Joint body and semiconductor device
By using a thin copper particle bonding body containing 65% by volume or more of copper in the semiconductor device, a sintered metal layer with high thermal conductivity and high bonding strength is solved, and the problem of insufficient connection reliability of the semiconductor device under high temperature conditions is achieved. Full connection reliability and high-temperature working ability in temperature cycle tests.
Patent Information
- Application Number
- CN202010311153.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2015-09-07
- Filing Date
- 2016-09-07
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2036-09-07
AI Technical Summary
The existing semiconductor devices lack connection reliability under high temperature conditions, especially in temperature cycle tests, the relationship between the sintered metal layer and the connection reliability is not clear, making it difficult to achieve sufficient connection reliability.
The copper paste for bonding containing flaky copper particles is used to form a sintered metal layer. The copper content reaches 65% by volume. The specific orientation structure optimization ensures the thermal conductivity and bonding strength of the sintered metal layer, and uses 65% by volume or more by volume. The copper density and parallel-oriented sheet structure disperses heat stress, improving connection reliability.
Under high temperature conditions, especially in temperature cycle tests, sufficient connection reliability is achieved, the high-temperature working ability and high capacity and space-saving characteristics of semiconductor devices are improved, and the chip shear strength and thermal conductivity are improved.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
[0001] This application is a divisional application with an application date of September 7, 2016, a priority date of September 7, 2015, a Chinese patent application number of 201680051537.8, and an invention name of “Joint body and semiconductor device”. Technical Field
[0002] The present invention relates to a junction body and a semiconductor device. Background Art
[0003] When manufacturing semiconductor devices, various bonding materials are used to bond semiconductor elements to lead frames (supporting members). In semiconductor devices, high-melting-point lead solder is used as a bonding material for bonding power semiconductors and LSIs that operate at high temperatures above 150°C. In recent years, due to the high capacity and space saving of semiconductor elements, the requirements for operating at high temperatures above 175°C have increased. At the joints formed by the high-melting-point lead solder layer, the heat resistance and thermal conductivity are insufficient, making it difficult to ensure connection reliability. On the other hand, with the strengthening of RoHS control, lead-free bonding materials are required.
[0004] Until now, the bonding of semiconductor elements using materials other than lead solder has been studied. For example, Patent Document 1 below proposes a technique for sintering silver nanoparticles at low temperature to form a sintered silver layer. It is known that such sintered silver has high connection reliability for power cycles.
[0005] As other materials, a technology for sintering copper particles to form a sintered copper layer has also been proposed. For example, the following patent document 2 discloses a copper paste for bonding containing copper oxide particles and a reducing agent as a bonding material for bonding a semiconductor element to an electrode. In addition, the following patent document 3 discloses a bonding material containing copper nanoparticles and copper micron particles or copper submicron particles or both.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent No. 4928639
[0009] Patent Document 2: Japanese Patent No. 5006081
[0010] Patent Document 3: Japanese Patent Application Publication No. 2014-167145
[0011] Non-patent literature
[0012] Non-patent document 1: R. Khazaka, L. Mendizabal, D. Henry: J. ElecTron. Mater, 43(7), 2014, 2459-2466 Summary of the invention
[0013] Technical problem to be solved by the invention
[0014] When the semiconductor device is operated at a high temperature, the connection reliability of the joint that joins the semiconductor element becomes an important issue. Compared with silver, copper has a higher shear elastic modulus (copper: 48GPa, silver: 30GPa) and a lower thermal expansion coefficient (copper: 17μm / (m·K), silver: 19μm / (m·K)). Therefore, the connection reliability of the semiconductor device described in the above patent document 2 and the electronic components described in the above patent document 3 may be better than the joint with a sintered silver layer described in the above patent document 1.
[0015] However, the inventors have found through their research that when the joint is a sintered metal layer, not only the physical properties of the constituent metal but also the morphology of the sintered metal layer itself will affect its connection reliability. In the above-mentioned patent documents 1 to 3, the relationship between the morphology of the sintered body layer and the connection reliability is still unclear, and in particular, a sintered metal layer that can fully obtain the connection reliability in a temperature cycle test including high temperature conditions has not yet been realized.
[0016] An object of the present invention is to provide a joint body and a semiconductor device including a sintered metal layer having sufficient connection reliability even in a temperature cycle test including high temperature conditions.
[0017] Means for solving technical problems
[0018] In order to solve the above-mentioned technical problems, the present inventors conducted intensive studies and found that a sintered metal layer formed by a specific copper paste for bonding containing flaky copper particles has excellent thermal conductivity and bonding strength and has a structure with sufficient connection reliability even in a temperature cycle test including high temperature conditions. Based on this knowledge, the present invention was completed.
[0019] That is, the present invention provides a joint body, which comprises a first component, a second component, and a sintered metal layer joining the first component and the second component, wherein the sintered metal layer contains a structure derived from flaky copper particles oriented approximately parallel to an interface between the first component or the second component and the sintered metal layer, and the copper content in the sintered metal layer is greater than 65 volume % based on the volume of the sintered metal layer.
[0020] In addition, in this specification, "thin sheet shape" includes a flat plate shape such as a plate shape and a scale shape.
[0021] The joint body of the present invention has sufficient connection reliability even in a temperature cycle test including high temperature conditions by including the above-mentioned sintered metal layer. The reason for obtaining such an effect is considered to be that the above-mentioned sintered metal layer has a density of copper of 65 volume % or more, thereby obtaining sufficient thermal conductivity and bonding strength, and at the same time, the structure containing a source of flaky copper particles oriented in a predetermined direction obtains the effects of dispersing thermal stress and making it difficult for the damage to spread even if a part of the sintered metal layer is damaged.
[0022] In the above-mentioned joint body, at least one of the first component and the second component may contain at least one metal selected from copper, nickel, palladium, silver, gold, platinum, lead, tin and cobalt on the surface in contact with the sintered metal layer. In this case, the adhesion between at least one of the first component and the second component and the sintered metal layer can be further improved.
[0023] The present invention also provides a semiconductor device comprising a first component, a second component, and a sintered metal layer connecting the first component and the second component, wherein at least one of the first component and the second component is a semiconductor element, wherein the sintered metal layer contains a structure derived from flaky copper particles oriented approximately parallel to an interface between the first component or the second component and the sintered metal layer, and the copper content in the sintered metal layer is greater than 65 volume % based on the volume of the sintered metal layer.
[0024] The semiconductor device of the present invention includes the sintered metal layer having sufficient connection reliability even in a temperature cycle test including high temperature conditions, so that high-temperature operability can be improved and it can cope with higher capacity and space saving of semiconductor elements.
[0025] In the semiconductor device, the die shear strength may be 30 MPa or more.
[0026] The present invention further provides a semiconductor device comprising a first electrode, a semiconductor element electrically connected to the first electrode, and a second electrode electrically connected to the semiconductor element via a metal wiring, wherein a sintered metal layer containing copper is provided between the semiconductor element and the metal wiring, and between the metal wiring and the second electrode.
[0027] The semiconductor device of the present invention includes the sintered metal layer having sufficient connection reliability even in a temperature cycle test including high temperature conditions, so that high-temperature operability can be improved and it can cope with higher capacity and space saving of semiconductor elements.
[0028] In the semiconductor device, the sintered metal layer is in contact with the metal wiring and contains a structure derived from flaky copper particles oriented approximately parallel to the interface with the metal wiring. The copper content in the sintered metal layer can be 65 volume % or more based on the volume of the sintered metal layer.
[0029] The present invention also provides a semiconductor device comprising a first heat conducting member, a second heat conducting member, and a semiconductor element arranged between the first heat conducting member and the second heat conducting member, wherein a sintered metal layer containing copper is provided between at least one of the first heat conducting member and the semiconductor element and between the semiconductor element and the second heat conducting member.
[0030] The semiconductor device of the present invention includes the sintered metal layer having sufficient connection reliability even in a temperature cycle test including high temperature conditions, so that high-temperature operability can be improved and it can cope with higher capacity and space saving of semiconductor elements.
[0031] In the above-mentioned semiconductor device, the sintered metal layer is in contact with the first heat-conducting member or the second heat-conducting member and contains a structure derived from flaky copper particles oriented approximately parallel to the interface of the first heat-conducting member or the second heat-conducting member. The copper content in the sintered metal layer can be 65 volume % or more based on the volume of the sintered metal layer.
[0032] Effects of the Invention
[0033] According to the present invention, it is possible to provide a bonded body and a semiconductor device including a sintered metal layer having sufficient connection reliability even in a temperature cycle test including high temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a schematic cross-sectional view showing an example of a typical form of a sintered metal layer in the bonded body according to the present embodiment.
[0035] Figure 2 This is a schematic cross-sectional view showing an example of a bonded body produced using the copper paste for bonding according to the present embodiment.
[0036] Figure 3 for Figure 1 The enlarged view is a schematic cross-sectional view showing a method for measuring the major diameter and thickness of a structure from which flaky copper particles are derived.
[0037] Figure 4 This is a schematic cross-sectional view showing a method of measuring the angle θ of the structure derived from the flaky copper particles of the joined body according to the present embodiment with respect to the joined surface.
[0038] Figure 5 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0039] Figure 6 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0040] Figure 7 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0041] Figure 8 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0042] Fig. 9 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0043] Fig.10 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0044] Fig.11 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0045] Fig.12 This is a schematic cross-sectional view showing an example of a semiconductor device manufactured using the copper paste for bonding according to the present embodiment.
[0046] Fig.13 This is a SEM image showing a cross section of the bonded body of Example 1.
[0047] Fig.14 This is a SEM image showing a cross section of the bonded body of Example 4.
[0048] Fig.15 : is a SEM image showing a cross section of the bonded body of Comparative Example 3.
[0049] Fig.16 3 is a SEM image showing a cross section of the bonded body of Comparative Example 6.
[0050] Fig.17 3 is a SEM image showing a cross section of the bonded body of Comparative Example 7.
[0051] Fig.18 3 is a SEM image showing a cross section of the bonded body of Comparative Example 8. DETAILED DESCRIPTION
[0052] Hereinafter, a mode for carrying out the present invention (hereinafter also referred to as "this embodiment") will be described in detail. The present invention is not limited to the following embodiment.
[0053] The following is a reference to the attached Figure 1 The preferred embodiment will be described in detail. In the drawings, the same or corresponding parts are given the same reference numerals, and repeated descriptions are omitted. In addition, the dimensional ratios of the drawings are not limited to the ratios shown in the drawings.
[0054] <Joint body>
[0055] The bonded body of this embodiment includes a first member, a second member, and a sintered metal layer bonding the first member and the second member, the sintered metal layer having a predetermined orientation structure, and the copper content in the sintered metal layer is 65 volume % or more based on the volume of the sintered metal layer.
[0056] Figure 1 This is a schematic cross-sectional view showing an example of a typical form of a sintered metal layer in the bonded body according to the present embodiment. Figure 1 The sintered metal layer shown includes sintered copper 1 having a structure derived from flaky copper particles (hereinafter sometimes referred to as “flaky structure”), sintered copper 2 derived from other copper particles, and pores 3 .
[0057] Figure 2 It is a schematic cross-sectional view showing an example of a bonded body according to the present embodiment. Figure 2 The bonded body 100 shown includes a first member 5 , a second member 6 , and a sintered metal layer 4 bonding the first member 5 and the second member 6 .
[0058] As the first component 5 and the second component 6, for example, there can be cited semiconductor elements such as IGBT, diode, Schottky diode, MOS-FET, thyristor, logic circuit, sensor, analog integrated circuit, LED, semiconductor laser, signal transmitter, lead frame, ceramic substrate with metal plate (such as DBC), LED package and other semiconductor element mounting substrate, metal wiring such as copper tape and metal frame, blocks such as metal blocks, power supply components such as terminals, heat dissipation plates, water cooling plates, etc.
[0059] The first component 5 and the second component 6 may also contain metal on the surfaces 7a and 7b in contact with the sintered metal layer 4. Examples of the metal include copper, nickel, silver, gold, palladium, platinum, lead, tin, and cobalt. One of these metals may be used alone, or two or more may be used in combination. In addition, the surface in contact with the sintered body may also be an alloy containing the above-mentioned metals. In addition to the above-mentioned metals, zinc, manganese, aluminum, beryllium, titanium, chromium, iron, and molybdenum may also be mentioned as the metal used in the alloy. As a component containing metal on the surface in contact with the sintered metal layer, for example, components with various metal platings, wires, chips with metal platings, heat sinks, ceramic substrates with metal plates, lead frames with various metal platings, or lead frames formed of various metals, copper plates, and copper foils may be mentioned. In addition, when the second component 6 is a semiconductor element, the first component 5 may also be a block with thermal conductivity and electrical conductivity such as a metal wiring such as a metal frame or a metal block.
[0060] The proportion of copper in the constituent elements of the sintered metal layer of the present embodiment, excluding light elements, may be 95 mass % or more, 97 mass % or more, 98 mass % or more, or 100 mass %. When the proportion of copper in the sintered metal layer is within the above range, the formation of intermetallic compounds or the precipitation of heterogeneous elements to the grain boundaries of metallic copper crystals can be suppressed, the properties of the metallic copper constituting the sintered metal layer tend to become hard, and more excellent connection reliability tends to be obtained.
[0061] The proportion of copper element in elements other than light elements can be quantified by scanning electron microscope-energy dispersive X-ray spectroscopy (SEM-EDX) measurement of the sintered metal layer, inductively coupled plasma-optical emission spectroscopy (ICP-OES) measurement, inductively coupled plasma-mass spectroscopy (ICP-MS) measurement, etc.
[0062] The sintered copper with a flaky structure of the present embodiment can be formed by sintering a copper paste for bonding containing flaky copper particles. Among them, the flaky shape includes flat plate shapes such as plate-like and scale-like. As a flaky structure, the ratio of the major diameter to the thickness can be 5 or more. The number average diameter of the major diameter of the flaky structure can be 2 μm or more, 3 μm or more, or 4 μm or more. When the shape of the flaky structure is within this range, the reinforcing effect brought by the flaky structure contained in the sintered metal layer is improved, and the bonding strength and connection reliability of the bonded body become more excellent.
[0063] The long diameter and thickness of the flaky structure can be obtained, for example, from the SEM image of the joint body. Below, an example is given of a method for measuring the long diameter and thickness of the flaky structure from the SEM image. The joint body is injected and cured in a manner that the sample is embedded as a whole with epoxy injection molding resin. The sample is cut near the cross section to be observed by the injection molding, and the cross section is ground by grinding and CP (cross section polishing machine) processing is performed. The cross section of the sample is observed at 5000 times using an SEM device. A cross-sectional image of the joint body is obtained (for example, 5000 times). In a densely connected portion and a straight, rectangular, or ellipsoidal portion, when the maximum length of the straight line contained in the portion is taken as the long diameter, and the maximum length of the straight line orthogonal to it and contained in the portion is taken as the thickness, the length of the long diameter is 1 μm or more and the ratio of the long diameter / thickness is 4 or more, and the flaky structure is regarded as a flaky structure. Using image processing software with a measurement function, the long diameter and thickness of the flaky structure can be measured. These average values were obtained by calculating the average of more than 20 points selected at random.
[0064] Figure 3 For Figure 1 The sintered copper 1 with a thin sheet structure is enlarged. Figure 3 In the example shown, the major diameter 9 of the laminar structure is given as the distance between two parallel straight lines selected in such a way that the distance between the two parallel straight lines is maximized among the two parallel straight lines circumscribing the laminar structure. The thickness 8 of the laminar structure is given as the distance between two parallel planes selected in such a way that the distance between the two parallel planes is maximized among the two parallel planes orthogonal to the two parallel straight lines giving the major diameter and circumscribing the laminar structure.
[0065] The image processing software is not particularly limited, and for example, Microsoft PowerPoint (manufactured by Microsoft Corporation) or ImageJ (manufactured by the National Institutes of Health, USA) can be used.
[0066] The degree of orientation of the structure derived from the flaky copper particles oriented substantially parallel to the interface between the first member or the second member and the sintered metal layer can be represented by the degree of orientation order S. The degree of orientation order S can be obtained by equation (1).
[0067] S=1 / 2×(3<cos 2 θ>-1) (1)
[0068] Where θ represents the angle between the interface and the thin sheet structure, <cos 2 θ> represents multiple cos 2 The average value of θ.
[0069] The orientation order S may be greater than 0.88 and less than 1.00, or greater than 0.90 and less than 1.00, or greater than 0.92 and less than 1.00. When the orientation order S is within this range, the flaky structure contained in the sintered metal layer is oriented approximately parallel to the bonding surface, and thus the bonding strength and connection reliability of the bonded body tend to be improved.
[0070] The degree of orientation order S can be obtained, for example, from an SEM image of the conjugate. Below, an example is given of a method for obtaining the degree of orientation order S from an SEM image. The SEM cross-sectional view of the conjugate is obtained by the same method as the determination of the major diameter and thickness of the flaky structure. For the obtained cross-sectional image, an image processing software having an angle determination function is used to determine the angle between the major diameter of the flaky structure and the interface. Figure 4 Schematic cross-sectional view showing a method of measuring the angle θ of the sheet-like structure to be joined relative to the joined body of the present embodiment. Figure 4 As shown, the angle θ of 50 or more randomly selected sintered copper sheets 1 having a flaky structure relative to the bonded surface of the chip 10 is measured and substituted into the formula (1) to obtain the orientation order S. The orientation order S takes a value of 0 to 1, 1 in a completely oriented state and 0 in a completely random state.
[0071] The image processing software is not particularly limited, and for example, Microsoft PowerPoint (manufactured by Microsoft Corporation) or ImageJ (manufactured by the National Institutes of Health, USA) can be used.
[0072] The proportion of the flaky structure relative to the whole structure can be obtained by the method described in the examples described later. That is, the cross-sectional area of the joint body is obtained from the SEM image of the joint body, and the cross-sectional area of the flaky structure is obtained from the major diameter and thickness of the flaky structure measured by the method, and the total cross-sectional area of the flaky structure is divided by the cross-sectional area of the joint body, thereby the proportion of the flaky structure relative to the whole structure can be obtained. The proportion of the flaky structure relative to the whole structure of the joint body of this embodiment obtained by the above method can be 10 to 40%, or 20 to 30%.
[0073] The content (volume ratio) of copper in the sintered metal layer can be 65% by volume or more based on the volume of the sintered metal layer. When the content of copper in the sintered metal layer is within the above range, it is possible to suppress the formation of larger pores inside the sintered metal layer, and the sintered copper connecting the thin sheet structure becomes loose. Therefore, when the content of copper in the sintered metal layer is within the above range, sufficient thermal conductivity is obtained, and the bonding strength between the component and the sintered metal layer is improved, and the connection reliability of the joint body becomes excellent. The content of copper in the sintered metal layer can be 67% by volume or more, and can also be 70% by volume or more, based on the volume of the sintered metal layer. The content of copper in the sintered metal layer can be 90% by volume or less from the perspective of the difficulty of the manufacturing process, based on the volume of the sintered metal layer.
[0074] When the composition of the material constituting the sintered metal layer is clear, for example, the copper content in the sintered metal layer can be obtained by the following procedure. First, the sintered metal layer is cut into a cuboid, and the longitudinal and transverse lengths of the sintered metal layer are measured using a vernier caliper or an external shape measuring device, and the thickness is measured using a film thickness meter to calculate the volume of the sintered metal layer. The apparent density M is obtained from the volume of the cut sintered metal layer and the weight of the sintered metal layer measured using a precision balance. 1 (g / cm 3 ). Use the obtained M 1 The density of copper is 8.96 g / cm 3 The copper content (volume %) in the sintered metal layer is calculated by the following formula (2).
[0075] The copper content in the sintered metal layer (volume %) = [(M 1 ) / 8.96]×100(2)
[0076] The bonding strength of the bonded body may be 10 MPa or more, 15 MPa or more, 20 MPa or more, or 30 MPa or more. The bonding strength can be measured using a universal Bond Tester (4000 series, manufactured by DAGE) or the like.
[0077] The thermal conductivity of the sintered metal layer can be 100 W / (m·K) or more, 120 W / (m·K) or more, or 150 W / (m·K) or more, from the viewpoint of heat release and connection reliability at high temperatures. The thermal conductivity can be obtained from the thermal diffusivity, specific heat capacity and density of the sintered metal layer. For example, the thermal diffusivity of the sintered metal layer is measured by a laser flash method (LFA467, manufactured by Netch), and the thermal conductivity [W / (m·K)] of the sintered metal layer at 25°C can be obtained by multiplying the thermal diffusivity, the specific heat capacity obtained by a differential scanning calorimeter (DSC8500, manufactured by PerkinElmer), and the density obtained in the same manner as above.
[0078] In the joint body (such as electronic equipment, etc.) of the present embodiment, even when the thermal stress generated by the difference in thermal expansion coefficient between the joined components is applied to the sintered metal layer (joining layer), high connection reliability can be maintained. As the reason, it is speculated that even if thermal stress is generated, the stress is dispersed by the thin sheet structure, so stress concentration is difficult to occur. In addition, even if a part of the porous sintered copper is destroyed, the destruction is stopped by the sintered copper with a thin sheet structure, so the connection reliability of the joint body is improved. In addition, since the sintered metal layer is a composition that fully contains metal copper connected by metal bonds, it can show high thermal conductivity and can quickly release heat when installing electronic equipment with high heat generation. Furthermore, since the sintered metal layer is firmly joined by metal bonds, it can show excellent joining strength for the components containing the above metal. In this way, the sintered metal layer of the present embodiment has a very effective property for the joining of electronic equipment with high heat generation such as power supply equipment, logic circuits, amplifiers, etc. The joint body using it allows higher input power and can be operated at a higher operating temperature.
[0079] <Method for producing a bonded body>
[0080] The joint body of the present embodiment can be manufactured, for example, by the following method. As a method for manufacturing the joint body, a method having the following steps can be cited: preparing a laminated body having a first member, a copper paste for joining, and a second member in sequence on one side in the direction in which the self-weight of the first member acts, and sintering the copper paste for joining under the self-weight of the first member, or under the self-weight of the first member and a pressure of 0.01 MPa or less.
[0081] The above-mentioned laminated body can be prepared, for example, by providing a copper paste for bonding on a necessary portion of the second member and then arranging the first member on the copper paste for bonding.
[0082] As a method for setting the copper paste for bonding at a necessary part of the second member, any method can be used as long as the copper paste for bonding is deposited. As such method, for example, screen printing, transfer printing, offset printing, inkjet printing, dispenser, jet dispenser, needle dispenser, comma coater, slit coater, die coater, gravure coater, slit coating, relief printing, gravure printing, gravure printing, stencil printing, soft engraving, rod coating, applicator, particle deposition method, spray coater, spin coater, dip coater, electrodeposition coating, etc. can be used. The thickness of the copper paste for bonding can be greater than 1 μm and less than 1000 μm, greater than 10 μm and less than 500 μm, greater than 50 μm and less than 200 μm, greater than 10 μm and less than 3000 μm, greater than 15 μm and less than 500 μm, greater than 20 μm and less than 300 μm, greater than 5 μm and less than 500 μm, greater than 10 μm and less than 250 μm, or greater than 15 μm and less than 150 μm.
[0083] The copper paste for bonding provided on the second member can also be properly dried from the viewpoint of suppressing the flow and pore generation during sintering. The gas environment during drying can be in the atmosphere, in an oxygen-free environment such as nitrogen and rare gas, or in a reducing environment such as hydrogen and formic acid. The drying method can be drying by placing at room temperature, heating drying, or reduced pressure drying. For example, heating drying or reduced pressure drying can use a heating plate, a warm air dryer, a warm air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, a hot plate pressurizing device, etc. The drying temperature and time can be appropriately adjusted according to the type and amount of the dispersion medium used. As the drying temperature and time, for example, it can be dried at 50°C or more and 180°C or less for more than 1 minute and less than 120 minutes.
[0084] As a method for placing the first member on the copper paste for bonding, for example, a chip mounter, a flip chip bonder, or a carbon or ceramic positioning jig can be mentioned. In addition, the drying step can be performed after the step of placing the first member.
[0085] The copper paste for bonding is sintered by heating the laminate. Sintering is performed by heating. For example, a hot plate, a warm air dryer, a warm air heating furnace, a nitrogen dryer, an infrared dryer, an infrared heating furnace, a far infrared heating furnace, a microwave heating device, a laser heating device, an electromagnetic heating device, a heater heating device, a steam heating furnace, etc. can be used for the heating treatment.
[0086] The gas environment during sintering may be an oxygen-free environment from the viewpoint of suppressing oxidation of the sintered body, the first component, and the second component. The gas environment during sintering may also be a reducing environment from the viewpoint of removing the surface oxides of the copper particles of the copper paste for bonding. As an oxygen-free environment, for example, the introduction of oxygen-free gases such as nitrogen and rare gases or vacuum may be cited. As a reducing environment, for example, pure hydrogen gas, a mixed gas of hydrogen and nitrogen as a representative of the composition gas, nitrogen containing formic acid gas, a mixed gas of hydrogen and rare gases, and a rare gas containing formic acid gas may be cited.
[0087] The maximum temperature during the heat treatment can be 250°C to 450°C, 250°C to 400°C, or 250°C to 350°C from the viewpoint of reducing thermal damage to the first member and the second member and improving the yield. When the maximum temperature is 200°C or higher and the maximum temperature holding time is 60 minutes or less, sintering tends to proceed sufficiently.
[0088] The holding time at the maximum temperature may be 1 minute to 60 minutes, 1 minute to less than 40 minutes, or 1 minute to less than 30 minutes, from the viewpoint of completely volatilizing the dispersion medium and improving the yield.
[0089] The pressure during bonding can be a condition in which the copper content (stacking ratio) in the sintered body reaches 65% by volume or more based on the sintered body. For example, by using the copper paste for bonding described below, the sintered metal layer of the present embodiment described above can be formed even without pressurization when the stack is sintered. At this time, sufficient bonding strength can be obtained only by the deadweight generated by the first component stacked on the copper paste for bonding or in a state where it is subjected to a pressure of less than 0.01MPa, preferably less than 0.005MPa in addition to the deadweight of the first component. When the pressure received during sintering is within the above range, since no special pressurizing device is required, the porosity can be reduced, and the bonding strength and connection reliability can be further improved without damaging the yield. As a method for subjecting the copper paste for bonding to a pressure of less than 0.01MPa, for example, a method of placing a heavy object on the first component can be cited.
[0090] (Copper paste for bonding)
[0091] An example of the copper paste for bonding used in the method for producing a bonded body according to the present embodiment is shown below.
[0092] The copper paste for bonding according to the present embodiment is a copper paste for bonding containing metal particles and a dispersion medium, and the metal particles include submicron copper particles and flaky micron copper particles.
[0093] (Metal Particles)
[0094] Examples of the metal particles of the present embodiment include submicron copper particles, flaky micron copper particles, other copper particles, and other metal particles.
[0095] (Submicron copper particles)
[0096] As submicron copper particles, copper particles having a particle size of 0.12 μm or more and 0.8 μm or less can be cited, for example, copper particles having a volume average particle size of 0.12 μm or more and 0.8 μm or less can be used. When the volume average particle size of the submicron copper particles is 0.12 μm or more, it is easy to obtain the effect of suppressing the synthesis cost of the submicron copper particles, good dispersibility, and suppressing the amount of surface treatment agent used. When the volume average particle size of the submicron copper particles is 0.8 μm or less, it is easy to obtain the effect of excellent sintering of the submicron copper particles. From the viewpoint of further exerting the above-mentioned effects, the volume average particle size of the submicron copper particles can be 0.15 μm or more and 0.8 μm or less, 0.15 μm or more and 0.6 μm or less, 0.2 μm or more and 0.5 μm or less, or 0.3 μm or more and 0.45 μm or less.
[0097] In this specification, the volume average particle size refers to the 50% volume average particle size. When calculating the volume average particle size of the copper particles, it can be obtained by the following method, etc.: using a light scattering particle size distribution measuring device (for example, a Shimadzu nanoparticle size distribution measuring device (SALD-7500nano, manufactured by Shimadzu Corporation)) to measure the material obtained by dispersing the copper particles as a raw material or the dry copper particles from which the volatile components are removed from the copper paste for bonding in a dispersion medium using a dispersant. When using a light scattering particle size distribution measuring device, hexane, toluene, α-terpineol, etc. can be used as the dispersion medium.
[0098] The submicron copper particles may contain 10% by mass or more of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less. From the viewpoint of the sinterability of the copper paste for bonding, the submicron copper particles may contain 20% by mass or more, 30% by mass or more, or 100% by mass of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less. When the content ratio of copper particles having a particle size of 0.12 μm or more and 0.8 μm or less in the submicron copper particles is 20% by mass or more, the dispersibility of the copper particles is further improved, and the increase in viscosity and the decrease in paste concentration can be further suppressed.
[0099] The particle size of the copper particles can be calculated by the following method. The particle size of the copper particles can be obtained, for example, from an SEM image. A powder of the copper particles is placed on a carbon tape for SEM using a spatula to prepare a SEM sample. The SEM sample is observed at 5000 times using an SEM device. A quadrilateral of the copper particles attached to the SEM image is prepared using image processing software, and one side is used as the particle size of the particle.
[0100] The content of the submicron copper particles can be 20% to 90% by mass, 30% to 90% by mass, 35% to 85% by mass, or 40% to 80% by mass, based on the total mass of the metal particles. When the content of the submicron copper particles is within the above range, the sintered metal layer of the present embodiment described above can be easily formed.
[0101] The content of submicron copper particles is based on the sum of the mass of the submicron copper particles and the mass of the flaky micron copper particles, and can be 20% by mass or more and 90% by mass or less. When the above-mentioned content of submicron copper particles is 20% by mass or more, the flaky micron copper particles can be fully filled, and the sintered metal layer of the above-mentioned present embodiment can be easily formed. When the above-mentioned content of submicron copper particles is 90% by mass or less, the volume shrinkage during sintering of the copper paste for bonding can be fully suppressed, so it is easy to form the sintered metal layer of the above-mentioned present embodiment. From the viewpoint of further exerting the above-mentioned effect, the content of submicron copper particles is based on the sum of the mass of the submicron copper particles and the mass of the flaky micron copper particles, and can be 30% by mass or more and 85% by mass or less, and can also be 35% by mass or more and 85% by mass or less, and can also be 40% by mass or more and 80% by mass or less.
[0102] The shape of the submicron copper particles is not particularly limited. As the shape of the submicron copper particles, for example, spherical, blocky, needle-like, flaky, roughly spherical and agglomerates thereof can be cited. From the viewpoint of dispersibility and filling, the shape of the submicron copper particles can be spherical, roughly spherical, or flaky. From the viewpoint of combustibility, dispersibility, and miscibility with flaky micron particles, the submicron copper particles can also be spherical or roughly spherical.
[0103] From the viewpoint of dispersibility, filling property and miscibility with flaky micron particles, the aspect ratio of submicron copper particles may be 5 or less, or 3 or less. In this specification, "aspect ratio" means the long side / thickness of a particle. The long side and thickness of a particle can be measured, for example, from a SEM image of the particle.
[0104] Submicron copper particles can be treated with a specific surface treatment agent. Examples of specific surface treatment agents include organic acids having 8 to 16 carbon atoms. Examples of organic acids having 8 to 16 carbon atoms include octanoic acid, methylheptanoic acid, ethylhexanoic acid, propylpentanoic acid, nonanoic acid, methyloctanoic acid, ethylheptanoic acid, propylhexanoic acid, decanoic acid, methylnonanoic acid, ethyloctanoic acid, propylheptanoic acid, butylhexanoic acid, undecanoic acid, methyldecanoic acid, ethylnonanoic acid, propyloctanoic acid, butylheptanoic acid, lauric acid, methylundecanoic acid, ethyldecanoic acid, propylnonanoic acid, butyloctanoic acid, pentylheptanoic acid, tridecanoic acid, methyldodecanoic acid, ethylundecanoic acid, propyldecanoic acid, butylnonanoic acid, pentyloctanoic acid, myristic acid, methyltridecanoic acid, ethyldodecanoic acid, propylundecanoic acid, butyldecanoic acid, pentylnonanoic acid, hexyloctanoic acid, pentadecanoic acid, methyltetradecanoic acid, ethyl Saturated fatty acids such as octenyl tridecanoic acid, propyl dodecanoic acid, butyl undecanoic acid, pentyl decanoic acid, hexyl nonanoic acid, palmitic acid, methyl pentadecanoic acid, ethyl tetradecanoic acid, propyl tridecanoic acid, butyl dodecanoic acid, pentyl undecanoic acid, hexyl decanoic acid, heptyl nonanoic acid, methyl cyclohexanoic acid, ethyl cyclohexanoic acid, propyl cyclohexanoic acid, butyl cyclohexanoic acid, pentyl cyclohexanoic acid, hexyl cyclohexanoic acid, heptyl cyclohexanoic acid, octyl cyclohexanoic acid, nonyl cyclohexanoic acid; octenyl acid, nonenyl acid, methyl nonenyl acid, decenoic acid, undecenoic acid, dodecenoic acid, tridecenoic acid, tetradecenoic acid, myristic acid, pentadecenoic acid, hexadecenoic acid, palmitoleic acid, 6(Z)-hexadecenoic acid (sapienic acid The organic acid may be used alone or in combination of two or more. By combining such an organic acid with the submicron copper particles, there is a tendency to balance the dispersibility of the submicron copper particles with the leaving property of the organic acid during sintering.
[0105] The treatment amount of the surface treatment agent can be an amount of one to three molecular layers attached to the surface of the submicron copper particles. This amount can be determined by the number of molecular layers attached to the surface of the submicron copper particles (n), the specific surface area of the submicron copper particles (A p )(Unit: m 2 / g), molecular weight of the surface treatment agent (M s ) (unit: g / mol), minimum coating area of surface treatment agent (S S )(Unit: m 2 / ) and Avogadro's constant (N A )(6.02×10 23 Specifically, the treatment amount of the surface treatment agent is calculated from the treatment amount of the surface treatment agent (mass %) = {(n·A p ·M s) / (S S ·N A +n·A p ·M s )}×100% formula is used to calculate.
[0106] The specific surface area of the submicron copper particles can be determined by measuring the dried submicron copper particles using the BET specific surface area measurement method. The minimum coating area of the surface treatment agent is 2.05×10 -19 m 2 / 1 molecule. In case of other surface treatment agents, for example, they can be measured by calculation by molecular model or by the method described in "Chemistry and Education" (Kamieda Jiebo, Inafuku Jun'o, Moriyama, 40(2), 1992, p114-117). An example of a quantitative method for a surface treatment agent is shown below. The surface treatment agent can be identified by a thermally desorbed gas-gas chromatograph mass spectrometer of a dry powder after the dispersion medium is removed from the copper paste for bonding, thereby determining the carbon number and molecular weight of the surface treatment agent. The carbon content ratio of the surface treatment agent can be analyzed by carbon content analysis. As a carbon content analysis method, for example, a high-frequency induction heating furnace combustion / infrared absorption method can be cited. The surface treatment amount can be calculated by the above formula based on the carbon number, molecular weight and carbon content ratio of the identified surface treatment agent.
[0107] The treatment amount of the surface treatment agent may be 0.07% by mass or more and 2.1% by mass or less, 0.10% by mass or more and 1.6% by mass or less, or 0.2% by mass or more and 1.1% by mass or less.
[0108] Commercially available submicron copper particles can be used. Examples of commercially available submicron copper particles include CH-0200 (manufactured by Mitsui Mining & Smelting Co., Ltd., with a volume average particle size of 0.36 μm), HT-14 (manufactured by Mitsui Mining & Smelting Co., Ltd., with a volume average particle size of 0.41 μm), CT-500 (manufactured by Mitsui Mining & Smelting Co., Ltd., with a volume average particle size of 0.72 μm), and Tn-Cu100 (manufactured by Taiyo Nippon Sanso Corporation, with a volume average particle size of 0.12 μm).
[0109] (Flake-like micron copper particles)
[0110] As the flaky micron copper particles, particles containing copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more can be cited. For example, copper particles with an average maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more can be used. When the average maximum diameter and aspect ratio of the flaky micron copper particles are within the above range, the volume shrinkage during sintering of the copper paste for bonding can be sufficiently reduced, thereby facilitating the formation of the sintered metal layer of the present embodiment described above. From the viewpoint of further exerting the above effect, the average maximum diameter of the flaky micron copper particles can be 1 μm or more and 10 μm or less, or 3 μm or more and 10 μm or less. The maximum diameter and average maximum diameter of the flaky micron copper particles can be obtained, for example, from the SEM image of the particles, as the major diameter X and the average value Xav of the major diameter of the flaky structure described later.
[0111] The flaky micron copper particles may contain 50% or more of copper particles having a maximum diameter of 1 μm or more and 20 μm or less. From the viewpoint of orientation in the joint body, reinforcement effect, and filling property of the joint paste, the flaky micron copper particles may contain 70% or more, 80% or more, or 100% of copper particles having a maximum diameter of 1 μm or more and 20 μm or less. From the viewpoint of suppressing poor jointing, the flaky micron copper particles preferably do not contain particles having a size exceeding the joint thickness, such as particles having a maximum diameter exceeding 20 μm.
[0112] The method of calculating the long diameter X of the flaky micron copper particles from the SEM image is exemplified. The powder of the flaky micron copper particles is placed on the carbon tape for SEM using a spatula to prepare a SEM sample. The SEM sample is observed at 5000 times using a SEM device. A rectangular image of the flaky micron copper particles externally connected to the SEM image is made using image processing software, and the long side of the rectangle is used as the long diameter X of the particle. Using multiple SEM images, the measurement is performed on more than 50 flaky micron copper particles to obtain the average value Xav of the long diameter.
[0113] The aspect ratio of the flaky micron copper particles may be greater than 4, or greater than 6. When the aspect ratio is within the above range, the flaky micron copper particles in the bonding copper paste are oriented substantially parallel to the bonding surface, and thus the volume shrinkage during sintering of the bonding copper paste can be suppressed, thereby facilitating the formation of the sintered metal layer of the present embodiment.
[0114] The content of the flaky micron copper particles can be 1% by mass or more and 90% by mass or less, 10% by mass or more and 70% by mass or less, or 20% by mass or more and 50% by mass or less, based on the total mass of the metal particles. When the content of the flaky micron copper particles is within the above range, the sintered metal layer of the present embodiment described above can be easily formed.
[0115] The sum of the content of the submicron copper particles and the content of the flaky micron copper particles can be 80% by mass or more based on the total mass of the metal particles. When the content of the submicron copper particles and the sum of the content of the micron copper particles are within the above range, the sintered metal layer of the present embodiment described above can be easily formed. From the viewpoint of further exerting the above effect, the sum of the content of the submicron copper particles and the content of the flaky micron copper particles can be 90% by mass or more, 95% by mass or more, or 100% by mass based on the total mass of the metal particles.
[0116] There is no particular limitation on whether or not the flaky micron copper particles are treated with a surface treatment agent. From the viewpoint of dispersion stability and oxidation resistance, the flaky micron copper particles can be treated with a surface treatment agent. The surface treatment agent can be removed during bonding. Examples of such surface treatment agents include aliphatic carboxylic acids such as palmitic acid, stearic acid, arachidic acid, and oleic acid; aromatic carboxylic acids such as terephthalic acid, pyromellitic acid, and o-phenoxybenzoic acid; aliphatic alcohols such as cetyl alcohol, stearyl alcohol, isobornyl cyclohexanol, and tetraethylene glycol; aromatic alcohols such as p-phenylphenol; alkylamines such as octylamine, dodecylamine, and stearylamine; aliphatic nitriles such as stearonitrile and decanoonitrile; silane coupling agents such as alkyl alkoxysilanes; polymer treatment materials such as polyethylene glycol, polyvinyl alcohol, polyvinyl pyrrolidone, and silicone oligomers. The surface treatment agent can be used alone or in combination of two or more.
[0117] The treatment amount of the surface treatment agent can be an amount of one molecular layer or more on the particle surface. The treatment amount of this surface treatment agent varies according to the specific surface area of the flaky micron copper particles, the molecular weight of the surface treatment agent, and the minimum coating area of the surface treatment agent. The treatment amount of the surface treatment agent is usually 0.001 mass % or more. The specific surface area of the flaky micron copper particles, the molecular weight of the surface treatment agent, and the minimum coating area of the surface treatment agent can be obtained using the above method.
[0118] When the copper paste for bonding is prepared only from the above-mentioned submicron copper particles, the dispersion medium has large volume shrinkage during drying and sintering, so it is easy to peel off from the bonded surface during sintering of the copper paste for bonding, and it is difficult to obtain sufficient chip shear strength and connection reliability in the bonding of semiconductor elements, etc. By using submicron copper particles and flaky micron copper particles together, the volume shrinkage of the copper paste for bonding is suppressed during sintering, so that the sintered metal layer of the above-mentioned present embodiment can be easily formed.
[0119] In the copper paste for bonding of the present embodiment, the content of the micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 contained in the metal particles is preferably 50% by mass or less, and more preferably 30% by mass or less, based on the total amount of the flaky micron copper particles with a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more. By limiting the content of the micron copper particles with an average maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2, the flaky micron copper particles in the copper paste for bonding are easily oriented roughly parallel to the bonding surface, and the volume shrinkage during sintering of the copper paste for bonding can be more effectively suppressed. As a result, the sintered metal layer of the present embodiment described above is easily formed. From the perspective of making it easier to obtain this effect, the content of micron copper particles with an average maximum diameter of 1 μm to 20 μm and an aspect ratio of less than 2 can be 20 mass % or less, or even 10 mass % or less, based on the total amount of flaky micron copper particles with a maximum diameter of 1 μm to 20 μm and an aspect ratio of 4 or more.
[0120] As the flaky micron copper particles of the present embodiment, commercially available products can be used. As commercially available flaky micron copper particles, for example, MA-C025 (manufactured by Mitsui Mining & Smelting Co., Ltd., with an average maximum diameter of 4.1 μm), 3L3 (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd., with a volume maximum diameter of 7.3 μm), 1110F (manufactured by Mitsui Mining & Smelting Co., Ltd., with an average maximum diameter of 5.8 μm), and 2L3 (manufactured by Fukuda Metal Foil Powder Industry Co., Ltd., with an average maximum diameter of 9 μm) can be cited.
[0121] In the copper paste for bonding of the present embodiment, as the micron copper particles to be compounded, flaky micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more can be used, and the content of micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 can be used, based on the total amount of the flaky micron copper particles, and preferably 30% or less. When commercially available flaky micron copper particles are used, particles containing flaky micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of 4 or more, and the content of micron copper particles having a maximum diameter of 1 μm or more and 20 μm or less and an aspect ratio of less than 2 can be selected, based on the total amount of the flaky micron copper particles, and preferably 50% or less and 30% or less.
[0122] (Other metal particles except copper particles)
[0123] As metal particles, other metal particles other than the above-mentioned submicron copper particles and micron copper particles may be contained, for example, particles of nickel, silver, gold, palladium, platinum, etc. may be contained. The volume average particle size of other metal particles may be 0.01 μm or more and 10 μm or less, 0.01 μm or more and 5 μm or less, or 0.05 μm or more and 3 μm or less. When other metal particles are contained, their content may be less than 20% by mass, or less than 10% by mass, based on the total mass of the metal particles, from the viewpoint of obtaining sufficient bonding. Other metal particles may also be contained. The shape of other metal particles is not particularly limited.
[0124] By including metal particles other than copper particles, a sintered metal layer formed by solid solution or dispersion of multiple metals can be obtained, thereby improving the mechanical properties of the sintered metal layer such as yield stress and fatigue strength, and the connection reliability is easily improved. In addition, by adding multiple metal particles, the bonding strength and connection reliability of the formed sintered metal layer relative to a specific bonded body can be easily improved.
[0125] (Dispersion Medium)
[0126] The dispersion medium is not particularly limited and may be a volatile dispersion medium. Examples of the volatile dispersion medium include monohydric and polyhydric alcohols such as pentanol, hexanol, heptanol, octanol, decanol, ethylene glycol, diethylene glycol, propylene glycol, butanediol, α-terpineol, and isobornylcyclohexanol (MTPH); ethylene glycol butyl ether, ethylene glycol phenyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, diethylene glycol isobutyl ether, diethylene glycol hexyl ether, triethylene glycol methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, diethylene glycol isopropyl methyl ether, triethylene glycol dimethyl ether, triethylene glycol butyl methyl ether, propylene glycol propyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ...methyl ether, dipropylene glycol ethyl ether, dipropylene glycol methyl ether, dipropylene glycol methyl Ethers such as alcohol propyl ether, dipropylene glycol butyl ether, dipropylene glycol dimethyl ether, tripropylene glycol methyl ether, and tripropylene glycol dimethyl ether; esters such as ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, dipropylene glycol methyl ether acetate (DPMA), ethyl lactate, butyl lactate, γ-butyrolactone, and propylene carbonate; amides such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide; aliphatic hydrocarbons such as cyclohexanone, octane, nonane, decane, and undecane; aromatic hydrocarbons such as benzene, toluene, and xylene; thiols having an alkyl group with a carbon number of 1 to 18; thiols having a cycloalkyl group with a carbon number of 5 to 7. Examples of the mercaptans having an alkyl group having 1 to 18 carbon atoms include ethyl mercaptan, n-propyl mercaptan, isopropyl mercaptan, n-butyl mercaptan, isobutyl mercaptan, tert-butyl mercaptan, pentyl mercaptan, hexyl mercaptan, and dodecyl mercaptan. Examples of the mercaptans having a cycloalkyl group having 5 to 7 carbon atoms include cyclopentyl mercaptan, cyclohexyl mercaptan, and cycloheptyl mercaptan.
[0127] The content of the dispersion medium may be 5 to 50 parts by mass based on 100 parts by mass of the total mass of the metal particles. When the content of the dispersion medium is within the above range, the copper paste for bonding can be adjusted to a more appropriate viscosity and the sintering of the copper particles is less likely to be inhibited.
[0128] (additive)
[0129] The copper paste for bonding may further contain, as required, a wettability enhancer such as a nonionic surfactant or a fluorine-based surfactant, a defoamer such as silicone oil, an ion scavenger such as an inorganic ion exchanger, or the like.
[0130] (Preparation of copper paste for bonding)
[0131] The copper paste for bonding can be prepared by mixing the above-mentioned submicron copper particles, micron copper particles, other metal particles and any additives in a dispersion medium. It can also be stirred after the components are mixed. The copper paste for bonding can adjust the maximum particle size of the dispersion by a classification operation.
[0132] The copper paste for bonding can be prepared by mixing submicron copper particles, a surface treatment agent, and a dispersion medium in advance, performing a dispersion treatment, preparing a dispersion of submicron copper particles, and then mixing micron copper particles, other metal particles, and any additives. Through this sequence, the dispersibility of submicron copper particles is improved, the miscibility with micron copper particles is improved, and the performance of the copper paste for bonding is further improved. Agglomerates in the dispersion of submicron copper particles can also be removed by a classification operation.
[0133] <Semiconductor device and method for manufacturing semiconductor device>
[0134] The semiconductor device of this embodiment comprises a first component, a second component, and a sintered metal layer joining the first component and the second component, wherein at least one of the first component and the second component is a semiconductor element, wherein the sintered metal layer has a prescribed orientation structure, and the copper content in the sintered metal layer is greater than 65 volume % based on the volume of the sintered metal layer.
[0135] As semiconductor elements, there can be cited power supply components formed by diodes, rectifiers, thyristors, MOS gate drivers, power switches, power MOSFETs, IGBTs, Schottky diodes, fast recovery diodes, etc., signal transmitters, amplifiers, LED components, etc. As components other than semiconductor elements, there can be cited semiconductor element mounting substrates such as lead frames, ceramic substrates with metal plates (such as DBC), LED packages, copper tapes, metal blocks, terminals, etc., power supply components, heat dissipation plates, water cooling plates, etc.
[0136] The sintered metal layer of the present embodiment may be the same as the sintered metal layer in the bonded body of the present embodiment described above.
[0137] From the perspective of subsequent process adaptability and connection reliability, the semiconductor device of this embodiment can have a chip shear strength of 10 MPa or more, 15 MPa or more, 20 MPa or more, or 30 MPa or more. The chip shear strength can be measured using a universal Bond Tester (4000 series, manufactured by DAGE) or the like.
[0138] Figure 5 This is a schematic cross-sectional view showing an example of a semiconductor device according to this embodiment. Figure 5 The semiconductor device 110 shown is formed by a semiconductor element 14 connected to a lead frame 11a via a sintered metal layer 4 and a mold resin 13 molded therein. The semiconductor element 14 is connected to the lead frame 11b via a wire 12.
[0139] As the semiconductor device of this embodiment, for example, there can be listed power supply components formed by diodes, rectifiers, thyristors, MOS gate drivers, power switches, power MOSFETs, IGBTs, Schottky diodes, fast recovery diodes, etc., signal transmitters, amplifiers, high-brightness LED components, sensors, etc.
[0140] The semiconductor device of this embodiment achieves high connection reliability when operating at high temperatures, improves heat dissipation due to high thermal conductivity, and high electrical conductivity, and can be preferably used in semiconductor devices using high heat dissipation semiconductor elements, semiconductor devices operating in high temperature environments, etc.
[0141] The semiconductor device can be manufactured in the same manner as the manufacturing method of the bonded body. That is, a method including the following steps is provided: preparing a laminated body having a first member, a bonding copper paste and a second member in sequence on one side of the direction in which the self-weight of the first member acts, at least one of the first member and the second member being a semiconductor element, and sintering the bonding copper paste under the self-weight of the first member or under the self-weight of the first member and a pressure of 0.01 MPa or less.
[0142] The above method can reduce the damage to the semiconductor element when a metal wiring or a bulk is bonded to the semiconductor element as the first member when the second member is a semiconductor element. A semiconductor device in which a metal wiring or a bulk is bonded to a semiconductor element is described below.
[0143] As an embodiment of the semiconductor device, there can be cited a device comprising a first electrode, a semiconductor element electrically connected to the first electrode, and a second electrode electrically connected to the semiconductor element via a metal wiring, and having a copper-containing sintered metal layer between the semiconductor element and the metal wiring, and between the metal wiring and the second electrode.
[0144] Figure 6 It is a schematic cross-sectional view showing an example of the above-mentioned semiconductor device. Figure 6The semiconductor device 200 shown in the figure includes an insulating substrate 21 having a first electrode 22 and a second electrode 24, a semiconductor element 23 bonded to the first electrode 22 via a sintered metal layer 4, and a metal wiring 25 electrically connecting the semiconductor element 23 and the second electrode 24. The metal wiring 25 and the semiconductor element 23, and the metal wiring 25 and the second electrode 24 are bonded respectively via the sintered metal layer 4. In addition, the semiconductor element 23 is connected to the third electrode 26 via a wire 27. The semiconductor device 200 includes a copper plate 28 on the side of the insulating substrate 21 opposite to the surface on which the above-mentioned electrodes and the like are mounted. The above-mentioned structure of the semiconductor device 200 is sealed by an insulator 29. The semiconductor device 200 has one semiconductor element 23 on the first electrode 22, and may also have two or more. In this case, the plurality of semiconductor elements 23 may be bonded to the metal wiring 25 via the sintered metal layer 4, respectively.
[0145] Figure 7 It is a schematic cross-sectional view showing another example of a semiconductor device. Figure 7 The semiconductor device 210 shown in the figure has a block 30 between the semiconductor element 23 and the metal wiring 25. The semiconductor element 23 and the block 30, and the block 30 and the metal wiring 25 are respectively bonded by a sintered metal layer 4. Figure 6 The structure is the same as that of the semiconductor device 200 shown in FIG.
[0146] Figure 8 It is a schematic cross-sectional view showing another example of a semiconductor device. Figure 8 The semiconductor device 220 shown in the figure further has a semiconductor element 23 and a block 30 on the first electrode 22 and a sintered metal layer 4 connecting them. Figure 7 The semiconductor device 220 has the same structure as the semiconductor device 210 shown in the figure. The semiconductor device 220 has two semiconductor elements on the first electrode 22, and can also have three or more. In this case, the three or more semiconductor elements 23 can be respectively connected to the metal wiring 25 through the block 30 through the sintered metal layer 4. Among them, the position of the block 30 can be appropriately changed, for example, it can be set between the first electrode 22 and the semiconductor element 23.
[0147] Examples of the insulating substrate 21 include ceramics such as alumina, aluminum nitride, and silicon nitride, highly thermally conductive particle / resin composites, polyimide resins, and polymaleimide resins.
[0148] Examples of the metals constituting the first electrode 22, the second electrode 24, and the third electrode 26 include copper, nickel, silver, gold, palladium, platinum, lead, tin, and cobalt. These metals may be used alone or in combination of two or more. In addition, the electrode may have an alloy containing the above-mentioned metals on the surface in contact with the sintered metal layer 4. Examples of the metals used in the alloy include zinc, manganese, aluminum, beryllium, titanium, chromium, iron, and molybdenum in addition to the above-mentioned metals.
[0149] As metal wiring, there can be mentioned metal frames having shapes such as strips, plates, cubes, cylinders, L-shaped, U-shaped, and E-shaped. As materials for metal wiring, there can be mentioned, for example, silver, copper, iron, aluminum, molybdenum, tungsten, tantalum, niobium, or alloys thereof. For oxidation resistance and adhesion, the surfaces of these metal wirings can also be coated with nickel, copper, gold, silver, etc. by plating, sputtering, etc. In addition, the width of the metal wiring can be 1 μm to 30 μm, and the thickness can be 20 μm to 5 mm.
[0150] As the block, those with excellent thermal conductivity and electrical conductivity are preferred, for example, silver, copper, iron, aluminum, molybdenum, tungsten, tantalum, niobium, or alloys thereof can be used. On the surface of the block, nickel, copper, gold, silver, etc. can also be coated by plating, sputtering, etc. for oxidation resistance and adhesion. By arranging the block on the semiconductor element, the heat release is further improved. The number of blocks can be appropriately changed.
[0151] Examples of the insulator 29 include silicone rubber, polymaleimide resin, polyimide resin, and polyamide-imide resin.
[0152] The sintered metal layer 4 is formed by sintering the above-mentioned copper paste for bonding. The sintered metal layer 4 is in contact with the metal wiring 25 and contains a structure derived from flaky copper particles oriented approximately parallel to the interface with the metal wiring 25. The content of copper in the sintered metal layer 4 can be 65% by volume or more based on the volume of the sintered metal layer. In addition, when the sintered metal layer 4 is in contact with the first electrode, the second electrode, the semiconductor element or the bulk, the sintered metal layer 4 contains a structure derived from flaky copper particles oriented approximately parallel to the interface with the first electrode, the second electrode, the semiconductor element or the bulk. The content of copper in the sintered metal layer 4 can be 65% by volume or more based on the volume of the sintered metal layer.
[0153] Figures 6 to 8 The semiconductor device shown can be used in a power supply unit that has a large capacity and is required to have high reliability.
[0154] Figures 6 to 8The semiconductor device shown can be manufactured, for example, by a method comprising the following steps: preparing an insulating substrate comprising a first electrode and a second electrode, arranging a bonding copper paste, a semiconductor element, a bonding copper paste as required, a block, and a bonding copper paste on the first electrode in sequence from the first electrode side, arranging a bonding copper paste on the second electrode, and arranging metal wiring on the bonding copper paste on the semiconductor element or the block and the bonding copper paste on the second electrode in a manner that connects these bonding copper pastes; and a step of sintering the bonding copper paste under the self-weight of each component or under the self-weight of each component and a pressure of less than 0.01 MPa.
[0155] According to such a manufacturing method, a semiconductor device can be manufactured without applying pressure, so bonding can be performed without deforming the metal wiring having a bridge portion, and even when a component having a smaller bonding area than the semiconductor element is bonded to the semiconductor element, damage to the semiconductor element can be further reduced.
[0156] Fig. 9 It is a schematic cross-sectional view showing still another example of a semiconductor device. Fig. 9 The semiconductor device 300 shown in the figure includes a first electrode 22, a semiconductor element 23 bonded to the first electrode 22 via a sintered metal layer 4, and a metal wiring 25 electrically connecting the semiconductor element 23 to a second electrode 24. The metal wiring 25 and the semiconductor element 23, and the metal wiring 25 and the second electrode 24 are bonded to each other via the sintered metal layer 4. In addition, the semiconductor element 23 is connected to the third electrode 26 via a wire 27. The above-mentioned structure of the semiconductor device 300 is sealed by a sealing material 31. The semiconductor device 300 has one semiconductor element 23 on the first electrode 22, and may have two or more. In this case, the plurality of semiconductor elements 23 can be bonded to the metal wiring 25 via the sintered metal layer 4, respectively.
[0157] Fig.10 It is a schematic cross-sectional view showing another example of a semiconductor device. Fig.10 The semiconductor device 310 shown in the figure has a block 30 between the semiconductor element 23 and the metal wiring 25. The semiconductor element 23 and the block 30, and the block 30 and the metal wiring 25 are respectively bonded by a sintered metal layer 4. Fig. 9 The semiconductor device 300 shown in FIG. 1 has the same structure. However, the position of the block 30 can be changed as appropriate, and for example, the block 30 can be provided between the first electrode 22 and the semiconductor element 23 .
[0158] Fig.11 It is a schematic cross-sectional view showing another example of a semiconductor device. Fig.11The semiconductor device 320 shown in the figure further includes a semiconductor element 23 and a block 30 on the first electrode 22, and a sintered metal layer 4 connecting them. Fig.10 The semiconductor device 320 has the same structure as the semiconductor device 310 shown in FIG. The semiconductor device 320 has two semiconductor elements on the first electrode 22, and may also have three or more semiconductor elements. In this case, the three or more semiconductor elements 23 can be respectively connected to the metal wiring 25 through the block 30 and the sintered metal layer 4. The position of the block 30 can be appropriately changed, for example, it can be set between the first electrode 22 and the semiconductor element 23.
[0159] Figures 9-11 The first electrode 22 and the second electrode 24 shown may be a lead frame, a copper plate, a copper-molybdenum sintered body, or the like.
[0160] Examples of the sealing material 31 include heat-resistant solid sealing materials and highly thermally conductive composite materials.
[0161] The sintered metal layer 4 may be the same as that described in connection with the semiconductor devices 200 to 220 .
[0162] Figures 9-11 The semiconductor device of the embodiment shown can be used for a miniaturized power supply module by using a lead frame or the like as the first electrode and the second electrode. This semiconductor device can be manufactured in the same manner as the above-mentioned method for manufacturing the semiconductor device.
[0163] Furthermore, another embodiment of a semiconductor device having a structure in which a bulk body is bonded to a semiconductor element will be described.
[0164] The semiconductor device may include a first heat conducting member, a second heat conducting member, and a semiconductor element disposed between the first heat conducting member and the second heat conducting member, wherein a sintered metal layer containing copper is provided between at least one of the first heat conducting member and the semiconductor element and between the semiconductor element and the second heat conducting member.
[0165] Fig.12 It is a schematic cross-sectional view showing an example of this embodiment. Fig.12The semiconductor device 400 shown has a first heat-conducting member 32, a semiconductor element 23 bonded to the first heat-conducting member 32 via a sintered metal layer 4, a block 30 bonded to the semiconductor element 23 via a sintered metal layer 4, and a second heat-conducting member 33 bonded to the block 30 via a sintered metal layer 4. The semiconductor element 23 is connected to an electrode 34 via a wire 35. The first heat-conducting member 32 and the second heat-conducting member of the semiconductor device 400 are sealed by a sealing material 31. The semiconductor device 400 has two semiconductor elements, or may have one or more than three, and the number of blocks may also be appropriately changed. Among them, the position of the block 30 may be appropriately changed, for example, it may be set between the first electrode 22 and the semiconductor element 23.
[0166] The heat conducting member has both the function of releasing the heat generated by the semiconductor element 23 to the outside and the function of serving as an electrode for electrically connecting the semiconductor element to the outside. For example, copper, aluminum, or an alloy thereof is used for such a heat conducting member.
[0167] The sintered metal layer 4 is formed by sintering the above-mentioned copper paste for bonding. The sintered metal layer 4 is in contact with the first heat conducting member 32 or the second heat conducting member 33, and contains a structure derived from flaky copper particles oriented approximately parallel to the interface with the first heat conducting member 32 or the second heat conducting member 33, and the content of copper in the sintered metal layer 4 can be 65 volume % or more based on the volume of the sintered metal layer. In addition, when the sintered metal layer 4 is in contact with the semiconductor element or the block, the sintered metal layer 4 contains a structure derived from flaky copper particles oriented approximately parallel to the interface with the semiconductor element or the block, and the content of copper in the sintered metal layer 4 can be 65 volume % or more based on the volume of the sintered metal layer.
[0168] Fig.12 The semiconductor device shown can have a double-sided cooling structure with excellent heat dissipation by having heat-conducting members on both sides of the semiconductor element. Such a semiconductor device can be manufactured by a method comprising the following steps: preparing a stacked body in which a copper paste for bonding, a semiconductor element, a copper paste for bonding, a block, a copper paste for bonding, and a second heat-conducting member are sequentially stacked on a first heat-conducting member from the first heat-conducting member side, and sintering the copper paste for bonding under the self-weight of each member or under the self-weight of each member and a pressure of 0.01 MPa or less. The stacked body can also be stacked in the reverse order to the above.
[0169] Example
[0170] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to the following examples.
[0171] <Measurement conditions>
[0172] (1) Determination of chip shear strength
[0173] On the copper plate (19×25×3mm 3 ) is placed on a stainless steel plate with a thickness of 70 μm and a metal mask with 3 rows and 3 columns of 3×3 mm square openings is applied using a metal scraper by stencil printing. On the applied copper paste for bonding is placed a titanium, nickel, 3×3 mm 2 A silicon chip (chip thickness: 600μm) with nickel on the surface to be bonded is gently pressed with small tweezers. It is installed in a tube furnace (manufactured by AVC Co., Ltd.), and argon gas flows in at 1L / min to replace the air with argon gas. After that, while hydrogen gas flows in at 300ml / min, the temperature is raised for 10 minutes, and sintering treatment is performed at 350℃ for 10 minutes to obtain a bonded body in which the copper plate and the silicon chip are bonded by a sintered metal layer. After that, the argon gas is replaced with 0.3L / min for cooling, and the bonded body is taken out into the air below 50℃.
[0174] The bonding strength of the bonded body was evaluated by die shear strength. Use a 1kN load cell. Energy Bond Tester (4000 series, manufactured by DAGE) was used to measure the silicon chip at a measuring speed of 500 μm / s and a measuring height of 100 μm. The die shear strength of the bonded body was measured by pressing in the horizontal direction. The average value of the measured values of 8 bonded bodies was calculated as Chip shear strength .
[0175] (2) Copper content in sintered metal layer (volume ratio)
[0176] A 15×15 mm thick Teflon (registered trademark) plate was set 2 Opening. Place the Teflon (registered trademark) plate on a glass plate, fill the opening with copper paste for bonding, and use a metal scraper to remove the copper paste overflowing from the opening. Remove the Teflon (registered trademark) plate, install it in a tube furnace, and heat it to 150°C while flowing argon gas at 0.3L / min. Keep it for 1 hour to remove the solvent. In this state, replace the gas with hydrogen at 300mL / min, raise the temperature to 350°C, and sinter for 60 minutes to obtain a sintered metal layer. Thereafter, replace the argon gas with 0.3L / min and cool it, and take the sintered metal layer out into the air at below 50°C. Peel off the plate-shaped sintered metal layer from the glass plate and grind it with sandpaper (No. 800) to obtain a 10×10mm 2 The plate sample is a flat plate sample with a size of . The length, width and thickness of the plate sample are measured, and the weight of the plate sample is measured. The density of the plate sample is calculated from these values, and the volume ratio of the metal copper is calculated using the following formula.
[0177] Copper content in the sintered metal layer (volume %) = density of the plate sample (g / cm 3 ) / 8.96(g / cm3 )×100(%)
[0178] (3) Cross-sectional morphological observation
[0179] The conjugate is fixed in a cup using a sample clamp (Samplklip I, Buehler), and epoxy injection resin (Epomatt, Refinetec Co., Ltd.) is flowed around until the entire sample is embedded, and the sample is left to stand in a vacuum dryer and decompressed for 1 minute for degassing. After that, the epoxy injection resin is cured at room temperature for 10 hours to prepare the sample. The sample is cut near the silicon chip using a Refinery Sol Esser (Refinetec Co., Ltd.). A grinding device (Refine Polisher Hv, Refinetec Co., Ltd.) with water-resistant grinding paper (Carbon Mac Paper, Refinetec Co., Ltd.) is used to grind to the vicinity of the center of the conjugate and produce a cross section. For the ground sample, the excess epoxy injection resin is shaved off to make a size that can be processed with an ion grinding device. An ion milling device (IM4000, manufactured by Hitachi High-Technologies Co., Ltd.) was used in the CP processing mode with an argon gas flow rate of 0.07 to 0.1 cm 3 The sample processed by size was cross-sectioned under the conditions of 1000 nm / min and 120 minutes of processing time to prepare a SEM sample. The cross section of the sintered metal layer of the SEM sample was observed with a SEM-EDX device (ESEM XL30, manufactured by Philips) at an applied voltage of 15 kV.
[0180] (4) Calculation of orientation order
[0181] The 3000-fold SEM image obtained in "(3) Cross-sectional morphological observation" is read using Image J (manufactured by the National Institutes of Health, USA). As the SEM image, an image of the bonding interface between the substrate or silicon chip and the sintered metal layer is used. Press the [T] key to display the ROI Manager window, and check the Show All check box. Select Straight Line from the main window. The longest length of the straight line contained in the linear, rectangular, or ellipsoidal part of the dense continuous part on the image is taken as the major axis; when the longest length of the straight line orthogonal to it and contained in the part is taken as the thickness, the case where the length of the major axis is greater than 1 μm and the ratio of the major axis / thickness is greater than 4 is determined to be a thin sheet structure. Click → drag a line from one end of the cross section of the thin sheet structure to the other end, and press the [T] key to log in to the ROI Manager window. Repeat this operation without repetition for the entire thin sheet structure on the screen. Among them, the thin sheet structure whose image is truncated when viewed from the end of the screen is not selected. Next, press the Measure button in the ROI Manager window. Since the measured angles are displayed in the Results window, use [File] → [Save As] to save them in a file. When the interface with the substrate or silicon chip is not horizontal relative to the image, measure its angle in the same way. Use Microsoft Excel to read the file storing the results. When the interface between the substrate or silicon chip and the sintered metal layer is not horizontal relative to the image, subtract the angle of the interface from the measured angles. For each angle θ, calculate cos 2 θ, find its average value <cos 2 θ>, substitute into S=1 / 2×(3<cos 2 θ>-1), calculate the orientation order S.
[0182] When S was 0.83 or more, it was determined as “existent” that the flaky structure was oriented substantially parallel to the interface between the member and the sintered metal layer.
[0183] (5) Calculation of the ratio of the major axis to the thickness of a thin sheet structure
[0184] Use Image J (manufactured by the National Institutes of Health, USA) to read the 5000x SEM image obtained in "Cross-sectional Morphology Observation". Select Straight Line from the main window. Draw a straight line from one end to the other of the scale at the bottom of the image (in this example, the scale represents 5μm) by clicking → dragging. Select [Analyze] → [Set Scale] from the main window to display the Set Scale window. Enter "5" in the Known Distance: box and "μm" in the Unit of length: box, and click the [OK] button. Press the [T] key to display the ROI Manager window, and select the check box for Show All. Determine the lamellar structure using the same method as (4). Draw a line from one end of the cross section of the lamellar structure on the image to the other end by clicking → dragging. Press the [T] key to log in to the ROI Manager window. Repeat this operation for the entire lamellar structure on the screen without duplication. However, do not select the lamellar structure whose image is cut off when viewed from the end of the screen. Next, press the Measure button in the ROI Manager window. Since the measured length is displayed in the Results window, use [File] → [Save As] to save it in a file. Similarly, measure the thickness direction length of the cross section of the thin-sheet structure on the image and save it in a file. Use Microsoft Excel to read the stored file and calculate the average value of the length measurement results. In this way, the average long diameter of the thin-sheet structure and the average thickness of the thin-sheet structure are obtained. Furthermore, the average long diameter of the thin-sheet structure is divided by the average thickness of the plate-like structure to obtain the "ratio of the number average length in the long axis direction of the thin-sheet structure to the number average length in the thickness direction".
[0185] (6) Ratio of copper in elements other than light elements
[0186] The SEM sample obtained in "(3) Cross-sectional morphological observation" is mounted in a SEM-EDX device, and the field of view is set within a working distance of 10 mm, at Spot: 4, an applied voltage of 15 kV, and 5000 times so that the entire screen becomes a sintered metal layer, and the focus is aligned. Enigma correction is performed as needed. Start the EDX measurement program "EDX Control", press the integration key, and perform integration for 5 minutes. The spectrum obtained in the measurement program is identified (automatically). At this time, the peaks of light elements (Li, Be, B, C, N, O) are excluded from the detection objects. Furthermore, a baseline is set (automatically), and then the composition ratio is calculated, and the composition ratio of each component is quantified so that the proportion of copper is "the proportion of copper elements in elements other than light elements".
[0187] (7) Thermal conductivity
[0188] The thermal diffusivity of the plate-shaped sample prepared in "(2) Volume ratio of metallic copper" was measured by a laser flash method (LFA467, manufactured by Netch). The thermal conductivity [W / (m·K)] of the silver sintered body at 25°C was determined by the product of the thermal diffusivity, the specific heat capacity obtained by a differential scanning calorimeter (DSC8500, manufactured by PerkinElmer), and the density determined in "(2) Volume ratio of metallic copper".
[0189] (8) Temperature cycle connection reliability test
[0190] The same method as in "(1) Die shear strength" was performed to obtain a copper plate (19×25×3 mm 3 ) and 4×8mm 2 A bonded body is prepared by bonding a silicon chip (chip thickness: 600 μm) whose bonding surface is nickel. After applying an adhesion improving material (HIMAL, manufactured by Hitachi Chemical Co., Ltd.) on the bonded body and drying it, it is sealed with a solid sealing material (CEL, manufactured by Hitachi Chemical Co., Ltd.) to obtain a temperature cycle test piece. The temperature cycle test piece is installed in a temperature cycle tester (TSA-72SE-W, manufactured by Espec Co., Ltd.), and a temperature cycle connection reliability test is carried out under the conditions of low temperature side: -40°C, 15 minutes, room temperature: 2 minutes, high temperature side: 200°C, 15 minutes, defrost cycle: automatic, number of cycles: 1000 cycles. Using an ultrasonic flaw detector (Insight-300, manufactured by Insight Co., Ltd.), a SAT image of the bonding state of the interface between the sintered metal layer and the substrate or chip before and after the temperature cycle connection reliability test is obtained to study whether there is peeling. When the peeling area of the bonded portion was less than 20% by area, it was rated as good (○); when it was 20% by area or more, it was rated as bad (×).
[0191] (9) Determination of the content ratio of flaky structures in the bonded body
[0192] Use Image J to read the same SEM image as the user in (5), and select [Image] → [Type] → [RGB color]. Next, use [Image] → [Adjust] → [Color Threshold] to call the Threshold Color window. In the Brightness curve of the Threshold Color window, align the lower limit of the brightness with the inflection point on the dark side of the distribution curve and the upper limit with the position of 100% on the light side. Then, press [Select] in the Threshold Color window to select the metal sintered body part in the SEM image. In this state, press [Analyze] → [Measure] to calculate the cross-sectional area of the sintered body part. On the other hand, multiply the major diameter and thickness of the thin-plate structure identified in (5) and sum them to calculate the cross-sectional area of the thin-plate structure part. The content ratio (%) of the thin-plate structure in the entire joint body is calculated by the formula {(cross-sectional area of the thin-plate structure part) / (cross-sectional area of the sintered body part)}×100.
[0193] (Example 1)
[0194] 5.2 g of α-terpineol (manufactured by Wako Pure Chemical Industries, Ltd.) and 6.8 g of isobornylcyclohexanol (MTPH, manufactured by Nippon Terpene Chemical Co., Ltd.) as a dispersion medium and 52.8 g of CH0200 (manufactured by Mitsui Mining and Smelting Co., Ltd., with a content of copper particles of 0.12 μm or more and 0.8 μm or less of 95% by mass) as submicron copper particles were mixed in a plastic bottle, and an ultrasonic homogenizer (US-600, manufactured by Nippon Seiki Co., Ltd.) was used to perform a treatment at 19.6 kHz, 600 W, and 1 minute to obtain a dispersion liquid. 35.2 g of MA-C025 (manufactured by Mitsui Mining and Smelting Co., Ltd., with a content of copper particles of 1 μm or more and 20 μm or less in maximum diameter of 100% by mass) as flaky micron copper particles was added to the dispersion liquid, and the mixture was stirred with a spatula until the dry powder disappeared. The plastic bottle was sealed and stirred at 2000 rpm for 2 minutes using a rotation-revolution type stirring device (Planetary Vacuum Mixer ARV-310, manufactured by Shinkey Co., Ltd.), and stirred at 2000 rpm for 2 minutes under reduced pressure to obtain a copper paste for bonding. Using this copper paste for bonding, a bonded body was prepared, and various measurements and analyses were performed.
[0195] (Examples 2 and 3)
[0196] Copper pastes for bonding were obtained in the same manner as in Example 1 except that the input amounts described in Table 1 were used. Using these copper pastes for bonding, bonded bodies were prepared, and various measurements and analyses were performed.
[0197] (Example 4)
[0198] A copper paste for bonding was obtained in the same manner as in Example 1 except that 35.2 g of 3L3 (manufactured by Fukuda Metal Foil Co., Ltd., with a content of copper particles having a maximum diameter of 1 μm or more and 20 μm or less) as flaky micron copper particles was used instead of MA-C025 as flaky micron copper particles. A bonded body was prepared using the copper paste for bonding, and various measurements and analyses were performed.
[0199] (Example 5)
[0200] A copper paste for bonding was obtained in the same manner as in Example 1 except that 35.2 g of 1110F (manufactured by Mitsui Mining & Smelting Co., Ltd., with a content of copper particles having a maximum diameter of 1 μm or more and 20 μm or less, being 100% by mass) as flaky micron copper particles was used instead of MA-C025 as flaky micron copper particles. A bonded body was prepared using the copper paste for bonding, and various measurements and analyses were performed.
[0201] (Example 6)
[0202] The same copper paste as in Example 4 was used as the bonding copper paste. Titanium, nickel, and gold were used to form the bonding paste in this order. 2 A bonded body was made of a silicon chip (chip thickness: 600 μm) with a gold surface, and "(1) Measurement of chip shear strength" was performed. 2 A silicon chip (chip thickness: 600 μm) whose bonding surface was gold was subjected to "(8) Temperature cycle connection reliability test".
[0203] (Example 7)
[0204] The same copper paste as in Example 4 was used as the bonding copper paste. Titanium, nickel, and silver were used to form the bonding paste in this order. 2 A bonded body was made of a silicon chip (chip thickness: 600 μm) with a gold surface, and "(1) Measurement of chip shear strength" was performed. 2 A silicon chip (chip thickness: 600 μm) whose bonding surface was silver was subjected to “(8) Temperature cycle connection reliability test”.
[0205] (Comparative Example 1)
[0206] A copper paste for bonding was obtained in the same manner as in Example 1 except that 35.2 g of Cu-HWQ3 μm (atomized powder, manufactured by Fukuda Metal Foil Powder Co., Ltd.) as pseudo-spherical particles was used as copper particles instead of MA-C025 as flaky micron copper particles. A bonded body was prepared using the copper paste for bonding, and various measurements and analyses were performed.
[0207] (Comparative Examples 2 to 5)
[0208] Copper pastes for bonding were obtained in the same manner as in Example 1 except for the composition described in Table 2. Using these copper pastes for bonding, bonded bodies were prepared, and various measurements and analyses were performed.
[0209] (Comparative Example 6)
[0210] A copper paste for bonding was obtained in the same manner as in Example 1 except that 52.8 g of spherical copper particles CS-10 (50% volume average particle size 1 μm, manufactured by Mitsui Mining & Smelting Co., Ltd.) were used instead of CH0200 as copper particles. A bonded body was prepared using the copper paste for bonding, and various measurements and analyses were performed.
[0211] (Comparative Example 7)
[0212] A copper paste for joining was obtained by adding 0.88 mass % of acetic acid (0.88 g) to the copper paste for joining of Example 1. A joined body was prepared using the copper paste for joining, and various measurements and analyses were performed.
[0213] (Comparative Example 8)
[0214] A copper paste for bonding was obtained in the same manner as in Example 1 except that 26.4 g of copper oxide particles (synthetic product) and 26.4 g of CHO200 were used instead of 52.8 g of CHO200 as copper particles. A bonded body was prepared using the copper paste for bonding, and various measurements and analyses were performed.
[0215] (Comparative Example 9)
[0216] A 100 μm thick sheet of high temperature lead solder (93.5Pb5Sn1.5Ag, manufactured by Senju Metal Industries, Ltd.) was cut into 3×3 mm 2 Size. On copper plate (19×25×3mm 3 ) is placed on a 3.5×3.5mm 2 The open carbon fixture is used to successively place the cut high temperature lead solder and 3×3mm 2 A silicon chip (chip thickness: 600μm) with a nickel surface to be bonded is installed in the opening of the carbon fixture. In a hydrogen oven, the copper plate and the silicon chip are heated under the conditions of a maximum temperature of 350°C in a hydrogen atmosphere, and a bonding sample is obtained by bonding the copper plate and the silicon chip with high-temperature lead solder. Various measurements and analyses are performed using this bonding sample.
[0217] (Comparative Example 10)
[0218] LM1 (Tokusen Kogyo Co., Ltd.) 75 g and AgC239 (Fukuda Metal Foil Powder Co., Ltd.) 25 g as silver particles, terpineol (Wako Pure Chemical Industries, Ltd.) 13.6 g as a dispersion medium, and stearic acid (Shin Nippon Rika Co., Ltd.) 1 g as an additive were weighed and mixed, and kneaded for 15 minutes using a Raikai machine to prepare a silver paste for bonding. The sintering treatment conditions were kept on a hot plate heated to 110° C. in air for 10 minutes and on a hot plate heated to 200° C. for 60 minutes to prepare a sintered silver bonding sample, and various measurements and analyses were performed.
[0219] The compositions of the bonding pastes prepared in Examples and Comparative Examples are shown in Tables 1 and 2. In addition, Tables 3 and 4 show the measurement results of Examples and Comparative Examples.
[0220]
[0221]
[0222]
[0223]
[0224] As shown in the results of the examples, when the sintered metal layer has a flaky structure and the copper content in the sintered metal layer is 65 volume % or more, the bonded body has excellent thermal conductivity, die shear strength, and connection reliability. Fig.13 and Fig.14 The SEM images of the joint bodies of Example 1 and Example 4 are shown. It can be seen that in the joint body of the example, in the copper sintered body, the gaps between the sintered copper 1 having a plurality of thin sheet structures oriented approximately parallel to the chip 15 or 16 are densely filled with the sintered copper 2 derived from the copper particles. In the example, the sintered metal layer has a thin sheet structure, which disperses the stress concentration, and the copper particles are firmly and densely bonded, so that a joint body with excellent chip shear strength is obtained.
[0225] On the other hand, the bonded body of the comparative example was inferior in thermal conductivity, die shear strength, or connection reliability. Figure 15 to Figure 18 The SEM images of the joint bodies of Comparative Examples 3 and Comparative Examples 6 to 8 are shown. From these results, it can be seen that when the copper content in the sintered metal layer is low, the number of voids 3 increases, the bonding between the sintered copper 1 having a thin sheet structure weakens, the bonding between the substrate and the chip and the sintered metal layer weakens, and the thermal conductivity of the joint body, the chip shear strength, or the connection reliability decreases. In addition, if Fig.17 and Fig.18As shown, in the bonded bodies of Comparative Examples 7 and 8, the sintered copper 1 having a thin sheet structure in the sintered body is not oriented approximately parallel to the substrate 17 or the chip, so stress is concentrated and not dispersed, which is considered to be the reason why the thermal conductivity, chip shear strength or connection reliability of the bonded body is reduced.
[0226] In Comparative Example 9 using high-temperature lead solder, although the chip shear strength and connection reliability are good, the thermal conductivity is low. In addition, in Comparative Example 10 using silver paste for connection, although the thermal conductivity and chip shear strength are good, the connection reliability is poor. These results show that the joint body of the present invention is superior in thermal conductivity, chip shear strength and connection reliability compared to the joint body using the conventional joint material.
[0227] Explanation of symbols
[0228] 1 Sintered copper with a lamellar structure
[0229] 2 Sintered copper from copper particles
[0230] 3 empty holes
[0231] 4 Sintered metal layer
[0232] 5. First Component
[0233] 6 Second component
[0234] 8 Thickness of the lamellar structure
[0235] 9 Long diameter of the lamellar structure
[0236] 10 Chip
[0237] 11a, 11b Lead frame
[0238] 12 Wire
[0239] 13 Casting resin
[0240] 14 Semiconductor components
[0241] 15 Chip (joined surface: gold),
[0242] 16 Chip (joined surface: silver)
[0243] 17 substrate
[0244] 100 Joint
[0245] 110 Semiconductor devices
[0246] 21 Insulation substrate
[0247] 22. First electrode
[0248] 23 Semiconductor components
[0249] 24 Second electrode
[0250] 25 Metal wiring
[0251] 26 Third electrode
[0252] 27 Wire
[0253] 28 Copper Plate
[0254] 29 Insulator
[0255] 30 blocks
[0256] 31 Sealing material
[0257] 32 first heat conducting member
[0258] 33 second heat conducting member
[0259] 34 Electrodes
[0260] 35 Wire
[0261] 200 Semiconductor devices
[0262] 210 Semiconductor devices
[0263] 220 Semiconductor devices
[0264] 300 Semiconductor devices
[0265] 310 Semiconductor devices
[0266] 320 Semiconductor devices
[0267] 400 Semiconductor devices
Claims
1. A bonded body comprising a first member, a second member, and a sintered metal layer bonding the first member and the second member. The sintered metal layer includes a structure derived from flaky copper particles having a maximum diameter of 1 μm to 20 μm and an aspect ratio of 4 or more, oriented substantially parallel to an interface between the first member or the second member and the sintered metal layer. The content of copper in the sintered metal layer is 65 volume % or more based on the volume of the sintered metal layer. The orientation order S of the structure derived from the flaky copper particles is 0.88 or more and 1.00 or less as determined by the following formula (1). S=1 / 2×(3<cos 2 θ>-1) (1) Where θ represents the angle between the interface and the lamellar structure, <cos 2 θ> represents multiple cos 2 The average value of θ.
2. The conjugate according to claim 1, wherein At least one of the first member and the second member contains at least one metal selected from the group consisting of copper, nickel, silver, gold, and palladium on a surface in contact with the sintered metal layer.
3. A semiconductor device comprising a first member, a second member, and a sintered metal layer bonding the first member and the second member, wherein at least one of the first member and the second member is a semiconductor element, wherein: The sintered metal layer includes a structure derived from flaky copper particles having a maximum diameter of 1 μm to 20 μm and an aspect ratio of 4 or more, oriented substantially parallel to an interface between the first member or the second member and the sintered metal layer. The content of copper in the sintered metal layer is 65 volume % or more based on the volume of the sintered metal layer. The orientation order S of the structure derived from the flaky copper particles is 0.88 or more and 1.00 or less as determined by the following formula (1). S=1 / 2×(3<cos 2 θ>-1) (1) Where θ represents the angle between the interface and the lamellar structure, <cos 2 θ> represents multiple cos 2 The average value of θ. The semiconductor device according to claim 3 , wherein the die shear strength is 30 MPa or more.
5. A semiconductor device comprising a first electrode, a semiconductor element electrically connected to the first electrode, and a second electrode electrically connected to the semiconductor element via a metal wiring, A sintered metal layer containing copper is provided between the semiconductor element and the metal wiring and between the metal wiring and the second electrode. The sintered metal layer is in contact with the metal wiring and contains a structure derived from flaky copper particles having a maximum diameter of 1 μm to 20 μm and an aspect ratio of 4 or more, oriented substantially parallel to an interface with the metal wiring. The content of copper in the sintered metal layer is 65 volume % or more based on the volume of the sintered metal layer. The orientation order S of the structure derived from the flaky copper particles is 0.88 or more and 1.00 or less as determined by the following formula (1). S=1 / 2×(3<cos 2 θ>-1) (1) Where θ represents the angle between the interface and the lamellar structure, <cos 2 θ> represents multiple cos 2 The average value of θ.
6. A semiconductor device comprising a first heat conducting member, a second heat conducting member, and a semiconductor element disposed between the first heat conducting member and the second heat conducting member, A sintered metal layer containing copper is provided between at least one of the first heat conducting member and the semiconductor element and between the semiconductor element and the second heat conducting member. The sintered metal layer is in contact with the first heat conducting member or the second heat conducting member and contains a structure derived from flaky copper particles having a maximum diameter of 1 μm to 20 μm and an aspect ratio of 4 or more, oriented substantially parallel to the interface of the first heat conducting member or the second heat conducting member, The content of copper in the sintered metal layer is 65 volume % or more based on the volume of the sintered metal layer. The orientation order S of the structure derived from the flaky copper particles is 0.88 or more and 1.00 or less as determined by the following formula (1). S=1 / 2×(3<cos 2 θ>-1) (1) Where θ represents the angle between the interface and the lamellar structure, <cos 2 θ> represents multiple cos 2 The average value of θ.