Surface coating materials, films, stacked structures, display devices, and products

By using the surface coating material of the terpolymer in Chemical Formula 1, the long chain structure is used to provide the brush effect, which solves the problem in the existing technology that it is difficult to improve the durability and fingerprint resistance of the functional layer at the same time, and achieves low friction coefficient and High durability effect.

CN111689696BActive Publication Date: 2024-10-01SAMSUNG ELECTRONICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201911248418.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-12
Filing Date
2019-12-09
Publication Date
2024-10-01
Estimated Expiration
2039-12-09

AI Technical Summary

Technical Problem

The functional layer of the existing touch screen panel has a high friction coefficient and poor durability, and is easily worn out due to frequent contact. It is also difficult to improve the durability at the same time when improving fingerprint resistance.

Method used

A terpolymer represented by Chemical Formula 1 is used as the surface coating material, including alkylene groups, polyoxyalkylene groups and hydrolyzable silane groups, providing a brush effect through a long chain structure, reducing the friction coefficient and improving durability .

Benefits of technology

The durability and fingerprint resistance of surface coating materials are significantly improved, the friction coefficient is reduced, and the service life of the functional layer is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111689696B_ABST
    Figure CN111689696B_ABST
Patent Text Reader

Abstract

Disclosed are a surface coating material, a film, a stacked structure, a display device, and an article, wherein the surface coating material includes a compound represented by Chemical Formula 1, and the article includes a glass substrate coated with the surface coating material. In Chemical Formula 1, each substituent is the same as defined in the detailed description. [Chemical Formula 1]#imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2019-0028223 filed in the Korean Intellectual Property Office on March 12, 2019, the entire contents of which are incorporated herein by reference. Technical Field

[0003] Surface coating (coating) materials, films, stacked structures, display devices, and articles are disclosed. Background Art

[0004] Portable electronic devices such as smart phones or tablet PCs (personal computers) may include functional layers with different functions. In particular, recently, as touch screen panels that recognize contact positions using fingers or tools have become popular, functional layers may be applied on the surface of a display panel to improve the surface slipping properties and tactile feel of the touch screen panel.

[0005] However, such a functional layer has poor durability and may be easily worn or damaged by frequent contact, so that its function may be quickly lost. Summary of the invention

[0006] One embodiment provides a surface coating material capable of improving durability due to a low coefficient of friction.

[0007] Another embodiment provides a film capable of improving durability.

[0008] Another embodiment provides a stack structure including the film.

[0009] Another embodiment provides a display device including the film or the stack structure.

[0010] Another embodiment provides an article coated with the surface coating material.

[0011] According to one embodiment, the surface coating material includes a compound represented by Chemical Formula 1.

[0012] [Chemical formula 1]

[0013]

[0014] In Chemical Formula 1,

[0015] R 1 -R 3 are independently hydrogen, halogen, hydroxyl, or substituted or unsubstituted C1-C20 alkoxy,

[0016] R is hydrogen or a substituted or unsubstituted C1-C20 alkyl group,

[0017] L 1 is a single bond, *-O-*, *-C(=O)O-*, *-NH-(CH 2 ) p1 -C(=O)O-*, *-S-(CH 2 ) p2 -*, or *-S-(CH 2 ) p2 -O-*,

[0018] L 2 is a single bond, a substituted or unsubstituted C1-C20 alkylene group, *-C(=O)-*, *-C(=O)NH-*, *-C(=O)(CH 2 ) p3 NH-*,*-NHC(=O)NH-*,*-C(=O)(CH 2 ) p4 NH(CH 2 ) p5 NH-*, *-(CH 2 ) p6 S-*, or

[0019] p1-p6 are independently integers ranging from 1 to 20,

[0020] n0 is an integer of 1 or 2,

[0021] n1 and n2 are independently integers ranging from 3 to 20,

[0022] n3 is an integer in the range 3-23, and

[0023] m is an integer in the range of 1-5.

[0024] In example embodiments, the compound represented by Chemical Formula 1 includes groups (also referred to as "parts") corresponding to the following Chemical Formulas 1-1 to 1-3. The sum of the weight average molecular weights of the group represented by Chemical Formula 1-1, the group represented by Chemical Formula 1-2, and the group represented by Chemical Formula 1-3 may be in the range of about 380 g / mol to about 1600 g / mol.

[0025] [Chemical formula 1-1]

[0026]

[0027] [Chemical formula 1-2]

[0028]

[0029] [Chemical formula 1-3]

[0030]

[0031] In some embodiments, the weight average molecular weight of the group represented by Chemical Formula 1-2 may be greater than each weight average molecular weight of the groups represented by Chemical Formula 1-1 and Chemical Formula 1-3.

[0032] In some embodiments, the group represented by Chemical Formula 1-1 may have a weight average molecular weight of about 140 g / mol to about 280 g / mol, the group represented by Chemical Formula 1-2 may have a weight average molecular weight of about 159 g / mol to about 1188 g / mol, and the group represented by Chemical Formula 1-3 may have a weight average molecular weight of about 28 g / mol to about 322 g / mol.

[0033] According to another embodiment, the film may include a polycondensation product of a compound represented by Chemical Formula 1. Chemical Formula 1 may be the same as described above.

[0034] In some embodiments, the film may be a coated film or a deposited film.

[0035] In some embodiments, the film may have a water contact angle of about 60° to about 80° and an oil contact angle of less than about 50°.

[0036] According to another embodiment, a stack structure including a substrate and the film is provided.

[0037] According to another embodiment, a display device including the film or the stack structure is provided.

[0038] According to another embodiment, an article coated with the surface coating material is provided.

[0039] The friction coefficient of the functional layer may be reduced and thus the durability may be improved.

[0040] According to another embodiment, the surface coating material may include a compound represented by Chemical Formula 1A.

[0041] [Chemical Formula 1A]

[0042]

[0043] In Chemical Formula 1A,

[0044] R is hydrogen or a substituted or unsubstituted C1-C20 alkyl group,

[0045] L 1 is a single bond, *-O-*, *-C(=O)O-*, *-NH-(CH 2 ) p1 -C(=O)O-*, *-S-(CH 2 )p2 -*, or *-S-(CH 2 ) p2 -O-*,

[0046] L 2 is a single bond, a substituted or unsubstituted C1-C20 alkylene group, *-C(=O)-*, *-C(=O)NH-*, *-C(=O)(CH 2 ) p3 NH-*,*-NHC(=O)NH-*,*-C(=O)(CH 2 ) p4 NH(CH 2 ) p5 NH-*, *-(CH 2 ) p6 S-*, or

[0047] p1-p6 are independently integers ranging from 1 to 20,

[0048] n is an integer ranging from 3 to 20,

[0049] n0 is an integer of 1 or 2,

[0050] A' is a C4-C21 alkyl group,

[0051] B' is a C3-C23 alkylene group,

[0052] C' is a hydrolyzable silane moiety, and

[0053] m is an integer in the range of 1-5.

[0054] In some embodiments, A' in Chemical Formula 1A may be a group represented by Chemical Formula 1-1A. In Chemical Formula 1-1A, n1 may be an integer ranging from 3 to 20.

[0055] [Chemical Formula 1-1A]

[0056]

[0057] In some embodiments, B' in Chemical Formula 1A may be a group represented by Chemical Formula 1-3. In Chemical Formula 1-3, n3 may be an integer ranging from 3 to 23.

[0058] [Chemical formula 1-3]

[0059]

[0060] In some embodiments, C' in Formula 1A can be composed of *-SiR 1 R 2 R 3 Indicates that R1 -R 3 They may independently be hydrogen, halogen, hydroxy, or substituted or unsubstituted C1-C20 alkoxy.

[0061] In some embodiments, Chemical Formula 1A may include a group represented by Chemical Formula 1-2. In addition, n2 may be in the range of 3 to 20. The weight average molecular weight of the group represented by Chemical Formula 1-2 may be greater than the weight average molecular weight of group B' in Chemical Formula 1A.

[0062] [Chemical formula 1-2]

[0063]

[0064] In some embodiments, an article may include a substrate (eg, a glass substrate) coated with one of the foregoing surface coating materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0065] Figure 1 To show a cross-sectional view of a display device according to an embodiment,

[0066] Figure 2 To show a cross-sectional view of a display device according to another embodiment,

[0067] Figure 3 FT-IR graphs of the compound of Synthesis Example 1, polypropylene glycol (PPG) acrylate, and N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane,

[0068] Figure 4 is a cross-sectional view showing an article according to another embodiment, and

[0069] Figure 5 A diagram illustrating the structure of a thin film coated on a substrate according to another embodiment. DETAILED DESCRIPTION

[0070] Example embodiments of the present disclosure will be described in detail below and can be easily performed by a person having ordinary skills in the relevant field. However, the structure of the actual application can be embodied in many different forms and will not be construed as limited to the example embodiments set forth herein.

[0071] In the accompanying drawings, the thickness of layers, films, panels, regions, etc. is exaggerated for clarity. In the specification, the same reference numerals always represent the same elements. It will be understood that when an element such as a layer, film, region, or substrate is referred to as being "on" another element, it may be on the other element or there may be intermediate elements. On the contrary, when an element is referred to as being "directly on" another element, there are no intermediate elements.

[0072] In the drawings, parts that are not related to the description are omitted for clarity of the embodiments, and the same or similar constituent elements are denoted by the same reference numerals throughout the specification.

[0073] As used herein, "alkylene" may be an alkanediyl group. "Alkyl" may be, for example, methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, tert-butyl, pentyl, hexyl, and the like.

[0074] As used herein, when no definition is otherwise provided, "substituted" may refer to a compound or group in which a hydrogen atom is replaced by a halogen atom, a hydroxyl group, a nitro group, a cyano group, an amino group, an azido group, an amidino group, a hydrazine group, a hydrazone group, a carbonyl group, a carbamoyl group, a thiol group, an ester group, a carboxyl group or a salt thereof, a sulfonic acid group or a salt thereof, a phosphoric acid group or a salt thereof, a C1-C20 alkyl group, a C2-C20 alkenyl group, a C2-C20 alkynyl group, a C6-C30 aryl group, a C7-C30 aralkyl group, a C1-C30 alkoxy group, a C1-C20 heteroalkyl group, a C3-C20 heteroaralkyl group, a C3-C30 cycloalkyl group, a C3-C15 cycloalkenyl group, a C6-C15 cycloalkynyl group, a C3-C30 heterocycloalkyl group, or a combination thereof.

[0075] As used herein, when no definition is otherwise provided, “hetero” may refer to 1 to 4 heteroatoms including N, O, S, Se, Te, Si, or P.

[0076] As used herein, when a specific definition is not otherwise provided, "*" represents the same or different atoms (including hydrogen atoms) or points at which chemical formulae are linked.

[0077] Hereinafter, "combination" refers to a mixture of two or more and a stack structure of two or more.

[0078] Hereinafter, a surface coating material according to an embodiment is described.

[0079] The surface coating material according to an embodiment includes a compound represented by Chemical Formula 1.

[0080] [Chemical formula 1]

[0081]

[0082] In Chemical Formula 1,

[0083] R 1 -R 3 are independently hydrogen, halogen, hydroxyl, or substituted or unsubstituted C1-C20 alkoxy,

[0084] R is hydrogen or a substituted or unsubstituted C1-C20 alkyl group,

[0085] L 1 is a single bond, *-O-*, *-C(=O)O-*, *-NH-(CH 2 ) p1 -C(=O)O-*, *-S-(CH 2 ) p2 -*, or *-S-(CH 2 ) p2 -O-*,

[0086] L 2 is a single bond, a substituted or unsubstituted C1-C20 alkylene group, *-C(=O)-*, *-C(=O)NH-*, *-C(=O)(CH 2 ) p3 NH-*,*-NHC(=O)NH-*,*-C(=O)(CH 2 ) p4 NH(CH 2 ) p5 NH-*, or *-(CH 2 ) p6 S-*, or

[0087] p1-p6 are independently integers ranging from 1 to 20,

[0088] n0 is an integer of 1 or 2,

[0089] n1 and n2 are independently integers ranging from 3 to 20,

[0090] n3 is an integer in the range 3-23, and

[0091] m is an integer in the range of 1-5.

[0092] Preferably, R 1 -R 3 At least two (eg, two or three) of the groups are independently hydrogen, substituted or unsubstituted C1-C20 alkoxy, halogen, or hydroxy, more preferably substituted or unsubstituted C1-C20 alkoxy or halogen.

[0093] For example, p1-p6 may independently be integers ranging from 2-20 or 3-20.

[0094] Since a composition including a siloxane compound composed of an alkylene group and an oxyalkylene group (oxyalkylene) has a low friction coefficient and thus excellent anti-fingerprint property, many attempts have been made to use the composition as a surface coating material, but displays treated with the conventional surface coating material look worn compared to the initial display surface after about three months due to poor durability even when inspected with the naked eye.

[0095] Therefore, attempts have been made to enhance durability by using a composition using a perfluoropolyether silane compound instead of the siloxane compound as a surface coating material. However, here, the durability is enhanced, but there is a problem that fingerprint resistance, such as diffuse reflection due to dirty fingerprints on the surface coating material, is greatly deteriorated.

[0096] However, the surface coating material according to the embodiment includes the compound represented by Chemical Formula 1 and thus may exhibit excellent anti-fingerprint properties and at the same time exhibit significantly improved durability.

[0097] Specifically, the compound represented by Chemical Formula 1 has a ternary copolymer (a copolymer of three groups having numbers n1, n2, and n3, respectively) skeleton and the following linear form: wherein the groups having numbers n1 and n3 are alkylene groups, the group having number n2 is polyoxyalkylene groups, and a silane group (a hydrolyzable silane moiety) is included at one end, and is therefore arranged on a substrate subjected to surface coating in the form of a long chain having a large molecular weight, where, since the chain is long, the chain (group having number n1; alkylene group) at the side farther from the substrate lies down in parallel with the substrate and thus provides a so-called brush effect. Therefore, the friction coefficient is reduced, and ultimately, the durability of the substrate coated with the surface coating material according to the embodiment can be significantly improved. This effect is achieved due to the structure of the compound represented by Chemical Formula 1 having a ternary copolymer skeleton consisting of alkylene-polyoxyalkylene-alkylene groups. For example, a compound having a binary copolymer skeleton may hardly provide a brush effect or the like, and even if provided, the brush effect is very slight.

[0098] For example, in the compound represented by Chemical Formula 1, the sum of the weight average molecular weights of the group represented by Chemical Formula 1-1 (a group having the number n1; an alkylene group), the group represented by Chemical Formula 1-2 (a group having the number n2; a polyoxyalkylene group), and the group represented by Chemical Formula 1-3 (a group having the number n3; an alkylene group) may be in the range of about 380 g / mol to about 1600 g / mol. When the sum of the weight average molecular weights of the three groups is within the range, the durability of the surface coating material including the compound may be further improved.

[0099] [Chemical formula 1-1]

[0100]

[0101] [Chemical formula 1-2]

[0102]

[0103] [Chemical formula 1-3]

[0104]

[0105] When the sum of the weight average molecular weights of the three groups is less than about 380 g / mol, the chain is not long enough to provide a brush effect, and thus, durability may not be improved due to deterioration of the friction coefficient, and when the sum of the weight average molecular weights of the groups is greater than about 1600 g / mol, the compound of the terpolymer skeleton represented by Chemical Formula 1 may be almost impossible to synthesize.

[0106] For example, the weight average molecular weight of the group represented by Chemical Formula 1-2 may be greater than each weight average molecular weight of the groups represented by Chemical Formula 1-1 and Chemical Formula 1-3. When the group represented by Chemical Formula 1-2 among the three groups has a larger weight average molecular weight than the other two groups, the chain at the side farther from the substrate, i.e., the alkylene group at the terminal of the compound, can easily lie parallel to the substrate and thus greatly improve durability.

[0107] For example, the group represented by Chemical Formula 1-1 may have a weight average molecular weight of about 140 g / mol to about 280 g / mol, the group represented by Chemical Formula 1-2 may have a weight average molecular weight of about 159 g / mol to about 1188 g / mol, such as 330 g / mol to 1188 g / mol, and the group represented by Chemical Formula 1-3 may have a weight average molecular weight of about 28 g / mol to about 322 g / mol.

[0108] The compound represented by Chemical Formula 1 has an alkyl group and a hydrolyzable silane moiety at each end and thus may be aligned in one direction, for example, in a direction perpendicular to a substrate coated with the surface coating material due to a surface energy difference at both ends.

[0109] The hydrolyzable silane moiety may be a silane group substituted by at least one hydrolyzable functional group, such as a silane group substituted by at least one substituted or unsubstituted C1-C20 alkoxy group, halogen, or hydroxyl group. The hydrolyzable silane moiety may be bonded to the substrate or underlying layer by hydrolysis and / or polycondensation during the coating or deposition process.

[0110] The group represented by Chemical Formula 1-2 among the three groups constituting the terpolymer may form a non-covalent interaction with an adjacent molecule. The non-covalent interaction is not a covalent bond and may be, for example, a hydrogen bond. In addition, in Chemical Formula 1, 1 and L 2 The linking groups represented by may also form non-covalent interactions such as hydrogen bonds with neighboring molecules (however, except for the following: L 1 Can be a single bond and L 2(may be an alkylene group).

[0111] For example, in Formula 1, R 1 -R 3 may be independently substituted or unsubstituted C1-C20 alkoxy, L 1 It can be *-C(=O)O-*, *-NH-(CH 2 ) p1 -C(=O)O-*, *-S-(CH 2 ) p2 -*, or *-S-(CH 2 ) p2 -O-*, and L 2 It may be a substituted or unsubstituted C1-C20 alkylene group, *-C(=O)-*, *-C(=O)NH-*, *-C(=O)(CH 2 ) p3 NH-*,*-NHC(=O)NH-*,*-C(=O)(CH 2 ) p4 NH(CH 2 ) p5 NH-*, or *-(CH 2 ) p6 S-*, and p1-p6 are independently integers ranging from 1-10, or 2-10, or 3-10.

[0112] According to another embodiment, the surface coating material may include a compound represented by Chemical Formula 1A.

[0113] [Chemical Formula 1A]

[0114]

[0115] In Chemical Formula 1A,

[0116] R is hydrogen or a substituted or unsubstituted C1-C20 alkyl group,

[0117] L 1 is a single bond, *-O-*, *-C(=O)O-*, *-NH-(CH 2 ) p1 -C(=O)O-*, *-S-(CH 2 ) p2 -*, or *-S-(CH 2 ) p2 -O-*,L 2 is a single bond, a substituted or unsubstituted C1-C20 alkylene group, *-C(=O)-*, *-C(=O)NH-*, *-C(=O)(CH 2 ) p3NH-*,*-NHC(=O)NH-*,*-C(=O)(CH 2 ) p4 NH(CH 2 ) p5 NH-*, *-(CH 2 ) p6 S-*, or p1-p6 are independently an integer ranging from 1-20, n is an integer ranging from 3-20, n0 is an integer ranging from 1 or 2, A' is a C4-C21 alkyl group, B' is a C3-C23 alkylene group, C' is a hydrolyzable silane moiety, and m is an integer ranging from 1-5.

[0118] A′ in Chemical Formula 1A may be a group represented by Chemical Formula 1-1A.

[0119] [Chemical Formula 1-1A]

[0120]

[0121] In Chemical Formula 1-1A, n1 is an integer ranging from 3 to 20.

[0122] B' in Chemical Formula 1A may be a group represented by Chemical Formulas 1-3 discussed above.

[0123] C' in Chemical Formula 1A can be composed of *-SiR 1 R 2 R 3 Indicates that R 1 -R 3 They may independently be hydrogen, halogen, hydroxy, or substituted or unsubstituted C1-C20 alkoxy.

[0124] Chemical Formula 1A may include a group represented by Chemical Formula 1-2. The weight average molecular weight of the group represented by Chemical Formula 1-2 may be greater than the weight average molecular weight of the group B' in Chemical Formula 1A.

[0125] According to another embodiment, a film including a polycondensation product of the compound represented by Chemical Formula 1 or 1A is provided.

[0126] In the compound represented by Chemical Formula 1 used to form the polycondensation product, the sum of the weight average molecular weights of the group represented by Chemical Formula 1-1, the group represented by Chemical Formula 1-2, and the group represented by Chemical Formula 1-3 may be in the range of about 380 g / mol to about 1600 g / mol. As described above, when the sum of the weight average molecular weights of the three groups is within the range, the durability of the surface coating material can be further improved.

[0127] For example, the weight average molecular weight of the group represented by Chemical Formula 1-2 may be greater than each weight average molecular weight of the groups represented by Chemical Formula 1-1 and Chemical Formula 1-3. Among the three groups, the group represented by Chemical Formula 1-2 has a larger weight average molecular weight than the other two groups, and the chain at the side farther from the substrate, that is, the alkylene group at the terminal, can easily lie down in a direction parallel to the substrate and thus further improve durability.

[0128] For example, the group represented by Chemical Formula 1-1 may have a weight average molecular weight of about 140 g / mol to about 280 g / mol, the group represented by Chemical Formula 1-2 may have a weight average molecular weight of about 159 g / mol to about 1188 g / mol, such as 330 g / mol to 1188 g / mol, and the group represented by Chemical Formula 1-3 may have a weight average molecular weight of about 28 g / mol to about 322 g / mol.

[0129] The aforementioned surface coating material can be formed into a film via coating by a solution process or via deposition by a dry process. Therefore, the film can be a coated film or a deposited film. According to one embodiment, a process for coating the surface coating material on a substrate such as a glass substrate (glass plate) is provided. Here, a primer layer can be further provided on the glass substrate. Specifically, the coated film can be obtained as follows: for example, a surface coating material dissolved or dispersed in a solvent is coated by a method of spin coating, slit coating, inkjet printing, or dipping, and then dried. The deposited film can be obtained, for example, by a method of thermal deposition, vacuum deposition, or chemical vapor deposition (CVD).

[0130] The film may be formed on a substrate and the substrate may be, for example, a ceramic or glass plate, but is not limited thereto.

[0131] Here, the hydrolyzable silane moiety of the compound represented by Chemical Formula 1 or its polycondensation product may be bonded at the substrate, and the alkyl group may be arranged at the surface (air). The compound represented by Chemical Formula 1 or its polycondensation product may be arranged in a direction substantially perpendicular to the substrate.

[0132] The compound represented by Chemical Formula 1 or a polycondensation product thereof is the same as above.

[0133] By including a compound represented by Chemical Formula 1, the film may have a low contact angle. Therefore, satisfactory slip properties, fingerprint resistance, and durability can be obtained. The film may, for example, have a contact angle of about 60° to about 80°, and, for example, less than or equal to about 79° within the range. Here, the contact angle can be measured using a sessile drop technique. The liquid for measuring the contact angle may be water, and a drop shape analyzer (DSA100, KRUSS, Germany) is used to measure the contact angle by dropping a desired (and / or alternatively predetermined) amount of (about 3ul) water droplets on the film.

[0134] On the other hand, the contact angle of the film can be measured by using diiodomethane instead of water. Here, for example, the contact angle can be less than about 50 °, for example, less than or equal to about 49 °. Here, the contact angle can be measured by using a sessile drop technique. The liquid for measuring the contact angle can be diiodomethane, and a drop shape analyzer (DSA100, KRUSS, Germany) is used to measure the contact angle by dropping (about 3ul) of diiodomethane of a desired (and / or alternatively predetermined) amount on the surface of the film.

[0135] The substrate and the film may form a stacked structure.

[0136] The stack structure may further include at least one layer between the substrate and the film.

[0137] The stacked structure may be a transparent film such as a transparent flexible film.

[0138] For example, the film or the stacked structure may be attached to a display panel. Here, the display panel and the film or the stacked structure may be directly combined or may be combined by inserting an adhesive. The display panel may be, for example, a liquid crystal panel or an organic light emitting panel, but is not limited thereto. The film or the stacked structure may be disposed on the observer side.

[0139] Figure 1 is a cross-sectional view of a display device according to an embodiment.

[0140] Reference Figure 1 , a display device 100 according to an embodiment includes a display panel 50 and a functional film 10A.

[0141] The display panel 50 may be, for example, an organic light emitting panel or a liquid crystal panel, such as a bendable display panel, a foldable display panel, or a rollable display panel.

[0142] The functional film 10A may include the film or stacked structure and may be disposed on the observer side.An additional layer may be further disposed between the display panel 50 and the functional film 10A and may include, for example, a single layer or multiple layers of a polymer layer and an optional transparent adhesive layer (not shown).

[0143] Figure 2 is a cross-sectional view of a display device according to another embodiment.

[0144] Reference Figure 2 , the display device 200 according to the present embodiment includes a display panel 50 , a functional film 10A, and a touch screen panel 70 provided between the display panel 50 and the functional film 10A.

[0145] The display panel 50 may be, for example, an organic light emitting panel or a liquid crystal panel, such as a bendable display panel, a foldable display panel, or a rollable display panel.

[0146] The functional film 10A may include the film or the stack structure and may be disposed on the observer side.

[0147] The touch screen panel 70 may be disposed adjacent to each of the functional film 10A and the display panel 50 to recognize a touched position and position change when touched by a human hand or an object through the functional film 10A and then output a touch signal. A driving module (e.g., a circuit, not shown) may monitor the touched position by the output touch signal, recognize an icon at the touched position, and control to execute a function corresponding to the recognized icon, and the function execution result is displayed on the display panel 50.

[0148] Additional layers may be further disposed between the touch screen panel 70 and the functional film 10A and may include, for example, a single layer or multiple layers of a polymer layer (not shown) and an optional transparent adhesive layer (not shown).

[0149] Additional layers may be further interposed between the touch screen panel 70 and the display panel 50 and may include, for example, a single layer or multiple layers of a polymer layer (not shown) and an optional transparent adhesive layer (not shown).

[0150] The functional film 10A including the aforementioned film or stacked structure may be applied to various electronic devices such as display devices such as smartphones, tablet PCs, cameras, touch screen devices, etc., but is not limited thereto.

[0151] Figure 4 The display article 100 includes a substrate 110 (eg, a glass substrate) coated with a functional film 10A including the aforementioned surface coating material and an optional primer layer 120 .

[0152] Another embodiment provides a product manufactured by coating the aforementioned surface coating material on a substrate such as a glass substrate (glass plate). Here, the product may include a mobile display device, a monitor, a television screen, a touch screen, an automobile glass, etc., but is not limited thereto.

[0153] Hereinafter, the embodiments are described in more detail with reference to Examples. However, these Examples are non-limiting, and the present scope is not limited thereto.

[0154] Synthesis Example: Preparation of Terpolymer

[0155] The terpolymers according to Synthesis Examples 1 to 35 are all terpolymers sequentially including A1 (alkylene), B (polyoxyalkylene), and A2 (alkylene). In Synthesis Examples 1 to 35, n is an integer ranging from 3 to 20, and n varies with the weight average molecular weight of the polyalkylene glycol compound.

[0156] Synthesis Example 1

[0157] (1) 40 ml of a chloroform solution in which 4.75 g (0.01 mol) of poly(propylene glycol) acrylate and 2.02 g (0.02 mol) of triethylamine were dissolved was placed in a 100 ml round-bottom flask equipped with a dropping funnel and a magnetic stirrer at room temperature. Subsequently, 2.1876 g (0.01 mol) of lauroyl chloride was added dropwise thereto, and the mixture was reacted at room temperature for 6 hours. The reaction product therefrom was washed three times with deionized water, and the organic layer therein was washed with anhydrous magnesium sulfate (anhydrous MgSO 4 After evaporation of chloroform, alkyl poly(propylene glycol) acrylate was obtained as a binary copolymer under reduced pressure (yield: about 90%).

[0158] (2) 0.8 g of the alkyl poly(propylene glycol) acrylate obtained in the step (1) was placed in a 5 ml vial, 0.4072 g of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane was added thereto, and the mixture was reacted at 60° C. for 3 hours to prepare a terpolymer having a silane group at the terminal (silane-terminated (terminated) triblock copolymer).

[0159]

[0160] Figure 3 It is the FT-IR chart of the compound poly(propylene glycol) acrylate and N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane of Synthesis Example 1.

[0161] Synthesis Example 2

[0162] Synthesis was performed according to the same method as Synthesis Example 1, except that 0.3548 g of 11-aminoundecyltrimethoxysilane was used instead of 0.4072 g of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane.

[0163]

[0164] Synthesis Example 3

[0165] (1) 33.173 g (0.0415 mol) of poly(propylene glycol) diacrylate (weight average molecular weight: 800 g / mol) was placed in a 100 ml round-bottom flask equipped with a magnetic stirrer. Subsequently, 2 g (0.0083 mol) of hexadecylamine was added thereto, and the mixture was reacted at 60° C. overnight. The reaction product therefrom was washed with hexane and extracted with acetonitrile to remove the polypropylene glycol diacrylate remaining therein. The acetonitrile extraction was repeated twice more to obtain a hexane layer, and the hexane was distilled off to obtain a binary copolymer.

[0166] (2) 0.5 g of the product obtained in step (1) (the binary copolymer) was reacted with 0.147 g of 11-aminoundecyltrimethoxysilane at 60° C. for 3 hours to prepare a ternary copolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0167]

[0168] Synthesis Example 4

[0169] Synthesis was performed according to the same method as Synthesis Example 1, except that 0.3539 g of N-(6-aminohexyl)aminopropyltrimethoxysilane was used instead of 0.4072 g of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane.

[0170]

[0171] Synthesis Example 5

[0172] (1) A binary copolymer was obtained according to the same method as in Synthesis Example 1, except that 3.0293 g of stearoyl chloride was used instead of 2.1876 g of lauroyl chloride.

[0173] (2) 0.8 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, 0.361 g of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane was added thereto, and the mixture was reacted at 60° C. for 3 hours to prepare a ternary copolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0174]

[0175] Synthesis Example 6

[0176] Synthesis was performed according to the same method as in Synthesis Example 5, except that 0.301 g of N-(6-aminohexyl)aminopropyltrimethoxysilane was used instead of 0.361 g of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane.

[0177]

[0178] Synthesis Example 7

[0179] Synthesis was performed according to the same method as in Synthesis Example 5, except that 0.3144 g of 11-aminoundecyltrimethoxysilane was used instead of 0.361 g of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane.

[0180]

[0181] Synthesis Example 8

[0182] Synthesis was performed according to the same method as in Synthesis Example 3, except that 0.1337 g of N-(6-aminohexyl)aminopropyltrimethoxysilane was used instead of 0.147 g of 11-aminoundecyltrimethoxysilane.

[0183]

[0184] Synthesis Example 9

[0185] Synthesis was performed according to the same method as in Synthesis Example 3, except that 0.1607 g of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane was used instead of 0.147 g of 11-aminoundecyltrimethoxysilane.

[0186]

[0187] Synthesis Example 10

[0188] (1) 40 ml of a chloroform solution in which 6.6 g (0.0044 mol) of poly(propylene glycol) allyl ether (weight average molecular weight: 1500 g / mol) and 0.809 g (0.008 mol) of triethylamine were dissolved was placed in a 100 ml round-bottom flask equipped with a dropping funnel and a magnetic stirrer at room temperature. Subsequently, 1.2117 g (0.004 mol) of a stearoyl chloride solution prepared by using 10 ml of chloroform as a solvent was added dropwise thereto, and the mixture was reacted at room temperature for 6 hours. The reaction product therefrom was washed three times with deionized water, and the organic layer therein was washed with anhydrous magnesium sulfate (anhydrous MgSO 4 After evaporating the chloroform, a binary copolymer was obtained under reduced pressure.

[0189] (2) 1 g of the binary copolymer obtained by step (1) was placed in a 5 ml vial, and 0.1834 g (0.0006 mol) of 11-mercaptoundecyltrimethoxysilane was added thereto. Subsequently, 0.5917 g of a solution prepared by dissolving 1 wt % of azobisisobutyronitrile (AIBN) in THF was added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0190]

[0191] Synthesis Example 11

[0192] (1) A 200 ml chloroform solution in which 17.6 g (0.0176 mol) of poly(propylene glycol) allyl ether (weight average molecular weight: 1000 g / mol) and 3.24 g (0.032 mol) of triethylamine were dissolved was placed in a 500 ml round-bottom flask equipped with a dropping funnel and a magnetic stirrer at room temperature. Subsequently, 4.8468 g (0.016 mol) of a stearoyl chloride solution prepared by using 50 ml of chloroform as a solvent was added dropwise thereto, and the mixture was reacted at room temperature for 6 hours. The reaction product therefrom was washed three times with deionized water, and then the organic layer therein was washed with anhydrous magnesium sulfate (anhydrous MgSO 4 After chloroform was evaporated therefrom, a binary copolymer was obtained under reduced pressure.

[0193] (2) 1 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, and 0.2558 g (0.0008 mol) of 11-mercaptoundecyltrimethoxysilane was added thereto. Subsequently, 0.628 g of a solution prepared by dissolving 1 wt % of AIBN in THF was added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a terpolymer having a silane group at the terminal (silane-terminated triblock copolymer).

[0194]

[0195] (In the general structures of Synthesis Examples 11 and 12, n is different from each other. n varies with the weight average molecular weight of the poly(propylene glycol) allyl ether.)

[0196] Synthesis Example 12

[0197] Synthesis was performed according to the same method as Synthesis Example 1, except that 0.2182 g of 3-aminopropyltrimethoxysilane was used instead of 0.4072 g of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane.

[0198]

[0199] Synthesis Example 13

[0200] (1) A 30 ml chloroform solution in which 2.6 g (0.004 mol) of polytetrahydrofuran (weight average molecular weight: 650 g / mol) and 0.81 g (0.008 mol) of triethylamine were dissolved was placed in a 100 ml round-bottom flask equipped with a dropping funnel and a magnetic stirrer at room temperature. Subsequently, 0.875 g (0.008 mol) of lauroyl chloride was added dropwise thereto, and the mixture was reacted at room temperature for 6 hours. The reaction product therefrom was washed three times with deionized water, and the organic layer therein was washed with anhydrous magnesium sulfate (anhydrous MgSO 4 After evaporating the chloroform, a binary copolymer was obtained under reduced pressure.

[0201] (2) 2.45 g of the binary copolymer obtained in step (1) dissolved in 2 g of ethyl acetate was placed in a 10 ml vial, and 0.6032 g of 3-isocyanatepropyltrimethoxysilane was added thereto. Dibutyltin dilaurate was used as a catalyst. The reactants were reacted at 60° C. for 3 hours to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0202]

[0203] Synthesis Example 14

[0204] (1) A binary copolymer was obtained according to the same method as in Synthesis Example 13 by using 1.2117 g of stearoyl chloride instead of 0.875 g of lauroyl chloride.

[0205] (2) 2.57 g of the binary copolymer obtained in step (1) dissolved in 2 g of ethyl acetate was placed in a 10 ml vial, and 0.5767 g of 3-isocyanatepropyltrimethoxysilane was added thereto. Dibutyltin dilaurate was used as a catalyst. The reactants were reacted at 60° C. for 3 hours to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0206]

[0207] Synthesis Example 15

[0208] (1) Polyoxyethylene (10) oleyl ether (Brij O10) was used as the binary copolymer.

[0209] (2) 2 g of the binary copolymer of step (1) dissolved in 2 g of ethyl acetate was placed in a 10 ml vial, and 0.5789 g of 3-isocyanatepropyltrimethoxysilane was added thereto. Dibutyltin dilaurate was used as a catalyst. The reactants were reacted at 70° C. for 3 hours to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0210]

[0211] Synthesis Example 16

[0212] (1) Polyoxyethylene (10) lauryl ether (Sigma Aldrich Co., Ltd.) was used as the binary copolymer.

[0213] (2) 2 g of the binary copolymer of step (1) dissolved in 2 g of ethyl acetate was placed in a 10 ml vial, and 0.6549 g of 3-isocyanatepropyltrimethoxysilane was added thereto. Dibutyltin dilaurate was used as a catalyst. The reactants were reacted at 70° C. for 3 hours to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0214]

[0215] Synthesis Example 17

[0216] (1) Polyoxyethylene (10) stearyl ether (Brij S10) was used as the binary copolymer.

[0217] (2) 2 g of the binary copolymer of step (1) dissolved in 4 g of ethyl acetate was placed in a 10 ml vial, and 0.5774 g of 3-isocyanatepropyltrimethoxysilane was added thereto. Dibutyltin dilaurate was used as a catalyst. The reactants were reacted at 70° C. for 3 hours to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0218]

[0219] Synthesis Example 18

[0220] (1) Polyoxyethylene (10) hexadecyl ether (Brij C10) was used as the binary copolymer.

[0221] (2) 1.33 g of the binary copolymer of step (1) dissolved in 4 g of ethyl acetate was placed in a 10 ml vial, and 0.4 g of 3-isocyanatepropyltrimethoxysilane was added thereto. Dibutyltin dilaurate was used as a catalyst. The reactants were reacted at 70° C. for 3 hours to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0222]

[0223] Synthesis Example 19

[0224] (1) Polyoxyethylene (4) lauryl ether (Brij L4) was used as the binary copolymer.

[0225] (2) 1 g of the binary copolymer of step (1) dissolved in 2 g of ethyl acetate was placed in a 10 ml vial, and 0.567 g of 3-isocyanatepropyltrimethoxysilane was added thereto. Dibutyltin dilaurate was used as a catalyst. The reactants were reacted at 70° C. for 3 hours to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0226]

[0227] Synthesis Example 20

[0228] (1) 15 g (0.021 mol) of polyoxyethylene (10) stearyl ether and 4.26 g (0.042 mol) of triethylamine were dissolved in 200 ml of dichloromethane. 3.82 g (0.042 mol) of acryloyl chloride was added dropwise thereto while stirring, and while adding, the temperature of the reactant was maintained at 0° C. to 5° C. Subsequently, after the mixture was stirred in an ice bath for 1 hour, the temperature was raised to 25° C., and the reactant was treated sequentially with 1 wt % aqueous hydrochloric acid solution (500 ml), water (500 ml), and 1 % aqueous sodium bicarbonate solution, and then with anhydrous magnesium sulfate (anhydrous MgSO 4 The dichloromethane was evaporated under reduced pressure to obtain a binary copolymer (off-white waxy solid).

[0229] (2) 1 g of the binary copolymer obtained in step (1), 0.4884 g of bis[3-(trimethoxysilyl)propyl]amine and a catalyst (ionic liquid [DABCO-PDO][Ac], 0.32 g of a 10 wt % ethanol solution) were mixed and reacted at 60° C. overnight.

[0230]

[0231] Synthesis Example 21

[0232] (1) A 100 ml chloroform solution in which 1.44 g (0.003 mol) of poly(ethylene glycol) allyl ether (weight average molecular weight: 480 g / mol) and 0.61 g (0.006 mol) of triethylamine were dissolved was placed in a 250 ml round-bottom flask equipped with a dropping funnel and a magnetic stirrer at room temperature. Subsequently, 0.9088 g (0.003 mol) of a stearoyl chloride solution prepared by using 50 ml of chloroform was added dropwise thereto, and the mixture was reacted at room temperature for 6 hours. The reaction product therefrom was washed three times with deionized water, and the organic layer therein was washed with anhydrous magnesium sulfate (anhydrous MgSO 4 After evaporation of chloroform under reduced pressure, a binary copolymer was obtained.

[0233] (2) 1.16 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, 10 μl of a platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex solution in xylene and 0.285 g (0.0023 mol) of trimethoxysilane were added thereto, and the mixture was purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0234]

[0235] Synthesis Example 22

[0236] (1) A binary copolymer was obtained according to the same method as step (1) of Synthesis Example 21, except that 2.25 g of poly(ethylene glycol) allyl ether (weight average molecular weight: 750 g / mol) was used instead of 1.44 g of poly(ethylene glycol) allyl ether (weight average molecular weight: 480 g / mol).

[0237] (2) 1.63 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, 10 μl of a platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex solution in xylene and 0.294 g (0.0024 mol) of trimethoxysilane were added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0238]

[0239] (In the general structures of Synthesis Examples 21 and 22, n is different from each other. n varies with the weight average molecular weight of the poly(ethylene glycol) allyl ether.)

[0240] Synthesis Example 23

[0241] 3.15g (0.028mol) potassium tert-butoxide and 10g (0.014mol) polyoxyethylene (10) stearyl ether (Brij S10) dissolved in 80ml tetrahydrofuran were mixed and stirred at 25°C for 30 minutes. 5.1g (0.042mol) allyl bromide was added to the mixture, and the obtained mixture was stirred again at 100°C for 5 hours. When the reaction was completed, the temperature was reduced to 25°C, and then the tetrahydrofuran was evaporated under reduced pressure. The undissolved material remaining after treating the residue with 100ml hot toluene was filtered and removed. Toluene was evaporated under reduced pressure, and unreacted allyl bromide was removed. The remaining material (oily residue) was dissolved in 300ml ethyl acetate, and then washed three times with 200ml water. The organic layer was washed with anhydrous magnesium sulfate (anhydrous MgSO 4 ) and dried, and ethyl acetate was evaporated under reduced pressure to obtain 9.9 g of a pale yellow oily binary copolymer.

[0242] (2) 5 g of the binary copolymer obtained in step (1) was placed in a 10 ml vial, 10 μl of a platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex solution in xylene and 1.222 g (0.01 mol) of trimethoxysilane were added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to obtain a ternary copolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0243]

[0244] Synthesis Example 24

[0245] (1) 1.95 g (0.017 mol) of potassium tert-butoxide and 10 g (0.0087 mol) of polyoxyethylene (20) stearyl ether (Brij S20) dissolved in 50 ml of tetrahydrofuran were mixed and stirred at 25° C. for 30 minutes. 2.02 g (0.0087 mol) of 11-bromo-1-undecene was added to the mixture, and the obtained mixture was stirred again at 100° C. for 48 hours. When the reaction was completed, the temperature was lowered to 25° C., and a 1 wt % aqueous hydrochloric acid solution was added thereto to adjust the pH to about 1. Then, tetrahydrofuran was evaporated under reduced pressure. The residue was dissolved using 250 ml of dichloromethane, and the solution was washed twice with 250 ml of water and 250 ml of an aqueous sodium bicarbonate solution. Dichloromethane was evaporated under reduced pressure. The residue was dissolved using 200 ml of methanol, and the solution was treated with charcoal and then filtered. After methanol was evaporated under reduced pressure, the residue was dissolved in 150 ml of toluene. The operation of evaporating toluene under reduced pressure at 90° C. was repeated twice. Nitrogen was introduced thereinto at 90° C. for 1 hour to remove the toluene residue and obtain a binary copolymer.

[0246] (2) 1 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, and 0.2468 g (0.0008 mol) of 11-mercaptoundecyltrimethoxysilane was added thereto. Subsequently, 0.6234 g of a solution prepared by dissolving 1 wt % of AIBN in THF was added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0247]

[0248] Synthesis Example 25

[0249] (1) 3.36 g (0.03 mol) of potassium tert-butoxide and 10.67 g (0.015 mol) of polyoxyethylene (10) stearyl ether (Brij S10) dissolved in 100 ml of tetrahydrofuran were mixed and stirred at 25° C. for 30 minutes. 3.5 g (0.015 mol) of 11-bromo-1-undecene was added thereto, and the obtained mixture was stirred again at 100° C. for 48 hours. When the reaction was completed, the temperature was cooled to 25° C., and a 1 wt % aqueous hydrochloric acid solution was added thereto to adjust the pH to about 1. Subsequently, tetrahydrofuran was evaporated under reduced pressure. After its residue was dissolved in 250 ml of dichloromethane, the solution was washed twice with 250 ml of water and 250 ml of an aqueous sodium bicarbonate solution. Dichloromethane was evaporated under reduced pressure. Its residue was dissolved using 200 ml of methanol, and the solution was treated with activated carbon and then filtered. Methanol was evaporated under reduced pressure, and the residue was dissolved in 150 ml of toluene. Toluene was evaporated under reduced pressure at 90° C., and this operation was repeated twice. Nitrogen was vented thereinto at 90° C. for 1 hour to remove the residual toluene and obtain a binary copolymer as a white waxy solid.

[0250] (2) 1 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, and 0.3752 g (0.0012 mol) of 11-mercaptoundecyltrimethoxysilane was added thereto. Subsequently, 0.6876 g of a solution prepared by dissolving 1 wt % of AIBN in THF was added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. to obtain a terpolymer including a silane group at the terminal (a silane-terminated triblock copolymer).

[0251]

[0252] Synthesis Example 26

[0253] 4.53 g of the binary copolymer according to step (1) of Synthesis Example 20 was placed in a 20 ml vial, and 1.98 g (0.0059 mol) of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane was added thereto. The mixture was stirred at 60° C. for 15 hours to obtain a terpolymer (light yellow waxy solid).

[0254]

[0255] Synthesis Example 27

[0256] (1) 10 g (0.0087 mol) of polyoxyethylene (20) stearyl ether and 1.75 g (0.0174 mol) of triethylamine were dissolved in 100 ml of a dichloromethane solution. While stirring, 1.57 g (0.0174 mol) of acryloyl chloride was added thereto in a dropwise manner, and while adding, the reactant was kept at 0° C. to 5° C. Subsequently, the mixture was stirred at 0° C. for 1 hour on an ice bath, heated to 25° C., treated sequentially with a 1 wt % aqueous hydrochloric acid solution (500 ml), water (500 ml), and a 1 % aqueous sodium bicarbonate solution, and treated with anhydrous magnesium sulfate (anhydrous MgSO 4 The dichloromethane was evaporated under reduced pressure to obtain a binary copolymer (off-white waxy solid).

[0257] 0.761 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, and 0.211 g (0.0063 mol) of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane was added thereto. The mixture was stirred at 60° C. for 15 hours to obtain a terpolymer (light yellow waxy solid).

[0258]

[0259] Synthesis Example 28

[0260] 1 g of the binary copolymer obtained in step (1) of Synthesis Example 25 was placed in a 5 ml vial, 10 μl of a platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex solution in xylene and 0.2123 g (0.00116 mol) of trimethoxysilane were added thereto, and the mixture was purged with nitrogen. The reaction was carried out at 60° C. overnight to obtain a ternary copolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0261]

[0262] Synthesis Example 29

[0263] (1) A 30 ml chloroform solution in which 2 g (0.0032 mol) of polyoxyethylene (10) lauryl ether and 0.646 g (0.0064 mol) of triethylamine were dissolved was placed in a 250 ml round-bottom flask equipped with a dropping funnel and a magnetic stirrer at room temperature. Subsequently, 0.6468 g (0.0032 mol) of undecenoyl chloride was added dropwise thereto, and the mixture was reacted at room temperature for 6 hours. The reaction product therefrom was washed three times with deionized water, and the organic layer therein was washed with anhydrous magnesium sulfate (anhydrous MgSO 4 The chloroform was evaporated under reduced pressure to obtain a binary copolymer.

[0264] 1.4589 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, 10 μl of a platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex solution in xylene and 0.3372 g (0.00276 mol) of trimethoxysilane were added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0265]

[0266] Synthesis Example 30

[0267] (1) 40.5 g (0.0646 mol) of polyoxyethylene (10) lauryl ether and 9.14 g (0.0905 mol) of triethylamine were dissolved in 500 ml of a dichloromethane solution. 7.01 g (0.0775 mol) of acryloyl chloride was added dropwise thereto while stirring, and while adding, the reactant was kept at 0° C. to 5° C. Subsequently, the mixture was stirred on an ice bath for 1 hour, heated to 25° C., treated (washed) with a 1 wt % aqueous hydrochloric acid solution (500 ml), water (500 ml), and a 1 % aqueous sodium bicarbonate solution in sequence, and washed with anhydrous magnesium sulfate (anhydrous MgSO 4 The dichloromethane was evaporated under reduced pressure to obtain a binary copolymer (off-white waxy solid).

[0268] (2) 1 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, and 0.4914 g (0.00147 mol) of N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane was added thereto. The mixture was stirred at 60° C. for 3 hours to obtain a ternary copolymer.

[0269]

[0270] Synthesis Example 31

[0271] 1 g of the binary copolymer obtained in step (1) of Synthesis Example 30 was placed in a 5 ml vial, and 0.4091 g (0.00147 mol) of N-(6-aminohexyl)-3-aminopropyltrimethoxysilane was added thereto. The mixture was stirred at 60° C. for 3 hours to obtain a ternary copolymer.

[0272]

[0273] Synthesis Example 32

[0274] 0.2 g of the binary copolymer obtained in step (1) of Synthesis Example 30 was placed in a 1 ml vial, and 0.0856 g (0.00029 mol) of 11-aminoundecyltrimethoxysilane was added thereto. The mixture was stirred at 60° C. for 3 hours to obtain a ternary copolymer.

[0275]

[0276] Synthesis Example 33

[0277] A 20 ml chloroform solution in which 2 g (0.008 mol) of poly(ethylene glycol) allyl ether (weight average molecular weight: 250 g / mol) and 1.619 g (0.016 mol) of triethylamine were dissolved was placed in a 50 ml round-bottom flask equipped with a dropping funnel and a magnetic stirrer at room temperature. Subsequently, 1.75 g (0.008 mol) of lauroyl chloride was added dropwise thereto, and the mixture was reacted at room temperature for 6 hours. The reaction product therefrom was washed three times with deionized water, and the organic layer therein was washed with anhydrous magnesium sulfate (anhydrous MgSO 4 The chloroform was evaporated under reduced pressure to obtain a binary copolymer.

[0278] 1 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, and 0.785 g (0.0025 mol) of 11-mercaptoundecyltrimethoxysilane was added thereto. Subsequently, 0.89 g of a solution obtained by dissolving 1 wt % of AIBN in THF was added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a terpolymer including a silane group at the terminal (a silane-terminated triblock copolymer).

[0279]

[0280] Synthesis Example 34

[0281] A binary copolymer was obtained according to the same method as in Synthesis Example 33, except that 2.423 g of stearoyl chloride was used instead of 1.75 g of lauroyl chloride.

[0282] 1 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, and 0.6109 g (0.0018 mol) of 11-mercaptoundecyltrimethoxysilane was added thereto. Subsequently, 0.8 g of a solution obtained by dissolving 1 wt % of AIBN in THF was added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0283]

[0284] Synthesis Example 35

[0285] 1 g of the binary copolymer obtained in step (1) of Synthesis Example 23 was placed in a 5 ml vial, and 0.4109 g (0.0013 mol) of 11-mercaptoundecyltrimethoxysilane was added thereto. Subsequently, 0.7 g of a solution obtained by dissolving 1 wt % of AIBN in THF was added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a terpolymer including a silane group at the terminal (silane-terminated triblock copolymer).

[0286]

[0287] Comparative Synthesis Example

[0288] Both of the binary copolymers according to Comparative Synthesis Examples 1 and 3 sequentially include B (polyoxyalkylene) and A2 (alkylene).

[0289] Comparative Synthesis Example 1

[0290] Commercially available 11-(2-methoxyethoxy)undecyltrimethoxysilane (Gelest, Inc.) was used.

[0291]

[0292] Comparative Synthesis Example 2

[0293] Commercially available perfluoropolyether silane OPTOOL UD509 (Daikin LLC.) was used.

[0294] Comparative Synthesis Example 3: Preparation of Binary Copolymer

[0295] A 200 ml chloroform solution in which 15 g (0.025 mol) of O-(2-aminopropyl)-O′-(2-methoxyethyl)propylene glycol (weight average molecular weight: 600 g / mol) and 4.0476 g (0.04 mol) of triethylamine were dissolved was placed in a 500 ml round-bottom flask equipped with a dropping funnel and a magnetic stirrer at room temperature. Subsequently, the mixture was moved to an ice bath, 5.068 g (0.025 mol) of 10-undecenoyl chloride was added dropwise thereto, and the reactant was reacted at room temperature for 3 hours. The reaction product therefrom was washed three times with deionized water, and the organic layer therein was washed with anhydrous magnesium sulfate (anhydrous MgSO 4 The chloroform was evaporated under reduced pressure to obtain a binary copolymer.

[0296] 1 g of the binary copolymer obtained in step (1) was placed in a 5 ml vial, 10 μl of a platinum (0)-1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex solution in xylene and 0.2407 g (0.00197 mol) of trimethoxysilane were added thereto, and the reactants were purged with nitrogen. The reaction was carried out at 70° C. overnight to prepare a binary copolymer including a silane group at the terminal (silane-terminated diblock copolymer).

[0297]

[0298] (n varies with the weight average molecular weight of O-(2-aminopropyl)-O'-(2-methoxyethyl)propanediol.)

[0299] Examples and Comparative Examples

[0300] Each copolymer of the Synthesis Example and the Synthesis Comparative Example was coated on a glass plate by electron beam vacuum deposition. Specifically, the copolymers obtained in the Synthesis Example and the Synthesis Comparative Example were placed in ethyl acetate or tetrahydrofuran solvent at a concentration of 50-70 wt %, and then mixed therewith to prepare a composition. Subsequently, the composition was electron beam vacuum deposited on a glass substrate to form The weight average molecular weights of the groups (A1, B, A2) in the copolymers used in the examples and comparative examples are shown in Table 1.

[0301] (Table 1)

[0302]

[0303]

[0304] Rating 1

[0305] The films of Examples 1-35 and Comparative Examples 1-3 were evaluated for durability.

[0306] The durability of the films was evaluated by measuring the contact angle.

[0307] The contact angle was evaluated by the sessile drop technique method and specifically by dropping water and diiodomethane on each film, respectively, and measuring using a drop shape analyzer (DSA100, KRUSS, Germany).

[0308] The friction coefficient was measured by using a FPT-F1 tester (Labthink Instruments Co., Ltd.).

[0309] The contact angle and friction coefficient results are shown in Table 2.

[0310] (Table 2)

[0311]

[0312]

[0313] Referring to Tables 1 and 2, the binary copolymer of Comparative Example 1 has a high friction coefficient and thus shows deteriorated durability compared to the terpolymers of Examples 1 to 35. In addition, even though the binary copolymer of Comparative Example 3 has a weight average molecular weight satisfying a specific range, the durability is still deteriorated compared to the terpolymer. In addition, referring to Comparative Example 2, when the perfluoro-based copolymer is used alone, the friction coefficient is reduced, but at the same time, its contact angle is significantly increased and thus causes a fingerprint smudging phenomenon, and therefore, diffuse reflection can easily occur.

[0314] Rating 2

[0315] The films of Example 1 and Comparative Examples 1 to 3 were evaluated for wear resistance. The wear resistance evaluation was performed by measuring the number of frictions until the film eased off by using a 6 mm wide polyurethane rubber with a load of 1 kg. The wear resistance evaluation results are shown in Table 3.

[0316] (Table 3)

[0317] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Number of frictions (times) 10000 1500 8000 3000

[0318] Referring to Table 3, the film of Example 1 exhibited excellent abrasion resistance compared with the films of Comparative Examples 1-3.

[0319] While the present disclosure has been described with respect to what are presently considered to be practical example embodiments, it will be understood that the inventive concepts are not limited to the disclosed embodiments. Rather, the inventive concepts are intended to cover various modifications and equivalent arrangements included within the spirit and scope of the appended claims.

[0320] <Description of Reference Numerals>

[0321] 10A: Functional film (layer)

[0322] 50: Display panel

[0323] 70: Touch screen panel

[0324] 100, 200: Display device

[0325] 110: Substrate

[0326] 120: Primer layer.

Claims

1. Surface coating materials, include: The compound represented by Chemical Formula 1: [Chemical formula 1] Wherein, in Chemical Formula 1, R 1 -R 3 are independently hydrogen, halogen, hydroxyl, or substituted or unsubstituted C1-C20 alkoxy, R is hydrogen or a substituted or unsubstituted C1-C20 alkyl group, L 1 is a single bond, *-O-*, *-C(=O)O-*, *-NH-(CH 2 ) p1 -C(=O)O-*, *-S-(CH 2 ) p2 -*, or *-S-(CH 2 ) p2 -O-*, L 2 is a single bond, a substituted or unsubstituted C1-C20 alkylene group, *-C(=O)-*, *-C(=O)NH-*, *-C(=O)(CH 2 ) p3 NH-*,*-NHC(=O)NH-*,*-C(=O)(CH 2 ) p4 NH(CH 2 ) p5 NH-*, *-(CH 2 ) p6 S-*, or p1-p6 are independently integers ranging from 1 to 20, n0 is an integer of 1 or 2, n1 is an integer in the range of 10-20, n2 is an integer in the range of 3-20, n3 is an integer in the range 3-23, and m is an integer in the range of 1-5.

2. The surface coating material according to claim 1, wherein the compound represented by Chemical Formula 1 comprises a portion represented by Chemical Formula 1-1, a portion represented by Chemical Formula 1-2, and a portion represented by Chemical Formula 1-3: [Chemical formula 1-1] [Chemical formula 1-2] [Chemical formula 1-3] and The sum of each weight average molecular weight of the moiety represented by Chemical Formula 1-1, the moiety represented by Chemical Formula 1-2, and the moiety represented by Chemical Formula 1-3 is in the range of 380 g / mol to 1600 g / mol. 3 . The surface coating material of claim 2 , wherein the weight average molecular weight of the moiety represented by Chemical Formula 1-2 is greater than each of the weight average molecular weights of the moieties represented by Chemical Formula 1-1 and Chemical Formula 1-3.

4. The surface coating material according to claim 2, wherein The weight average molecular weight of the part represented by Chemical Formula 1-1 is 140 g / mol to 280 g / mol, The weight average molecular weight of the part represented by Chemical Formula 1-2 is 159 g / mol to 1188 g / mol, and The weight average molecular weight of the moiety represented by Chemical Formula 1-3 is 42 g / mol to 322 g / mol.

5. Products, include: A glass substrate coated with the surface coating material according to any one of claims 1 to 4.

6. Membrane, include: A polycondensation product of a compound represented by Chemical Formula 1: [Chemical formula 1] Wherein, in Chemical Formula 1, R 1 -R 3 are independently hydrogen, halogen, hydroxyl, or substituted or unsubstituted C1-C20 alkoxy, R is hydrogen or a substituted or unsubstituted C1-C20 alkyl group, L 1 is a single bond, *-O-*, *-C(=O)O-*, *-NH-(CH 2 ) p1 -C(=O)O-*, *-S-(CH 2 ) p2 -*, or *-S-(CH 2 ) p2 -O-*, L 2 is a single bond, a substituted or unsubstituted C1-C20 alkylene group, *-C(=O)-*, *-C(=O)NH-*, *-C(=O)(CH 2 ) p3 NH-*,*-NHC(=O)NH-*,*-C(=O)(CH 2 ) p4 NH(CH 2 ) p5 NH-*, *-(CH 2 ) p6 S-*, or p1-p6 are independently integers ranging from 1 to 20, n0 is an integer of 1 or 2, n1 is an integer in the range of 10-20, n2 is an integer in the range of 3-20, n3 is an integer in the range 3-23, and m is an integer in the range of 1-5.

7. The film of claim 6, wherein Chemical Formula 1 comprises a portion represented by Chemical Formula 1-1, a portion represented by Chemical Formula 1-2, and a portion represented by Chemical Formula 1-3, [Chemical formula 1-1] [Chemical formula 1-2] [Chemical formula 1-3] and The sum of each weight average molecular weight of the moiety represented by Chemical Formula 1-1, the moiety represented by Chemical Formula 1-2, and the moiety represented by Chemical Formula 1-3 is in the range of 380 g / mol to 1600 g / mol. 8 . The film of claim 7 , wherein the weight average molecular weight of the moiety represented by Chemical Formula 1-2 is greater than each of the weight average molecular weights of the moieties represented by Chemical Formula 1-1 and Chemical Formula 1-3.

9. The film of claim 7, wherein The weight average molecular weight of the part represented by Chemical Formula 1-1 is 140 g / mol to 280 g / mol, The weight average molecular weight of the part represented by Chemical Formula 1-2 is 159 g / mol to 1188 g / mol, and The weight average molecular weight of the moiety represented by Chemical Formula 1-3 is 42 g / mol to 322 g / mol.

10. The film of claim 6, wherein the film is a coated film or a deposited film.

11. The film of claim 6, wherein the film has a water contact angle of 60° to 80° and an oil contact angle of less than 50°.

12. Stacked structure, including substrate, and A membrane as claimed in any one of claims 6 to 11.

13. A display device comprising the film according to any one of claims 6 to 11 or the stacked structure according to claim 12.

14. Surface coating materials, include: A compound represented by Chemical Formula 1A, [Chemical Formula 1A] Wherein, in Chemical Formula 1A, R is hydrogen or a substituted or unsubstituted C1-C20 alkyl group, L 1 is a single bond, *-O-*, *-C(=O)O-*, *-NH-(CH 2 ) p1 -C(=O)O-*, *-S-(CH 2 ) p2 -*, or *-S-(CH 2 ) p2 -O-*, L 2 is a single bond, a substituted or unsubstituted C1-C20 alkylene group, *-C(=O)-*, *-C(=O)NH-*, *-C(=O)(CH 2 ) p3 NH-*,*-NHC(=O)NH-*,*-C(=O)(CH 2 ) p4 NH(CH 2 ) p5 NH-*, *-(CH 2 ) p6 S-*, or p1-p6 are independently integers ranging from 1 to 20, n is an integer ranging from 3 to 20, n0 is an integer of 1 or 2, A' is a group represented by Chemical Formula 1-1A: [Chemical Formula 1-1A] In Chemical Formula 1-1A, n1 is an integer ranging from 10 to 20, B' is a C3-C23 alkylene group, C' is a hydrolyzable silane moiety, and m is an integer in the range of 1-5.

15. The surface coating material according to claim 14, wherein Chemical formula 1A includes a moiety represented by Chemical formula 1-2: [Chemical formula 1-2] n is in the range of 3-20, and The weight average molecular weight of the moiety represented by Chemical Formula 1-2 is greater than the weight average molecular weight of the group B' in Chemical Formula 1A.

16. Products, include: A glass substrate coated with the surface coating material according to any one of claims 14 to 15.