A wet pre-selection process for copper-containing magnetite ore
Through wet magnetic separation and hydrocyclone classification technology, the problem of copper elements being thrown out prematurely in the pre-selection process of copper-containing magnet ores has been solved, achieving efficient recovery of resources and reducing production costs, and improving the efficiency of mineral processing.
Patent Information
- Application Number
- CN202010720968.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-07-24
AI Technical Summary
In the pre-selection process of copper-containing magnet ores in the prior art, the copper element is thrown out prematurely, resulting in waste of resources and high beneficiation costs.
Wet magnetic separation process is used for pre-selection, combined with ball milling and hydrocyclone classification, and screening and closed-circuit grinding systems are used to achieve effective recovery of copper elements and comprehensive utilization of resources, reduce subsequent grinding volume and improve mineral processing efficiency.
It achieves the collection of copper elements as much as possible, reduces the cost of mineral processing, improves the grade of iron concentrate, avoids the loss of copper elements in the tailings, and improves production efficiency.
Smart Images

Figure CN111841880B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of magnetite ore dressing, and more specifically, relates to a wet pre-selection process for copper-containing magnetite ore. Background Art
[0002] With the acceleration of domestic mining resources mining speed year by year, my country's mining resources have become less rich ores, more poor ores, poor ore properties, fine crystal size, and difficult separation. Faced with the actual situation of "poor, fine, and mixed" ore, traditional mineral processing technology has gradually been replaced by efficient, intelligent and targeted design of mineral processing technology for different ore properties. With the deterioration of ore properties and the decrease of mining grade year by year, the operating cost of the mineral processing plant has been greatly affected. Due to the low grade of ore, the ore entering the mill has a low grade, a large amount of ore entering the mill, high grinding cost, and low efficiency. In view of this situation, the pre-grinding pre-selection process for poor ore has become an indispensable part of the mineral processing process of the mineral processing plant.
[0003] If the conventional magnetic pulley dry selection pre-selection tailings discarding technology is used for the raw iron ore containing copper magnetite, since chalcopyrite is a weakly magnetic mineral, it will enter the tailings together with the gangue minerals, resulting in a large loss of copper elements in the tailings, resulting in a waste of copper resources and affecting the economic benefits of the enterprise.
[0004] After searching, the Chinese patent publication number is CN107876214A, and the publication date is April 6, 2018. A method for separating copper-containing magnetite ore is disclosed, which solves the problems of high copper loss rate in magnetic separation operation and excessive sulfur content in iron concentrate in the traditional "first magnetic and then flotation" process. The technical scheme of the invention is carried out in the following manner: (1) After the raw ore is ground, a weak magnetic roughing is first performed, and a part of it is obtained by weak magnetic separation tailings, and a part of it enters the magnetic field screening machine for selection to obtain iron concentrate and magnetic field screening machine tailings; (2) The weak magnetic separation tailings and magnetic field screening machine tailings are flotated to obtain copper concentrate and tailings. The invention is aimed at copper-containing skarn-type magnetite ore, and the method of weak magnetic roughing-magnetic field screening machine selection is used to recover iron, and the magnetic separation tailings are then flotated to recover copper. However, the invention does not have a pre-selection operation, the raw ore is directly ground, and the "early throwing when possible" is not implemented, and the ore dressing cost is relatively high. Summary of the invention
[0005] 1. Problems to be solved
[0006] In view of the problem that the copper element is discarded too early in the pre-selection process of copper-containing magnetite ore in the prior art, resulting in waste of resources, the present invention provides a wet pre-selection process for copper-containing magnetite ore, which adopts wet magnetic separation, and screens the tailings separated by wet magnetic separation, and the above-screen products are sold as building materials; the under-screen products and a stage of ball mill discharge are fed to a hydrocyclone to form a closed-circuit grinding. The overflow product of the hydrocyclone enters the subsequent separation operation to separate magnetite and chalcopyrite. The present invention implements a pre-grinding pre-selection process for copper-containing magnetite and implements "early discarding when possible", which not only achieves the effect of energy saving and consumption reduction, but also comprehensively utilizes tailings as building materials, and also achieves the technical effect of collecting all the copper elements that should be collected.
[0007] 2. Technical solution
[0008] To solve the above problems, the present invention adopts the following technical solutions.
[0009] A wet pre-selection process for copper-containing magnetite ore, the steps are as follows:
[0010] Step 1: Crushing and screening: The copper-containing magnetite ore is crushed, and the crushed product is screened, and the screened product is the copper-containing magnetite ore crushed ore product;
[0011] Step 2, wet coarse particle selection and ball milling: the screened copper magnetite particles are subjected to wet magnetic separation, and the concentrate product after magnetic separation is fed into a ball mill for ball milling;
[0012] Step 3: Screening of tailings products: The tailings separated by wet magnetic separation are screened. The screened products have low copper content and can be directly discharged, which can reduce the grinding amount of subsequent ball milling operations, save mineral processing production costs, and avoid the loss of copper elements as much as possible;
[0013] Step 4: hydrocyclone classification: the discharged ore after ball milling in step 2 and the undersize product after screening in step 3 are fed into the hydrocyclone for classification, and the sediment of the hydrocyclone is returned to the ball mill for re-grinding; the overflow product of the hydrocyclone enters the subsequent separation operation for separation of magnetite and chalcopyrite.
[0014] Furthermore, it is suitable for copper-containing magnetite ores with a TFe content of not less than 20%, a magnetic rate of not less than 65%, and a copper content of not more than 0.12%. If this process is used when the copper content is too high, the loss of copper after tailings are discarded in step three is large, and it is impossible to achieve both the purpose of discarding the copper-containing magnetite as early as possible and recovering as much copper as possible.
[0015] Furthermore, in step one, a three-stage one-closed-circuit crushing process is adopted, and the crushing particle size is -12mm; in step two, the feed concentration is 30-40%, the magnetic field strength is 0.4-0.5T, and the feed concentration in the ball mill is 70-80%; in step three, the screened products after screening are sold as building materials, and the tailings are fully utilized.
[0016] Furthermore, the mesh size of the vibrating screen used for screening in step three is 0.5-0.8 mm, with 0.5 mm being the best. The products on the screen are discarded and the products under the screen are returned to the ball mill. The mesh size of 0.5 mm can enrich the copper element in the copper-containing magnetite ore, so as to achieve the goal of both early disposal of the copper-containing magnetite tailings and full recovery of the copper element in the tailings.
[0017] Furthermore, the undersize product of the vibrating screen and the discharge product of the ball mill are fed into the same pump pool and fed into the hydrocyclone through a slurry pump.
[0018] Furthermore, the magnetic separator is an internal magnetic separation downstream magnetic separator, and its feed particle size is preferably not higher than 12 mm; the ball mill is an overflow ball mill, and the ball mill and the hydrocyclone form an integrated closed-circuit grinding and grading system; the vibrating screen is preferably a linear vibrating screen.
[0019] 3. Beneficial effects
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] (1) A wet pre-selection process for copper-containing magnetite of the present invention adds a pre-selection screening process consisting of wet coarse particle magnetic separation and vibrating screen screening between finely crushed products and a first-stage ball milling and grading system, which not only realizes wet tailings discarding of copper-containing magnetite, reduces the grinding amount of subsequent ball milling operations, and saves ore dressing production costs, but also comprehensively utilizes the coarse particle tailings on the screen, and the underscreen products with high copper content are returned to the grinding and grading system, effectively avoiding the loss of copper metal in the tailings, and also achieving the effect of enriching copper elements, thereby achieving the purpose of reducing costs and increasing efficiency;
[0022] (2) A wet pre-selection process for copper-containing magnetite ore of the present invention is applicable to copper-containing magnetite ore with a TFe content of not less than 20%, a magnetic rate of not less than 65%, and a copper content of not more than 0.12%. The inventors found in actual application that if the copper content is too high, exceeding 0.12%, the copper loss after discarding the tailings in step 3 is large when using this process, and the technical effect of both discarding the copper-containing magnetite early and collecting the copper can be achieved. However, for copper-containing magnetite with a copper content of not more than 0.12%, the present process can increase the TFe percentage while keeping the copper loss below 0.005%, which is negligible.
[0023] (3) In a wet pre-selection process for copper-containing magnetite ore of the present invention, the mesh size of the vibrating screen for screening in step 3 is 0.5-0.8 mm, wherein the mesh size of 0.5 mm is optimal, the product on the screen is discarded, and the product under the screen is returned to the ball mill. The inventors have found in practice that the mesh size of 0.5 mm can enrich the copper element in the copper-containing magnetite ore, and can achieve the technical effect of both early discarding of the copper-containing magnetite tailings and full collection of the copper element in the tailings;
[0024] (4) In a wet pre-selection process for copper-containing magnetite ore of the present invention, the undersize product of the vibrating screen and the discharge product of the ball mill are fed into the same pump pool and fed into the hydrocyclone through a slurry pump, thereby achieving the purpose of automated cyclic production and improving production efficiency;
[0025] (5) In the wet pre-selection process of copper-containing magnetite ore of the present invention, the ball mill and the hydrocyclone form an integrated closed-circuit grinding and classification system, which has a circulating closed-circuit production and high grinding and classification efficiency; the vibrating screen is preferably a linear vibrating screen, which has high screening efficiency for the products of wet magnetic separation. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a pre-selection process flow chart of the present invention. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with specific embodiments and drawings.
[0028] Example 1
[0029] like Figure 1 As shown, the iron ore of this embodiment has a TFe grade of 38.45% in the raw iron ore, a magnetic iron content of 81.33% in the ore, and a copper content of 0.053%. The pre-selection process is as follows:
[0030] 1. Crushing: The raw ore is crushed by a three-stage one-closed-circuit crushing process. The particle size of the crushed product is -12mm (i.e., passing through a 12mm mesh sieve), and the sieved material is copper magnetite ore particles;
[0031] 2. Wet coarse particle selection and ball milling: The screened copper magnetite particles are subjected to wet magnetic separation, with a magnetic field strength of 0.45T and a feed concentration of 35%. The yield of the magnetic tailings product is 23.97% (TFe content 11.78%, Cu 0.10%); the TFe grade of the magnetic concentrate is 46.86%; the concentrate product after magnetic separation is fed into a ball mill for ball milling;
[0032] 3. Screening of tailings products: The tailings separated by wet magnetic separation are screened with a screen size of 0.5mm. The over-screen product with an original ore yield of 13.90% is sold as a building material product, reducing the grinding amount of subsequent ball milling operations; after testing, the TFe content in the product is only 11.14%, and the copper content is 0.078%; the under-0.5mm product has TFe11.78% and Cu0.13%, and the copper element is effectively enriched in the under-screen product; that is, the 13.90% over-screen tailings product accounts for a small proportion and has a low copper content, so it can be directly discharged as a building material, reducing the grinding amount of subsequent ball milling operations, saving the ore dressing production cost, and avoiding the loss of copper as much as possible;
[0033] 4. Hydrocyclone classification: The discharged ore and the discharged ore product after ball milling in step 2 are fed into the hydrocyclone for classification, and the sedimentation sand of the hydrocyclone is returned to the ball mill for regrinding. The grinding concentration of the ball mill is 70-80%, and the ball mill and the hydrocyclone form a closed circuit; the overflow product of the hydrocyclone enters the subsequent separation operation for magnetite and chalcopyrite separation. After testing, the yield of the overflow product of the hydrocyclone (to the original ore) is 86.10%, the TFe grade is 42.86%, and the Cu is 0.049%.
[0034] By adopting the pre-selection process of this embodiment, the TFe grade in the raw ore is increased by 4.41 percentage points, the Cu content is only reduced by 0.004 percentage points, and tailings with a yield of 13.90% are obtained (TFe content 11.14%, Cu content 0.078%, which can be sold as building materials products), thereby achieving the purpose of reducing costs and increasing efficiency.
[0035] Example 2
[0036] like Figure 1 As shown, the copper-containing magnetite ore of this embodiment has a TFe grade of 25.32%, a magnetic iron occupancy rate of 77.85% in the ore, and a copper content of 0.058%. The pre-selection process is as follows:
[0037] 1. Crushing: The raw ore is crushed by a three-stage one-closed-circuit crushing process. The particle size of the crushed product is -12mm (i.e., passing through a 12mm mesh sieve), and the sieved material is copper magnetite ore particles;
[0038] 2. Wet coarse particle selection and ball milling: The screened copper magnetite particles are subjected to wet magnetic separation, with a magnetic field strength of 0.48T and a feed concentration of 35%. The yield of the magnetic tailings product is 37.59% (TFe content 10.81%, Cu 0.098%); the TFe grade of the magnetic concentrate is 34.06%; the screened product of the concentrate product after magnetic separation is fed into a ball mill for ball milling;
[0039] 3. Screening of tailings products: The tailings separated by wet magnetic separation are screened with a screen size of 0.5mm. The over-screen product with an original ore yield of 20.67% is sold as a building material product, reducing the grinding amount of subsequent ball milling operations; after testing, the TFe content in the product is only 9.41%, and the copper content is 0.068%; the under-screen -0.5mm product has TFe12.53% and Cu0.135%, and the copper element is effectively enriched in the under-screen product; that is, the 20.67% over-screen tailings product accounts for a small proportion, and the copper content is low, so the tailings can be directly discharged as building materials, reducing the grinding amount of subsequent ball milling operations, saving the ore dressing production cost, and avoiding the loss of copper elements as much as possible;
[0040] 4. Hydrocyclone classification: The discharged ore and the discharged ore product after ball milling in step 2 are fed into the hydrocyclone for classification, and the sedimentation sand of the hydrocyclone is returned to the ball mill for regrinding. The grinding concentration of the ball mill is 70-80%, and the ball mill and the hydrocyclone form a closed circuit; the overflow product of the hydrocyclone enters the subsequent separation operation for magnetite and chalcopyrite separation. After testing, the yield of the overflow product of the hydrocyclone (to the original ore) is 79.33%, the TFe grade is 29.47%, and the Cu is 0.055%.
[0041] By adopting the pre-selection process of this embodiment, the TFe grade in the raw ore is increased by 4.15 percentage points, the Cu content is only reduced by 0.003 percentage points, and tailings with a yield of 20.67% are obtained (TFe content 9.41%, Cu content 0.068%, which can be sold as building materials products), thereby achieving the purpose of reducing costs and increasing efficiency.
[0042] Example 3
[0043] like Figure 1 As shown, the copper-containing magnetite ore of this embodiment has a TFe grade of 30.66%, a magnetic iron occupancy rate of 65.85% in the ore, and a copper content of 0.12%. The pre-selection process is as follows:
[0044] 1. Crushing: The raw ore is crushed by a three-stage one-closed-circuit crushing process. The particle size of the crushed product is -12mm (i.e., passing through a 12mm mesh sieve), and the sieved material is copper magnetite ore particles;
[0045] 2. Wet coarse particle selection and ball milling: The copper magnetite ore particles after screening are subjected to wet magnetic separation. The magnetic separator uses an internal magnetic separation downstream magnetic separator with a magnetic field strength of 0.5T and a feed concentration of 40%. The yield of the magnetic tailings product is 30.35% (TFe content 8.87%, Cu 0.138%). The TFe grade of the magnetic concentrate obtained is 35.36%. The screened product of the concentrate product after magnetic separation is fed into a ball mill for ball milling. The ball mill is an overflow type ball mill.
[0046] 3. Screening of tailings products: The tailings separated by wet magnetic separation are screened by linear vibrating screen with a screen size of 0.5mm. The over-screen product with an ore yield of 17.33% is sold as a building material product, reducing the grinding amount of subsequent ball milling operations. After testing, the TFe content in the product is only 9.78%, and the copper content is 0.128%; the under-0.5mm product has TFe 15.44% and Cu 0.225%, and the copper element is effectively enriched in the under-screen product; that is, the 17.33% over-screen tailings product accounts for a small proportion, and the copper content is low, so the tailings can be directly discharged as building materials, reducing the grinding amount of subsequent ball milling operations, saving the ore dressing production cost, and avoiding the loss of copper elements as much as possible.
[0047] 4. Hydrocyclone classification: the discharged ore and the discharged ore products after ball milling in step 2 are fed into the hydrocyclone for classification, the sedimentation of the hydrocyclone is returned to the ball mill for regrinding, the undersize product of the vibrating screen and the discharged ore products of the ball mill are fed into the same pump pool and fed into the hydrocyclone through a slurry pump, the grinding concentration of the ball mill is 70-80%, the ball mill and the hydrocyclone form a closed circuit, and constitute an integrated closed-circuit grinding and classification system; the overflow product of the hydrocyclone enters the subsequent separation operation for magnetite and chalcopyrite separation, and the yield of the overflow product of the hydrocyclone (to the original ore) is 82.67%, the TFe grade is 36.77%, and the Cu is 0.115%.
[0048] By adopting the pre-selection process of this embodiment, the TFe grade in the raw ore is increased by 6.11 percentage points, the Cu content is only reduced by 0.005 percentage points, and tailings with a yield of 17.33% are obtained (TFe content is 9.78%, Cu content is 0.128%, and can be sold as building materials products), thereby achieving the purpose of reducing costs and increasing efficiency.
[0049] Comparative Example
[0050] The copper-containing magnetite ore of this embodiment has a TFe grade of 31.16%, a magnetic iron occupancy rate of 68.15% in the ore, a copper element content of 0.13%, and the pre-selection process steps are the same as those of Example 3.
[0051] In step three, an over-screen product with an ore yield of 16.21% is obtained. After testing, the TFe content in the product is 10.22%, and the copper content is 0.147%. The product with a copper content of 0.147% has certain flotation and smelting value. If the product is sold as a building material, it will still cause a waste of copper. Therefore, combined with Example 3, if the copper content exceeds 0.12%, it is not suitable to use this process.
[0052] The examples described in the present invention are merely descriptions of the preferred implementation modes of the present invention, and are not intended to limit the concept and scope of the present invention. Without departing from the design concept of the present invention, various modifications and improvements made to the technical solutions of the present invention by engineers and technicians in this field should all fall within the protection scope of the present invention.
Claims
1. A wet pre-selection process for copper-containing magnetite ore, characterized in that: Here are the steps: Step 1: Crushing and screening: The copper-containing magnetite ore is crushed, and the crushed product is screened, and the screened product is the copper-containing magnetite ore particles; Step 2, wet coarse particle selection and ball milling: the copper-containing magnetite ore particles after screening are subjected to wet magnetic separation, and the magnetic separator is an internal magnetic separation downstream magnetic separator, and the concentrate product after magnetic separation is fed into a ball mill for ball milling; Step 3: Screening of tailings products: The tailings separated by wet magnetic separation are screened, and the mesh size of the vibrating screen is 0.5mm; Step 4: hydrocyclone classification: the discharged ore after ball milling in step 2 and the undersize product after screening in step 3 are fed into the hydrocyclone for classification, and the sediment of the hydrocyclone is returned to the ball mill for re-grinding; the overflow product of the hydrocyclone enters the subsequent separation operation for separation of magnetite and chalcopyrite.
2. A wet pre-selection process for copper-containing magnetite ore according to claim 1, characterized in that: It is applicable to copper-containing magnetite ores with TFe content not less than 20%, magnetic rate not less than 65%, and copper content not higher than 0.12%.
3. A wet pre-selection process for copper-containing magnetite ore according to claim 1, characterized in that: In step one, a three-stage one-closed-circuit crushing process is adopted, and the crushing particle size is -12mm; in step two, the feed concentration is 30-40%, the magnetic field strength is 0.4-0.5T, and the ball mill grinding concentration is 70-80%; in step three, the sieved products are sold as building materials.
4. A wet pre-selection process for copper-containing magnetite ore according to claim 3, characterized in that: The undersize product of the vibrating screen and the discharge product of the ball mill are fed into the same pump pool and then fed into the hydrocyclone through a slurry pump.
5. A wet pre-selection process for copper-containing magnetite ore according to claim 4, characterized in that: The feed particle size of the magnetic separator is preferably not higher than 12 mm; the ball mill is an overflow type ball mill, and the ball mill and the hydrocyclone form an integrated closed-circuit grinding and grading system; the vibrating screen is preferably a linear vibrating screen.