multi-layer structure, including an insulating rubber layer, an insulating base layer, an insulating middle layer, a thermal diffusion layer and a heat dissipation layer, which are joined through chemical bonds and use hollow fillers and thermally expandable liquid hydrocarbons to achieve high thermal insulation and uniformity Thermal conduction ensures the stability and durability of the thermoelectric conversion chip.
It achieves efficient thermoelectric conversion, avoids concave and convex deformation, improves thermoelectric conversion efficiency and temperature distribution uniformity, enhances the durability and durability of the device, and is suitable for installation on curved surface equipment.
Smart Images

Figure CN111344874B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a thermoelectric conversion device having a thermoelectric conversion chip and a thermoelectric module layer of a heat insulating rubber surrounding the thermoelectric conversion chip, and exhibiting a Peltier effect or a Seebeck effect. Background Art
[0002] It is known that a thermoelectric conversion element pair consisting of an n-type semiconductor element and a p-type semiconductor element exhibits the Peltier effect in which heat is generated at one end and heat is absorbed at the other end by applying a voltage between the two semiconductor elements, or the Seebeck effect in which a voltage is generated due to the temperature difference between one end and the other end of the thermoelectric conversion element pair. In particular, a thermoelectric conversion chip consisting of a plurality of thermoelectric conversion element pairs sandwiched between substrates is used as a heating source or cooling source for equipment or appliances such as a refrigerator or a CPU (central processing unit) cooler by utilizing the Peltier effect.
[0003] As an example of such a thermoelectric conversion chip, a thermoelectric conversion module is disclosed in Patent Document 1, in which a plurality of thermoelectric conversion element pairs are electrically connected and arranged in series on a flexible insulating film such as a polymer film or a rubber sheet as a substrate, and an output terminal is formed at a heat-generating end at one end and a heat-absorbing end at the other end. The thermoelectric conversion modules can be bent and twisted, so they can be installed not only on a flat surface of a device or an appliance, but also along a curved surface.
[0004] As an example of using the thermoelectric conversion chip of the thermoelectric conversion module of Patent Document 1 on a curved surface of a device, Patent Document 2 discloses an example of installing the thermoelectric conversion chip by dividing it into multiple pieces along the ring of a car steering wheel. The steering wheel is heated or cooled by the thermoelectric conversion chip through the ring, and the user can hold the ring to operate it without feeling cold or hot in cold or hot weather. Thus, the flexible thermoelectric conversion chip can be used in devices that the user directly contacts.
[0005] The thermoelectric conversion chip can be assembled in a thermoelectric conversion device and installed in a device or an appliance. Figure 7 As shown, the thermoelectric conversion chip 61 is disposed so as to be sandwiched between a rubber substrate side sheet 64 and a surface side sheet 65. By fixing the substrate side sheet 64 to the device substrate 67, the conventional thermoelectric conversion device 60 is mounted in a device or the like.
[0006] The gap between the surface side sheet 65 and the device substrate 67 is a cavity 66. In the thermoelectric conversion element pair 61a, if the heat generated at the heat-generating end 62 is transferred to the heat-absorbing end 63, it will not only cause a significant decrease in the heat generation and heat absorption efficiency, but also hinder the movement of carriers between semiconductor elements and eventually cause damage. Therefore, the conventional thermoelectric conversion device 60 uses the air in the cavity 66 to insulate the heat-generating end 62 and the heat-absorbing end 63 of the thermoelectric conversion element pair 61a. Figure 7 As shown by the white arrows, when the surface side sheet 65 on the cavity 66 is pressed, the surface side sheet 65 is supported by the thermoelectric conversion chip 61 and bends toward the cavity 66 , so the upper surface of the conventional thermoelectric conversion device 60 is deformed into a concavo-convex shape.
[0007] In the case where the conventional thermoelectric conversion device 60 is mounted on an appliance that is directly contacted by the user, such as the ring portion of a steering wheel, the uneven deformation will cause discomfort to the user due to poor touch. In addition, due to the unevenness, whenever the surface side sheet 65 is pressed, stress is concentrated on the edge of the thermoelectric conversion chip 61, and the surface side sheet 65 is damaged or the edge of the thermoelectric conversion chip 61 is crushed, thereby damaging the thermoelectric conversion function. In addition, since the surface side sheet 65 made of rubber has poor thermal conductivity, the heat generated by the thermoelectric conversion chip 61 is only retained in the surface side sheet 65 and directly above the thermoelectric conversion chip 61. Therefore, the heat cannot be evenly diffused to the entire surface of the surface side sheet 65, resulting in uneven temperature distribution.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2000-286463
[0011] Patent Document 2: Japanese Patent Application Publication No. 2004-291889 Summary of the invention
[0012] Technical problem to be solved by the invention
[0013] The present invention is completed to solve the above-mentioned technical problems, and its purpose is to provide a thermoelectric conversion device, which diffuses heat evenly on the surface, can insulate the heat-generating end and the heat-absorbing end of the thermoelectric conversion element pair without causing concave-convex deformation caused by pressing, and has high durability by being joined with a sheet that clamps the thermoelectric conversion chip with high strength.
[0014] Technical solutions adopted to solve technical problems
[0015] The thermoelectric conversion device completed to achieve the above-mentioned purpose comprises a thermoelectric module layer, an insulating base layer and an insulating intermediate layer, a heat diffusion layer, and a heat dissipation layer. In the thermoelectric module layer, a heat-insulating rubber containing a rubber component and a hollow filler having a plurality of mutually independent voids surrounds a thermoelectric conversion chip; the insulating base layer and the insulating intermediate layer sandwich the thermoelectric module layer and are heat-conductive insulating sheets; the heat diffusion layer overlaps with the insulating intermediate layer and has higher thermal conductivity than the insulating base layer and the insulating intermediate layer; the heat dissipation layer overlaps with the heat diffusion layer and has thermal conductivity; at least one pair of these adjacent layers are bonded to each other by chemical bonds.
[0016] In the thermoelectric converter, it is preferred that the hollow filler has a shell made of resin, and a thermally expandable liquid hydrocarbon is sealed in an internal space of the shell.
[0017] In the thermoelectric conversion device, the thermal insulation rubber and the thermoelectric conversion chip may have the same thickness.
[0018] In the thermoelectric converter, the heat diffusion layer is preferably formed of at least one selected from the group consisting of aluminum, copper, graphite, heat conductive rubber, heat conductive elastomer, and the heat conductive insulating sheet.
[0019] In the thermoelectric converter, the heat diffusion layer preferably has a thickness of 0.01 to 0.5 mm.
[0020] In the thermoelectric conversion device, the thermoelectric conversion chip may include: a thermoelectric conversion element pair consisting of an n-type semiconductor element and a p-type semiconductor element, electrodes sandwiching a plurality of the thermoelectric conversion element pairs, and an insulating sheet overlapped and bonded to the electrodes.
[0021] In the thermoelectric converter, it is preferred that the rubber component is silicone rubber, and a silane coupling film is attached to the outer surface of the hollow filler.
[0022] The thermoelectric converter may include a circuit layer between the thermoelectric module layer and the insulating intermediate layer, the circuit layer being electrically connected to the thermoelectric conversion chip.
[0023] Effects of the Invention
[0024] In the thermoelectric converter of the present invention, the thermoelectric converter chip is surrounded by the heat insulating rubber having high heat insulating properties by including hollow fillers, so that the heat generated in the thermoelectric converter chip is not lost, and the thermoelectric converter has high thermoelectric conversion efficiency. In addition, since the thermoelectric converter does not have a cavity for heat insulation, even if the thermoelectric converter is pressed, the surface of the heat dissipation layer as the outermost layer of the thermoelectric converter will not be deformed in a concave and convex shape due to the thickness of the thermoelectric converter chip.
[0025] Since the thermoelectric converter has a simple structure in which a plurality of layers are stacked and joined together, it can be manufactured quickly at low cost and with high yield.
[0026] In the thermoelectric converter, the heat generated by the thermoelectric converter chip is diffused in the surface direction by the heat diffusion layer having high thermal conductivity, so that the temperature distribution on the surface of the heat dissipation layer can be made uniform.
[0027] In a thermoelectric converter, when the joint surfaces of stacked layers are firmly bonded by chemical bonds, there is no separation between the layers due to bending or twisting, and the device can be mounted on a curved surface of equipment or devices with high durability.
[0028] In a thermoelectric converter, when the hollow filler has a resin shell and a heat-expandable liquid hydrocarbon sealed in the inner space thereof, the hollow filler expands uniformly by heating to form voids of uniform diameter in the thermal insulation rubber, so that the rubber component in the thermal insulation rubber is not unevenly distributed, and high thermal insulation due to the voids and high strength due to the dispersed existence of the rubber component can be achieved at the same time.
[0029] In a thermoelectric converter, when the rubber component is silicone rubber and a silane coupling agent is attached to the outer surface of the hollow filler, the two are firmly bonded to form a heat-insulating rubber with higher strength, thereby exhibiting higher durability.
[0030] In the thermoelectric converter, when a circuit layer is provided between the thermoelectric module layer and the insulating intermediate layer, the thermoelectric conversion chips in the thermoelectric module layer can be controlled to achieve desired timing and temperature by connecting the control device to the wiring of the circuit layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic partially cutaway perspective view showing a thermoelectric converter to which the present invention is applied.
[0032] Figure 2 This is a schematic cross-sectional view showing a thermoelectric converter to which the present invention is applied.
[0033] Figure 3 It is a plan view showing the positions of temperature measurement points in a temperature distribution test and a temperature change test using a thermoelectric converter to which the present invention is applied.
[0034] Figure 4 The graphs show the results of a heat absorption control temperature distribution test of a thermoelectric converter of an example to which the present invention is applied and a thermoelectric converter of a comparative example to which the present invention is not applied.
[0035] Figure 5 The graphs show the results of a heat generation control temperature distribution test of a thermoelectric converter of an example to which the present invention is applied and a thermoelectric converter of a comparative example to which the present invention is not applied.
[0036] Figure 6 The graphs show the results of a heat absorption control temperature change test and a heat generation control temperature change test of a thermoelectric converter of an example to which the present invention is applied and a thermoelectric converter of a comparative example to which the present invention is not applied.
[0037] Figure 7 This is a schematic cross-sectional view showing a conventional thermoelectric converter to which the present invention is not applied. DETAILED DESCRIPTION
[0038] Hereinafter, embodiments of the present invention will be described in detail, but the scope of the present invention is not limited to these embodiments.
[0039] Figure 1 1 is a schematic partially cutaway perspective view of an embodiment of a thermoelectric converter 1 of the present invention. In the thermoelectric converter 1, an insulating base layer 10, a thermoelectric module layer 20, an insulating intermediate layer 30, a heat diffusion layer 40, and a heat dissipation layer 50 are stacked in this order. A thermoelectric converter chip 21 is disposed in the center of the thermoelectric module layer 20.
[0040] These adjacent layers, namely the insulating base layer 10 and the thermoelectric module layer 20, the thermoelectric module layer 20 and the insulating intermediate layer 30, the insulating intermediate layer 30 and the heat diffusion layer 40, and the heat diffusion layer 40 and the heat dissipation layer 50, are bonded by chemical bonds. This bonding is different from bonding by intermolecular forces or physical anchoring effects of adhesives or binders, for example. The layers are bonded by covalent bonds as chemical bonds, so they are extremely strong, and the layers will not peel off by pressing, bending or twisting applied to the thermoelectric converter 1. Moreover, the heat generated by the thermoelectric converter chip 21 does not move between layers via adhesives or binders, so no heat loss occurs when moving between layers. Therefore, the thermoelectric converter 1 has a high thermoelectric conversion efficiency.
[0041] The thermoelectric module layer 20 includes a thermoelectric conversion chip 21 and a heat insulating rubber 22 surrounding the side surfaces of the thermoelectric conversion chip 21. The thermoelectric conversion chip 21 and the heat insulating rubber 22 have the same thickness.
[0042] Figure 2 Schematic cross-sectional view of the thermoelectric converter 1 is shown in FIG. The heat insulating rubber 22 includes a rubber component 22a and hollow fillers 22b uniformly dispersed in the rubber component 22a.
[0043] The rubber component 22a is preferably a silicone rubber. The silicone rubber has high flexibility and flexural fatigue resistance in a wide temperature range from -40°C to 200°C. Therefore, the thermoelectric conversion device 1 can be bent and installed along the curved surface of equipment or the like, and expansion caused by thermal shock can be prevented. The number average molecular weight of the silicone rubber is preferably from 10,000 to 1,000,000. The hollow filler 22b is spherical and has a shell made of a soft and gas-barrier thermoplastic resin such as a vinylidene chloride resin or an acrylic resin. A small amount of thermally expandable liquid hydrocarbon is enclosed in the internal space of the shell.
[0044] Most of the volume of the internal space of the shell constituting the hollow filler 22b is occupied by air. Thereby, voids formed by air are formed in the heat insulating rubber 22, and thus the heat insulating rubber 22 has high heat insulation equivalent to that of air. Thereby, the heat generated at the heat generating end 23 of the thermoelectric conversion chip 21 does not diffuse to the heat insulating rubber 22, but is transferred in the insulating intermediate layer 30 and the heat diffusion layer 40 and efficiently conducted to the heat dissipation layer 50 as the outermost layer. Therefore, the thermoelectric conversion device 1 can perform thermoelectric conversion with high efficiency.
[0045] As such a hollow filler 22b, thermally expandable microcapsules are preferred, and specific examples include Matsumoto Microsphere (registered trademark) F, FN, F-E, F-DE, and MFL (manufactured by Matsumoto Yushi Yakuhin Co., Ltd., trade name); KUREHA Microsphere (manufactured by Kureha Corporation, trade name); Expancel (manufactured by Nippon Metal Co., Ltd. (Nippon Ferlite Co., Ltd.), registered trademark); ADVANCELL (registered trademark) EM, HB, and NS (manufactured by Sekisui Chemical Co., Ltd., trade name).
[0046] In addition, by making the thermoelectric conversion chip 21 and the heat insulating rubber 22 have the same thickness, the thermoelectric module layer 20 is formed into a rectangular parallelepiped without unevenness on all surfaces. In addition, the thermoelectric module layer 20 does not have voids around the thermoelectric conversion chip 21. Thereby, even when the heat dissipation layer 50 is pressed, the upper surface of the thermoelectric conversion device 1 does not deform into an uneven shape like a conventional thermoelectric conversion device. Therefore, the pressing force is not concentrated on the edge of the thermoelectric conversion chip 21 but is dispersed, so that peeling of the heat dissipation layer 50 disposed on the surface layer or breakage of the edge of the thermoelectric conversion chip does not occur. In addition, even when it is installed on the ring portion of an automobile steering wheel, the touch of the user is not impaired.
[0047] Furthermore, since the hollow filler 22b has a shell, the hollow fillers 22b are not combined with each other but are independent of each other. That is, the voids in the heat-insulating rubber 22 are not connected and are evenly dispersed in the rubber component 22a, so the distance between the voids is roughly equal in the heat-insulating rubber 22. Therefore, the rubber component 22a is also evenly present in the heat-insulating rubber 22, so when the thermoelectric converter 1 is bent or pressed, stress is dispersed in the rubber component 22a to absorb the impact. Moreover, the voids in the heat-insulating rubber 22 are formed by the hollow filler 22b having a soft shell, so unlike a porous rubber having only a plurality of voids, it has not only the elasticity derived from the rubber component 22a, but also the softness derived from the shell of the hollow filler 22b. As a result, combined with the bonding of the rubber component 22a and the hollow filler 22b, the heat-insulating rubber 22 will not crack or break due to external forces such as pressing, bending or twisting even under repeated heating and cooling conditions. In addition, since the gaps in the heat insulating rubber 22 are formed by the hollow filler 22b, water can be prevented from penetrating from the outside due to the presence of the gaps. Therefore, the heat insulating rubber 22 has high strength and waterproofness, and by surrounding the thermoelectric conversion chip 21 to support it, it can not only prevent damage and water penetration, but also give the thermoelectric conversion device 1 strength and bending fatigue resistance.
[0048] A silane coupling film containing a silane coupling agent can be attached to the outer surface of the hollow filler 22b. Thus, the rubber component 22a made of silicone rubber and the hollow filler 22b can be firmly bonded through molecular bonding via the silane coupling agent. In addition, the hollow filler 22b can include a variety of hollow fillers with different average particle sizes, materials or expansion coefficients.
[0049] Molecular bonding that firmly bonds the rubber component 22a and the hollow filler 22b refers to a chemical reaction based on covalent bonds between the functional groups in the molecules of the molecular adhesive such as the silane coupling agent and the silicone rubber of the rubber component 22a as the adherend, so that the rubber component 22a and the hollow filler 22b are bonded by covalent bonds based on single or multiple molecular adhesive molecules. The molecular adhesive is an adhesive having two functional groups that chemically reacts with the rubber component 22a and the hollow filler 22b to form a covalent bond, and is a general term for such bifunctional molecules.
[0050] As molecular binders, specifically, there can be mentioned:
[0051] Amino-containing compounds such as triethoxysilylpropylamino-1,3,5-triazine-2,4-dithiol (TES) and aminoethylaminopropyltrimethoxysilane;
[0052] A triazine compound having a trialkoxysilylalkylamino group such as a triethoxysilylpropylamino group and a mercapto group or an azide group, a triazine compound represented by the following chemical formula (1),
[0053] [Chemistry 1]
[0054]
[0055] (In the chemical formula (1), W is a spacer group, for example, an alkylene group or an aminoalkylene group which may have a substituent, or a direct bond. Y is an OH group or a reactive functional group which generates an OH group by hydrolysis or detachment, for example, a trialkoxyalkyl group. -Z is -N3 or -NR 1 R 2 (Among them, R 1 , R 2 the same or different, H or alkyl), -R 3 Si(R 4 ) m (OR 5 ) 3-m [R 3 ,R 4 is an alkyl group, R 5 is H or alkyl, and m is 0 to 2]. In addition, alkylene, alkoxy, and alkyl are linear, branched, and / or cyclic hydrocarbon groups having 1 to 12 carbon atoms and which may have a substituent;
[0056] a thiol compound having a trialkoxysilylalkyl group;
[0057] Epoxy compounds having a trialkoxysilylalkyl group;
[0058] From CH2=CH-Si(OCH3)2-O-[Si(OCH3)2-O-] n -Si(OCH3)2-CH=CH2 (n=1.8 to 5.7) Silane coupling agents such as vinyl alkoxysiloxane polymers exemplified above.
[0059] The silane coupling agent may, for example, be a silane coupling agent such as a vinyl alkoxysiloxane polymer; or an amino group-containing silane coupling agent having an alkoxy group. Specific examples of such silane coupling agents include vinyl triethoxysilane (KBE-1003), N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane (KBM-602), N-2-(aminoethyl)-3-aminopropyl trimethoxysilane (KBM-603), N-2-(aminoethyl)-3-aminopropyl triethoxysilane (KBE-603), 3-aminopropyl trimethoxysilane (KBM-903), 3-aminopropyl triethoxysilane (KBE-903), 3-triethoxysilyl-N-(1,3-dimethyl-butylene) propylamine (KBE-9103), N-phenyl-3-aminopropyl trimethoxysilane (KBM-573), N-(vinylbenzyl)-2 -Aminoethyl-3-aminopropyltrimethoxysilane hydrochloride (KBM-575) as an example of an amino group-containing alkoxysilyl compound (the above are manufactured by Shin-Etsu Silicone Co., Ltd.; product name), in addition, amino group-containing alkoxysilyl compounds exemplified by 3-aminopropyltrimethoxysilane (Z-6610), 3-aminopropyltrimethoxysilane (Z-6611), 3-(2-aminoethyl)aminopropyltrimethoxysilane (Z-6094), 3-phenylaminopropyltrimethoxysilane (Z-6883), and N-[3-(trimethoxysilyl)propyl]-N'-[(vinylphenyl)methyl-1,2-ethylenediamine hydrochloride (Z-6032) (the above are manufactured by Dow Corning Toray Industries, Ltd.; product name) can be preferably used.
[0060] The silicone rubber as the rubber component 22a is preferably a three-dimensional silicone rubber, and specifically, addition cross-linked silicone rubber, peroxide cross-linked silicone rubber, and condensation cross-linked silicone rubber can be exemplified. In addition, non-silicone rubber can be used, and a blend of silicone rubber and non-silicone rubber can also be used. The three-dimensional silicone rubber is a silicone rubber obtained by placing these rubber raw material compositions into a forming mold to make them cross-linked.
[0061] Examples of the addition crosslinking silicone rubber of the rubber component 22a include vinyl methyl siloxane / polydimethyl siloxane copolymer (molecular weight: 500,000 to 900,000), vinyl-terminated polydimethyl siloxane (molecular weight: 10,000 to 200,000), vinyl-terminated diphenyl siloxane / polydimethyl siloxane copolymer (molecular weight: 10,000 to 100,000), vinyl-terminated diethyl siloxane / polydimethyl siloxane copolymer (molecular weight: 10,000 to 50,000), vinyl-terminated trifluoropropyl methyl siloxane / polydimethyl siloxane copolymer (molecular weight: 10,000 to 100,000), vinyl-terminated polyphenyl methyl siloxane (molecular weight: 10,000 to 10,000), vinyl methyl siloxane / dimethyl siloxane copolymer (molecular weight: 10,000 to 10,000), and vinyl methyl siloxane / dimethyl siloxane copolymer (molecular weight: 10,000 to 10,000). Compositions of polysiloxanes containing a vinyl group such as trimethylsiloxane copolymers, trimethylsiloxane-terminated dimethylsiloxane / vinylmethylsiloxane / diphenylsiloxane copolymers, trimethylsiloxane-terminated dimethylsiloxane / vinylmethylsiloxane / bistrifluoropropylmethylsiloxane copolymers, and trimethylsiloxane-terminated polyvinylmethylsiloxane, and H-terminated polysiloxanes (molecular weight: 5000 to 100000), methyl H siloxane / dimethylsiloxane copolymers, polymethyl H siloxane, polyethyl H siloxane, H-terminated polyphenyl (dimethyl H siloxy) siloxane, methyl H siloxane / phenylmethylsiloxane copolymers, and methyl H siloxane / octylmethylsiloxane copolymers,
[0062] Silicone rubber obtained by a composition of amino group-containing polysiloxanes such as aminopropyl-terminated polydimethylsiloxane, aminopropylmethylsiloxane / dimethylsiloxane copolymer, aminoethylaminoisopropylmethylsiloxane / dimethylsiloxane copolymer, aminoethylaminopropylmethoxysiloxane / dimethylsiloxane copolymer, and dimethylamino-terminated polydimethylsiloxane, epoxy group-containing polysiloxanes such as glycidyl-terminated polydimethylsiloxane and (cyclohexyloxyethyl)methylsiloxane / dimethylsiloxane copolymer, acid anhydride group-containing polysiloxanes such as succinic anhydride-terminated polydimethylsiloxane, and isocyanate group-containing compounds such as tolyl diisocyanate and 1,6-hexamethylene diisocyanate.
[0063] The peroxide cross-linked silicone rubber of the rubber component 22a is not particularly limited as long as it is a cross-linked silicone rubber synthesized using an organic silicon raw material compound that can be cross-linked with a peroxide cross-linking agent. Specific examples include polydimethylsiloxane (molecular weight: 500,000 to 900,000), vinyl methylsiloxane / polydimethylsiloxane copolymer (molecular weight: 500,000 to 900,000), vinyl-terminated polydimethylsiloxane (molecular weight: 10,000 to 200,000), vinyl-terminated diphenylsiloxane / polydimethylsiloxane copolymer (molecular weight: 10,000 to 100,000), vinyl-terminated diethylsiloxane / polydimethylsiloxane copolymer (molecular weight: 10,000 to 50,000), vinyl-terminated trifluoropropylmethylsiloxane / polydimethylsiloxane copolymer (molecular weight: 10,000 to 100,000), vinyl-terminated polyphenylmethylsiloxane (molecular weight: 10,000 to 10,000), vinyl methyl Siloxane / dimethylsiloxane copolymer, trimethylsiloxane-terminated dimethylsiloxane / vinylmethylsiloxane copolymer, trimethylsiloxane-terminated dimethylsiloxane / vinylmethylsiloxane / diphenylsiloxane copolymer, trimethylsiloxane-terminated dimethylsiloxane / vinylmethylsiloxane / bistrifluoropropylmethylsiloxane copolymer, trimethylsiloxane-terminated polyvinylmethylsiloxane, methacryloxypropyl-terminated polydimethylsiloxane, acryloxypropyl-terminated polydimethylsiloxane, (methacryloxypropyl)methylsiloxane / dimethylsiloxane copolymer, (acryloxypropyl)methylsiloxane / dimethylsiloxane copolymer.
[0064] Examples of the peroxide crosslinking agent used for crosslinking include ketone peroxides, diacyl peroxides, hydroperoxides, dialkyl peroxides, peroxyketals, alkyl peresters, and percarbonates. More specifically, examples include ketone peroxides, peroxyketals, hydroperoxides, dialkyl peroxides, peroxycarbonates, peroxyesters, benzoyl peroxide, dicumyl peroxide, dibenzoyl peroxide, tert-butyl hydroperoxide, di-tert-butyl hydroperoxide, di(dicyclobenzoyl)peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, benzophenone, Michler's ketone, ethyl dimethylaminobenzoate, and benzoin ethyl ether.
[0065] The amount of the peroxide crosslinking agent can be appropriately selected according to the type of silicone rubber obtained, the required functions and characteristics of the heat insulating rubber 22, but is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 2 parts by mass, relative to 100 parts by mass of the silicone rubber. If it is less than this range, the crosslinking degree is too low and it cannot be used as silicone rubber. On the other hand, if it is more than this range, the crosslinking degree is too high, resulting in a decrease in the elasticity of the silicone rubber.
[0066] As the condensation cross-linking silicone rubber of the rubber component 22a, there can be mentioned a composition of a single condensation component composed of silanol-terminated polydimethylsiloxane (molecular weight: 0.05 ten thousand to 200 thousand) synthesized in the presence of a tin catalyst or a zinc catalyst, a silanol-terminated polydiphenylsiloxane, a silanol-terminated polytrifluoromethylsiloxane, a silanol-terminated diphenylsiloxane / dimethylsiloxane copolymer, etc.; these silanol-terminated polysiloxanes and tetraacetoxysilane, triacetoxymethylsilane, di-tert-butoxydiacetoxysilane, vinyltriacetoxysilane, tetraethoxysilane, triethoxymethylsilane, bis(triethoxysilyl)silane The present invention relates to a condensation-crosslinked silicone rubber comprising a composition of a crosslinking agent such as 1,4-dimethylaminomethylsilane, ...
[0067] Examples of the non-silicone rubber of the rubber component 22a include butyl rubber, ethylene propylene rubber, ethylene propylene diene rubber, polyurethane rubber, fluororubber, acrylic rubber, butadiene rubber, styrene-butadiene rubber, acrylonitrile-butadiene rubber, chloroprene rubber, isoprene rubber, natural rubber, 1,2-polybutadiene, styrene-based thermoplastic elastomers, olefin-based thermoplastic elastomers, polyester-based thermoplastic elastomers, and polyurethane-based thermoplastic elastomers. These may be used alone or in combination.
[0068] The thermoelectric conversion chip 21 has: a thermoelectric conversion element pair 21a composed of an n-type semiconductor element 21a1 and a p-type semiconductor element 21a2, a first electrode 21b and a second electrode 21c that sandwich and electrically connect the two semiconductor elements 21a1 and 21a2 at their upper and lower ends, and insulating sheets 21d and 21e that overlap and bond with the two electrodes 21b and 21c, respectively. The n-type semiconductor element 21a1 and the p-type semiconductor element 21a2 are spaced apart from each other, and are connected to the first electrode 21b at their upper ends by welding. On the other hand, the n-type semiconductor element 21a1 in the thermoelectric conversion element pair 21a is spaced apart from the p-type semiconductor element 21a2 of another adjacent thermoelectric conversion element pair 21a, and are connected to the second electrode 21c at their lower ends by welding. By repeating these connections, a plurality of thermoelectric conversion element pairs 21a are arranged in a serial pattern.
[0069] The thermoelectric conversion element pair 21a and the two electrodes 21b, 21c are supported by the insulating sheets 21d, 21e. Thus, the thermoelectric conversion chip 21 has flexibility by having a so-called skeleton structure in which the n-type semiconductor element 21a1 and the p-type semiconductor element 21a2 are arranged with a gap between each other and supported by the insulating sheets 21d, 21e. By applying a voltage to the thermoelectric conversion chip 21, heat is generated at the heat-generating end 23 of the thermoelectric conversion element pair 21a, which is the upper end side, and the heat-absorbing end 24, which is the lower end side, is cooled. At this time, the heat generated at the heat-generating end 23 and transferred to the insulating intermediate layer 30 is blocked by the heat-insulating rubber 22 having a high heat-insulating property and does not move to the heat-absorbing end 24 side, so that the heat generated by the heat transfer to the heat-absorbing end 24 and the decrease in heat absorption efficiency or the damage of the thermoelectric conversion element pair 21a can be prevented. In addition, the number of thermoelectric conversion element pairs 21 a in the thermoelectric conversion chip 21 can be appropriately increased or decreased according to the size, shape, and output power of the thermoelectric conversion device 1 , and can be one or more.
[0070] As materials for the two semiconductor elements 21a1, 21a2 of the thermoelectric conversion element pair 21a, there can be cited bismuth tellurium-based thermoelectric conversion materials such as Bi-Sb-Te-Se; silicide-based thermoelectric conversion materials such as Mn-Si and Mg-Si; Si-Ge-based thermoelectric conversion materials such as Si-Ge; oxide-based thermoelectric conversion materials such as NaCo2O4, (Ca, Sr, Bi)2Co2O5, (ZnO)5(In-Y)2O3, and (Zn-Al)O; lead tellurium-based thermoelectric conversion materials such as PbTe; TAGS-based thermoelectric conversion materials such as GeTe-AgSbTe2; and cobalt-based thermoelectric conversion materials such as Ce-Fe-Co-Sb, and Yb-Co-ptPb-Sb.
[0071] The thickness of the thermoelectric module layer 20 is preferably 0.1 to 5.0 mm, more preferably 1.0 to 2.0 mm. The thickness can be appropriately set according to the thickness of the thermoelectric conversion chip 21. In addition, the thermoelectric module layer 20 may have a plurality of thermoelectric conversion chips 21.
[0072] The insulating base layer 10 and the insulating intermediate layer 30 sandwiching the thermoelectric module layer 20 in the thickness direction are formed of a heat conductive insulating sheet having thermal conductivity and electrical insulation. Thus, heat transfer caused by heat generation or heat absorption generated in the thermoelectric conversion chip 21 of the thermoelectric module layer 20 can be efficiently generated, and short circuits of the two electrodes 21b and 21c and leakage from the two electrodes can be prevented.
[0073] The thermally conductive insulating sheet having an insulating base layer 10 and an insulating intermediate layer 30 is formed of a thermally conductive insulating composition having a matrix and a thermally conductive filler dispersed in the matrix. The thermally conductive insulating sheets of the insulating base layer 10 and the insulating intermediate layer 30 may be of the same type or of different types. The thermal conductivity of the thermally conductive insulating sheet is preferably greater than 1 W / m·K, and more preferably 1 to 5 W / m·K. When the thermal conductivity of the thermally conductive insulating sheet is less than 1 W / m·K, the insulating base layer 10 and the insulating intermediate layer 30 having sufficient thermal conductivity cannot be obtained, and the heat generation and heat absorption efficiency of the thermoelectric converter 1 deteriorate. In addition, the thermal conductivity is a value at 30°C.
[0074] In addition, the thickness of the insulating base layer 10 and the insulating intermediate layer 30 is preferably 0.01 to 10 mm, more preferably 0.05 to 2 mm. The thickness of the insulating base layer 10 and the insulating intermediate layer 30 may be the same or different from each other if they are within this range. If the thickness is less than 0.01 mm, the strength is insufficient, so the operability during the manufacture of the thermoelectric converter 1 is poor. On the other hand, if the thickness exceeds 10 mm, the flexibility of the thermoelectric converter 1 is impaired, resulting in poor thermal conductivity.
[0075] As the matrix of the heat-conductive insulating composition of the insulating base layer 10 and the insulating intermediate layer 30, silicone rubber similar to the rubber component 22a and non-silicone rubber can be mentioned. In addition, as the heat-conductive filler, magnesium oxide (MgO), aluminum oxide (Al2O3), aluminum nitride (AlN), boron nitride (BN), silicon nitride (Si3N4), diamond, carbon, fullerene, and graphite can be mentioned. Only one type of heat-conductive filler can be used, or a combination of multiple types can be used. The content of the heat-conductive filler in the heat-conductive insulating sheet is preferably 50 to 95% by mass, and more preferably 65 to 90% by mass.
[0076] The heat diffusion layer 40 stacked on the insulating intermediate layer 30 has a higher thermal conductivity than the insulating base layer 10 and the insulating intermediate layer 30. Therefore, the heat diffusion layer 40 can efficiently and quickly move the heat generated at the heat generating end 23 of the thermoelectric conversion chip 21 and moved to the insulating intermediate layer 30 in the horizontal direction, and evenly diffuse it to the entire heat dissipation layer 50. Thereby, the temperature of the surface of the heat dissipation layer 50 rises evenly without unevenness.
[0077] As the material of the thermal diffusion layer 40, for example, aluminum (270 W / m·K (30°C)), copper (400 W / m·K (30°C)), graphite (130 W / m·K (30°C, surface direction)), and high thermal conductivity rubber and high thermal conductivity elastomer (5-10 W / m·K (30°C)) can be mentioned. In addition, as the material of the thermal diffusion layer 40, a thermally conductive insulating sheet that is the material of the insulating base layer 10 and the insulating intermediate layer 30 can be used. These materials can be used alone or in a plurality of forms, which can be overlapped or arranged. The thickness of the thermal diffusion layer 40 is preferably 0.01-0.5 mm, and more preferably 0.05-0.3 mm. In the case where the thermal diffusion layer 40 is formed of a metal material such as aluminum or copper, if the thickness is within this range, the flexibility of the thermoelectric converter 1 will not be impaired, and the rigidity of the metal material can be used to support each layer 10, 20, 30, 50, thereby improving the bending fatigue resistance of the thermoelectric converter 1.
[0078] The heat dissipation layer 50 stacked on the thermal diffusion layer 40 transfers the heat transferred from the thermal diffusion layer 40 to the heated object. Therefore, the material of the heat dissipation layer 50 preferably has high thermal conductivity, and specifically, the heat conductive insulating composition used as the material of the insulating base layer 10 and the insulating intermediate layer 30 can be exemplified. The heat dissipation layer 50 is exposed on the surface of the device or appliance or is directly touched by the user of the device, etc., so the material is preferably easy to process and does not damage the appearance design of the device, etc. and the touch of the user. As the material of the heat dissipation layer 50, in addition to the heat conductive insulating composition, resins such as polyethylene, polypropylene and polyurethane, woven fabrics, non-woven fabrics, wood and leather can be exemplified.
[0079] The thermoelectric converter 1 can be manufactured as follows.
[0080] First, a rubber raw material composition that will become the rubber component 22a of the thermal insulation rubber 22 and a hollow filler 22b whose outer surface is covered with a molecular adhesive by coating or impregnating in a molecular adhesive in advance are kneaded. The hollow filler 22b before heating has a sharp particle size distribution within the range of an average particle size of 5 to 50 μm, and its shape is roughly spherical. The hollow filler 22b has a uniform particle size and shape, so it is uniformly diffused in the rubber raw material composition by kneading. In the thermal insulation rubber 22, the content of the hollow filler 22b is preferably 5 to 60% by mass, more preferably 15 to 50% by mass, and further preferably 20 to 30% by mass. If the content of the hollow filler 22b is too low, a thermal insulation rubber 22 with sufficient thermal insulation and flexibility cannot be obtained. On the other hand, if the content of the hollow filler 22b is too high, the strength of the thermal insulation rubber 22 is reduced, and cracks or breaks are prone to occur.
[0081] Next, a predetermined amount of the kneaded product is placed in a mold maintained at a predetermined temperature and heated for a predetermined time, and at the same time, pressurized under the same conditions as the thermoelectric conversion chip 21 in thickness after molding. In this way, the rubber raw material composition is cured by crosslinking. At this time, the shell of the hollow filler 22b formed by a soft thermoplastic resin is softened by heating. In addition, the heat-expandable liquid hydrocarbon enclosed in its internal space becomes gas and increases in volume, and the internal pressure of the hollow filler 22b is greater than its external pressure, and the hollow filler 22b expands 50 to 100 times in volume ratio like a balloon. The hollow filler 22b has a uniform expansion rate because the shells are all formed with the same thickness, and the shells are formed into spheres, so the pressure of the vaporized heat-expandable liquid hydrocarbons is uniformly applied to the entire shell. As a result, for example, unlike bubbles of uneven shape and diameter formed by the foaming of the foaming agent contained in the rubber component, a void with a uniform shape and diameter can be formed. The conditions such as the heating temperature and the heating time vary depending on the type and characteristics of the addition reaction, but heating is preferably performed at 0 to 200° C. for 1 minute to 24 hours.
[0082] After a predetermined time, the solidified product is removed from the mold and cooled. As a result, the heat-expandable liquid hydrocarbon of the hollow filler 22b returns to liquid, while its shell maintains the size when expanded. Thus, the insulating rubber 22 is formed to include uniformly distributed voids with uniform diameter. A laser cutter is used to cut a predetermined position of the insulating rubber 22 to a size for embedding the thermoelectric conversion chip 21. The thermoelectric conversion chip 21 is embedded therein to obtain the thermoelectric module layer 20.
[0083] A heat conductive filler is added to the above-mentioned rubber raw material composition and kneaded, and the insulating base layer 10 , the insulating intermediate layer 30 , and the heat dissipation layer 50 are molded in the same manner as the method for producing the heat insulating rubber 22 .
[0084] The aluminum sheet is cut by a cutter under conditions to form the same outer shape as the layers 10 , 20 , 30 , 50 , thereby forming the heat diffusion layer 40 .
[0085] A surface active treatment such as corona discharge treatment, plasma treatment, ultraviolet irradiation treatment or excimer treatment is applied to one surface of the insulating base layer 10 and both surfaces of the thermoelectric module layer 20, so that hydroxyl groups are newly generated, expanded and exposed as reactive functional groups on their surfaces. The hydroxyl groups as reactive functional groups are dispersed on their joint surfaces together with the hydroxyl groups originally exposed on the joint surfaces of the insulating base layer 10 and the thermoelectric module layer 20. The surfaces of the two layers 10 and 20 are made to face each other and fixed with a clamp (not shown) to align them so that they overlap and contact. They are pressed at high temperature for crimping. Thereby, the hydroxyl groups form direct ether bonds with each other through dehydration, so that the surfaces of the two layers 10 and 20 are chemically bonded to each other, thereby joining the two layers 10 and 20.
[0086] When the two layers 10 and 20 are joined, they can be covalently bonded under normal pressure, but can also be covalently bonded under reduced pressure or pressure. The covalent bonding can be carried out under reduced pressure or vacuum conditions, for example, 50 torr or less, more specifically 50 to 10 torr, or less than 10 torr, more specifically less than 10 torr to 1×10 -3 torr, preferably less than 10torr~1×10 - 2 Under a vacuum condition of 0.1 torr, the gas medium at the contact interface is removed, or stress (load), such as 10 to 200 kgf, is applied to the contact interface, and the contact interface is further heated to promote the approach of reactive groups such as hydroxyl groups of the two layers 10 and 20.
[0087] The corona discharge treatment applied to the two layers 10 and 20 is performed using, for example, an atmospheric pressure corona surface modification device (manufactured by Shinko Electric Instruments Co., Ltd., product name: Corona Master) under conditions such as power supply: AC100V, output voltage: 0 to 20 kV, oscillation frequency: 0 to 40 kHz for 0.1 to 60 seconds, and temperature 0 to 60° C. Such corona discharge treatment can be performed in a wet state with water, alcohols, acetones, esters, or the like.
[0088] The surface activation treatment may be an atmospheric pressure plasma treatment. In this case, an atmospheric pressure plasma generator (manufactured by Panasonic Corporation, product name: Aiplasma) is used, for example, under conditions of a plasma treatment speed of 10 to 100 mm / s, a power supply of 200 or 220 V AC (30 A), compressed air of 0.5 MPa (1 NL / min), 10 kHz / 300 W to 5 GHz, a power of 100 W to 400 W, and an irradiation time of 0.1 to 60 seconds.
[0089] The surface activation treatment may be an ultraviolet irradiation treatment (a conventional UV treatment or an excimer UV treatment that generates ozone by UV irradiation). The ultraviolet irradiation treatment is performed by using an excimer lamp light source (manufactured by Hamamatsu Photonics Co., Ltd., product name: L11751-01) at, for example, a cumulative light intensity of 50 to 1500 mJ / cm 2 Next proceed.
[0090] In addition, both surfaces of the two layers 10 and 20 to be bonded may be subjected to a surface activation treatment, or only one surface may be subjected to a surface activation treatment.
[0091] After both surfaces of the insulating intermediate layer 30 are subjected to surface activation treatment, the insulating intermediate layer 30 is overlapped and crimped with the insulating base layer 10 with the thermoelectric module layer 20 sandwiched therebetween. The thermal diffusion layer 40 and the heat dissipation layer 50 are similarly bonded to obtain the thermoelectric converter 1.
[0092] As the bonding between the adjacent layers 10, 20, 30, 40, 50, direct chemical bonding by surface active treatment is shown, but the bonding may also be indirect bonding via a molecular adhesive. As the molecular adhesive, the same molecular adhesive as the silane coupling agent attached to the outer surface of the hollow filler 22b can be used. In this case, the layers 10, 20, 30, 40, 50 can be attached by spraying or applying the molecular adhesive to the surfaces to be bonded, or by immersing the layers 10, 30, 40, 50 and the heat insulating rubber 22 in a solution of the molecular adhesive.
[0093] As another example of the molecular binder, there can be mentioned a polysiloxane compound containing a reactive group schematically represented by the following chemical formula (2).
[0094] [Chemistry 2]
[0095]
[0096] (In the chemical formula (2), p and q are 0 or a number from 2 to 200, r is 0 or a number from 2 to 100, and p+q+r>2. -A 1 ,-A 2 and -A 3 is selected from -CH3, -C2H5, -CH=CH2, -CH(CH3)2, -CH2CH(CH3)2, -C(CH3)3, -C6H5 or -C6H 12 , and -OCH3, -OC2H5, -OCH=CH2, -OCH(CH3)2, -OCH2CH(CH3)2, -OC(CH3)3, -OC6H5 and -OC6H 12 , any of the reactive groups capable of reacting with hydroxyl groups. 1 and -B 2 is selected from -N(CH3)COCH3 or -N(C2H5)COCH3, and -OCH3, -OC2H5, -OCH=CH2, -OCH(CH3)2, -OCH2CH(CH3)2, -OC(CH3)3, -OC6H5, -OC6H 12, -OCOCH3, -OCOCH(C2H5)C4H9, -OCOC6H5, -ON=C(CH3)2 and -OC(CH3)=CH2, any of the reactive groups that can react with hydroxyl groups. 1 )(-B 1 )} p -、-{O-Ti(-A 2 )(-B 2 )} q -and-{O-Al(-A 3 )} r -A in the repeating unit 1 ,-A 2 ,-A 3 ,-B 1 and-B 2 At least one of the above-mentioned reactive groups is a group that reacts with the hydroxyl groups on the surface when the layers 10, 20, 30, 40, 50 are bonded). The repeating unit of the compound may be a block copolymer or a random copolymer.
[0097] In this case, each layer 10, 30, 40, 50 and the heat-insulating rubber 22 can be attached thereto by immersing them in a solution of polysiloxane containing reactive groups that react with hydroxyl groups. In addition, the solution is applied or sprayed on the outer surface of the insulating sheet 21d, 21e of the thermoelectric conversion chip 21. Then, by heat treatment, the polysiloxane containing reactive groups is combined with the hydroxyl groups on the surface of each layer 10, 20, 30, 40, 50 to form a monolayer molecular film, and as a result, the reactive groups with other hydroxyl groups to be bonded are amplified. As a result of the chemical bonding of the hydroxyl groups on one surface of each layer 10, 20, 30, 40, 50 with the polysiloxane containing reactive groups, the hydroxyl groups of each layer 10, 20, 30, 40, 50 are indirectly bonded through the polysiloxane containing reactive groups, thereby bonding each layer 10, 20, 30, 40, 50 to each other. When the polysiloxane compound containing a reactive group is attached to both the thermoelectric conversion chip 21 and the heat insulating rubber 22, it is preferred to perform a spraying treatment on the polysiloxane solution containing a reactive group instead of a dipping treatment, followed by a drying treatment and, if necessary, a heating treatment. The polysiloxane compound containing a reactive group can be attached to the outer surface of the hollow filler 22b as a silane coupling film.
[0098] In addition, when the heating and cooling effects caused by the heat generation and heat absorption of the thermoelectric conversion chip 21 do not need to be exhibited on the insulating base layer 10 side, the insulating base layer 10 can be formed of a heat insulating material. In addition, the insulating base layer 10 and the thermoelectric module layer 20 can also be joined by an adhesive or a bonding agent.
[0099] When the thicknesses of the thermoelectric conversion chip 21 and the heat insulating rubber 22 are different, the thicknesses of the thermoelectric conversion chip 21 and the heat insulating rubber 22 can be made equal by overlapping a spacer on the insulating sheets 21 d and 21 e .
[0100] The thermoelectric conversion device 1 can be used as a heating source for a steering wheel heater or a heating sheet by, for example, being installed in the ring portion of a steering wheel of a car or on the supporting surface of a sheet with the heat dissipation layer 50 facing outward. In addition, by installing the thermoelectric conversion device 1 inside a helmet or protective clothing, the inside of the cold-proof clothing can be quickly heated, thereby reducing the burden on the body of a user working in a cold place such as a freezer.
[0101] By arranging the heat absorbing end 24 of the thermoelectric conversion chip 21 toward the heat dissipation layer 50, the thermoelectric conversion device 1 can generate a cooling phenomenon on the surface of the heat dissipation layer 50. In this case, by installing the thermoelectric conversion device 1 inside the ring of the steering wheel and the inside of the helmet or protective clothing, it is possible to prevent the temperature inside the helmet or protective clothing from rising in summer or in hot places, reduce the burden on the user's body caused by heat or summer heat, and prevent burns or heat stroke.
[0102] Thus, in the thermoelectric conversion device 1, the adjacent layers 10, 20, 30, 40, and 50 are firmly bonded to each other by chemical bonds, so that even if bent, peeling does not occur between the layers. In addition, by surrounding the thermoelectric conversion chip 21 with the heat insulating rubber 22 having the same thickness as the thermoelectric conversion chip 21, no gap is required for heat insulation, so the surface of the heat dissipation layer 50 is not deformed into an uneven shape due to the pressing force applied to the heat dissipation layer 50, or the thermoelectric conversion chip 21 is not damaged. Therefore, the thermoelectric conversion device 1 is suitable for use in instruments such as steering wheels and protective clothing, and does not impair the touch of their users.
[0103] The thermoelectric conversion device 1 can be used not only as a heating source or a cooling source, but also as a voltage generator using the Seebeck effect. In this case, the heat dissipation layer 50 on the heat-generating end 23 side is in contact with a high-temperature component, and the insulating base layer 10 on the heat-absorbing end 24 side is in contact with a low-temperature component. The thermoelectric conversion chip 21 generates a voltage using the temperature difference between the high-temperature component and the low-temperature component.
[0104] The thermoelectric converter 1 may have a circuit layer between the thermoelectric module layer 20 and the insulating intermediate layer 30. The circuit layer has wiring that electrically relays the thermoelectric conversion chip 21 and, for example, a control device that is disposed outside the thermoelectric converter 1. A portion of the wiring of the circuit layer is joined to each electrode 21b, 21c of the thermoelectric conversion chip 21 by, for example, soldering in a manner that allows conduction, and another portion of the wiring is electrically connected to the control device. In this case, the thermoelectric converter 1 can be operated at a desired time or temperature by a signal generated by the control device. The circuit layer is formed by applying wiring of a conductor such as copper to the surface of the insulating intermediate layer 30 opposite to the thermoelectric module layer 20 using a printing method such as screen printing, flexographic printing, inkjet printing, and offset printing.
[0105] Example
[0106] Hereinafter, examples of the present invention will be described in detail, but the scope of the present invention is not limited to these embodiments.
[0107] (Example 1)
[0108] 100 parts by mass of dimethyl silicone rubber (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: 3320-20) as the rubber component 22a, 40 parts by mass of heat-expandable microcapsules (manufactured by Matsumoto Oil Pharmaceutical Co., Ltd., product name: Matsumoto Microsphere F-36-D (average particle size 13 μm), and 20 parts by mass of F-36LVD (average particle size 16 μm) of the same company) as the hollow filler 22a, and 0.1 parts by mass of curing accelerator a (manufactured by Asahi Kasei Wacker Silicone Co., Ltd., product name: Cat. Ep) were mixed and kneaded, and cured by pressurizing and heating with a compression molding machine, and the cured product was cut with a laser cutter. In this way, a 50×50 mm square and 2 mm thick heat insulating rubber 22 was obtained. A 4×4 mm square was cut from the central part of the heat insulating rubber 22 to make a hole in which the thermoelectric conversion chip 21 could be embedded. The thermal conductivity of the heat insulating rubber 22 was measured using a thermal conductivity meter (manufactured by Kyoto Electronics Co., Ltd., product name: QTM-500) in accordance with JIS R2616-2000, and the result was 0.44 W / m·K.
[0109] A square of 50×50 mm was cut out from a 0.1 mm thick aluminum sheet using a cutter to serve as the heat diffusion layer 40 .
[0110] Magnesium oxide (MgO) and aluminum oxide (Al2O3) as heat conductive fillers were dispersed in dimethyl silicone rubber to form a flexible sheet of 0.5 mm thickness formed of heat conductive rubber, and a composition for insulating base layer 10, insulating intermediate layer 30, heat dissipation layer 50 and insulating sheets 21d, 21e was obtained. It was cured by applying pressure and heating, and the cured product was cut using a laser cutter. In this way, a 50×50 mm square and 0.5 mm thick insulating base layer 10, insulating intermediate layer 30 and heat dissipation layer 50 were obtained. Similarly, 4×4 mm square and 0.5 mm thick insulating sheets 21d, 21e were obtained. The thermal conductivity of each layer 10, 30, 50 and insulating sheets 21d, 21e was measured in the same way as the heat insulating rubber 22, and the result was 3.0 W / m·K.
[0111] An ethanol solution of vinyl triethoxysilane (manufactured by Shin-Etsu Silicone Co., Ltd., product name: KBE-1003) as a molecular binder was applied to the outer surfaces of the insulating sheets 21d and 21e sandwiching the plurality of thermoelectric conversion element pairs 21a, and then heated and washed with ethanol. In this way, the thermoelectric conversion chip 21 with the outer surfaces of the insulating sheets 21d and 21e modified was obtained.
[0112] The thermoelectric conversion chip 21 with modified surface is embedded in the hole of the heat insulating rubber 22 to produce the thermoelectric module layer 20. The surfaces to be joined of each layer 10, 20, 30, 40, 50 are subjected to corona discharge treatment to generate hydroxyl groups. The layers 10, 20, 30, 40, 50 are overlapped in sequence so that the hydroxyl generating surfaces abut against each other and clamped with a clamp. At this time, the thermoelectric module layer 20 is arranged in such a way that the heat absorbing end 24 of the thermoelectric conversion chip 21 is located on the insulating intermediate layer 30 side, and is joined with a molecular adhesive. In this way, the following is obtained: Figure 1 and 2 The thermoelectric converter 1 shown (length×width×thickness=50×50×2 mm).
[0113] (Comparative Example 1)
[0114] The insulating base layer, the thermoelectric conversion chip, and the heat dissipation layer were bonded by molecular bonding in the same manner as in Example 1, except that the thermal insulation rubber was not arranged on the thermoelectric module layer, and the insulating intermediate layer 30 and the heat diffusion layer 40 were not laminated. Thus, the thermoelectric conversion device of Comparative Example 1 (length × width × thickness = 50 × 50 × 2 mm) was obtained.
[0115] Table 1 shows the structures of the thermoelectric conversion devices of Example 1 and Comparative Example 1.
[0116] [Table 1]
[0117] Table 1
[0118]
[0119] (Heat absorption control temperature distribution test)
[0120] like Figure 3 As shown, thermocouples are installed on the surface of the heat dissipation layer 50 of the thermoelectric conversion device 1 of Example 1, that is, at the positions of measuring points A to C. The position coordinates of each point are measuring point A: x, y = 25, 25 mm, measuring point B: x, y = 15, 15 mm, measuring point C: x, y = 5, 5 mm. Measuring point A is directly above the thermoelectric conversion chip. Using a DC regulated power supply, a voltage of 0.45 V is applied to the thermoelectric conversion chip 21 to cool the heat absorption end 24 side. The temperature of each measuring point is recorded using a data recorder. The temperature distribution test of Comparative Example 1 was carried out in the same manner as in Example 1. Figure 4 This is a graph showing the change over time of the temperature difference ΔT (° C.) between Example 1 and Comparative Example 1. The temperature difference ΔT (° C.) is the difference between the temperature at each measurement point and the room temperature, and is represented by the following formula (1).
[0121] ΔT (°C) = (temperature at each measuring point) - (room temperature) ... (1)
[0122] Figure 4 (a) shows Example 1, Figure 4 (b) shows Comparative Example 1, where the horizontal axis of the graph represents time (minutes) and the vertical axis represents temperature difference ΔT (° C.). Table 2 shows the temperature 5 minutes after the start of voltage application.
[0123] [Table 2]
[0124] Table 2
[0125]
[0126] The thermoelectric converter of Example 1 has a smaller temperature difference between points and exhibits a uniform temperature distribution than the thermoelectric converter of Comparative Example 1. The thermoelectric converter of Example 1 has excellent thermoelectric conversion efficiency and temperature distribution uniformity because it has a heat diffusion layer.
[0127] (Example 2)
[0128] A thermoelectric converter of Example 2 was produced in the same manner as in Example 1, except that the thermoelectric module layer 20 was produced so that the heat generating end 23 of the thermoelectric conversion chip 21 was located on the insulating intermediate layer 30 side.
[0129] (Comparative Example 2)
[0130] The thermoelectric converter of Comparative Example 1 was turned upside down, and a thermocouple was mounted on the heat generating end side of the thermoelectric converter chip, that is, on the surface of the insulating base layer, to obtain a thermoelectric converter of Comparative Example 2.
[0131] Table 3 shows the structures of the thermoelectric conversion devices of Example 2 and Comparative Example 2.
[0132] [Table 3]
[0133] Table 3
[0134]
[0135] (Heat control temperature distribution test)
[0136] In the same manner as the endothermic controlled temperature distribution test, a voltage was applied to the thermoelectric conversion chip of Example 2 to generate heat at the heating end 23 side, and the temperature at each measurement point was measured. The temperature difference ΔT (°C) was calculated according to formula (1). The thermoelectric conversion chip of Comparative Example 2 was also measured in the same manner as Example 1. The results of Example 2 are shown in Figure 5 (a), the results of Comparative Example 2 are shown in Figure 5 (b) Table 4 shows the temperature 5 minutes after the start of voltage application.
[0137] [Table 4]
[0138] Table 4
[0139]
[0140] The thermoelectric converter of Example 2 has a smaller temperature difference between each point and shows a uniform temperature distribution than the thermoelectric converter of Comparative Example 2. The thermoelectric converter of Example 2 has excellent thermoelectric conversion efficiency and temperature distribution uniformity because it has a heat diffusion layer. On the other hand, in Comparative Example 2, only the measurement point A directly above the thermoelectric conversion chip shows a local temperature rise, and no uniform temperature distribution is observed.
[0141] (Comparative Example 3)
[0142] A thermoelectric conversion device (length×width×thickness=50×50×2 mm) of Comparative Example 3 without molecular bonding was manufactured in the same manner as Example 1 except that a thermoelectric module layer having thermoelectric conversion chips without surface modification was used and each layer was bonded with an acrylic adhesive.
[0143] (Comparative Example 4)
[0144] A thermoelectric converter device of Comparative Example 4 (length×width×thickness=50×50×2 mm) was obtained in the same manner as in Example 1, except that the thermal insulation rubber was not used in the thermoelectric module layer produced in Example 1, in which the thermoelectric conversion chip was surrounded by air instead of the thermal insulation rubber.
[0145] Table 5 shows the structures of the thermoelectric conversion devices of Example 1 and Comparative Examples 3 and 4.
[0146] [Table 5]
[0147] Table 5
[0148]
[0149] (Endothermic control temperature change test)
[0150] The heat dissipation layer of the thermoelectric converters of Example 1 and Comparative Examples 3 and 4 was cooled in the same manner as in the endothermic controlled temperature distribution test except that the applied voltage was set to 0.6 V. The temperature difference ΔT (°C) at 5 minutes after the start of voltage application at each measuring point A to C was calculated according to equation (1). The results are shown in Figure 6 (a) From Figure 6 (a) It can be seen that the temperature of Example 1 is significantly lower than that of Comparative Example 3 in which molecular bonding is not applied, so it can be seen that molecular bonding can suppress the interlayer transfer loss of heat and improve the thermoelectric conversion efficiency. In addition, Example 1 shows higher cooling than Comparative Example 4 in which no thermal insulation rubber is used, so it can be seen that the thermal insulation rubber has a thermal insulation effect equal to or higher than that of air.
[0151] (Comparative Example 5)
[0152] A thermoelectric conversion device (length×width×thickness=50×50×2 mm) of Comparative Example 5 without molecular bonding was manufactured in the same manner as Example 2 except that a thermoelectric module layer having thermoelectric conversion chips without surface modification was used and each layer was bonded with an acrylic adhesive.
[0153] (Comparative Example 6)
[0154] A thermoelectric converter device of Comparative Example 6 (length×width×thickness=50×50×2 mm) was obtained in the same manner as in Example 1, except that the thermal insulation rubber was not used in the thermoelectric module layer produced in Example 2, in which the thermoelectric conversion chip was surrounded by air instead of the thermal insulation rubber.
[0155] Table 6 shows the structures of the thermoelectric conversion devices of Example 2 and Comparative Examples 5 and 6.
[0156] [Table 6]
[0157] Table 6
[0158]
[0159] (Heat control temperature change test)
[0160] The heat dissipation layer of the thermoelectric converters of Example 2 and Comparative Examples 5 and 6 was heated in the same manner as in the endothermic controlled temperature change test. The temperature at 5 minutes after the start of voltage application was measured at each measuring point A to C, and the temperature difference ΔT (°C) was calculated according to formula (1). The results are shown in Figure 6 (b) According to Figure 6 (b) It can be seen that there is almost no difference between Example 2 and Comparative Example 5 in which molecular bonding is not applied.
[0161] The presence or absence of molecular bonding produced a difference in the endothermic control temperature change test, but on the other hand, did not produce a difference in the exothermic control temperature change test. This is believed to be due to the following reasons. First, in the thermoelectric converter, the following formula (2) holds true.
[0162] Q H >Q C ……(2)
[0163] Among them, Q H is the heat generated in the heat dissipation layer, Q C is the amount of heat absorbed in the heat dissipation layer. Q H and Q C Each of them includes at least the heat generated by the internal impedance of the thermoelectric conversion element pair (Q r ), and the heat loss caused by the heat transfer resistance between layers (Q λ ). Q r It shows a large value at high temperature and a small value at low temperature, so formula (2) always holds. λ With Q r In comparison, the temperature dependence is low and can be considered as a constant value.
[0164] In the endothermic controlled temperature change test, because Q r <Q λ Established, so Q λ Q r Q C The contribution of Q C On the other hand, in the heating control temperature change test, because Q r >Q λ Established, so Q r Q λ Q H The contribution of molecular bonding to Q is large, that is, since the heat generated by the internal impedance of the thermoelectric conversion element pair is greater than the heat loss generated by the heat transfer impedance between the layers, the presence or absence of molecular bonding has a significant effect on Q H Not easy to make a difference.
[0165] from Figure 6 (b) It is found that Example 2 having the heat-insulating rubber exhibits heat generation equivalent to that of Comparative Example 6 having no heat-insulating rubber, and thus it is found that the heat-insulating rubber has a heat-insulating effect equal to or greater than that of air.
[0166] Possibility of industrial application
[0167] The thermoelectric conversion device of the present invention does not cause concave-convex deformation on the surface by pressing, bending and twisting, so it is suitable for being installed on the curved surface of equipment or appliances that the user directly contacts and used as a heat pump.
[0168] Thermoelectric conversion devices apply voltage to thermoelectric conversion chips and use the Peltier effect, which generates heat at one end of the thermoelectric conversion element pair and absorbs heat at the other end. They can be used as heating or cooling sources for equipment and appliances such as cold storage, steering wheel heaters, and heating pads.
[0169] Thermoelectric conversion devices can use the Seebeck effect to generate voltage by setting a temperature difference between the two ends of the thermoelectric conversion chip, and are used to generate electricity for devices driven by small amounts of electricity, such as watches.
[0170] Explanation of symbols
[0171] 1 is a thermoelectric conversion device, 10 is an insulating base layer, 20 is a thermoelectric module layer, 21 is a thermoelectric conversion chip, 21a is a thermoelectric conversion element pair, 21a1 is an n-type semiconductor element, 21a2 is a p-type semiconductor element, 21b is a first electrode, 21c is a second electrode, 21d and 21e are insulating sheets, 22 is a heat insulating rubber, 22a is a rubber component, 22b is a hollow filler, 23 is a heat generating end, 24 is a heat absorbing end, 30 is an insulating intermediate layer, 40 is a heat diffusion layer, 50 is a heat dissipation layer, 60 is a conventional thermoelectric conversion device, 61 is a thermoelectric conversion chip, 61a is a thermoelectric conversion element pair, 62 is a heat generating end, 63 is a heat absorbing end, 64 is a substrate side sheet, 65 is a surface side sheet, 66 is a cavity, 67 is a device substrate, and A, B, and C are measuring points.
Claims
1. A thermoelectric module layer, comprising a thermoelectric conversion chip and a heat-insulating rubber, wherein the thermoelectric conversion chip has a thermoelectric conversion element pair consisting of an n-type semiconductor element and a p-type semiconductor element, and electrodes sandwiching a plurality of the thermoelectric conversion element pairs, wherein the thermoelectric conversion element pairs are connected to the electrodes, characterized in that: The heat-insulating rubber is a pressurized and heated cured product containing a rubber component as a silicone rubber and hollow fillers that are independent of each other and expand to form a plurality of voids, the heat-insulating rubber surrounds the thermoelectric conversion element pair and the electrode of the thermoelectric conversion chip, and the thermoelectric conversion chip has an insulating sheet that overlaps and is bonded to the electrode, The hollow filler includes a resin shell and a thermally expandable liquid hydrocarbon sealed in an internal space of the shell.
2. The thermoelectric module layer according to claim 1, characterized in that The thermoelectric module layer is used in a thermoelectric conversion device, which includes: an insulating base layer and an insulating intermediate layer which sandwich the thermoelectric module layer and are heat-conductive insulating sheets; a heat diffusion layer which overlaps with the insulating intermediate layer and has higher thermal conductivity than the insulating base layer and the insulating intermediate layer; and a heat dissipation layer which overlaps with the heat diffusion layer and has thermal conductivity, wherein these adjacent layers are bonded to each other by chemical bonds.
3. The thermoelectric module layer according to claim 1, characterized in that The resin is a vinylidene chloride resin or an acrylic resin.
4. The thermoelectric module layer according to claim 1, characterized in that The thickness of the heat insulating rubber is the same as the thickness of the thermoelectric conversion chip in which the thermoelectric conversion element pair and the electrodes are surrounded by the insulating rubber.
5. The thermoelectric module layer according to claim 2, characterized in that The heat diffusion layer is formed of at least one selected from aluminum, copper, graphite, heat conductive rubber, and heat conductive elastomer.
6. The thermoelectric module layer according to claim 2, characterized in that The thickness of the heat diffusion layer is 0.01-0.5 mm.
7. The thermoelectric module layer according to any one of claims 1 to 6, characterized in that A silane coupling film is attached to the outer surface of the hollow filler.
8. The thermoelectric module layer according to claim 2, characterized in that A circuit layer conductively connected to the thermoelectric conversion chip is provided between the thermoelectric module layer and the insulating intermediate layer.
9. A thermoelectric conversion device, characterized in that: have: The thermoelectric module layer according to claim 1; an insulating base layer and an insulating intermediate layer which are heat-conductive insulating sheets sandwiching the thermoelectric module layer; a heat diffusion layer overlapping the insulating intermediate layer and having higher thermal conductivity than the insulating base layer and the insulating intermediate layer; and a heat dissipation layer overlapping the heat diffusion layer and having thermal conductivity, Adjacent layers are bonded to each other by chemical bonds, so that the thermoelectric conversion device is used as a heating source or a cooling source, or is used to generate voltage.