A lost foam casting mold and casting method for a knife tooth seat
By using a combination of sprue and inner runner in the lost foam casting technology of the cutter tooth seat, bottom-up pouring and plume flushing of molten metal are realized, which solves the problem of poor surface quality and inconsistent mechanical properties of castings in the existing technology. problem, significantly improving the casting quality and service life of the cutter tooth holder.
Patent Information
- Application Number
- CN202010297121.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-15
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-04-15
Smart Images

Figure CN111468675B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of blade tooth seat casting, in particular to a blade tooth seat lost foam casting mold and a casting method. Background Art
[0002] As one of the key components in the coal mining industry, the cutter tooth seat is usually cast horizontally using sand molds. Since there are many inverted teeth on the drum and multiple risers are set along the length of the sand mold, there are too many inverted tooth cutting surfaces formed by pouring, a large amount of grinding workload, poor surface quality of castings, and increased metal liquid consumption. At the same time, horizontal casting can easily cause the structure on one side of the inverted tooth to be loose, and the mechanical properties are inconsistent with the other side of the inverted tooth, which reduces the service life of the cutter tooth seat. Summary of the invention
[0003] In view of this, in view of the above-mentioned shortcomings, it is necessary to propose a lost foam casting mold for a cutter tooth seat.
[0004] It is also necessary to propose a lost foam casting method for a cutter tooth seat.
[0005] A lost foam casting mold for a tooth seat comprises a tooth seat blank mold and a casting system blank mold, wherein the tooth seat blank mold comprises a roller, a first inverted tooth, and a second inverted tooth, wherein the roller is a hollow cylinder, wherein the first inverted tooth and the second inverted tooth are arranged end to end on both sides of the roller opposite to each other, and the casting system blank mold comprises a sprue, an entgate, and a pouring cup, wherein the entgate has two layers, an upper layer and an lower layer, wherein the sprue is vertically arranged along the axis direction of the roller, wherein one end of the sprue extends to the outside of one end of the roller, and the other end of the sprue is flush with the other end of the roller, wherein one end of the entgate is connected to the sprue, and the other end of the entgate is connected to the roller, and the pouring cup is connected to one end of the sprue.
[0006] Preferably, the first inverted teeth and the second inverted teeth are arranged in several groups end to end in the length direction of the drum, and the first inverted teeth and the second inverted teeth have the same structure. The first inverted teeth are arc-shaped, and the bottom is connected to the outer wall of the drum, and an L-shaped groove is provided at the end of the arc-shaped surface. The first inverted teeth are also provided with several chamfers on both sides of the L-shaped groove, and the first inverted teeth are also provided with a triangular groove on the side close to the chamfer.
[0007] Preferably, several ingates are arranged along the vertical direction of the straight runner, and the ingates include a first ingate, a second ingate, and a third ingate. One end of the first ingate is connected to the straight runner, and the other end of the first ingate is connected to a roller close to the side of the L-shaped groove of the first inverted tooth. One end of the second ingate is connected to the straight runner, and the other end of the second ingate is connected to a roller close to the side of the triangular groove of the second inverted tooth. One end of the third ingate is connected to the straight runner, and the other end of the third ingate is connected to a roller close to the first inverted tooth and the second inverted tooth on the opposite side of the head and tail.
[0008] Preferably, the angle between the first ingating channel, the second ingating channel and the third ingating channel is 120°.
[0009] Preferably, the first ingrate, the second ingrate and the third ingrate are also inclined at a small angle along the sprue direction, and the inclination angle is 5-30°.
[0010] Preferably, the sprue is further provided with a first riser and a second riser on both sides close to the pouring cup, the first riser is connected to one end of the roller and the first inverted tooth end, and the second riser is connected to one end of the roller and the second inverted tooth end.
[0011] A lost foam casting method for a cutter tooth seat comprises the following steps:
[0012] 1) Make the white mold of the cutter seat and the white mold of the pouring system;
[0013] 2) The sprue is vertically arranged inside the drum, so that the axis of the sprue coincides with the axis of the drum, the sprue is extended to one end of the outside of the drum and connected to the pouring cup, one end of a plurality of ingates is bonded to the sprue, the other end of a plurality of ingates is bonded to the drum, and the external slag collection bag is bonded to the other end of the sprue, and the first riser is bonded to the other end of the drum and the first inverted tooth end, and the second riser is bonded to the other end of the drum and the second inverted tooth end, so as to form a double-riser vertical casting mold for a cutter tooth seat;
[0014] 3) The bonded double-riser vertical casting mold of the tooth seat is coated with refractory material and dried to form a lost foam casting mold of the tooth seat;
[0015] 4) Place the dried lost foam casting mold of the cutter tooth seat vertically inside the sand box;
[0016] 5) Place the sand box on the vibrating casting platform, fill the sand inside the sand box, turn on the vibration and simultaneously perform negative pressure suction on the sand box;
[0017] 6) After the sand filling is completed, the sand box is sealed;
[0018] 7) Pour the molten metal from top to bottom along the pouring cup, straight runner, and several inner runners. The molten metal flows from bottom to top in the white mold of the blade seat to form a blade seat casting.
[0019] This scheme changes the sand box casting into lost foam casting, and sets a straight runner and several groups of ingates inside the drum to pour the molten metal from bottom to top in the white mold of the cutter tooth seat. The first ingates, the second ingates, and the third ingates in the ingates not only transport the molten metal to the drum, but also cause the molten metal to form a local vortex inside the drum to flush away the bubbles, scum and other impurities remaining in the drum, the first inverted tooth, and the second inverted tooth, thereby greatly improving the casting quality. The first riser and the second riser are respectively set at the connection between the end of the drum and the end of the first inverted tooth and the end of the second inverted tooth, so as to discharge the molten metal with impurities in time. Through the above methods, the casting quality of the cutter tooth seat is greatly improved, the internal structure is evenly distributed, the density is good, the mechanical properties on both sides are consistent, and the service life of the cutter tooth seat is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is an axial schematic diagram of the lost foam casting mold for the tooth holder.
[0021] Figure 2 for Figure 1 Axial view from the other direction.
[0022] Figure 3 Schematic diagram of the white mold of the pouring system.
[0023] In the figure: a roller 11, a first inverted tooth 12, an L-shaped groove 121, a triangular groove 122, a second inverted tooth 13, a pouring system white mold 20, a sprue 21, an entrant 22, a first entrant 221, a second entrant 222, a third entrant 223, a pouring cup 23, a first riser 24, a second riser 25; and an external slag collecting bag 100. DETAILED DESCRIPTION
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0025] See also Figures 1 to 3The present invention proposes a lost foam casting mold for a cutter tooth seat, including a cutter tooth seat white mold and a pouring system white mold 20, wherein the cutter tooth seat white mold includes a roller 11, a first inverted tooth 12, and a second inverted tooth 13, wherein the roller 11 is a hollow cylinder, wherein the first inverted tooth 12 and the second inverted tooth 13 are arranged end to end on both sides of the roller 11, and wherein the pouring system white mold 20 includes a sprue 21, an entrail 22, and a pouring cup 23, wherein the entrail 22 is an upper and lower two-layer structure, wherein the sprue 21 is a lower and upper two-layer structure, wherein the entrail 2 ... 1 is vertically arranged along the axis direction of the drum 11, one end of the sprue 21 extends to the outside of one end of the drum 11 and is connected to the pouring cup 23, so that the molten metal is transported to the sprue 21 during pouring, the other end of the sprue 21 is flush with the other end of the drum 11, the cross section of the sprue 21 is circular, one end of the entgate 22 is connected to the sprue 21, the other end of the entgate 22 is connected to the drum 11, and the pouring cup 23 is connected to one end of the sprue 21.
[0026] Specifically, the white mold of the tooth seat is directly engraved by a three-axis engraving machine, wherein the number of first inverted teeth 12 and second inverted teeth 13 arranged end to end is a group. According to actual production needs, a plurality of white molds of the tooth seat can be engraved by the three-axis engraving machine, and then the plurality of white molds of the tooth seat are bonded into a white mold of the tooth seat having a plurality of groups of first inverted teeth 12 and second inverted teeth 13. In the above manner, the three-axis engraving machine can be fully utilized to produce white molds of the tooth seat with complex structures, and the quality and precision of the white molds of the tooth seat can be significantly improved, and the amount of raw materials of the white mold can be reduced, and there is no need to purchase expensive high-end equipment such as five-axis engraving, thereby greatly reducing the production cost of the white mold of the tooth seat.
[0027] Specifically, the sprue 21, the entgate 22 and the pouring cup 23 in the pouring system white mold 20 are directly carved by a three-axis engraving machine. The pouring system white mold 20 is also provided with a first riser 24 and a second riser 25. The first riser 24 and the second riser 25 are separately carved by the three-axis engraving machine. The carved sprue 21, the entgate 22, the pouring cup 23, the first riser 24 and the second riser 25 are then bonded to the drum 11 and the first inverted teeth 12 and the second inverted teeth 13 on both sides thereof. The formed tooth seat lost foam casting mold has the advantages of high precision, low cost and high pouring efficiency.
[0028] Furthermore, the first inverted teeth 12 and the second inverted teeth 13 are arranged in a plurality of groups end to end in the length direction of the drum 11, and the number of the first inverted teeth 12 and the second inverted teeth 13 arranged end to end can be adjusted according to actual needs, such as two groups. The first inverted teeth 12 and the second inverted teeth 13 have the same structure. The first inverted teeth 12 are in an arc surface, and the bottom thereof is connected to the outer wall of the drum 11, and an L-shaped groove 121 is provided at the end of the arc surface, and the height thereof is adjusted according to actual needs. The first inverted teeth 12 are also provided with a plurality of chamfers on both sides close to the L-shaped groove 121, and the chamfers are one of edge-to-corner or rounded chamfers or a combination thereof, and are symmetrically distributed on both sides of the arc surface. The first inverted teeth 12 are also provided with a triangular groove 122 on the side close to the chamfer, and a round chamfer is also provided at the connection between the groove and the arc surface of the first inverted tooth 12.
[0029] Specifically, the structures of the first inverted teeth 12 and the second inverted teeth 13 are relatively complex. If horizontal sand casting is used, the first inverted teeth 12 and the second inverted teeth 13 may easily have defects such as shrinkage, pores, and uneven internal structure.
[0030] Furthermore, the ingates 22 are provided with a plurality of ingates 22 along the vertical direction of the sprue 21, and the ingates 22 include a first ingates 221, a second ingates 222, and a third ingates 223. One end of the first ingates 221 is connected to the sprue 21, and the other end of the first ingates 221 is connected to the roller 11 near the side of the L-shaped groove 121 of the first inverted tooth 12, so that the molten metal in the sprue 21 is transported to the roller 11 near the side of the L-shaped groove 121 of the first inverted tooth 12 through the first ingates 221. One end of the second ingates 222 is connected to the sprue 21, and the second ingates 223 is connected to the roller 11 near the side of the L-shaped groove 121 of the first inverted tooth 12. The other end of the runner 222 is connected to the roller 11 on the side of the triangular groove 122 close to the second inverted tooth 13, so that the molten metal in the straight runner 21 is transported to the roller 11 on the side of the triangular groove 122 close to the second inverted tooth 13 through the second ingrowing 222. One end of the third ingrowing 223 is connected to the straight runner 21, and the other end of the third ingrowing 223 is connected to the roller 11 on the side opposite to the first inverted tooth 12 and the second inverted tooth 13, so that the molten metal in the straight runner 21 is transported to the roller 11 on the side opposite to the first inverted tooth 12 and the second inverted tooth 13 through the third ingrowing 223.
[0031] Specifically, the first ingrate 221, the second ingrate 222, and the third ingrate 223 have rectangular cross sections, and the molten metal is transported to the inside of the drum 11 through the first ingrate 221, the second ingrate 222, and the third ingrate 223 and flows to the first inverted tooth 12 and the second inverted tooth 13. Since the angle between the first ingrate 221, the second ingrate 222, and the third ingrate 223 is 120°, the molten metal flows from the first ingrate 221, the second ingrate 222, and the third ingrate 223 to the drum 11 and the first inverted tooth 12 and the second inverted tooth 13. 3 flows at a slow speed, so that the density of the molten metal inside the drum 11 and the first inverted tooth 12 and the second inverted tooth 13 is consistent, ensuring that the two sides of the cutter tooth seat formed after casting have consistent mechanical properties. At the same time, when the molten metal flows through the first ingrate 221 to the drum 11 and the first inverted tooth 12 close to the L-shaped groove 121, the molten metal is hindered by the cross section of the L-shaped groove 121 of the first inverted tooth 12, and tends to flow toward the drum 11 close to the third ingrate 223, which partially increases the flow speed of the molten metal in the first inverted tooth 12, so that the molten metal is completely filled in The first inverted tooth 12 with a complex structure is formed at each place, and a vortex is formed inside the drum 11. When the molten metal flows to the drum 11 and the second inverted tooth 13 near the side of the triangular groove 122 through the second ingates 222, the molten metal first flows to the two sides of the second inverted tooth 13 after passing through the drum 11, and is blocked by the L-shaped groove 121 of the second inverted tooth 13 when it flows to the L-shaped groove 121 of the second inverted tooth 13, and the speed is slowed down. It is restricted by the shell of the second inverted tooth 13, and when it is completely filled in the second inverted tooth 13, a vortex is formed inside it; through the first ingates 221, the second ingates 222, and the third ingates 223 to the same horizontal The cross-sectional roller 11, the first inverted tooth 12, and the second inverted tooth 13 convey the molten metal. The molten metal vortex velocity near the first ingrate 221 in the roller 11 is different from the molten metal vortex velocity near the second ingrate 222 and the molten metal conveying velocity near the third ingrate 223, which causes the molten metal to form a local vortex flushing inside the roller 11 to flush away the bubbles, slag and other impurities remaining in the roller 11, the first inverted tooth 12, and the second inverted tooth 13, so that the molten metal floats on the surface of the molten metal and is then discharged to the outside through the first riser 24, the second riser 25, and the external slag collecting bag 100.
[0032] Furthermore, the included angle among the first ingating channel 221 , the second ingating channel 222 , and the third ingating channel 223 is 120°.
[0033] Furthermore, the first ingrate 221, the second ingrate 222, and the third ingrate 223 are also inclined at a small angle along the direction of the sprue 21, and the inclination angle is 5-30 degrees.
[0034] Specifically, after the molten metal enters the mold through the lower ingrowth 22, its temperature is relatively low, and it is prone to problems such as local solidification and structural defects. The present solution also makes the first ingrowth 221, the second ingrowth 222, and the third ingrowth 223 tilt at a small angle of 5 to 30 degrees toward the sprue 21, and transports the molten metal from the upper ingrowth 22 to the inside of the mold to locally accelerate the flow rate of the molten metal, thereby replenishing the molten metal temperature of the lower ingrowth 22, maintaining the overall stability of the molten metal temperature in the mold, avoiding local solidification of the molten metal due to excessive temperature difference or too low temperature, and preventing structural defects after the molten metal solidifies.
[0035] Furthermore, the sprue 21 is provided with a first riser 24 and a second riser 25 on both sides close to the pouring cup 23. The first riser 24 is connected to one end of the roller 11 and the end of the first inverted tooth 12 to discharge the molten metal and impurities at one end of the roller 11 and the end of the first inverted tooth 12 in time. The second riser 25 is connected to one end of the roller 11 and the end of the second inverted tooth 13 to discharge the molten metal and impurities at one end of the roller 11 and the end of the second inverted tooth 13 in time.
[0036] The present invention also proposes a lost foam casting method for a cutter tooth seat, which comprises the following steps:
[0037] 1) Make the white mold of the blade tooth seat and the white mold of the pouring system 20;
[0038] 2) vertically setting the sprue 21 inside the drum 11 so that the axis of the sprue 21 coincides with the axis of the drum 11, extending the sprue 21 to one end of the outside of the drum 11 and connecting it to the pouring cup 23, bonding one end of a plurality of ingates 22 to the sprue 21, bonding the other end of a plurality of ingates 22 to the drum 11, bonding the external slag collection bag 100 to the other end of the sprue 21, bonding the first riser 24 to one end of the drum 11 and the end of the first inverted tooth 12, bonding the second riser 25 to one end of the drum 11 and the end of the second inverted tooth 13, forming a double-riser vertical casting mold for a cutter tooth seat;
[0039] 3) The bonded double-riser vertical casting mold of the tooth seat is coated with refractory material and dried to form a lost foam casting mold of the tooth seat;
[0040] 4) Place the dried lost foam casting mold of the cutter tooth seat vertically inside the sand box;
[0041] 5) Place the sand box on the vibrating casting platform, fill the sand inside the sand box, turn on the vibration and simultaneously perform negative pressure suction on the sand box;
[0042] 6) After the sand filling is completed, the sand box is sealed;
[0043] 7) The molten metal is poured from top to bottom along the pouring cup 23, the sprue 21, and the plurality of inner runners 22. The molten metal flows from bottom to top in the cutter tooth seat white mold to form a cutter tooth seat casting.
[0044] Specifically, the pouring cup 23 is connected to one end of the sprue 21 to timely transport the molten metal to the sprue 21. The pouring cup 23 is a hollow cone with a diameter no larger than that of the first riser 24 and the second riser 25 to increase the flow rate of the molten metal in the sprue 21 and improve the casting quality.
[0045] The present invention controls the number of risers to 2, the first riser 24 is connected to one end of the roller 11 and the end of the first inverted tooth 12, so as to quickly discharge the molten metal with impurities in the roller 11 and the first inverted tooth 12 in time, and prevent the impurities from being retained in one end of the roller 11, and the second riser 25 is connected to one end of the roller 11 and the end of the second inverted tooth 13, so as to quickly discharge the molten metal with impurities in the roller 11 and the second inverted tooth 13 in time, and prevent the impurities from being retained in one end of the roller 11. Through the above methods, the casting quality of the cutter tooth seat is greatly improved, the internal structure is evenly distributed, the density is good, the mechanical properties on both sides are consistent, and the service life of the cutter tooth seat is significantly improved.
[0046] The modules or units in the device of the embodiment of the present invention may be combined, divided or deleted according to actual needs.
[0047] What is disclosed above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. A person skilled in the art can understand that all or part of the processes of the above embodiments and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.
Claims
1. A lost foam casting mold for a blade tooth seat, Features: It includes a cutter tooth seat blank mold and a pouring system blank mold. The cutter tooth seat blank mold includes a roller, a first inverted tooth, and a second inverted tooth. The roller is a hollow cylinder. The first inverted tooth and the second inverted tooth are arranged end to end on both sides of the roller. The pouring system blank mold includes a sprue, an entgate, and a pouring cup. The entgate is an upper and lower layer. The sprue is vertically arranged along the axis of the roller. One end of the sprue extends to the outside of one end of the roller. The other end of the sprue is flush with the other end of the roller. One end of the entgate is connected to the sprue, and the other end of the entgate is connected to the roller. The pouring cup is connected to one end of the sprue. The first inverted teeth and the second inverted teeth are arranged in a plurality of groups end to end in the length direction of the drum. The first inverted teeth and the second inverted teeth have the same structure. The first inverted teeth are arc-shaped, the bottom is connected to the outer wall of the drum, and an L-shaped groove is provided at the end of the arc-shaped surface. The first inverted teeth are also provided with a plurality of chamfers on both sides close to the L-shaped groove, and a triangular groove is also provided on the side of the first inverted teeth close to the chamfer. The ingates are provided with a plurality of them along the vertical direction of the straight runner, and the ingates include a first ingates, a second ingates, and a third ingates, one end of the first ingates is connected to the straight runner, and the other end of the first ingates is connected to a roller close to one side of the L-shaped groove of the first inverted tooth, one end of the second ingates is connected to the straight runner, and the other end of the second ingates is connected to a roller close to one side of the triangular groove of the second inverted tooth, one end of the third ingates is connected to the straight runner, and the other end of the third ingates is connected to a roller close to the first inverted tooth and the second inverted tooth on the opposite side of the head and tail; The angle between the first ingating channel, the second ingating channel and the third ingating channel is 120°; The first ingrate, the second ingrate and the third ingrate are also inclined at a small angle along the sprue direction, and the inclination angle is 5-30 degrees.
2. The lost foam casting mold for the blade tooth seat according to claim 1, Features: The sprue is also provided with a first riser and a second riser on both sides close to the pouring cup. The first riser is connected to one end of the roller and the first inverted tooth end, and the second riser is connected to one end of the roller and the second inverted tooth end.