Electronic component packaging and manufacturing method thereof
By adopting a sequential stacking structure of metal particle layer, copper plating layer and nickel plating layer in electronic component packaging, combined with polymer layer processing, the problem of easy peeling of the plating layer is solved and excellent electromagnetic wave shielding effect is achieved.
Patent Information
- Application Number
- CN201980006586.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-02-27
- Filing Date
- 2019-02-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-02-21
AI Technical Summary
Existing electronic components are packaged with a plating layer on the sealing body as a shielding layer, but it is easy to peel off, resulting in poor electromagnetic wave noise shielding effect.
A sequential stacking structure of metal particle layer, copper plating layer and nickel plating layer is used as the shielding layer, and the polymer layer and metal particle layer are processed on the surface of the sealing body to improve the adhesion force and electromagnetic wave shielding.
It significantly improves the adhesion between the shielding layer and the sealing body and the electromagnetic wave shielding effect, and enhances the noise shielding performance of electronic component packaging.
Smart Images

Figure CN111492472B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to electronic component packaging and a method for manufacturing the same. Background Art
[0002] In recent years, semiconductor packages called system-in-package (SiP) have been widely used in portable information terminals such as smartphones, in which an IC and multiple electronic components are installed in one semiconductor package to operate as a functional block. Such semiconductor packages prevent malfunctions caused by external noise while implementing electromagnetic wave noise countermeasures to avoid becoming a noise source themselves. For example, Patent Document 1 discloses an electronic component package having multiple plating layers as layers for shielding electromagnetic wave noise, but does not involve a system-in-package.
[0003] However, in the above-mentioned electronic component package, although a plating layer is directly provided as a shielding layer on a sealing body that seals the electronic component, there is a disadvantage that the plating layer is easily peeled off from the sealing body.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2005-109306 Summary of the invention
[0007] Problems to be solved by the invention
[0008] The problem to be solved by the present invention is to provide an electronic component package and a method for manufacturing the same, wherein a copper plating layer and a nickel plating layer are provided as a shield layer on a sealing body that seals an electronic component, and the shield layer and the sealing body have excellent adhesion.
[0009] Methods for solving problems
[0010] The inventors of the present invention have conducted active research to solve the above-mentioned problems, and as a result, have found that in an electronic component package having a sealed electronic component and a sealing body with an epoxy resin, and a shielding layer formed on the sealing body, the shielding layer is a layer stacked in the order of a metal particle layer, a copper plating layer, and a nickel plating layer starting from the sealing body side, the shielding layer has significantly excellent adhesion with the sealing body, and has excellent electromagnetic wave shielding properties, thereby completing the present invention.
[0011] That is, the present invention provides an electronic component package and a method for manufacturing the same, wherein the electronic component package is an electronic component package having an electronic component, a sealing body and a shielding layer, wherein the electronic component is mounted on a circuit substrate having a grounding pattern, the sealing body seals the electronic component and has an epoxy resin, and the shielding layer is formed on the sealing body. The electronic component package is characterized in that the shielding layer is a layer stacked in the order of a metal particle layer, a copper plating layer, and a nickel plating layer starting from the sealing body side, and the shielding layer is grounded to the grounding pattern.
[0012] Effects of the Invention
[0013] The electronic component package of the present invention can also be suitably used as, for example: a semiconductor package provided with a shielding layer in order to improve the shielding effect of the electromagnetic wave noise of the semiconductor device; an integrated module that integrates the functions of a high-frequency module, a front-end module including a filter, a communication module for sending and receiving, etc. into one function and has a high-density installation of multiple modules. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a diagram showing the entirety of an electronic component package with a shielding layer.
[0015] Figure 2 To express Figure 1 FIG. 1 is a diagram of a cross section (AA) of an electronic component package.
[0016] Figure 3 This is a diagram showing a cross section of an electronic component package in which a polymer layer is provided on the surface of a sealing body.
[0017] Figure 4 This is a cross-sectional view showing a state in which a polymer layer is provided on the surface of a sealing body, a slit portion is formed along a predetermined dividing line, and a metal particle layer is provided thereon. It should be noted that a copper plating layer and a nickel plating layer are finally laminated in sequence on the metal particle layer to form the electronic component package of the present invention. DETAILED DESCRIPTION
[0018] The electronic component package of the present invention is an electronic component package having an electronic component, a sealing body and a shielding layer, wherein the electronic component is mounted on a circuit substrate having a grounding pattern, the sealing body seals the electronic component and has an epoxy resin, and the shielding layer is formed on the sealing body. The electronic component package is characterized in that the shielding layer is a layer stacked in the order of a metal particle layer, a copper plating layer, and a nickel plating layer starting from the sealing body side, and the shielding layer is grounded to the grounding pattern.
[0019] The circuit board having the ground pattern is preferably configured such that a portion of the ground pattern is exposed on the surface of the sealing body. By connecting a shielding layer described later to the ground pattern, excellent electromagnetic wave shielding properties can be obtained.
[0020] As the circuit substrate with the ground pattern, at least two layers of ground patterns and wiring patterns may be formed on a substrate made of an insulating material such as glass epoxy resin. In addition, when the circuit substrate has two or more layers, it is preferred that the layers are electrically connected by through holes.
[0021] In addition, as the above-mentioned circuit substrate with a ground pattern, the following can also be used: a circuit substrate for mounting at least two semiconductor devices in a planar or three-dimensional arrangement on a substrate including an insulating material; a circuit substrate for an integrated module in which the functions of a high-frequency module, a front-end module including a filter, a communication module for sending and receiving, etc. are integrated into one function and a plurality of modules are installed at a high density.
[0022] Examples of materials for the circuit board having a ground pattern include glass epoxy resin, liquid crystal polymer, fluororesin represented by polytetrafluoroethylene, silicone resin, polyimide resin, polyimide resin, polybenzoic acid resin, and the like. Photosensitive insulating materials such as azole resin, build-up films of thermosetting epoxy resin, or materials with glass cloth added to the build-up films, etc., can be used as the base material alone, or two or more materials can be composited and used as the base material.
[0023] In the present invention, after the electronic components are mounted on the circuit substrate having the ground pattern, a sealing body is formed by a material having an epoxy resin. As the material having the epoxy resin, a material obtained by curing a thermosetting epoxy resin with a curing agent such as a phenolic curing agent, a cyanate curing agent, an active ester curing agent, or a material obtained by adding an inorganic filler represented by silica particles to the material, and other commonly used sealing materials can be used. As a method for forming the sealing body, transfer molding and compression molding can be cited, and a method of sealing using a sealing resin sheet and a laminator or a pressing device can also be cited.
[0024] In addition, in order to further improve the adhesion with the metal particle layer described later and the polymer layer described later, the surface of the above-mentioned seal can be surface treated by, for example, a plasma discharge treatment method such as a corona discharge treatment method; a dry treatment method such as an ultraviolet treatment method; a wet treatment method using water, an acidic or alkaline liquid, an organic solvent, etc. In addition, although the above-mentioned patent document 1 records that the surface of the seal is roughened with a chemical, it is preferred not to roughen the surface of the seal in the present invention.
[0025] Next, in the present invention, a metal particle layer is provided to form a shielding layer on the seal. The metal particle layer is to make the seal close to the copper plating layer described later, and also functions as a plating base layer for forming the copper plating layer described later, and is used as a catalyst for electroless copper plating or a base conductive layer for electroplating copper.
[0026] In the present invention, in order to further improve the adhesion between the seal and the shielding layer, a polymer layer is preferably provided between the seal and the metal particle layer. As the polymer forming the polymer layer, various resins such as polyurethane resin, vinyl resin, acrylic resin, urethane-acrylic composite resin, epoxy resin, imide resin, amide resin, melamine resin, phenolic resin, polyvinyl alcohol, polyvinyl pyrrolidone, etc. can be listed.
[0027] Among the resins used as the above-mentioned polymer, polyurethane resins, acrylic resins, urethane-acrylic composite resins, and epoxy resins are preferred, and more preferably, one or more resins selected from the group consisting of polyurethane resins having a polyether structure, polyurethane resins having a polycarbonate structure, polyurethane resins having a polyester structure, acrylic resins, urethane-acrylic composite resins, and epoxy resins are more preferred. In addition, urethane-acrylic composite resins are further preferred because they can obtain wiring patterns with excellent adhesion and conductivity.
[0028] In addition, the metal particle layer is composed of metal particles dispersed by a polymer dispersant described later, and when the polymer dispersant contains a compound (b1) having a reactive functional group [Y] described later, the polymer forming the polymer layer is preferably a compound (a1) having a functional group [X], and the functional group [X] is reactive with the reactive functional group [Y]. Examples of the compound (a1) having the reactive functional group [X] include compounds having an amino group, an amide group, an alkanolamide group, a carboxyl group, a carboxylic anhydride group, a carbonyl group, an acetoacetyl group, an epoxy group, an alicyclic epoxy group, an oxetane ring, a vinyl group, an allyl group, a (meth)acryloyl group, a (blocked) isocyanate group, an (alkoxy)silyl group, and a silsesquioxane compound.
[0029] In particular, when the compound (b1) having a reactive functional group [Y] in the polymer dispersant described later in the above-mentioned metal particle layer uses a compound having a basic group containing a nitrogen atom described later, and the polymer forming the above-mentioned polymer layer has a carboxyl group, a carbonyl group, an acetoacetyl group, an epoxy group, an alicyclic epoxy group, an alkanolamide group, an isocyanate group, a vinyl group, a (meth)acryloyl group, or an allyl group as a reactive functional group [X], it is possible to further improve the adhesion between the finally obtained sealing body and the above-mentioned shielding layer, and thus it is preferred.
[0030] The polymer layer is preferably provided on the entire surface of the sealing body in the form of a thin film, but in order to connect the ground pattern of the electronic component package and the shielding layer, it is preferred to avoid the ground pattern exposed from the sealing body and provide the polymer layer. In addition, the polymer layer is preferably not formed in the part of the electronic component package where the shielding layer is not formed. The so-called part of the electronic component package where the shielding layer is not formed includes, for example, the circuit substrate side of the electronic component package opposite to the shielding layer, the part where the solder ball is formed, and the predetermined part where the solder ball is to be formed.
[0031] When the polymer forming the polymer layer is applied to the surface of the seal, a fluid obtained by dissolving or dispersing the polymer in a solvent is used. Examples of the coating method include coating, dipping, roller coating, spin coating, rotation, spraying, dispenser, inkjet printing, pad printing, reverse printing, flexographic printing, screen printing, gravure printing, gravure lithography, and the like.
[0032] Furthermore, when applying the fluid containing the polymer, the fluid may be applied after protecting the portion where the polymer layer is not to be applied with a masking tape or a sealing material.
[0033] Next, the fluid containing the polymer is dried after being applied to form the polymer layer. The drying is performed to volatilize the solvent contained in the fluid containing the polymer. The drying is preferably performed at a temperature range of 80 to 300° C. for about 1 to 200 minutes.
[0034] The thickness of the polymer layer formed using the polymer is preferably in the range of 5 to 5,000 nm in order to further improve the adhesion between the seal and the metal particle layer described later, and is more preferably in the range of 10 to 200 nm in order to achieve excellent adhesion between the finally obtained shielding layer and the seal.
[0035] The metal particle layer forming the barrier layer in the present invention is preferably composed of metal particles dispersed in a polymer dispersant, because of excellent adhesion to the sealing body and the polymer layer.
[0036] The polymer dispersant is preferably a polymer having a functional group coordinated to the metal particles. Examples of the functional group include a carboxyl group, an amino group, a cyano group, an acetoacetyl group, a phosphorus atom-containing group, a thiol group, a thiocyano group, and a glycine group.
[0037] In order to improve the adhesion with the sealing body and the polymer layer, the polymer dispersant preferably contains a compound (b1) having a reactive functional group [Y].
[0038] The reactive functional group [Y] possessed by the above-mentioned compound (b1) is a functional group that participates in the bonding with the epoxy group, phenolic hydroxyl group, hydroxyl group present in the above-mentioned sealing body, or the reactive functional group [X] in the above-mentioned polymer. As specific examples, there can be listed compounds having amino group, amide group, alkanolamide group, carboxyl group, carboxylic anhydride group, carbonyl group, acetoacetyl group, epoxy group, alicyclic epoxy group, oxetane ring, vinyl group, allyl group, (meth)acryloyl group, (blocked) isocyanate group, (alkoxy)silyl group, etc., silsesquioxane compounds, etc.
[0039] In order to further improve the adhesion with the sealing body and the polymer layer, the reactive functional group [Y] is preferably a basic group containing a nitrogen atom.
[0040] Examples of the nitrogen atom-containing basic group include an imino group, a primary amino group, and a secondary amino group.
[0041] In addition, by using a compound having a plurality of basic groups containing nitrogen atoms in one molecule as the above-mentioned compound (b1), one of the basic groups containing nitrogen atoms participates in the bonding with the epoxy group present in the above-mentioned sealant or the above-mentioned reactive functional group [X] possessed by the polymer forming the above-mentioned polymer layer, and the other contributes to the interaction with the metal particles contained in the above-mentioned metal particle layer, which can further improve the adhesion between the final metal plating layer described later and the above-mentioned sealant, and is therefore preferred.
[0042] The compound having a nitrogen atom-containing basic group is preferably a polyalkyleneimine or a polyalkyleneimine having a polyoxyalkylene structure containing an oxyethylene unit, since the dispersion stability of the metal particles and the adhesion to the polymer layer can be further improved.
[0043] The polyalkylene imine having the above structure may be a polyalkylene imine in which polyethylene imine and polyoxyalkylene are linearly bonded, or a polyalkylene imine in which the polyoxyalkylene is grafted to a side chain of a main chain of the polyethylene imine.
[0044] Specific examples of the polyalkylene imine having the above-mentioned polyoxyalkylene structure include: block copolymers of polyethylene imine and polyethylene oxide; polyalkylene imine in which a polyethylene oxide structure is introduced by addition reaction of ethylene oxide to a part of the imino groups present in the main chain of polyethylene imine; polyalkylene imine obtained by reacting an amino group of polyalkylene imine, a hydroxyl group of polyoxyethylene glycol, and an epoxy group of an epoxy resin; and the like.
[0045] Examples of commercially available products of the polyalkylene imine include “PAO2006W”, “PAO306”, “PAO318”, and “PAO718” of the “Epomin (registered trademark) PAO series” manufactured by Nippon Shokubai Co., Ltd.
[0046] The number average molecular weight of the polyalkylene imine is preferably in the range of 3,000 to 30,000.
[0047] When the reactive functional group [Y] possessed by the above-mentioned compound (b1) is a carboxyl group, an amino group, a cyano group, an acetoacetyl group, a phosphorus atom-containing group, a thiol group, a thiocyanate group, a glycine group, etc., these functional groups also function as functional groups that coordinate with metal particles, so the above-mentioned compound (b1) can also be used as a polymer dispersant for metal particles.
[0048] Next, as the metal particles constituting the above-mentioned metal layer, transition metals or their compounds can be listed, and among the above-mentioned transition metals, ionic transition metals are preferred. As the above-mentioned ionic transition metals, for example, metals such as copper, silver, gold, nickel, palladium, platinum, cobalt, or composites of these metals can be listed. These metal particles can be used alone or in combination of two or more. In addition, among these metal particles, silver particles are preferred, especially from the perspective of fewer operational problems such as oxidative degradation and cost.
[0049] As the above-mentioned metal particles, it is preferred to use granular metal particles with an average particle size of 1 to 20,000 nm; when using metal nanoparticles with an average particle size of 1 to 200 nm, compared with the case of using metal particles with an average particle size of micrometer level, in the copper plating process described later, the copper plating precipitation when used as a catalyst for electroless copper plating and the resistance value when used as a base layer for electroplated copper can be further reduced, and thus it is more preferred. It should be noted that in the present invention, the average particle size is the volume average value obtained by diluting the above-mentioned conductive material (b2) with a dispersing good solvent and measuring it by a dynamic light scattering method. This measurement can use "Nanotrac UPA" manufactured by Microtrac.
[0050] In order to form the metal particle layer, the seal is preferably coated by various coating methods described below, and therefore, it is preferably used as a metal particle dispersion obtained by dispersing metal particles in various solvents. Examples of the solvent include aqueous media such as distilled water, ion exchange water, pure water, and ultrapure water; and organic solvents such as alcohol solvents, ether solvents, ketone solvents, and ester solvents.
[0051] Examples of the alcohol solvent or ether solvent include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, heptanol, hexanol, octanol, nonanol, decanol, undecanol, dodecanol, tridecanol, tetradecanol, pentadecanol, stearyl alcohol, allyl alcohol, cyclohexanol, terpineol, terpineol, dihydroterpineol, 2-ethyl-1,3-hexanediol, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, propylene glycol, dipropylene glycol, 1,2-diol, 1,3-hexanediol, 1,4-diol, 1,6-diol, 1,8 ... ,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, propylene glycol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monobutyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, propylene glycol monopropyl ether, dipropylene glycol monopropyl ether, propylene glycol monobutyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monobutyl ether, etc.
[0052] Examples of the ketone solvent include acetone, cyclohexanone, methyl ethyl ketone, etc. Examples of the ester solvent include ethyl acetate, butyl acetate, 3-methoxybutyl acetate, 3-methoxy-3-methyl-1-butyl acetate, etc. Examples of other organic solvents include hydrocarbon solvents such as toluene, especially hydrocarbon solvents having 8 or more carbon atoms.
[0053] Examples of the hydrocarbon solvent having 8 or more carbon atoms include nonpolar solvents such as octane, nonane, decane, dodecane, tridecane, tetradecane, cyclooctane, xylene, mesitylene, ethylbenzene, dodecylbenzene, tetralin, and trimethylphenylcyclohexane, which can be used in combination with other solvents as needed. Furthermore, solvents such as mineral spirits and solvent naphtha can also be used in combination as a mixed solvent.
[0054] The metal particle dispersion can be prepared, for example, by mixing the polymer dispersant, the metal particles, and the solvent as required. Specifically, it can be prepared by adding a pre-modulated metal ion solution to a medium in which a compound having a polyalkylene imine chain, a hydrophilic segment, and a hydrophobic segment is dispersed, and reducing the metal ions.
[0055] Furthermore, in the metal particle dispersion, a surfactant, a defoaming agent, a rheology adjusting agent, etc. may be added as needed to improve the dispersion stability of the conductive substance in an aqueous medium, an organic solvent, or the like, and the wettability to the coating surface.
[0056] The metal particle layer may be provided in the form of a thin film on the entire surface and the side surface of the sealing body, but in order to connect the ground pattern of the electronic component package with the shielding layer, the metal particle layer needs to be provided in a manner in contact with the ground pattern exposed from the sealing body. In addition, the metal particle layer is preferably not formed at a portion of the electronic component package where the shielding layer is not formed. The so-called portion of the electronic component package where the shielding layer is not formed includes, for example, a portion of the electronic component package where a solder ball is formed on the opposite side of the shielding layer, a predetermined portion where a solder ball is to be formed, and the like.
[0057] The metal particle layer may be disposed on the entire surface of the seal where the shielding layer is to be formed, or the metal particle dispersion may be patterned by a coating method described later. When the metal particle layer forms a pattern, since the copper plating layer and the nickel plating layer described later are only formed on the pattern of the metal particle layer, the shielding layer itself can be patterned. The pattern of the metal particle layer may be formed in a portion without the metal particle layer within a range that does not hinder the electromagnetic wave shielding property. For example, a pattern in which the metal particle layer has dotted openings, a pattern in which the metal particle layer is arranged in a grid shape, or other various patterns may be formed.
[0058] When the metal particle dispersion is applied to the surface and side of the seal, the coating method includes, for example, coating method, dipping method, roller coating method, spin coating method, rotation method, spraying method, dispenser method, inkjet printing method, pad printing method, reverse printing method, flexographic printing method, screen printing method, gravure printing method, gravure lithography method, etc. When forming the pattern of the metal particle layer, it is preferred to use inkjet printing method, pad printing method, reverse printing method, flexographic printing method, screen printing method, gravure printing method, gravure lithography method.
[0059] Among the above-mentioned coating methods, it is particularly preferable to select a coating method that forms the metal particle layer uniformly as a thin film, and it is preferable to select a dipping method, a spin coating method, a spray method, an inkjet printing method, or a flexographic printing method.
[0060] In addition, when applying the above-mentioned metal particle dispersion, the metal particle dispersion may be applied after the portion where the metal particle layer is not formed is protected with a shielding tape or a sealing material. Examples of the above-mentioned shielding tape and sealing material include shielding adhesive tape for plating, shielding tape for printed circuit boards, dicing tape used in semiconductor wafer processing, and thermal release sheets for electronic component processes. It is preferred to select a material that can protect the portion where the shielding layer is not formed after the sealing material is applied to the portion where the shielding layer is not formed and the metal particles are applied, so that the portion where the shielding layer is not formed can be protected during the metal plating process described later.
[0061] Next, the metal particle dispersion is dried after being applied in order to form a metal particle layer. The drying is performed in order to volatilize the solvent contained in the metal particle dispersion. Furthermore, when used as a conductive layer for electroplated copper described later, it is performed in order to form a conductive metal particle layer by making the metal particles close and bonded to each other. The drying is preferably performed at a temperature range of 80 to 300°C for about 1 to 200 minutes. Here, in order to obtain a metal particle layer (plating base layer) having excellent adhesion to the sealant and the polymer layer, it is more preferred to set the drying temperature to a range of 100 to 200°C.
[0062] The drying may be performed in the air, but in order to prevent all oxidation of the metal particles, part or all of the drying process may be performed in a reducing atmosphere.
[0063] The drying step can be performed using, for example, an oven, a hot air drying furnace, an infrared drying furnace, laser irradiation, microwaves, light irradiation (a flash irradiation device), or the like.
[0064] The metal particle layer formed using the metal particle dispersion by the above method preferably contains 80 to 99.9% by mass of the conductive material and 0.1 to 20% by mass of the polymer dispersant in the pattern.
[0065] The thickness of the metal layer formed using the metal particle dispersion is preferably in the range of 5 to 500 nm in order to reduce the activity (plating precipitation) as a plating catalyst in the electroless copper plating step described later and the resistance value of the conductive layer in the electrolytic copper plating step.
[0066] The copper-plated layer constituting the shielding layer of the present invention can be used to shield electric field noise. As a method for forming the copper-plated layer, for example, wet plating methods such as electroless copper plating and electrolytic copper plating can be cited, and these plating methods can also be combined to form the copper-plated layer. For example, a method in which the above-mentioned metal particle layer is used as an electroless copper plating catalyst to perform electroless copper plating, and the electroless copper plating layer is used as a conductive layer to perform electrolytic copper plating; the above-mentioned metal particle layer can be used as a conductive layer to perform electrolytic copper plating.
[0067] Among the above-mentioned plating methods, the electrolytic copper plating method is more preferable because the adhesion between the metal particle layer and the copper plating layer formed by the above-mentioned plating method is further improved and the productivity of the copper plating step is excellent.
[0068] The electroless plating method is a method of, for example, forming an electroless copper plating layer including a metal film by bringing an electroless copper plating solution into contact with the metal particle layer to deposit copper metal contained in the electroless copper plating solution.
[0069] Examples of the electroless copper plating solution include an electroless copper plating solution containing copper, a reducing agent, and a solvent such as an aqueous medium or an organic solvent.
[0070] Examples of the reducing agent include dimethylaminoborane, hypophosphorous acid, sodium hypophosphite, dimethylamine borane, hydrazine, formaldehyde, sodium borohydride, and phenol.
[0071] In addition, as the above-mentioned electroless copper plating solution, as needed, an electroless copper plating solution containing a complexing agent such as a monocarboxylic acid such as acetic acid and formic acid; a dicarboxylic acid compound such as malonic acid, succinic acid, adipic acid, maleic acid, and fumaric acid; a hydroxycarboxylic acid compound such as malic acid, lactic acid, glycolic acid, gluconic acid, and citric acid; an amino acid compound such as glycine, alanine, iminodiacetic acid, arginine, aspartic acid, and glutamic acid; an organic acid such as an aminopolycarboxylic acid compound such as iminodiacetic acid, nitrilotriacetic acid, ethylenediaminediacetic acid, ethylenediaminetetraacetic acid, and diethylenetriaminepentaacetic acid, or a soluble salt (sodium salt, potassium salt, ammonium salt, etc.) of these organic acids, an amine compound such as ethylenediamine, diethylenetriamine, and triethylenetetraamine, etc.
[0072] The electroless copper plating solution is preferably used at a temperature in the range of 20 to 98°C.
[0073] The above-mentioned electrolytic copper plating method is, for example, a method as follows: electricity is applied while an electrolytic copper plating solution is in contact with the metal constituting the above-mentioned metal particle layer, or the surface of the electroless copper plating layer formed by the above-mentioned electroless copper plating, so that metals such as copper contained in the above-mentioned electrolytic copper plating solution are precipitated on the above-mentioned metal particle layer provided at the cathode, or the surface of the electroless copper plating layer formed by the above-mentioned electroless copper plating, thereby forming an electrolytic copper plating layer.
[0074] Examples of the copper electroplating solution include, for example, copper electroplating solutions containing copper sulfide, sulfuric acid, and an aqueous medium. Specifically, examples include copper electroplating solutions containing copper sulfate, sulfuric acid, and an aqueous medium.
[0075] The copper electroplating solution is preferably used at a temperature in the range of 20 to 98°C.
[0076] Among the above-mentioned plating methods, electroplating copper is preferred because it does not use highly toxic substances and has good workability. In addition, electroplating copper can shorten the plating time compared to electroless copper plating, and the control of the plated film thickness is easy, so it is preferred.
[0077] The thickness of the copper-plated layer formed by the copper plating method is preferably in the range of 0.5 to 30 μm due to its excellent electric field shielding properties. In addition, when the copper-plated layer is formed by the electroplating method, the thickness of the layer can be adjusted by controlling the treatment time, current density, and the amount of plating additives used in the plating treatment process.
[0078] The nickel-plated layer constituting the shielding layer of the present invention can be used to shield magnetic field noise. In addition, the nickel-plated layer can also be used to prevent oxidation degradation and corrosion of the surface of the copper-plated layer. As a method for forming the nickel-plated layer, for example, wet plating methods such as electroless nickel plating and electroplating nickel can be cited, and these plating methods can also be combined to form the nickel-plated layer. From the perspective of excellent magnetic field shielding properties, the nickel layer is preferably formed by electroplating nickel.
[0079] It is also possible to stack plating layers of different metals on the nickel-plated layer. For example, if a gold-plated layer, a tin-plated layer, or a chrome-plated layer is provided, corrosion of the surface of the nickel-plated layer can be prevented. In addition, the metal particle layer may be formed on the nickel-plated layer as a protective film. As the metal particle layer, for example, a silver nanoparticle layer may be cited. Furthermore, a resin film may be formed on the nickel-plated layer as a protective film. As the resin film, the resins exemplified as the polymer adhesion layer may be cited.
[0080] The thickness of the nickel plating layer formed by the above-mentioned nickel plating method is preferably in the range of 0.5 to 10 μm because of excellent magnetic field shielding properties.
[0081] Next, a method for manufacturing an electronic component package of the present invention is described. As a manufacturing method, for example, the following manufacturing method can be cited: a dispersion containing metal particles is applied to the surface of a sealed body of an electronic component package having an electronic component mounted on a circuit substrate having a ground pattern and a sealed body that seals the electronic component and has an epoxy resin, and the dispersion is dried to form a metal particle layer, a copper plating layer is formed on the metal particle layer by one or more selected from the group consisting of electroless copper plating and electrolytic copper plating, and a nickel plating layer is formed by one or more selected from the group consisting of electroless nickel plating and electrolytic nickel plating, thereby forming a shielding layer having a metal particle layer, a copper plating layer, and a nickel plating layer.
[0082] Here, as a manufacturing method, a fluid containing a polymer is coated on the surface of the above-mentioned sealing body and dried to form a polymer layer, a dispersion containing metal particles is coated on the above-mentioned polymer layer and dried to form a metal particle layer, and then, a manufacturing method of forming the above-mentioned shielding layer having the above-mentioned copper plating layer and nickel plating layer is preferred because the above-mentioned sealing body and the above-mentioned shielding layer have excellent adhesion.
[0083] The polymer layer is preferably provided on the entire surface of the sealing body in the form of a thin film, but in order to connect the ground pattern of the electronic component package and the shielding layer, it is preferred to avoid the ground pattern exposed from the sealing body and provide the polymer layer. In addition, the polymer layer is preferably not formed in the part of the electronic component package where the shielding layer is not formed. The so-called part of the electronic component package where the shielding layer is not formed includes, for example, the circuit substrate side of the electronic component package opposite to the shielding layer, the part where the solder ball is formed, and the predetermined part where the solder ball is to be formed.
[0084] As a method for forming the above-mentioned metal particle layer on the surface of the above-mentioned sealing body and the above-mentioned polymer adhesion layer, the method of coating or printing the metal particle dispersion liquid and the method of drying can be implemented by the above-mentioned exemplified methods. When the above-mentioned metal particles are nanoparticles such as silver nanoparticles, they can be dried by the above-mentioned method to fuse the metal particles with each other to form a conductive layer, which functions as a plating base layer in the above-mentioned electroplating, and is therefore preferred.
[0085] As a method for forming the above-mentioned polymer layer on the surface of the above-mentioned sealing body, a method of applying or printing a fluid containing a polymer or a method of drying can be implemented by the methods exemplified above, and the polymer can be cured by heating or using ultraviolet rays as needed to form the polymer layer.
[0086] In addition, in the manufacturing method of the above-mentioned electronic component package, as a method for forming a shielding layer before the above-mentioned electronic component package is singulated, the following manufacturing method can be listed: after the above-mentioned polymer layer is formed, a part of the above-mentioned sealing body is cut from the above-mentioned polymer layer in a manner that the above-mentioned ground pattern is exposed to form a slit portion at a predetermined dividing line, after a metal particle layer is formed on the surface of the above-mentioned polymer layer and the cut surface of the slit portion, a copper plating layer and a nickel plating layer are formed to form a shielding layer, and the electronic component is singulated using the above-mentioned slit portion.
[0087] The above-mentioned manufacturing method is preferable because it can efficiently manufacture the above-mentioned shielding layer for packaging a large number of the above-mentioned electronic components and has excellent productivity.
[0088] Here, the slit portion formed on the predetermined dividing line is provided to connect the ground pattern contained in the circuit substrate of the electronic component package and the shielding layer composed of a metal particle layer, a copper plating layer and a nickel plating layer. When forming the metal particle layer, it is preferred to apply a fluid containing metal particles in a manner that contacts the ground pattern to form the metal particle layer.
[0089] The slits formed on the planned dividing lines may be formed before the electronic component package is sealed or after the electronic component package is sealed and fixed to a support. The support may be made of the same material as the temporary fixing substrate described below.
[0090] In addition, in the manufacturing method of the above-mentioned electronic component package, as a method for forming a shielding layer after the above-mentioned electronic component package is singulated, the following manufacturing method can be listed: after the above-mentioned polymer layer is formed, the electronic components sealed by the sealed body are singulated by cutting from the above-mentioned polymer layer, the singulated electronic components are temporarily fixed to a temporarily fixed substrate, after a metal particle layer is formed on the surface of the above-mentioned polymer layer of the singulated electronic components and the cut surface produced by cutting, a copper plating layer and a nickel plating layer are formed to form a shielding layer, after the above-mentioned shielding layer is grounded to the above-mentioned grounding pattern, the singulated electronic components are taken out from the above-mentioned temporarily fixed substrate.
[0091] Here, as the above-mentioned temporary fixing base material, for example, there can be cited a fluororesin adhesive film with a fluororesin film as a support as an adhesive sheet or adhesive film that is bonded to a support; a shielding adhesive tape for plating; a shielding tape for a printed circuit board; a dicing tape used in semiconductor wafer processing; a thermal release sheet for an electronic component process, etc. The above-mentioned temporary fixing base material can also be used for the purpose of protecting the above-mentioned portion where the above-mentioned shielding layer is not formed.
[0092] Next, the method of forming a copper-plated layer or a nickel-plated layer on the metal particle layer by electroplating or electroless plating can be implemented by the wet plating method exemplified above. In particular, when the electroplating method is used, it is preferred due to productivity, mechanical properties of the obtained metal film, cost, and excellent magnetic field shielding properties when nickel is plated.
[0093] The electronic component package of the present invention manufactured in this manner can be used as an electronic component package in the above-exemplified applications.
[0094] Example
[0095] Hereinafter, the present invention will be described in detail by way of examples.
[0096] (Preparation Example 1: Preparation of Metal Particle Dispersion Liquid)
[0097] In a mixed solvent of 30 parts by mass of ethylene glycol and 70 parts by mass of ion exchange water, a compound obtained by adding polyethylene oxide to polyethyleneimine was used as a dispersant to disperse silver particles having an average particle size of 30 nm, and then ion exchange water, ethanol and a surfactant were added to adjust the viscosity to 10 mPa·s to prepare a metal particle dispersion. It should be noted that the metal particle dispersion contains metal particles and a polymer dispersant having a basic group containing a nitrogen atom as a reactive functional group.
[0098] (Manufacturing Example 1: Manufacture of Resin for Polymer Layer)
[0099] In a reaction container equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, and a thermometer, 100 parts by mass of a polycarbonate polyol (a polycarbonate diol having an acid group equivalent of 1,000 g / equivalent obtained by reacting 1,4-cyclohexanedimethanol with a carbonate) 9.7 parts by mass of 2,2-dimethylolpropionic acid, 5.5 parts by mass of 1,4-cyclohexanedimethanol, and 51.4 parts by mass of dicyclohexylmethane diisocyanate were reacted in a mixed solvent of 111 parts by mass of methyl ethyl ketone to obtain an organic solvent solution of a urethane prepolymer having an isocyanate group at a molecular terminal.
[0100] Next, 7.3 parts by mass of triethylamine was added to the organic solvent solution of the polyurethane resin to neutralize part or all of the carboxyl groups of the polyurethane resin, and 355 parts by mass of water was further added and stirred sufficiently to obtain an aqueous dispersion of the polyurethane resin.
[0101] Next, 4.3 parts by mass of a 25% by mass aqueous solution of ethylenediamine was added to the aqueous dispersion and stirred to extend the chains of the polyurethane resin particles. The mixture was then aged and desolvated to obtain an aqueous dispersion of polyurethane resin having a solid content concentration of 30% by mass.
[0102] In a reaction vessel equipped with a stirrer, a reflux cooling tube, a nitrogen inlet tube, a thermometer, a dropping funnel for dropping a monomer mixture, and a dropping funnel for dropping a polymerization catalyst, 140 parts by mass of deionized water and 100 parts by mass of the aqueous dispersion of the polyurethane resin obtained above were placed, and the temperature was raised to 80° C. while blowing nitrogen. In the reaction vessel heated to 80° C., a monomer mixture containing 60 parts by mass of methyl methacrylate, 10 parts by mass of n-butyl acrylate, and 30 parts by mass of N-n-butoxymethyl acrylamide, and 20 parts by mass of an aqueous ammonium persulfate solution (concentration: 0.5% by mass) were dropped from each dropping funnel over 120 minutes while stirring and maintaining the temperature in the reaction vessel at 80±2° C., thereby performing polymerization.
[0103] After the addition was completed, the mixture was stirred at the same temperature for 60 minutes, and then the temperature in the reaction container was cooled to 40° C., and then deionized water was added so that the non-volatile component became 20% by mass, and then filtered with a 200-mesh filter cloth to obtain a polymer layer resin containing a carboxyl group and an N-n-butoxymethylacrylamide group as reactive functional groups.
[0104] (Preparation Example 2: Preparation of a Fluid Containing a Polymer Layer Resin)
[0105] 90 parts by mass of ethanol were mixed with 10 parts by mass of the polymer layer resin obtained in the production of the polymer layer resin, and stirred to obtain a fluid containing the polymer layer resin.
[0106] (Example 1)
[0107] The electronic components mounted on the circuit board with the ground pattern are sealed with a semiconductor sealing resin composition containing epoxy resin, phenolic resin curing agent and filler. The metal particle dispersion prepared in Preparation Example 1 is applied to the surface of the sealed body with a spray device (a spray device with a nozzle tip QTKA (flow size 0.1L / min) of a nozzle manufactured by Spraying Systems Japan Co., Ltd.) so that the thickness of the dried film as the metal particle layer becomes 150nm. Then, it is dried at 180°C for 10 minutes to form a metal particle layer. The surface resistance value of the metal particle layer is 4Ω / □.
[0108] Next, phosphorus-containing copper was set as an anode on the metal particle layer formed by the above method, and an electroplating solution containing copper sulfate was used at a current density of 2.5 A / dm 2 The copper electroplating was performed for 10 minutes to laminate a 5 μm thick copper plating layer on the surface of the metal particle layer. As the copper electroplating solution, 70 g / L of copper sulfate, 200 g / L of sulfuric acid, 50 mg / L of chloride ions, and 5 mL / L of an additive ("Top Lucina SF-M" manufactured by Okuno Pharmaceutical Industry Co., Ltd.) were used.
[0109] Next, on the copper-plated layer formed by the above method, nickel sulfate was supplied with nickel ions while a current density of 2 A / dm 2 Nickel electroplating was performed for 5 minutes to laminate a nickel plated layer with a thickness of 2 μm on the copper plated layer, thereby forming a shield layer.
[0110] (Example 2)
[0111] The electronic components mounted on the circuit board with the ground pattern were sealed with a semiconductor sealing resin composition containing epoxy resin, phenolic resin curing agent and filler. On the surface of the sealed body, the fluid containing the polymer layer resin prepared in Preparation Example 2 was applied with a spray device (a spray device equipped with a nozzle tip QTKA (flow size 0.1 L / min) of a nozzle manufactured by Spraying Systems Japan Co., Ltd.) so that the film thickness after drying as the polymer layer became 200 nm. Then, it was dried at 150°C for 10 minutes to form a polymer layer.
[0112] Next, the metal particle dispersion prepared in Preparation Example 1 was applied to the polymer layer formed by the above method using a spray device (a spray device equipped with a nozzle tip QTKA (flow rate size 0.1 L / min) manufactured by Spraying Systems Japan Co., Ltd.) so that the thickness of the metal particle layer after drying became 150 nm. Then, the metal particle layer was formed by drying at 180° C. for 10 minutes. The surface resistance value of the metal particle layer was 4Ω / □.
[0113] Next, copper electroplating and nickel electroplating were performed on the metal particle layer formed by the above method in the same manner as in Example 1 to form a barrier layer including a 5 μm thick copper plated layer and a 2 μm thick nickel plated layer.
[0114] (Example 3)
[0115] The electronic components mounted on the circuit substrate with a ground pattern are sealed with a semiconductor sealing resin composition containing an epoxy resin, a phenolic resin curing agent and a filler. Next, a shielding adhesive tape for plating is attached to the circuit substrate side of the sealed body of the sealed electronic components where the shielding layer is not formed. Next, a fluid containing the polymer layer resin prepared in Preparation Example 2 is applied to the surface of the sealed body using a spray device (a spray device having a nozzle tip QTKA (flow size 0.1 L / min) of a nozzle manufactured by Spraying Systems Japan Contract Co., Ltd.) so that the film thickness after drying as the polymer layer becomes 200 nm. Then, it is dried at 150°C for 10 minutes to form a polymer layer.
[0116] Next, the surface of the polymer layer formed by the above method was half-cut along the planned dividing line using a diamond knife of a dicing device to form a slit portion. It was confirmed that there was no polymer layer in the slit portion and the ground line of the circuit board was exposed.
[0117] Next, for the sealant formed with the polymer layer obtained above and half-cut to form the slit portion, the metal particle dispersion prepared in the preparation example 1 was printed. The metal particle dispersion was printed using an inkjet printer (inkjet tester EB100 manufactured by Konica Minolta IJ Co., Ltd., evaluation print head KM512L, discharge volume 14pL), initially printing along the slit portion, and then printing the entire surface of the sealant. Then, it was dried at 150°C for 10 minutes to form a metal particle layer. The film thickness of the metal particle layer was 80nm based on the average film thickness at each location.
[0118] Next, electroless copper plating was performed on the metal particle layer formed by the above method to form an electroless copper plating film with a thickness of 0.2 μm. It should be noted that the electroless copper plating was performed as follows: ARG copper (manufactured by Okuno Pharmaceutical Industry Co., Ltd.) was prepared in a bath under standard recommended conditions (ARG copper 1: 30 mL / L, ARG copper 2: 15 mL / L, ARG copper 3: 200 mL / L), and the bath temperature was maintained at 45° C. The substrate formed with the metal particle layer was immersed in the bath for 15 minutes to precipitate the copper plating film.
[0119] Next, electrolytic copper plating and electrolytic nickel plating were performed on the electroless copper plating layer formed by the above method in the same manner as in Example 1 to form a barrier layer including a 5 μm thick copper plating layer and a 2 μm thick nickel plating layer.
[0120] (Example 4)
[0121] The electronic components mounted on the circuit board with the ground pattern were sealed with a semiconductor sealing resin composition containing an epoxy resin, a phenolic resin curing agent and a filler. Next, a fluid containing a resin for the polymer layer (A-1) was applied to the surface of the sealed body using a spray device (a spray device having a nozzle tip QTKA (flow size 0.1 L / min) of a nozzle manufactured by Spraying Systems Japan Co., Ltd.) so that the film thickness after drying as the polymer layer became 200 nm. Then, it was dried at 120°C for 10 minutes to form a polymer layer.
[0122] Next, the surface of the polymer layer formed by the above method was cut into a size of 10 mm in the vertical direction and 10 mm in the horizontal direction along the dividing line using a diamond knife of a cutting device and then singulated. In the portion of the singulated sealed body contacted by the diamond knife, it was confirmed that there was no polymer layer and the grounding wire of the circuit substrate was exposed. Next, 40 singulated sealed bodies were attached to a thermal peeling sheet for electronic component process at intervals of 2 mm.
[0123] Next, the metal particle dispersion prepared in Example 1 was printed on the surface of the sealing body attached to the thermal release sheet for the electronic component process by the above method. The metal particle dispersion was printed using an inkjet printer (inkjet tester EB100 manufactured by Konica Minolta IJ Co., Ltd., evaluation print head KM512L, discharge volume 14 pL), and was also printed on the surface of the sealing body, the side cut out by cutting, and the surface of the thermal release sheet for the electronic component process to which the sealing body was attached. Then, it was dried at 100°C for 10 minutes to form a metal particle layer. The film thickness of the metal particle layer was 90nm in terms of the average film thickness at each location.
[0124] Next, electroless copper plating was performed on the metal particle layer formed by the above method in the same manner as in Example 3 to form an electroless copper plating layer having a thickness of 0.2 μm.
[0125] Next, electrolytic copper plating and electrolytic nickel plating were performed on the electroless copper plating layer formed by the above method in the same manner as in Example 1 to form a barrier layer including a 5 μm thick copper plating layer and a 2 μm thick nickel plating layer.
[0126] (Comparative Example 1)
[0127] The electronic components mounted on the circuit substrate with the ground pattern are sealed with a semiconductor sealing resin composition comprising an epoxy resin, a phenolic resin curing agent and a filler. In order to roughen the surface of the seal, hydrofluoric acid is used to dissolve the filler in the seal and perform a roughening treatment on the surface of the seal. The above-mentioned roughening treatment uses a reagent obtained by dissolving 150 g / L of ammonium fluoride in 1000 mL / L of 62% nitric acid. The roughening treatment temperature is set to 40 ° C, and the roughening treatment time is 20 minutes.
[0128] Next, the sealed body roughened by the above method was immersed in a catalyst solution of a tin dichloride protective colloid solution containing palladium as an electroless copper plating catalyst (an aqueous solution containing 40 mL / L of "Catalyst C" manufactured by Okuno Pharmaceutical Co., Ltd. and 180 mL / L of 35% hydrochloric acid) at 30° C. for 3 minutes. Next, the sealed body was immersed in an aqueous solution containing 100 mL / L of 98% sulfuric acid at 40° C. for 3 minutes to activate the electroless copper plating catalyst.
[0129] Next, electroless copper plating was performed on the sealed body subjected to the roughening treatment, provision of the electroless copper plating catalyst and activation treatment in the above-mentioned manner in the same manner as in Example 3 to form an electroless copper plating layer having a thickness of 0.2 μm.
[0130] Next, electrolytic copper plating and electrolytic nickel plating were performed on the electroless copper plating layer formed by the above method in the same manner as in Example 1 to form a barrier layer including a 5 μm thick copper plating layer and a 2 μm thick nickel plating layer.
[0131] (Comparative Example 2)
[0132] The electronic components mounted on the circuit board with the ground pattern were sealed with a semiconductor sealing resin composition containing an epoxy resin, a phenolic resin curing agent and a filler. The surface of the sealed body was sputtered by a film forming method of magnetron sputtering. By the sputtering method, a copper film with a thickness of 0.2 μm was formed.
[0133] Next, copper electroplating and nickel electroplating were performed on the copper film formed by the above method in the same manner as in Example 1 to form a barrier layer including a 5 μm thick copper plated layer and a 2 μm thick nickel plated layer.
[0134] <Measurement of Adhesion (Peel Strength) of Shielding Layer>
[0135] For the electronic component package formed with each shielding layer obtained above, the peel strength between the seal and the shielding layer was measured using "Autograph AGS-X 500N" manufactured by Shimadzu Corporation. It should be noted that the lead width used in the measurement was set to 1 mm and the peeling angle was set to 90°. In addition, the measurement of the peel strength in the present invention was implemented based on the measured value when the thickness of the shielding layer was 7 μm.
[0136] <Measurement of Adhesion Strength of Shielding Layer after Heating (Peel Test)>
[0137] The electronic component packages on which the shielding layers obtained above were formed were heated by being stored in a dryer set at 150° C. for 168 hours. After heating, the peel strength was measured by the same method as above.
[0138] <Evaluation of Heat Resistance>
[0139] Using the peel strength values before and after heating measured as described above, the retention rates before and after heating were calculated, and the heat resistance was evaluated based on the following criteria.
[0140] A: The retention rate is 80% or more.
[0141] B: The retention rate is 70% or more and less than 80%.
[0142] C: The retention rate is 50% or more and less than 70%.
[0143] D: The retention rate is less than 50%.
[0144] Table 1 shows the results of measuring the peel strength of the shield layer before and after heating and the results of evaluating the heat resistance of the electronic component packages on which the shield layers obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were formed.
[0145] [Table 1]
[0146]
[0147] The results shown in Table 1 confirm that the shielding layers obtained in Examples 1 to 4 of the electronic component package formed with the shielding layer of the present invention have high peel strength between the sealing body and the shielding layer, slight decrease in peel strength after heating, high retention rate of peel strength after heating, and excellent heat resistance.
[0148] On the other hand, the electronic component package having the shielding layer obtained in Comparative Example 1 is an example in which the metal plating film is formed after the sealing body is roughened, but it is confirmed that the peel strength is very low both before and after heating.
[0149] In addition, the electronic component package having the shield layer formed thereon obtained in Comparative Example 2 is an example in which a metal layer is formed on a support by sputtering and then metal plating is performed, but it was confirmed that the peel strength was extremely low both before and after heating.
[0150] Explanation of symbols
[0151] 1…Circuit board
[0152] 2…Shielding layer
[0153] 3…Metal Particle Layer
[0154] 4…Copper plating
[0155] 5…Nickel layer
[0156] 6…Ground pattern
[0157] 7…Wiring pattern
[0158] 8…Connection pad with another circuit board etc.
[0159] 9…Electronic components such as semiconductor devices
[0160] 10…Polymer layer.
Claims
1. A method for manufacturing an electronic component package, It is characterized in that A fluid containing a polymer is applied and dried on the surface of a sealed body of an electronic component package having an electronic component mounted on a circuit substrate having a ground pattern and a sealed body that seals the electronic component and has an epoxy resin to form a polymer layer, a dispersion liquid containing metal particles is applied and dried on the polymer layer to form a metal particle layer, a copper plating layer is formed on the metal particle layer by one or more selected from the group consisting of electroless copper plating and electrolytic copper plating, and a nickel plating layer is formed by one or more selected from the group consisting of electroless nickel plating and electrolytic nickel plating, thereby forming a shielding layer having a metal particle layer, a copper plating layer and a nickel plating layer, After the polymer layer is formed, the electronic components sealed by the sealed body are singulated by cutting from the polymer layer, and the singulated electronic components are temporarily fixed to a temporarily fixed substrate. After a metal particle layer is formed on the surface of the polymer layer of the singulated electronic components and the cut surface produced by cutting, a copper plating layer and a nickel plating layer are formed to form a shielding layer. After the shielding layer is grounded to the grounding pattern, the singulated electronic components are taken out from the temporarily fixed substrate.
Citation Information
Patent Citations
Electronic component package and its manufacturing method
JP2005109306A
Semiconductor Device And Manufacturing Method Of The Semiconductor Device
CN104064553A
Metallic copper dispersion, method for manufacturing same, and usage for same
CN105473259A
Stacked body, conductive pattern, electronic circuit, and production method for stacked body
CN105517788A
Moulded circuit module, and production method therefor
CN107006138A