Intensive mixer blade

The powder plasma arc cladding process forms a layer-by-layer surfacing wear-resistant layer of nickel-based wear-resistant alloy and tungsten carbide carbide particles on the surface of the blade, which solves the low bond strength and high temperature damage of the tungsten carbide wear-resistant layer and the base material. The problem is that it improves wear resistance and impact resistance, and achieves green manufacturing and low-cost remanufacturing.

CN111905586BActive Publication Date: 2024-12-03WEIHAI HAOYANG MASCH MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010780737.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-06
Publication Date
2024-12-03
Estimated Expiration
2040-08-06

AI Technical Summary

Technical Problem

In the prior art, the bonding strength of the tungsten carbide wear-resistant layer and the blade base material is low and easy to fall off. The solid state migration and diffusion of tungsten carbide at high temperature affects the wear resistance, making it difficult to maintain wear resistance in a strong mixer environment. .

Method used

The powder plasma arc cladding process is used to form a layer-by-layer welding and wear-resistant layer of nickel-based wear-resistant alloy and tungsten carbide carbide particles on the surface of the blade to ensure uniform distribution of tungsten carbide carbide particles, reduce high-temperature damage, and improve wear-resistant The bonding force between the layer and the base material.

Benefits of technology

The high wear resistance and impact resistance of the blade surface are achieved, the risk of the wear-resistant layer falling off and the cost of remanufacturing is reduced. The process is green additive manufacturing, which supports multiple reuse of the base material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111905586B_ABST
    Figure CN111905586B_ABST
Patent Text Reader

Abstract

The present invention provides a blade for a strong mixer, which is used to solve the problem in the prior art that the wear-resistant layer formed by welding a single component of tungsten carbide on the blade surface of a steel base material is easy to fall off from the steel base material. The blade includes a steel base material located inside, and a wear-resistant layer located on the surface of the base material. A powder plasma arc cladding process is used to melt a nickel-based wear-resistant alloy on the blade surface and tungsten carbide cemented carbide particles are added for layer-by-layer cladding. The wear-resistant layer is in a microscopic state: the tungsten carbide cemented carbide particles are evenly distributed in the wear-resistant layer without sinking to the bottom; the tested dilution rate of the joint between the wear-resistant layer and the base material is 3%-5%. The present invention is the first to use the (WC+Ni60) mixed wear-resistant material powder plasma arc cladding process for the domestic production of blades, and the blades can especially meet the use requirements of strong mixers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of blade wear-resistant layer forming method, in particular to a strong mixer blade with a wear-resistant layer. Background Art

[0002] A wear-resistant layer 00 is formed by welding or coating at the part of the blade 10 that is susceptible to wear, so as to improve the wear resistance of the blade. This is a common method in the industry. Figure 1 and Figure 2 .

[0003] For example, Chinese patent CN201120502286.5 discloses a blade for a high-speed mixing device, including a blade body, one end of the blade body is a free end, and the other end is connected to a blade shaft, and a connecting end for connecting to a main shaft is provided on the blade shaft, and a tungsten carbide wear-resistant layer is welded on the free end surface and the upper and lower sides of the blade body. When the blade rotates, the parts most susceptible to wear are the upper and lower sides of the blade body and the surface of the free end. A tungsten carbide wear-resistant layer is provided on the easily worn parts, and the thickness of the tungsten carbide wear-resistant layer is 1mm to 4mm; the tungsten carbide wear-resistant layer extends 20-60mm along the length direction of the blade. The above parameters can ensure that the blade is wear-resistant while keeping the overall manufacturing cost low.

[0004] In fact, the melting point of tungsten carbide is about 2800-3000℃; the particle size is 60-100 mesh (0.15-0.25mm); the hardness is Hv1700-2200, and its wear resistance is second only to diamond, making it a superior product among wear-resistant materials.

[0005] The above technical solution mentions the provision of a tungsten carbide wear-resistant layer, which is a wear-resistant layer of a single component (tungsten carbide), and requires high temperature to complete melt surfacing. This technology utilizes the high hardness and high wear resistance of tungsten carbide, which is its advantage. However, the bonding strength between the single-component tungsten carbide wear-resistant layer and the blade parent material is low, that is, the welding performance is poor, which is very unfavorable for maintaining wear resistance under strong impact in the use environment of the intensive mixer. This strong impact may even cause the overall detachment of the cladding layer, that is, there is a possibility of the overall detachment of the tungsten carbide wear-resistant layer. Therefore, as a blade used in a intensive mixer, the separation of this tungsten carbide wear-resistant layer from the blade parent material is very dangerous.

[0006] At the same time, because the melting point of tungsten carbide is around 2800-3000℃, when tungsten carbide is clad on the surface of the base material, the C atoms in the tungsten carbide will migrate and diffuse in the solid state under the action of high temperature, which has a direct impact on the wear resistance of tungsten carbide.

[0007] Therefore, simply welding tungsten carbide on the blade surface to form a wear-resistant layer has defects. That is, the wear-resistant principle of the above-mentioned tungsten carbide wear-resistant layer is to use the wear-resistant properties of tungsten carbide to resist the wear of the material, but it introduces the defects of poor welding performance and easy overall shedding of the wear-resistant layer.

[0008] How to solve this problem? In order to solve the problem of detachment between the tungsten carbide wear-resistant layer and the blade base material, the following technology provides a solution:

[0009] CN201110087226.6 discloses a method for repairing ship propeller blades. For worn blades, the worn edge of the blade can be welded up by gas welding. The material of the welding wire used is required to be the same as that of the propeller, and then the surface of the welded area is polished. The specific process is:

[0010] 1) The worn area on the leading edge of the propeller blade body is welded by electric welding to form a welded area, and then repaired by hand using a portable grinder and manual trimming to restore the original shape of the blade body;

[0011] 2) For the defective blade body, a slightly larger casting with the same material as the propeller is cast in advance according to the shape of the defect, and then its shape, size and thickness are manually matched, and the edge welds should be processed with appropriate welding chamfers; then they are welded together using oxygen-acetylene manual welding, and finally they are manually polished and trimmed to the same shape as the original blade body.

[0012] That is, in theory, this can be effectively avoided by setting the blade material and the part to be repaired to the same material. However, for blades made of tungsten carbide, the brittleness of tungsten carbide will have an adverse effect on the toughness of the blades. And the use of tungsten carbide as the overall blade material is not suitable for use as an impact-resistant blade, considering its impact resistance, toughness and cost, especially its impact toughness and bending strength are far worse than high-speed steel, making it only a theoretical possibility. Therefore, in the existing field of strong mixer blade technology, there is no precedent for using a single component of tungsten carbide as a blade base material.

[0013] In fact, the present invention still follows the technical route of coating a wear-resistant layer on the surface of high-strength steel to provide a blade with higher wear resistance and a manufacturing process thereof.

[0014] Based on this, as the blades are made of conventional steel, the inventor has not retrieved any related technology or literature that uses a mixed wear-resistant material of tungsten carbide particles and nickel-based wear-resistant alloy supplemented by a powder plasma arc surfacing process to enhance the wear resistance of the blade surface. Summary of the invention

[0015] In order to solve the shortcomings of the prior art, the present invention provides a blade for solving the problem in the prior art that the wear-resistant layer formed by welding a single component of tungsten carbide on the blade surface of the steel base material is easily detached from the steel base material, and further improving the wear resistance and impact resistance of the wear-resistant layer in the new technology.

[0016] The technical solution adopted by the present invention to solve the technical problem is:

[0017] A strong mixer blade, the blade comprises a steel base material located inside, and a wear-resistant layer located on the surface of the base material, characterized in that the wear-resistant layer is formed by melting a nickel-based wear-resistant alloy on the blade surface by a powder plasma arc cladding process and adding tungsten carbide cemented carbide particles for layer-by-layer cladding, and the wear-resistant layer is in a microscopic state:

[0018] The tungsten carbide hard alloy particles are evenly distributed in the wear-resistant layer without sinking to the bottom;

[0019] The high-magnification metallographic photograph of the wear-resistant layer shows that the hard phases in the cladding layer include tungsten carbide cemented carbide particles, Cr7C3 particles, and NiB particles, and the hard phase area of ​​the three particles accounts for 60-70%;

[0020] The test dilution rate of the bonding part between the wear-resistant layer and the base material is 3%-5%.

[0021] Furthermore, the average microhardness of tungsten carbide particles is Hv=1982, the average microhardness of Cr7C3 particles is Hv=1326, and the average microhardness of NiB particles is Hv=1153.

[0022] Furthermore, in the surfacing process, the weight ratio of the tungsten carbide hard alloy particles to the nickel-based wear-resistant alloy is 40-60%.

[0023] Furthermore, the thickness of the wear-resistant layer on the material-facing surface of the blade is 6 mm, and that on the remaining parts is 4 mm.

[0024] Furthermore, the thickness of the single layer of surfacing is 2 mm.

[0025] The beneficial effects of the present invention are:

[0026] 1. For the first time, the (WC+Ni60) mixed wear-resistant material powder plasma arc surfacing process method was used for the domestic production of blades, and the blades can especially meet the use requirements of strong mixers.

[0027] 2. The blades in the present invention are manufactured using a powder plasma arc cladding process, which falls within the scope of green additive manufacturing. The gene for remanufacturing is embedded in the initial manufacturing, and the cladding remanufacturing can be repeated. The parent material blank can be reused 3-4 times, and the second, third, and fourth remanufacturing costs are only 1 / 4 of the initial manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a schematic diagram of the installation of the blades and blade shafts.

[0029] Figure 2 This is the positional relationship between the blade and the wear-resistant layer (longitudinal section).

[0030] Figure 3 is the positional relationship between the blade and the wear-resistant layer (cross surface).

[0031] Figure 4 It is a schematic diagram of the sinking phenomenon of WC cemented carbide particles during the cladding process in the prior art.

[0032] Figure 5 The wear-resistant mechanism is that WC cemented carbide particles are filled and embedded in the molten nickel-based wear-resistant alloy.

[0033] Figure 6 Schematic diagram of the powder plasma arc surfacing principle.

[0034] Figure 7 This is a dimensional drawing of the nozzle.

[0035] Figure 8 This is a comparison chart of argon arc welding and plasma arc morphology.

[0036] Fig. 9 Schematic diagram of temperature field of argon arc welding and plasma arc.

[0037] Fig.10 This is a metallographic micrograph of the wear-resistant layer (1000μm unit).

[0038] Fig.11 Metallographic micrograph of the wear-resistant layer (100 μm unit).

[0039] In the figure:

[0040] 00 wear-resistant layer, 01 tungsten carbide particles, 02 fusion line, 021 decarburized layer, 03 cladding metal, 04 material surface, 05 Cr7C3 and NiB particles,

[0041] 10 blades,

[0042] 20 base material,

[0043] Figure 5 In the figure, 31 is a tungsten electrode, 32 is alloy powder, and 33 is a nozzle. DETAILED DESCRIPTION

[0044] This embodiment is dedicated to the localization of the manufacture of impact-resistant blades used in strong mixers, and introduces a method for surfacing the wear-resistant layer of blades. This method is especially aimed at the study of the wear-resistant performance of the blade facing surface. The main idea of ​​the wear-resistant manufacturing solution of the blade facing surface is: powder plasma arc cladding process + nickel-based wear-resistant alloy + WC cemented carbide particles (tungsten carbide cemented carbide particles). That is, the powder plasma arc cladding process is used to perform layer-by-layer surfacing on the surface of the blade, and the WC cemented carbide particles are filled and embedded in the molten nickel-based wear-resistant alloy, and the WC cemented carbide particles are uniformly arranged in the nickel-based wear-resistant alloy as much as possible.

[0045] In reality, WC cemented carbide particles are not uniformly distributed in the nickel-based wear-resistant alloy during the surfacing process, and are not uniformly distributed. The high temperature caused by welding will cause solid migration of C atoms (carbon atoms) in the WC cemented carbide particles. Therefore, in the implementation of this embodiment, there are two technical difficulties: first, how to ensure that the WC cemented carbide particles are dispersed and evenly distributed, and second, how to avoid the damage to the WC cemented carbide particles caused by high-temperature surfacing and minimize the damage as much as possible.

[0046] WC cemented carbide particles: that is, tungsten carbide cemented carbide particles, which have the following characteristics: melting point: about 2800-3000℃; particle size: 60-100 mesh (0.15-0.25mm); hardness Hv1700-2200, wear resistance is second only to diamond, and it is a superior product among wear-resistant materials.

[0047] Since the specific gravity of tungsten carbide particles is nearly twice that of ordinary carbon steel, there is always a phenomenon of sinking to the bottom during the cladding process (refer to Figure 4 ), a large number of tungsten carbide cemented carbide particles 01 are deposited near the fusion line 02. This non-uniform sedimentation is very unfavorable to the combination of the cladding layer and the base material 20, and may cause the entire cladding layer to fall off. At the same time, from the perspective of wear resistance, it is also hoped that the tungsten carbide cemented carbide particles are evenly distributed in the thickness direction of the cladding layer. However, it is difficult to achieve this in reality, which is also a problem that must be faced.

[0048] About the mechanism of destruction of tungsten carbide particles 01: During the powder plasma arc cladding process, tungsten carbide particles will inevitably be damaged, especially the protruding corners of tungsten carbide particles are melted, although the other flat parts of the cemented carbide particles are not melted in the high-temperature molten pool, but under the action of high temperature, the surface C atoms (carbon atoms) of tungsten carbide particles have solid migration and diffusion phenomenon. This solid migration of C atoms is an unfavorable factor, and the hazards are as follows:

[0049] First, decarburization on the surface of tungsten carbide cemented carbide particles will lead to a decrease in the wear resistance of the wear-resistant layer.

[0050] Secondly, the solid migration and diffusion of C atoms into the base metal (nickel-based wear-resistant alloy) will cause the embrittlement of the surfacing single layer, which is very easy to break and peel off, which is an unfavorable factor.

[0051] After research and analysis, it is impossible to completely eliminate this solid migration and diffusion phenomenon. What can be done is to minimize the solid migration of C atoms on the surface of cemented carbide particles to maximize the wear resistance of tungsten carbide cemented carbide particles, which requires modification of the process.

[0052] Nickel-based wear-resistant alloy: low melting point (about 1000°C), easy to melt, good solubility with WC cemented carbide particles, insensitive to carbon, and can dissolve C atoms that migrate and diffuse from WC cemented carbide particles. This is the reason for choosing nickel-based wear-resistant alloy.

[0053] Tungsten carbide particles 01 play the role of anti-wear skeleton and are the main force in anti-wear. Figure 5 , Figure 5 The middle arrow simulates the direction of the material impacting the blade in the intensive mixer; the nickel-based wear-resistant alloy as a base metal is also a wear-resistant alloy, and also acts as a "binder", that is, the WC carbide particles are bonded and embedded in the cladding metal 03 (molten nickel-based wear-resistant alloy); the two are interdependent and have a "lip-tooth" relationship. The quality of wear resistance depends on the distribution and area proportion of WC particles; the more the number and the more evenly distributed, the higher the wear resistance.

[0054] Wear theory of nickel-based wear-resistant alloy combined with tungsten carbide particles:

[0055] For example, SiO2 and Ai2O3 are conventional abrasives, and their hardness is generally expressed in Mohs hardness. There is no same unit as WC carbide particles, so they cannot be directly compared. However, in long-term production practice, we have learned that the hardness of SiO2 and Ai2O3 is slightly lower than that of WC carbide particles, and the Ha / Hm value is slightly to the right of K2. Theoretically, WC carbide particles are in the low wear zone.

[0056] Powder plasma arc cladding process: plasma arc has concentrated energy (105-106W / cm2), high temperature (18000-24000℃), short high temperature residence time, and little impact on the parent material and tungsten carbide cemented carbide particles. It is one of the high-energy beams (the other two are laser and electron beam); it is energy-saving and material-saving, green and low-carbon, and is an environmentally friendly cladding process.

[0057] Comparison chart of argon arc welding and plasma arc Figure 8 .

[0058] In order to solve these technical difficulties, the following work was done:

[0059] The general principle is to first debug an arc suitable for surfacing with WC carbide particles, and then explore feasible process parameters on this basis. The arc used for this surfacing is different from ordinary welding. Ordinary welding arcs have high energy, high density, concentrated heat, small heating range, and strong penetration. They can penetrate 10mm thick steel plates, which are obviously not suitable for this surfacing process.

[0060] From a macroscopic point of view, compared with the welding arc, the cladding arc is more flexible, the arc temperature is lower, and it is necessary to avoid high arc energy density and strong penetration (see Fig. 9 ). Too high energy density will cause serious burning of WC carbide particles and lose wear resistance, and too strong penetration will cause a high dilution rate and a decrease in wear resistance. These are to be avoided in WC carbide particle surfacing. At present, there is no mature complete set of powder plasma arc surfacing equipment in China, and there is no practical process parameter reference. The surfacing technology for WC carbide particles is more difficult than the usual iron-based, nickel-based, and cobalt-based alloy powder surfacing, and the required process conditions are more stringent. It is necessary to ensure a low dilution rate and to ensure that the WC carbide particles are burned as little as possible, so as to maximize the excellent wear resistance of WC carbide particles.

[0061] Summarizing previous work experience, the following statements are made for the flexible plasma arc suitable for cladding of WC cemented carbide particles: First, the size of the molten pool (heating range) formed by the arc used for cladding should be in a circular area with a diameter of d = 6 mm to 10 mm (closely related to the cladding efficiency). Second, the melting depth is within 0.5 mm (closely related to the dilution rate). Third, the molten pool is stable and does not "bubble", and obvious anode spots can be observed. Fourth, the plasma flame impacts a small inverted cone-shaped pit at the anode spot of the molten pool. Fifth, the anode spot is stable and does not jump. Sixth, the base material melts rapidly where the arc reaches, and the liquid metal solidifies rapidly after leaving, and the liquid pool stays as short as possible. Meeting or approaching these six statements can achieve WC cemented carbide particle cladding.

[0062] There are two main hardware factors that affect the above six points: welding power supply and plasma welding gun. The following experiment is carried out on the influence of welding power supply and plasma welding gun on arc characteristics to explore what configuration of welding power supply and welding gun is suitable for powder plasma arc cladding of WC cemented carbide particles.

[0063] The process is as follows:

[0064] First, select a nozzle with an aperture of H = 6 mm, a compression ratio of 1:1, and a compression angle of β = 60°. Figure 7 ; Test plate size 100 × 200 × 15mm, material 16Mn; No powder feeding, current 80 amperes, fusion welding test plate. Surfacing speed 600mm / min.

[0065] 1. Welding power supply

[0066] We have tried different frequencies of inverter DC power supplies, from 10,000 Hz (10k) to 40,000 Hz (40k), to observe the changes in the plasma arc state caused by different frequencies. Changes in the arc will definitely be reflected in the molten pool and the weld bead formation. Observing the molten pool state and weld bead formation can indirectly judge the arc state. As the frequency increases, the arc electromagnetic compression gradually increases and the energy increases; at 10,000 Hz (10k) and 20,000 Hz (20k), the molten pool is calm and the weld bead is formed normally, and at 20,000 Hz (20k), there is a slight undercut; at 30,000 Hz (30k), there is serious undercut, the molten pool rolls frequently, the weld bead becomes narrower, the arc is noisy, and the weld bead does not meet the requirements when observed with the naked eye; at 40,000 Hz (40k), there are dense pores of different sizes on the weld bead, the surface is severely oxidized, and the undercut worsens. 30,000 Hz (30k) and 40,000 Hz (40k) are excluded. The 10K and 20K samples were cut from the cross section of the weld to observe the penetration depth. The 10K sample has a bowl-shaped fusion line, shallow fusion depth and large fusion width. The 20K sample has a similar fusion line shape, deep fusion depth and small fusion width. From the experimental results, it is more reasonable to choose a 10K power source.

[0067] 2. No-load voltage

[0068] The no-load voltage of conventional welding machines is 65V. The no-load voltage is increased to three levels, 75V, 85V, and 95V, with a frequency of 10,000 Hz (10k). Other parameters remain unchanged, and the changes in the arc and molten pool are observed. At the conventional 65V no-load voltage, the arc is soft and a little floating, the arc stiffness is not enough, and the melting capacity is insufficient. As the no-load voltage increases, the arc energy is obviously increasing. It is manifested in the expansion of the molten pool size, the firmness and strength of the arc, the anode spots and inverted cone pits are becoming more and more obvious, the "arc core" at the center of the arc is clearly visible, and the molten pool is calm and does not bubble; cut the sample and observe that the 75V, 85V, and 95V, the size of the melt width increases successively, the increase in the depth of melt is not large, the fusion line is bowl-shaped, and there is no "finger-like" melt depth and "pen tip-like" melt depth. It can be seen from this that the changes brought about by increasing the no-load voltage are positive, and this arc state and molten pool state are exactly what we are pursuing.

[0069] Let's sort out the effects of frequency and no-load voltage changes on arc morphology and molten pool state. When the frequency increases from 10k to 40k, the arc energy increases in the form of enhanced electromagnetic compression, smaller arc column diameter, and greater energy density; it can be observed intuitively that the molten pool size decreases, the molten depth increases, and the arc's "digging" ability increases. Such changes are beneficial to welding, but harmful to surfacing. High frequency cannot be used for surfacing arcs, 10k is more suitable, and 20k or more is a bit too large and is not recommended. When the no-load voltage increases from 65v to 95v, the arc energy also increases in the form of increased arc column diameter, and the energy density remains basically unchanged; the intuitive performance is that the molten pool size increases, the molten depth increases slightly, and the arc's "digging" ability remains basically unchanged. The change brought about by the change from small to large no-load voltage is not conducive to welding, but is beneficial to surfacing. Summarizing the above experimental results, it is concluded that for this project, under the premise of using the selected welding gun nozzle size, the power supply frequency of 10k and the no-load voltage of 90v are appropriate.

[0070] 3. Welding gun

[0071] The core component of the welding gun is the nozzle. The core of the nozzle is three dimensions: the hole diameter H of the compression hole, the hole length L, and the compression angle β (reference Figure 7 ).

[0072] Among them, the arc compression is strong when the hole diameter H is small, the arc compression is strengthened when the hole length L is large, and the arc compression is strong when the compression angle β is small, and vice versa. There are three considerations for choosing a nozzle with an aperture of H = 6mm in this project. First, it tends to obtain a flexible plasma arc, lower and widen the temperature field of the welding arc, and the arc temperature should not be too high. The effective heating area is larger, which is conducive to reducing WC burning loss; second, it is to obtain a larger molten pool to reduce the loss of alloy powder during powder feeding; especially WC cemented carbide particles, WC cemented carbide particles have a large specific gravity, irregular shape, multiple edges and corners, and are not smoothly transported. It is impossible for all WC cemented carbide particles to fall on the theoretically designed landing point. 10%-20% of WC cemented carbide particles fall outside the molten pool and are lost. A large molten pool can reduce losses; nickel-based powders and WC cemented carbide particles are very expensive, and effective use of resources is an important issue that must be considered; the third point is to adjust the % landing point to the edge area of ​​the molten pool, away from the high temperature area in the center of the arc, which is conducive to reducing % burning loss. When the aperture is 7mm, the compression effect is very weak, which can basically be defined as weak plasma and is unusable; the available aperture range is between 5-6mm, and there is not much room for adjustment. The powder utilization rate of the 5mm aperture will be lower, and the WC carbide particles will be burned more, so the nozzle diameter of 6mm is selected.

[0073] In this way, the hardware indicators of the equipment are determined, power supply frequency 10k, no-load voltage 90v, nozzle size H=6, L=6, β=60°, reference Figure 7When welding on the test plate with a current of 80 amperes, the diameter of the molten pool is about 7 mm, the melting depth is 0.5-1.0 mm, the arc is stable, and the molten pool is calm, which meets the requirements of the above six statements.

[0074] 4. Surfacing process parameters

[0075] The selection of process parameters should serve the theme of reducing the burning of WC carbide particles. The general principle is fast, thin weld layer, and multi-layer welding. Fast surfacing speed and short high-temperature residence time of the molten pool can reduce the burning of WC carbide particles; argon arc welding and flux-cored arc welding have both had cases of WC carbide particle surfacing. Their arc temperatures are much lower than plasma, and WC carbide particles have different degrees of burning. Therefore, the author believes that the residence time of the molten pool has a greater impact on the burning of WC carbide particles, and the process parameters should focus on speed; WC carbide particles have a large specific gravity, and it is an inevitable trend for them to settle to the bottom after entering the molten pool. A thin weld layer only slows down this trend, and cannot fundamentally eliminate it. The thicker the surfacing layer, the more serious the settlement.

[0076] Schematic diagram of the surfacing layer of the impeller blade of the strong mixer, reference Figure 2 .

[0077] Actual welding process parameters: current = 90A, tungsten electrode diameter d = 3.2mm, retraction L = 6mm, nozzle to workpiece height = 8mm, voltage = 28.5v, ion gas Q1 = 3.7L / min, powder feeding gas Q2 = 6L / min, surfacing speed = 600mm / min, single layer 2mm. The current of the second and third layers is reduced to 80A, and the others remain unchanged.

[0078] The judgment of WC cemented carbide particle burning is that the protruding corners of WC cemented carbide particles melt in the high-temperature molten pool, and the remaining C atoms on the flat surface migrate to the molten pool to form a decarburized layer (reference Figure 2 ), the wear resistance of this part drops sharply, and the degree of burning is usually judged by the thickness of the decarburized layer. The second is to test the microhardness of the WC cemented carbide particles and compare them with the original hardness value at the factory.

[0079] The surfacing materials include: Ni60 alloy powder (nickel-based wear-resistant alloy), particle size 60-120 mesh, 60% cast WC (WC hard alloy particles), particle size 60-80 mesh, factory hardness Hv2100.

[0080] The above process parameters were used for actual welding, and a blade was randomly selected to take samples from the wear-resistant layer for analysis. The results are as follows:

[0081] The average macroscopic hardness is HRC63.7. High-magnification metallographic photos show that the hard phases in the cladding layer are WC particles, decarburized layer, Cr7C3, and NiB. The average microhardness of WC is Hv=1982, the average microhardness of Cr7C3 is Hv=1326, and the average microhardness of NiB is Hv=1153. The area of ​​the three hard phases accounts for about 60-70%. Among them, the particle size of Cr7C3 and NiB is relatively small, which is represented by 05 in the figure. The white fine particles distributed in stars are Cr7C3 and NiB, which are evenly distributed in the cladding metal 03. The burning of WC cemented carbide particles, from Fig.11 and Fig.10 It can be seen that the decarburized layer 021 of C cemented carbide particle 02 is very thin, with only slight burning and little loss of wear resistance.

[0082] from Figure 10 to Figure 11 The distribution of C cemented carbide particles in the wear-resistant layer, as well as the cross-sectional diagram of the wear-resistant layer show that the distribution of C cemented carbide particles tends to be less on the top and more on the bottom. Overall, it is fairly uniform and meets the composite requirements.

[0083] Fusion line condition: From the low-magnification photograph of the cross section of the cut sample, it can be seen that the fusion line is a slightly curved curve. The wear-resistant layer is well bonded to the base material, and the test dilution rate is 3-5%.

[0084] The wear resistance of the wear-resistant layer depends on the hardness, distribution and quantity of the hard phase. The higher the hardness, the more uniform the distribution and the more quantity of the hard phase, the better the wear resistance. The hard phase Cr7C3 of the high-carbon and high-chromium wear-resistant alloy has the same hardness as above, and the area accounts for only 25-35%. Compared with the two, the former has a higher hardness, a larger quantity and a clear advantage.

[0085] The thickness of the wear-resistant layer of the 04 surface facing the material is designed to be 6mm, and the thickness of the other parts is 4mm. Figure 2 and Figure 3 , carbide particles 40-60% by weight.

[0086] This blade is particularly suitable for strong mixers, which can be used in aerated brick production, steel industry, glass industry, and rubber industry. This technology uses a powder plasma arc cladding process to manufacture blades, which belongs to the category of green manufacturing. The gene of remanufacturing is buried during the initial manufacturing. The blank can be reused 3-4 times. The second, third, and fourth remanufacturing costs are only 1 / 4 of the initial manufacturing, which has a positive contribution to the effective use of resources, the reduction of greenhouse gas emissions, and the reduction of PM2.5 concentration.

[0087] Embodiment 2

[0088] As a direction for further research and implementation examples, the WC cemented carbide particles are subjected to freezing (reducing C precipitation) pretreatment. Specifically, before welding, the tungsten carbide cemented carbide particles are subjected to liquid nitrogen cooling pretreatment. Specifically, the tungsten carbide cemented carbide particles are pre-cooled using liquid nitrogen. The temperature of the tungsten carbide cemented carbide particles is controlled between -20° and 0° by controlling the amount of liquid nitrogen used. Through the pre-cooling treatment, the temperature of the particles is reduced to a reasonable level to offset the adverse effects of the high temperature of the powder plasma arc cladding process on the tungsten carbide cemented carbide particles, so that under the action of high temperature, the solid-state migration and diffusion phenomenon of carbon atoms on the surface of the tungsten carbide cemented carbide particles can be effectively further curbed.

[0089] However, what is described above is only a specific embodiment of the present invention and should not be used to limit the scope of implementation of the present invention. Therefore, the replacement of equivalent components, or equivalent changes and modifications made according to the scope of protection of the present invention should still fall within the scope covered by the claims of the present invention.

Claims

1. A strong mixer blade, the blade comprising a steel base material located inside and a wear-resistant layer located on the surface of the base material, characterized in that: The wear-resistant layer is formed by melting the nickel-based wear-resistant alloy on the blade surface by using a powder plasma arc cladding process and adding tungsten carbide hard alloy particles for layer-by-layer cladding. The wear-resistant layer is in a microscopic state: The high-magnification metallographic photograph of the wear-resistant layer shows that the hard phases in the cladding layer include tungsten carbide cemented carbide particles, Cr7C3 particles, and NiB particles, and the hard phase area of ​​the three particles accounts for 60-70%; The power frequency used in the surfacing welding is 10k, the no-load voltage is 90v, the nozzle size is H=6, L=6, β=60º, the current is 90A, the tungsten electrode diameter d=3.2mm, the retraction amount L=6mm, the height from the nozzle to the workpiece is 8mm, the voltage is 28.5v, the ion gas Q1=3.7L / min, the powder feeding gas Q2=6L / min, the surfacing speed is 600mm / min, the single layer thickness is 2mm, the second and third layer currents are reduced to 80A, and the others remain unchanged; The tungsten carbide hard alloy particles are evenly distributed in the wear-resistant layer without sinking to the bottom; The test dilution rate of the bonding area between the wear-resistant layer and the base material is 3%-5%.

2. The intensive mixer blade according to claim 1, characterized in that: The average microhardness of tungsten carbide particles is Hv=1982, the average microhardness of Cr7C3 particles is Hv=1326, and the average microhardness of NiB particles is Hv=1153.

3. The intensive mixer blade according to claim 1, characterized in that: The weight ratio of the tungsten carbide hard alloy particles to the nickel-based wear-resistant alloy in the surfacing process is 40-60%.

4. The intensive mixer blade according to claim 1, characterized in that: The thickness of the wear-resistant layer on the material-facing surface of the blade is 6 mm, and that on the other parts is 4 mm.