A radiation-resistant VDMOS device and its preparation method
By injecting or diffusing heavy metal ions into the well region of the VDMOS device and annealing activation, a doping infiltration zone is formed, which solves the problem of insufficient anti-single-particle burning ability in the prior art, improves the radiation resistance of the device and maintains the radiation resistance and controls the high performance.
Patent Information
- Application Number
- CN202010735219.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-28
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-07-28
AI Technical Summary
When the prior art improves the anti-single-particle burning capability of power VDMOS devices, it is difficult to ensure the device's own performance indicators, and the radiation-resistant reinforcement measures have a great impact.
By implanting or diffusion of heavy metal ions multiple times in the well region of the VDMOS device, a heavy metal ions implantation or diffusion region with a doping concentration decreasing from one side of the substrate to the other side of the substrate, and annealing activation process is performed to enhance the radiation of the device Induce the recombination rate of electron hole pairs and reduce the charge collection efficiency under high electric fields.
It effectively improves the anti-single-particle burning capability of power devices, while ensuring high-performance indicators of VDMOS devices, and is compatible with processes, making the steps simple and easy to operate.
Smart Images

Figure CN111863941B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electronic devices, and in particular to a radiation-resistant VDMOS device and a preparation method thereof. Background Art
[0002] With the widespread application of electronic devices and the increasing expansion of human space activities, the importance of the impact of the space environment and nuclear radiation environment on electronic devices has become increasingly prominent. The space environment and nuclear radiation environment are important causes of equipment anomalies and failures. Among them, the impact of the radiation environment on equipment is the most prominent. The incident particles can penetrate the external protective structure of the equipment and produce ionizing radiation damage, displacement radiation damage, single particle events, and internal charging and discharging effects in the electronic components in the cabin. These effects will cause the performance degradation or failure of electronic components, and in severe cases even cause equipment failure.
[0003] Power VDMOS devices are a type of electronic devices widely used in radiation environments. Under the influence of radiation environments, power VDMOS devices will produce a variety of complex radiation damage effects, such as single particle effect, ionization effect, displacement effect, ionization / displacement synergistic effect, etc., which make power VDMOS devices sensitive to damage in equipment electronic systems. In fact, equipment failures and even accidents during service are always caused by the "short board effect", which is closely related to the damage to key sensitive devices or materials. The loss of power VDMOS devices will directly affect the life and reliability of the equipment. Therefore, it is of great significance to study the radiation effects of VDMOS power devices and design the corresponding production process of radiation-resistant devices.
[0004] Radiation hardening refers to the optimization of various structures, circuits, and layout levels to avoid the hazards of radiation or control radiation damage within an acceptable range for the entire system. Considering the complexity of the radiation environment, the means of radiation hardening are also very diverse, including reinforcement measures for individual effects, general radiation hardening methods suitable for various radiation occasions, radiation shielding to prevent accidents, and equipment self-inspection measures to remedy the situation. However, the current radiation hardening of power VDMOS devices, especially the improvement of single-particle burnout resistance, is limited, and will affect the performance indicators of the power VDMOS devices themselves to a certain extent. Summary of the invention
[0005] The problem solved by the present invention is how to effectively improve the single particle burnout resistance of a power VDMOS device in a radiation environment and ensure the performance index of the power VDMOS device itself.
[0006] In order to solve at least one aspect of the above problems, the present invention provides a method for preparing a radiation-resistant VDMOS device, comprising: after completing the etching of the source contact hole of the VDMOS device, multiple times injecting or diffusing heavy metal ions into the well region through the source contact hole to form a heavy metal ion injection or diffusion zone in the well region, and the doping concentration of the heavy metal ion injection or diffusion zone decreases from the side away from the substrate to the side close to the substrate.
[0007] Preferably, the number of times of injecting or diffusing the heavy metal ions into the well region is 2-5 times.
[0008] Preferably, the concentration of the heavy metal ions injected or diffused each time is 1e17cm -3 -1e20cm -3 .
[0009] Preferably, the heavy metal ions are distributed in the trap region in the form of a cone, a cylinder, a cube or a cuboid.
[0010] Preferably, the cross-sectional shape of the heavy metal ion implantation or diffusion region is circular, annular, rectangular, square or trapezoidal.
[0011] Preferably, an annealing activation treatment is performed after each injection of the heavy metal ions, wherein the annealing atmosphere includes at least one of N2, O2 and H2, the annealing temperature is 800°C-1300°C, and the annealing time is 2min-200min.
[0012] Preferably, before each injection or diffusion of the heavy metal ions, a photolithography process is performed to etch out the source region contact region.
[0013] Preferably, the heavy metal ions include at least one of gold ions, copper ions and platinum ions.
[0014] The method for preparing the radiation-resistant VDMOS device provided by the present invention has the following beneficial effects compared with the prior art:
[0015] The present invention performs multiple heavy metal ion implantation or diffusion on the epitaxial layer. Since the heavy metal ion impurities are deep energy level impurities, recombination centers can be generated, thereby increasing the recombination rate of radiation-induced electron-hole pairs in the epitaxial layer, reducing the charge collection efficiency under high electric fields, and guiding the instantaneous large current generated by the incident high-energy particles in the device out of the power device, thereby improving the single particle burnout resistance of the power device, and at the same time ensuring the high performance indicators of the VDMOS device itself. In addition, the present invention is compatible with the conventional preparation method of the power VDMOS device in terms of process, has simple steps, and is easy to operate.
[0016] The present invention also provides a radiation-resistant VDMOS device, which is manufactured by the method for manufacturing the radiation-resistant VDMOS device as described above.
[0017] Preferably, the radiation-resistant VDMOS device includes a substrate, an epitaxial layer formed on the substrate, a well region formed in the epitaxial layer and arranged close to the upper surface of the epitaxial layer, and a source region formed in the well region and close to both sides of the upper surface of the epitaxial layer, and also includes a heavy metal ion injection or diffusion region formed in the well region.
[0018] The beneficial effects of the radiation-resistant VDMOS device provided by the present invention compared with the prior art are the same as the preparation method of the radiation-resistant VDMOS device, which will not be described in detail here. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of the cross-sectional structure of etching the source region and contact region of the VDMOS device in an embodiment of the present invention;
[0020] Figure 2 It is a schematic diagram of the cross-sectional structure of a VDMOS device in an embodiment of the present invention in which heavy metal ions are injected once;
[0021] Figure 3 It is a schematic diagram of the cross-sectional structure of the secondary injection of heavy metal ions into the VDMOS device in an embodiment of the present invention;
[0022] Figure 4 It is a schematic diagram of the cross-sectional structure of the VDMOS device after three injections of heavy metal ions in an embodiment of the present invention. DETAILED DESCRIPTION
[0023] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0024] The embodiment of the present invention provides a method for preparing a radiation-resistant VDMOS device, comprising: after etching the source contact hole of the VDMOS device, multiple injection or diffusion of heavy metal ions into the well region through the source contact hole, forming a heavy metal ion injection or diffusion region in the well region, and the doping concentration of the heavy metal ion injection or diffusion region decreases from the side away from the substrate to the side close to the substrate. The heavy metal ions include at least one of gold ions (Au), copper ions (Cu), and platinum ions (Pt).
[0025] In this embodiment, before etching the source contact hole, the conventional manufacturing process of the power VDMOS device is used to form an epitaxial layer, a well region, a source region, etc. on the substrate. The substrate can be P-type or N-type, and the well region is located in the epitaxial layer and is arranged close to the upper surface of the epitaxial layer. The source region is located in the well region and is arranged close to the upper surface of the epitaxial layer. Figure 1One of the embodiments is shown, providing an N-type substrate, forming an N-type epitaxial layer on the N-type substrate, injecting doped P-type ions on the N-type epitaxial layer to form a P-type well region, injecting doped N-type ions on both sides of the upper surface of the P-type well region, annealing to form an N-type source region, etching a source contact hole, and injecting or diffusing heavy metal ions into the P-type well region to form a heavy metal ion injection or diffusion region. After injecting or diffusing heavy metal ions into the well region, a source, a drain and a gate are respectively formed on the epitaxial layer to complete the preparation of the VDMOS device, wherein the steps before and after the preparation of the heavy metal ion injection or diffusion region are all prior art and will not be repeated here.
[0026] VDMOS devices are generally used in spacecraft power systems, and spacecraft operate in space. Various high-energy particles, cosmic rays and other radiation in space can cause damage to VDMOS devices. The radiation effects that the radiation environment may produce on VDMOS devices mainly include single-particle burnout and single-particle gate breakdown. Among them, the single-particle burnout effect is that under the condition of electric field irradiation, high-energy particles in space are incident on the VDMOS device and a large number of electron-hole pairs are generated in the VDMOS device along the particle trajectory. Under the action of drift and diffusion effects, holes enter the emitter of the inherent parasitic tube, and electrons flow to the collector to form a transient current. When the voltage between the collector and the emitter is higher than the breakdown voltage of the parasitic tube, the collector current of the parasitic tube undergoes avalanche multiplication, causing the device to burn out.
[0027] In the present embodiment, when preparing the VDMOS device, heavy metal ion impurities are injected or diffused into the well region. When the heavy metal ion impurities enter the epitaxial layer, new defect energy levels are generated in the energy band of the semiconductor in the epitaxial layer. A large number of defect energy levels become the recombination centers of electron-hole pairs, and the energy level is a deep energy level located near the center of the forbidden band, which is an effective recombination center, and plays a recombination role on the electrons and holes generated by radiation, reduces the collection effect of the charge, reduces the irradiation current, and guides the instantaneous large current generated in the device by the high-energy particles incident from the space out of the device. In addition, in the present embodiment, by multiple injection or diffusion of heavy metal ion impurities, a concentration distribution that decreases from the side far from the substrate to the side close to the substrate is formed in the well region. In this way, after the drain electrode is prepared later, the area with the largest doping concentration distribution in the heavy metal ion injection or diffusion area is far away from the electrode, so as to avoid the heavy metal ion impurities as a recombination center to recombine electrons or holes and concentrate near the electrode, which has a greater impact on the overall performance of the device. Therefore, this embodiment not only ensures the high performance index of the VDMOS device itself, but also can effectively improve the single-event burnout resistance of the VDMOS device, thereby achieving the purpose of reducing the radiation damage of the VDMOS device.
[0028] This embodiment effectively increases the recombination rate of radiation-induced electron-hole pairs in the epitaxial layer by multiple heavy metal ion injections or diffusions in the epitaxial layer, reduces the charge collection efficiency under high electric fields, and effectively improves the single-particle burnout resistance of the power device. In addition, the heavy metal ions injected or diffused in this embodiment are common metals in the manufacture of semiconductor devices, and have good process compatibility with the manufacturing process of semiconductor devices. Therefore, it is a process reinforcement technology that is easy to implement and realize. In addition, this embodiment is compatible with the preparation method of conventional power VDMOS devices, with simple steps and easy operation. The VDMOS device prepared by the method provided in this embodiment can greatly improve the radiation resistance of the transistor, which is of great significance to the ground simulation application and research of the space and nuclear radiation environmental effects of materials and devices, and has obvious advantages in the research of space and nuclear radiation environmental effects and the application of radiation resistance reinforcement technology.
[0029] Furthermore, the formation of the heavy metal ion injection or diffusion zone specifically includes: injecting or diffusing heavy metal ions into the well region multiple times on the source contact hole by injection, diffusion, physical vapor deposition, chemical vapor deposition, magnetron sputtering and other methods, and annealing and activating after each injection of heavy metal ions.
[0030] The number of heavy metal ion injection or diffusion is 2-5 times, preferably 5 times. According to the number of heavy metal ion injection or diffusion, different concentration gradients are formed in the heavy metal ion injection or diffusion area, and the smaller the concentration difference between the concentration gradients, the more conducive to the recombination effect, so as to reduce the charge collection efficiency.
[0031] The concentration of heavy metal ions injected or diffused each time is 1e17cm -3 -1e20cm -3 , of course, it can also be less than 1e17cm -3 or greater than 1e20cm -3 This is mainly related to the type of device. For devices with relatively large current, the amount of each injection or diffusion is relatively large. For devices with relatively small current, the amount of each injection or diffusion is relatively small. This embodiment only gives the amount of each injection or diffusion of most devices at 1e17cm -3 -1e20cm -3 .
[0032] The depth of the heavy metal ions injected or diffused each time may not exceed the well region. However, for some devices with thin well regions, such as high-frequency tubes, the injection or diffusion depth is difficult to control and the injection or diffusion depth may exceed the well region.
[0033] The distribution form of the heavy metal ion impurities in the well region can be a cone, a cylinder, a cube or a cuboid, and the cross-sectional shape of the heavy metal ion injection or diffusion region can be a circle, a donut, a rectangle, a square or a trapezoid. For example, when the heavy metal ion impurities are distributed in the well region in a cylindrical or conical shape, the cross-sectional shape of the heavy metal ion injection or diffusion region is a circle, and when the heavy metal ion impurities are distributed in the well region in a cuboid shape, the cross-sectional shape of the heavy metal ion injection or diffusion region is a rectangle. By adjusting the energy of the injected or diffused heavy metal ions, the distribution form of the heavy metal ion impurities in the well region can be changed. Preferably, the distribution form of the heavy metal ions in the well region is an inverted cone, so that the doping concentration of the heavy metal ion injection or diffusion region away from the substrate is the largest, and the doping concentration of the heavy metal ion injection or diffusion region is the smallest, that is, the heavy metal ion impurities will not be concentrated near the electrode, avoiding affecting the performance of the device.
[0034] The types of heavy metal ion impurities injected or diffused can be the same or different. Considering the complexity of the process, generally, the same type of ion impurities are used for injection or diffusion. However, when a distribution form such as an inverted cone shape needs to be injected or diffused, multiple ion impurities can be used for injection or diffusion.
[0035] Each time the heavy metal ions are injected and then annealed for activation, the annealing atmosphere includes at least one of N2, O2 and H2, the annealing temperature is 800° C.-1300° C., and the annealing time is 2 min-200 min.
[0036] Furthermore, before each injection or diffusion of heavy metal ions, the device needs to be photolithographically processed to etch out the source region and contact region. The etching method can be dry etching, wet etching or plasma etching.
[0037] The following is a detailed description through specific implementation methods.
[0038] Example 1
[0039] like Figure 1 , 2 As shown in FIG. 1 , after the source contact hole of the VDMOS device is etched, heavy metal ion impurities are diffused into the well region on the source contact hole by magnetron sputtering, and the diffusion concentration is 1e18 cm -3 , the diffusion depth is 4 / 5 of the well region, and the injected heavy metal ions are Au;
[0040] Perform an annealing process and a photolithography process, wherein the annealing atmosphere is N2, the annealing temperature is 1000°C, and the annealing time is 50 minutes;
[0041] like Figure 3 As shown in Figure 2, heavy metal ion impurities are diffused into the well region by magnetron sputtering, with a diffusion concentration of 1e18cm -3, the diffusion depth is 2 / 5 of the well region, and the injected heavy metal ions are Au;
[0042] Perform secondary annealing and secondary photolithography, wherein the annealing atmosphere is N2, the annealing temperature is 1000°C, and the annealing time is 50min;
[0043] like Figure 4 As shown in the figure, heavy metal ion impurities are diffused into the well region three times by magnetron sputtering, with a diffusion concentration of 1e18cm -3 , the diffusion depth is 1 μm in the well region, and the injected heavy metal ions are Au;
[0044] Three annealing treatments and three photolithography treatments were performed to etch out the entire source contact area, wherein the annealing atmosphere was N2, the annealing temperature was 1000°C, and the annealing time was 50 minutes.
[0045] Example 2
[0046] The difference between this embodiment and embodiment 1 is that the number of times of injecting or diffusing heavy metal ions is 5 times.
[0047] Example 3
[0048] The difference between this embodiment and embodiment 1 is that the concentration of the injected or diffused heavy metal ions is 1e20 cm -3 .
[0049] Example 4
[0050] The difference between this embodiment and embodiment 1 is that the concentration of the injected or diffused heavy metal ions is 1e17 cm -3 .
[0051] Example 5
[0052] The difference between this embodiment and embodiment 1 is that the concentration of the injected or diffused heavy metal ions is less than 1e17 cm -3 .
[0053] Example 6
[0054] The difference between this embodiment and the first embodiment is that the depth of each injection or diffusion of heavy metal ions is 1 μm in the well region.
[0055] Although the disclosure is disclosed as above, the protection scope of the disclosure is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the disclosure, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. A method for preparing a radiation-resistant VDMOS device, characterized in that: include: After the source contact hole of the VDMOS device is etched, heavy metal ions are injected or diffused into the well region multiple times through the source contact hole to form a heavy metal ion injection or diffusion zone in the well region, and the doping concentration of the heavy metal ion injection or diffusion zone decreases from the side away from the substrate to the side close to the substrate.
2. The method for preparing a radiation-resistant VDMOS device according to claim 1, characterized in that: The number of times of injecting or diffusing the heavy metal ions into the well region is 2-5 times.
3. The method for preparing a radiation-resistant VDMOS device according to claim 1, characterized in that: The concentration of the heavy metal ions injected or diffused each time is 1e17cm -3 -1e20cm -3 .
4. The method for preparing a radiation-resistant VDMOS device according to claim 1, characterized in that: The heavy metal ions are distributed in the trap region in the form of a cone, a cylinder, a cube or a cuboid.
5. The method for preparing a radiation-resistant VDMOS device according to claim 1, characterized in that: The cross-sectional shape of the heavy metal ion implantation or diffusion region is circular, annular, rectangular, square or trapezoidal.
6. The method for preparing a radiation-resistant VDMOS device according to any one of claims 1 to 5, characterized in that: After each injection of the heavy metal ions, an annealing activation treatment is performed, wherein the annealing atmosphere includes at least one of N2, O2 and H2, the annealing temperature is 800°C-1300°C, and the annealing time is 2min-200min.
7. The method for preparing a radiation-resistant VDMOS device according to any one of claims 1 to 5, characterized in that: Before each injection or diffusion of the heavy metal ions, photolithography is performed to etch out the source region and contact region.
8. The method for preparing a radiation-resistant VDMOS device according to any one of claims 1 to 5, characterized in that: The heavy metal ions include at least one of gold ions, copper ions and platinum ions.
9. A radiation-resistant VDMOS device, characterized in that: The radiation-resistant VDMOS device is manufactured by the method for manufacturing the radiation-resistant VDMOS device according to any one of claims 1 to 8.
10. The radiation-resistant VDMOS device according to claim 9, characterized in that: It includes a substrate, an epitaxial layer formed on the substrate, a well region formed in the epitaxial layer and arranged close to the upper surface of the epitaxial layer, and a source region formed in the well region and close to both sides of the upper surface of the epitaxial layer, and also includes a heavy metal ion injection or diffusion region formed in the well region.