Alkaline storage battery and method for manufacturing the same

By engaging the protruding part of the separator with the receiving part of the active material layer in the alkaline storage battery, the problem of increased electrolyte flow resistance caused by the polymer layer is solved, and the rapid supply of electrolyte and the uniformity of the electrode reaction are achieved. .

CN111937219BActive Publication Date: 2024-10-01TOYOTA INDUSTRIES CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980023198.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-04-05
Filing Date
2019-03-19
Publication Date
2024-10-01
Estimated Expiration
2039-03-19

AI Technical Summary

Technical Problem

In alkaline batteries, the presence of the polymer-containing layer causes the openings on the separator surface to narrow, increasing the electrolyte flow resistance, which may lead to uneven electrode reactions and increased internal resistance.

Method used

Multiple foil electrodes and separators are alternately stacked, and the protruding portion of the separator is engaged with the receiving portion of the active material layer through a compression process to ensure rapid supply of electrolyte and avoid the formation of gaps.

Benefits of technology

It effectively suppresses the formation of gaps between the separator and the active material layer, ensures the rapid supply of electrolyte, and reduces the unevenness and internal resistance of the electrode reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111937219B_ABST
    Figure CN111937219B_ABST
Patent Text Reader

Abstract

An alkaline storage battery comprises: a plurality of foil electrodes, each of which has a metal foil and an active material layer disposed on one or both sides of the metal foil, and is disposed so that the active material layers face each other; and a separator interposed between the active material layers. The separator has a protrusion protruding toward the active material layer. In addition, the active material layer has a receiving portion for receiving the protrusion of the separator. The protrusion of the separator engages with the receiving portion when entering the receiving portion of the active material layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an alkaline storage battery and a method for manufacturing the same. Background Art

[0002] For example, alkaline storage batteries are sometimes used as batteries for vehicles such as forklifts, hybrid vehicles, and electric vehicles. Such alkaline storage batteries have an electrode assembly formed by stacking a plurality of positive electrodes and negative electrodes with a separator. As a separator, a porous material such as a nonwoven fabric or a microporous membrane is used, and an electrolyte is retained in the pores of the separator. In addition, the separator is configured to be in close contact with the electrode, so that the electrolyte retained in the separator can be quickly supplied to the electrode.

[0003] When charging and discharging an alkaline storage battery, gas is sometimes generated from the positive electrode or the negative electrode. If the pressure inside the alkaline storage battery increases due to the generation of gas, a gap may be generated between the separator and the electrode, resulting in uneven electrode reaction. In order to avoid this problem, a technology has been proposed in which a polymer-containing layer containing a water-absorbing and adhesive polymer is interposed between the positive electrode and the separator and between the negative electrode and the separator (Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2003-45477 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] In the case where a polymer layer is provided between an electrode and a separator as in the alkaline secondary battery of patent document 1, the polymer constituting the polymer layer can adhere to the peripheral edge of the opening on the separator surface. Due to the presence of the polymer, the opening diameter on the separator surface is easy to narrow compared with the case without the polymer layer. In addition, depending on the amount of the polymer attached to the peripheral edge of the opening, the opening of the separator may also be completely closed.

[0009] Therefore, when a polymer-containing layer is provided on the surface of the separator, the flow resistance of the electrolyte from the separator to the electrode increases compared to when no polymer-containing layer is provided, and the supply of the electrolyte from the separator to the electrode may be delayed. As a result, uneven electrode reaction may occur in the active material layer, leading to an increase in the internal resistance of the alkaline secondary battery.

[0010] The present invention has been made in view of this background, and aims to provide an alkaline storage battery and a method for manufacturing the same, which can suppress the formation of a gap between an active material layer and a separator and can quickly supply an electrolyte from a separator to an active material layer.

[0011] Solutions for solving problems

[0012] One aspect of the present invention is an alkaline storage battery having:

[0013] A plurality of foil electrodes including a metal foil and an active material layer disposed on one or both surfaces of the metal foil, and disposed such that the active material layers face each other; and

[0014] A separator is disposed between the active material layers.

[0015] The separator is a nonwoven fabric having a plurality of fibers as protrusions protruding toward the active material layer.

[0016] The active material layer includes a plurality of active material particles bonded to each other and gaps formed between the active material particles as receiving portions for receiving the protrusions of the spacers.

[0017] The fibers are engaged in the gap.

[0018] The cumulative 50% particle size D [μm] of the active material particles based on volume, the average pore size A [μm] of the separator, and the average fiber diameter B [μm] of the separator satisfy the relationship of the following formula (1):

[0019] 0.2<D / (A+B)<1.5…(1).

[0020] Another aspect of the present invention is a method for manufacturing an alkaline storage battery. The alkaline storage battery is the alkaline storage battery of the above aspect. The method for manufacturing an alkaline storage battery comprises:

[0021] a lamination step of alternately laminating the foil electrodes and the separators to produce an electrode assembly, and impregnating the foil electrodes and the separators with an electrolyte; and

[0022] The compression step compresses the electrode assembly in a stacking direction thereof, thereby pressing a portion of the separator into the active material layer and causing the protrusion to engage with the receiving portion.

[0023] Effects of the Invention

[0024] The alkaline storage battery has a plurality of foil electrodes and separators, and the foil electrodes and separators are alternately stacked. The separator has a protrusion protruding toward the active material layer side of the foil electrode, and the active material layer has a receiving portion for receiving the protrusion of the separator. In addition, the protrusion of the separator is engaged with the receiving portion in a state of entering the receiving portion of the active material layer. By engaging the separator with the active material layer in this way, the separator can be held in the active material layer, and the formation of a gap between the separator and the active material layer is suppressed.

[0025] In addition, as described above, the alkaline storage battery holds the separator on the active material layer by engaging the protruding portion of the separator with the receiving portion of the active material layer. Therefore, there is no need to provide a layer such as an adhesive layer between the separator and the active material layer to improve the adhesion between the separator and the active material layer. Therefore, according to the alkaline storage battery, the electrolyte can be quickly supplied from the separator to the active material layer.

[0026] As described above, according to the alkaline storage battery, the formation of a gap between the electrode and the separator can be suppressed, and the electrolyte solution can be quickly supplied from the separator to the active material layer.

[0027] In addition, in the manufacturing method of the alkaline storage battery, after the electrode assembly impregnated with the electrolyte is produced in the lamination step, the electrode assembly is compressed in the compression step. By performing the compression step in a state where the electrolyte is impregnated in the electrode assembly, a part of the separator can be easily pressed into the active material layer, so that the protrusion and the receiving portion are engaged.

[0028] As a result of the above, according to the method for manufacturing the alkaline storage battery, the alkaline storage battery can be easily manufactured. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a cross-sectional view showing the main parts of the alkaline storage battery of Example 1.

[0030] Figure 2 yes Figure 1 An enlarged view of the protrusion formed on the separator and the accommodation portion formed on the positive electrode active material layer.

[0031] Figure 3 This is a photograph in lieu of a drawing of a positive electrode active material layer in Example 1 in which a mesh-like accommodation portion is formed.

[0032] Figure 4 This is a partially enlarged cross-sectional view of the interface between the separator and the positive electrode active material layer before the compression step in Example 1.

[0033] Figure 5 This is a three-dimensional diagram of the spacer in Example 2.

[0034] Figure 6 This is a partially enlarged cross-sectional view of the interface between the separator and the positive electrode active material layer before the compression step in Example 2.

[0035] Figure 7 This is a partially enlarged cross-sectional view of the interface between the separator and the positive electrode active material layer after the compression step in Example 2 is completed. DETAILED DESCRIPTION

[0036] The foil electrode in the alkaline storage battery has a metal foil as a current collector and an active material layer formed on one or both sides of the metal foil. The alkaline storage battery may be a foil electrode of any type as long as it has one or more cells and the cells are cells in which the positive electrode active material layer and the negative electrode active material layer as active material layers face each other through a separator.

[0037] For example, the alkaline storage battery may include a positive electrode having a positive electrode active material layer as an active material layer on one or both sides of a metal foil, and a negative electrode having a negative electrode active material layer as an active material layer on one or both sides of the metal foil. When these unipolar electrodes are used as foil electrodes, a single cell can be formed by alternately stacking the positive electrode and the negative electrode with a separator therebetween.

[0038] Alternatively, the foil electrode may be a bipolar electrode having a positive electrode active material layer as an active material layer disposed on one surface of the metal foil and a negative electrode active material layer as an active material layer disposed on the other surface of the metal foil. In this case, by a simple structure of stacking a plurality of bipolar electrodes with a separator interposed therebetween, the positive electrode active material layer and the negative electrode active material layer can be placed face to face with the separator interposed therebetween.

[0039] When bipolar electrodes are used, the number of cells relative to the total number of electrodes can be increased compared to when monopolar electrodes are used. Therefore, the total number of electrodes can be reduced compared to monopolar electrodes, and the size of the alkaline storage battery in the stacking direction of the foil electrodes and the separator can be further reduced.

[0040] On the other hand, when a bipolar electrode is used, a single cell is formed between adjacent metal foils, so the width of the single cell in the stacking direction of the foil electrode and the separator is narrower than that of the above-mentioned unipolar electrode. Therefore, in this case, there is a problem that when gas is generated from the positive electrode active material layer or the negative electrode active material layer, the internal pressure of the single cell is likely to increase.

[0041] However, as described above, the alkaline storage battery can firmly hold the separator to the active material layer by the engagement between the protrusion of the separator and the receiving portion of the active material layer. Therefore, even when the bipolar electrode is used as a foil electrode, the separator can be prevented from peeling off from the active material layer.

[0042] Therefore, the alkaline storage battery described above can not only further reduce the size of the alkaline storage battery in the stacking direction of the foil electrode and the separator, but also suppress separation of the separator from the active material layer by using the bipolar electrode as the foil electrode.

[0043] In the alkaline storage battery, the separator has a protrusion protruding toward the active material layer, and the active material layer has a receiving portion for receiving the protrusion of the separator. The protrusion engages with the receiving portion when entering the receiving portion. In other words, the protrusion is held in the receiving portion in a state where at least a portion of the protrusion is embedded in the receiving portion or in a state where the protrusion is intertwined with the receiving portion.

[0044] The shapes of the protrusion and the accommodation portion are not particularly limited, and may have any shape as long as the protrusion and the accommodation portion can be engaged with each other.

[0045] The protrusion may be pressed into both the positive electrode active material layer and the negative electrode active material layer and engage with the receiving portion formed in these active material layers, or may be pressed into either the positive electrode active material layer or the negative electrode active material layer and engage with the receiving portion formed in the active material layer.

[0046] Preferably, the protrusion is engaged with the receiving portion formed in the positive electrode active material layer. In an alkaline storage battery, gas is more likely to be generated from the positive electrode active material layer than from the negative electrode active material layer, so a gap is likely to be generated between the positive electrode active material layer and the separator. Therefore, by engaging the protrusion with the receiving portion formed in the positive electrode active material layer, the formation of a gap between the positive electrode active material layer and the separator can be more effectively suppressed.

[0047] Alternatively, the protrusion may be pre-set on the separator before it overlaps with the foil electrode. In this case, by compressing the electrode assembly in its stacking direction after the separator and the foil electrode are overlapped to produce the electrode assembly, the protrusion can be pressed into the active material layer and the receiving portion can be formed on the active material layer while the protrusion is engaged with the receiving portion. Similarly, the receiving portion may be pre-set on the active material layer of the foil electrode before it overlaps with the separator. In this case, by compressing the electrode assembly in its stacking direction, the separator can be pressed into the receiving portion and the protrusion can be formed on the separator while the protrusion is engaged with the receiving portion. Furthermore, it is also possible that the protrusion is pre-set on the separator, and the receiving portion is pre-set on the active material layer.

[0048] In addition, by appropriately combining the material of the separator and the structure of the active material layer, it is not necessary to pre-set the protrusion or the receiving portion, and the protrusion and the receiving portion can be formed by a simple operation of compressing the electrode assembly in the stacking direction, so that the protrusion and the receiving portion are engaged. From this point of view, it is preferred to use a non-woven fabric having many fibers as a separator and having an active material layer as follows: the active material layer has many active material particles bonded to each other and gaps formed between these active material particles.

[0049] By pressing the separator including the nonwoven fabric onto the active material layer including many active material particles, the gaps between the active material particles existing on the surface of the active material layer become the receiving portion, and the fibers of the separator can be pressed into the gaps between the active material particles. As a result, while a part of the fibers of the separator protrudes toward the active material layer to form a protrusion, the protrusion can be embedded in the above-mentioned gap as the receiving portion, so that the protrusion and the receiving portion are engaged.

[0050] In addition, since the fibers of the nonwoven fabric are randomly entangled with each other, by pressing the fibers into the active material layer, a protrusion extending in a mesh shape can be formed on the separator, and a mesh-shaped receiving portion corresponding to the protrusion can be formed on the active material layer. Then, by engaging the protrusion extending in a mesh shape with the receiving portion, the separator can be more firmly held on the active material layer, and the formation of a gap between the separator and the active material can be more effectively suppressed.

[0051] Furthermore, in this case, the protrusion and the receiving portion can be formed by a simple operation of compressing the electrode assembly in the stacking direction, so there is no need to preliminarily set the protrusion on the separator or set the receiving portion on the active material layer. Therefore, the complication of the manufacturing process caused by these operations can be avoided.

[0052] In the above case, it is preferred that the cumulative 50% particle size D [μm] of the active material particles based on volume, the average pore size A [μm] of the spacer, and the average fiber diameter B [μm] of the spacer satisfy the relationship of the following formula (1).

[0053] 0.2<D / (A+B)<1.5…(1)

[0054] In this case, the gaps between the active material particles on the surface of the active material layer are easily matched with the intervals between the fibers constituting the separator. Therefore, by compressing the electrode assembly in the stacking direction, the fibers of the separator can be more easily pressed into the gaps between the active material particles. As a result, the separator can be more firmly held in the active material layer, and the formation of a gap between the separator and the active material can be more effectively suppressed.

[0055] When the cumulative 50% particle size D of the active material particles, the average pore size A of the separator, and the average fiber diameter B do not satisfy the above formula (1), the gaps between the active material particles and the intervals between the fibers of the separator are difficult to match compared to the case where the above formula (1) is satisfied. Therefore, in this case, compared to the case where the cumulative 50% particle size D of the active material particles, the average pore size A of the separator, and the average fiber diameter B satisfy the relationship of the above formula (1), it is possible that a gap is easily formed between the separator and the positive electrode active material layer.

[0056] In addition, in the above case, it is preferred that the average fiber diameter B [μm] of the separator is smaller than the cumulative 50% particle diameter D [μm] of the active material particles based on the volume. In this case, the fibers exposed on the surface of the separator are easy to enter the gaps between the active material particles present on the surface of the active material layer. Therefore, by compressing the electrode assembly in the stacking direction, the fibers exposed on the surface of the separator can be more easily pressed into the gaps between the active material particles. As a result, the separator can be more firmly held in the active material layer, and the formation of a gap between the separator and the active material can be more effectively suppressed.

[0057] Next, specific aspects of each component of the above-mentioned alkaline storage battery will be described.

[0058] The metal foil as a current collector is a chemically inert electron conductor used to allow current to continue to flow through the electrode during the discharge or charging of the alkaline storage battery. As the material of the metal foil, a metal that can withstand the voltage used to react the active material can be used. As the material of the metal foil, for example, single metals such as silver, copper, gold, aluminum, tungsten, cobalt, zinc, nickel, iron, platinum, tin, indium, titanium, ruthenium, tantalum, chromium, molybdenum, stainless steel, aluminum alloys and other alloys can be used. In addition, as the metal foil, a metal foil that has been subjected to surface treatment such as nickel-plated copper foil and nickel-plated stainless steel foil can also be used.

[0059] When the alkaline storage battery is a nickel-metal hydride storage battery, nickel foil, nickel-plated copper foil, or nickel-plated stainless steel foil is preferably used as the metal foil. For example, the thickness of the metal foil can be appropriately set within a range of 5 to 100 μm.

[0060] The active material layer is disposed on one or both sides of the metal foil. The active material layer generally contains a plurality of active material particles and a binder for bonding the active material particles to each other and to the metal foil. The active material layer may also contain additives such as a conductive aid as required.

[0061] The specific composition of the active material layer can be appropriately set according to the structure of the alkaline storage battery and the polarity of the active material layer. For example, when the active material layer is a positive electrode active material layer of a nickel-hydrogen storage battery, nickel hydroxide or nickel hydroxide doped with a metal can be used as the positive electrode active material particles. As the metal doped in the nickel hydroxide, for example, group 2 elements such as magnesium and calcium, group 9 elements such as cobalt, rhodium, and iridium, and group 12 elements such as zinc and cadmium can be used. The positive electrode active material particles can also be surface treated by a known method for nickel-hydrogen storage batteries.

[0062] For example, the cumulative 50% particle size of the positive electrode active material particles based on volume can be appropriately set from 1 to 100 μm. The cumulative 50% particle size of the positive electrode active material particles based on volume is preferably 3 to 50 μm, more preferably 5 to 30 μm, and further preferably 7 to 18 μm. In addition, the above-mentioned cumulative 50% particle size based on volume is a value calculated based on the particle size distribution measured by a laser diffraction particle size distribution meter.

[0063] For example, the content of the positive electrode active material particles in the positive electrode active material layer can be appropriately set within a range of 75 to 99 mass %. The content of the positive electrode active material particles is preferably 80 to 97 mass %, and more preferably 85 to 95 mass %.

[0064] Alternatively, the positive electrode active material layer of the nickel-metal hydride storage battery may contain one or two of metal cobalt and cobalt compounds as conductive additives. As the cobalt compound, for example, cobalt hydroxide may be used. The metal cobalt and cobalt compounds may be contained in the positive electrode active material layer as their powders, or may be attached to the surface of the positive electrode active material particles.

[0065] For example, the content of the metal cobalt and the cobalt compound in the positive electrode active material layer can be appropriately set within the range of 0.5 to 10 mass %. The content of the metal cobalt and the cobalt compound is preferably 1 to 7 mass %, and more preferably 2 to 5 mass %.

[0066] The positive electrode active material layer of the nickel-metal hydride storage battery may further contain a conductive agent other than metal cobalt and cobalt compounds. The conductive agent may be a metal such as nickel or copper, a metal oxide or hydroxide thereof, carbon black, black lead, carbon fiber or other carbon material.

[0067] Alternatively, the positive electrode active material layer of the nickel-hydrogen storage battery may further include a positive electrode additive for improving battery characteristics. As the positive electrode additive, for example, niobium compounds such as Nb2O5, tungsten compounds such as WO2, WO3, Li2WO4, Na2WO4, and K2WO4, ytterbium compounds such as Yb2O3, titanium compounds such as TiO2, yttrium compounds such as Y2O3, zinc compounds such as ZnO, calcium compounds such as CaO, Ca(OH)2, and CaF2, oxides of rare earth elements other than the above elements, etc. may be used.

[0068] For example, the content of the positive electrode additive in the positive electrode active material layer can be appropriately set within a range of 0.1 to 10% by mass, and preferably 0.5 to 5% by mass.

[0069] In the case where the active material layer is the negative electrode active material layer of a nickel-hydrogen storage battery, a hydrogen storage alloy can be used as the negative electrode active material particle. As the hydrogen storage alloy, for example, the following can be used: AB5 type hydrogen storage alloy having a hexagonal CaCu5 type crystal structure, AB2 type hydrogen storage alloy having a hexagonal MgZn2 type crystal structure or a cubic MgCu2 type crystal structure, AB type hydrogen storage alloy having a cubic CsCl type crystal structure, A2B type hydrogen storage alloy having a hexagonal Mg2Ni type crystal structure, solid solution type hydrogen storage alloy having a body-centered cubic crystal structure, etc. In addition, as the hydrogen storage alloy, for example, AB3 type hydrogen storage alloy, A2B7 type hydrogen storage alloy, A5B 19 The invention also provides hydrogen storage alloys having a crystal structure formed by combining an AB5 type crystal structure and an AB2 type crystal structure, etc. These hydrogen storage alloys may be used alone or in combination of two or more.

[0070] More specifically, as AB5 type hydrogen storage alloys, for example, LaNi5, CaCu5, MmNi5, etc. can be used. In addition, the above-mentioned Mm is a symbol representing the so-called mixed rare earth metal (misch metal). As AB2 type hydrogen storage alloys, for example, MgZn2, ZrNi2, ZrCr2, etc. can be used. As AB type hydrogen storage alloys, for example, TiFe, TiCo, etc. can be used. As A2B type hydrogen storage alloys, for example, Mg2Ni, Mg2Cu, etc. can be used. As solid solution type hydrogen storage alloys, for example, Ti-V, V-Nb, Ti-Cr, etc. can be used.

[0071] As the AB3 type hydrogen storage alloy, for example, CeNi3 or the like can be used. As the A2B7 type hydrogen storage alloy, for example, Ce2Ni7 or the like can be used. As the A5B 19 Type hydrogen storage alloys, such as Ce5Co 19 、Pr5Co 19Part of the constituent elements in these hydrogen storage alloys may be replaced by other elements.

[0072] The negative electrode active material particles may be subjected to a known surface treatment used in nickel-metal hydride storage batteries. For example, the negative electrode active material particles may be subjected to an alkaline treatment by being immersed in an alkaline aqueous solution.

[0073] For example, the cumulative 50% particle size of the negative electrode active material particles based on volume can be appropriately set within the range of 1 to 100 μm. The cumulative 50% particle size of the negative electrode active material particles is preferably 3 to 50 μm, more preferably 5 to 30 μm, and further preferably 7 to 18 μm.

[0074] The content of the negative electrode active material particles in the negative electrode active material layer can be appropriately set, for example, in the range of 85 to 99 mass %. The content of the negative electrode active material particles is preferably 90 to 98 mass %.

[0075] Alternatively, the negative electrode active material layer of the nickel-hydrogen storage battery may further include a conductive aid including a chemically inert electronic conductor. As the conductive aid, for example, metals such as cobalt, nickel, and copper, oxides and hydroxides of these metals, carbon black, black lead, carbon fibers, and other carbon materials may be used. These conductive aids may be included in the negative electrode active material layer as powders, or may be attached to the surface of the negative electrode active material particles.

[0076] For example, the content of the conductive aid in the negative electrode active material layer can be appropriately set within a range of 0.1 to 5 mass %, preferably 0.2 to 3 mass %, more preferably 0.3 to 1 mass %.

[0077] Alternatively, the negative electrode active material layer of the nickel-metal hydride storage battery may further include a negative electrode additive for improving battery characteristics. As the negative electrode additive, for example, fluorides of rare earth elements such as CeF3 and YF3, bismuth compounds such as Bi2O3 and BiF3, and indium compounds such as In2O3 and InF3 may be used. In addition, the above-mentioned positive electrode additive may also be used as a negative electrode additive.

[0078] For example, the content of the negative electrode additive in the negative electrode active material layer can be appropriately set within a range of 0.1 to 10% by mass, and preferably 0.5 to 5% by mass.

[0079] As the binder contained in the active material layer, for example, fluorine-containing resins such as polyvinylidene fluoride, polytetrafluoroethylene and fluororubber, polyolefins such as polypropylene and polyethylene, imide resins such as polyimide and polyamide-imide, cellulose derivatives such as carboxymethyl cellulose, methyl cellulose and hydroxypropyl cellulose, (meth)acrylic resins containing (meth)acrylic acid derivatives such as polyacrylic acid, polyacrylate, polymethacrylic acid and polymethacrylate as monomer units, styrene butadiene rubber, etc. can be used.

[0080] For example, the content of the binder in the active material layer can be appropriately set within the range of 0.1 to 15 mass %. The content of the binder is preferably 1 to 10 mass %, and more preferably 2 to 7 mass %.

[0081] Preferably, the active material layer further includes carboxymethyl cellulose as a thickener. The active material layer containing carboxymethyl cellulose is easily softened by being impregnated with the electrolyte compared to before being impregnated with the electrolyte. Therefore, by impregnating the electrolyte into the active material layer containing carboxymethyl cellulose, a part of the separator can be more easily pressed into the active material layer. As a result, the separator can be more firmly held in the active material layer, and the formation of a gap between the separator and the active material can be more effectively suppressed.

[0082] As the separator, porous films, nonwoven fabrics, and woven fabrics including insulators that are chemically stable to the electrolyte can be used. As the insulator constituting the separator, for example, synthetic resins such as polytetrafluoroethylene, polypropylene, polyethylene, ethylene-propylene copolymers, polyimide, polyamide, polyester, and polyacrylonitrile, polysaccharides such as cellulose and straight-chain starch, and natural polymers such as silk protein, keratin, lignin, and suberin can be used. These insulators can be used alone or in combination of two or more.

[0083] In addition, the separator may be subjected to a hydrophilization treatment such as sulfonation treatment, corona treatment, fluorine gas treatment, plasma treatment, or the like.

[0084] When the alkaline storage battery is a nickel-hydrogen storage battery, a nonwoven fabric made of polyolefin such as polypropylene, polyethylene, or ethylene-propylene copolymer is preferably used as a separator. In this case, the average pore size of the nonwoven fabric is preferably 10 to 25 μm. In addition, the average fiber diameter of the nonwoven fabric is preferably 2 to 10 μm.

[0085] The average pore size of the nonwoven fabric can be calculated by the bubble point method specified in JIS K3832: 1990. The average fiber diameter of the nonwoven fabric is the average value of the fiber diameters of 10 fibers randomly selected from the SEM image obtained by observing the surface of the nonwoven fabric with a scanning electron microscope.

[0086] When making the above alkaline storage battery,

[0087] The following method for manufacturing an alkaline storage battery can be adopted, which has the following characteristics:

[0088] a lamination step of alternately laminating the foil electrodes and the separators to produce an electrode assembly, and impregnating the foil electrodes and the separators with an electrolyte; and

[0089] The compression step compresses the electrode assembly in a stacking direction thereof, thereby pressing a portion of the separator into the active material layer and causing the protrusion to engage with the receiving portion.

[0090] In the lamination process, the operation of alternately laminating the foil electrode and the separator and the operation of impregnating the foil electrode and the separator with the electrolyte may be performed in any order. For example, after the foil electrode and the separator are alternately laminated to form an electrode assembly, the electrolyte may be impregnated into the electrode assembly. In addition, after the foil electrode and the separator are impregnated with the electrolyte, the foil electrode and the separator may be alternately laminated to form an electrode assembly.

[0091] As the electrolyte, a known electrolyte for alkaline storage batteries can be used. When the alkaline storage battery is a nickel-metal hydride storage battery, an aqueous solution of an alkali metal hydroxide such as lithium hydroxide, sodium hydroxide, potassium hydroxide, etc. can be used as the electrolyte. These alkali metal hydroxides can be used alone or in combination of two or more.

[0092] In addition, the electrolyte may further contain alkali metal halides such as LiF, LiCl, LiBr, LiI, NaF, NaCl, NaBr, NaI, KF, KCl, KBr, and KI.

[0093] In the compression step, the electrode assembly is compressed in the stacking direction of the foil electrode and the separator. In the compression step, the end face of the electrode assembly in the stacking direction can be directly compressed, or the end face of the electrode assembly in the stacking direction can be covered with another member such as a housing, and the electrode assembly can be compressed through the member. In the latter case, by increasing the rigidity of the member disposed on the end face of the electrode assembly, the entire electrode assembly can be uniformly compressed.

[0094] In the compression step, the electrode assembly is preferably compressed in the stacking direction at a pressure of 0.1 MPa to 1.5 MPa, more preferably at a pressure of 0.15 MPa to 1.3 MPa, and even more preferably at a pressure of 0.2 MPa to 1.0 MPa.

[0095] When the pressure applied to the electrode assembly is less than 0.1 MPa, the compression amount of the electrode assembly is insufficient, so it may be difficult to engage the protrusion with the receiving portion. When the pressure applied to the electrode assembly exceeds 1.5 MPa, the compression amount of the separator is too large, which may cause the porosity of the separator to decrease. As a result, it is difficult for the electrolyte to move in the separator, which may increase the resistance of the alkaline storage battery.

[0096] Example 1

[0097] use Figure 1 to Figure 4 An example of the above alkaline storage battery is described below. Figure 1 As shown, the alkaline storage battery 1 of this example comprises: a plurality of foil electrodes 11 (11b, 11n, 11p), which comprises a metal foil 2 and active material layers 3 (3p, 3n) arranged on one or both sides of the metal foil 2, and arranged so that the active material layers 3 face each other; and a separator 4 interposed between the active material layers 3. Figure 2 As shown in FIG. 1 , the separator 4 has a protrusion 41 protruding toward the active material layer 3. Figure 2 and Figure 3 As shown in FIG. 1 , the active material layer 3 has a receiving portion 31 for receiving the protruding portion 41 of the separator 4. Figure 2 As shown, the protrusion 41 of the separator is engaged with the receiving portion 31 in a state of entering the receiving portion 31 of the active material layer 3 .

[0098] The following describes in detail the structure of the alkaline storage battery 1 of this example. The alkaline storage battery 1 of this example is a nickel-hydrogen storage battery. Figure 1 As shown, the alkaline storage battery 1 comprises: an electrode assembly 10 formed by stacking a plurality of foil electrodes 11 with a separator 4 interposed therebetween; a restraining member 12 abutting against the ends of the electrode assembly 10 in the stacking direction to restrain the electrode assembly 10; and a sealing material 13 covering the side circumference of the electrode assembly 10. The electrode assembly 10 comprises terminal electrodes 11n and 11p disposed at both ends in the stacking direction and a plurality of bipolar electrodes 11b disposed between the terminal electrodes 11n and 11p as foil electrodes 11. In addition, the electrode assembly 10 is impregnated with an electrolyte.

[0099] The bipolar electrode 11b includes a rectangular metal foil 2, a positive electrode active material layer 3p as an active material layer 3 provided on one surface of the metal foil 2, and a negative electrode active material layer 3n as an active material layer 3 provided on the other surface of the metal foil 2. The positive electrode active material layer 3p and the negative electrode active material layer 3n are provided in a region inside the peripheral edge portion 21 of the metal foil 2. The peripheral edge portion 21 of the metal foil 2 is retained by the sealing material 13. The metal foil 2 in this example is specifically a nickel foil having a thickness of 50 μm.

[0100] like Figure 2 As shown, the positive electrode active material layer 3p contains a plurality of positive electrode active material particles 32p. The receiving portion 31 in the positive electrode active material layer 3p is the gap between the positive electrode active material particles 32p. The positive electrode active material layer 3p contains: 95 parts by mass of nickel hydroxide as the positive electrode active material particles 32p, 1 part by mass of metal cobalt as a conductive auxiliary agent, 2 parts by mass of styrene butadiene rubber as a binder, 1 part by mass of carboxymethyl cellulose as a thickener, and 1 part by mass of Y2O3 as an oxygen inhibitor.

[0101] Although not shown in the figure, the surface of the nickel hydroxide as the positive electrode active material particle 32p is covered with cobalt oxide. The cumulative 50% particle size of the positive electrode active material particle 32p based on volume is 15 μm. Figure 2 In the description, for the sake of convenience, the description of the conductive additive, the adhesive, the thickener and the oxygen inhibitor is omitted.

[0102] The mass per unit area of ​​the positive electrode active material layer 3p is 30 mg / cm 2 The thickness is 100 μm. The apparent density of the positive electrode active material layer 3p, that is, the density including the voids in the positive electrode active material layer 3p, is 3.0 g / cm 3 .

[0103] The negative electrode active material layer 3n contains a plurality of negative electrode active material particles, 96 parts by mass of hydrogen storage alloy as negative electrode active material particles, 3 parts by mass of styrene butadiene rubber as a binder, and 1 part by mass of carboxymethyl cellulose as a thickener.

[0104] The mass per unit area of ​​the negative electrode active material layer 3n is 45 mg / cm 2 The thickness is 90 μm. In addition, the apparent density of the negative electrode active material layer 3n is 5.0 g / cm 3 .

[0105] like Figure 1 As shown, of the two terminal electrodes 11n and 11p, the first terminal electrode 11p disposed at one end in the stacking direction has the same structure as the bipolar electrode 11b except that it does not have the negative electrode active material layer 3n. In addition, the second terminal electrode 11n disposed at the other end in the stacking direction has the same structure as the bipolar electrode 11b except that it does not have the positive electrode active material layer 3p.

[0106] These foil electrodes 11 are arranged in such a manner that the positive electrode active material layer 3p and the negative electrode active material layer 3n are alternately arranged in the stacking direction. In addition, the separator 4 is interposed between the positive electrode active material layer 3p and the negative electrode active material layer 3n. Thus, between the metal foils 2, a single cell C is formed in which the positive electrode active material layer 3p and the negative electrode active material layer 3n face each other through the separator 4. In addition, in the electrode assembly 10 of this example, a plurality of single cells C are electrically connected in series via the metal foil 2.

[0107] like Figure 2 As shown, the separator 4 of this example is a rectangular nonwoven fabric including polyolefin fibers 42. The average pore size of the separator 4 of this example is 10 μm, and the average fiber diameter is 5 μm.

[0108] The protrusion 41 in the separator 4 of this example is a part of the fiber 42 exposed on the surface of the separator 4. Figure 2 As shown in the example in FIG. 1 , the fiber 42 as the protrusion 41 is pressed into the gap between the positive electrode active material particles 32p in the positive electrode active material layer 3p, and a part of the fiber 42 is embedded in the gap between the positive electrode active material particles 32p. As a result, the fiber 42 as the protrusion 41 is engaged with the gap between the positive electrode active material particles 32p as the receiving portion 31. Figure 3 As shown, the accommodation portion 31 of this example is in a mesh shape.

[0109] Metal restraint members 12 are disposed at both ends of the electrode assembly 10 in the stacking direction. The restraint members 12 are held by a holding plate (not shown) in contact with the metal foils 2 of the terminal electrodes 11n and 11p. The electrode assembly 10 of this example is configured to be electrically connectable to an external circuit via the restraint members 12.

[0110] The alkaline storage battery 1 of this example can be manufactured, for example, by the following method. First, a stacking step is performed in which the foil electrodes 11 (11b, 11n, 11p) and the separators 4 are alternately stacked and the electrolyte is impregnated into the foil electrodes 11 and the separators 4. In this example, after the foil electrodes 11 and the separators 4 are alternately stacked to manufacture the electrode assembly 10, the electrolyte is impregnated into each foil electrode 11 and the separator 4 from a liquid injection port (not shown).

[0111] Thereafter, a compression step is performed to compress the electrode assembly 10 in the stacking direction thereof, so that, for example, Figure 2 As shown in FIG. 1 , the fibers 42 exposed on the surface of the separator 4 can be pressed into the gaps between the positive electrode active material particles 32p. As a result, the fibers 42 as the protrusions 41 can be embedded in the gaps between the positive electrode active material particles 32p as the receiving portions 31, and the protrusions 41 can be engaged with the receiving portions 31. Figure 3As shown, the accommodation portion 31 of this example is depressed into a groove shape by being pressed by the fiber 42 serving as the protrusion 41 .

[0112] Next, the effects of the alkaline storage battery 1 of this example will be described. The alkaline storage battery 1 of this example has a plurality of foil electrodes 11 and separators 4, and the foil electrodes 11 and separators 4 are alternately stacked. The separator 4 has a protrusion 41 protruding toward the positive electrode active material layer 3p side of the foil electrode 11, and the positive electrode active material layer 3p has a receiving portion 31 for receiving the protrusion 41 of the separator 4. Furthermore, the protrusion 41 of the separator 4 is engaged with the receiving portion 31 of the positive electrode active material layer 3p. By engaging the separator 4 with the positive electrode active material layer 3p in this way, the separator 4 can be held on the positive electrode active material layer 3p, and the formation of a gap between the separator 4 and the positive electrode active material layer 3p can be suppressed.

[0113] In addition, as described above, the alkaline storage battery 1 holds the separator 4 on the positive electrode active material layer 3p by engaging the protrusion 41 of the separator 4 with the receiving portion 31 of the positive electrode active material layer 3p, so there is no need to provide a layer such as an adhesive layer between the separator 4 and the positive electrode active material layer 3p for improving the adhesion between the separator 4 and the positive electrode active material layer 3p. Therefore, according to the alkaline storage battery 1, the electrolyte can be quickly supplied from the separator 4 to the active material layer 3.

[0114] The separator 4 of this example is a nonwoven fabric having many fibers 42, and the positive electrode active material layer 3p has many positive electrode active material particles 32p bonded to each other and gaps formed between the positive electrode active material particles 32p. In addition, the fibers 42 as the protrusions 41 engage with the gaps between the positive electrode active material particles 32p as the receiving portions 31. By combining the material of the separator 4 with the structure of the positive electrode active material layer 3p in this way, it is not necessary to pre-set the protrusions 41 or the receiving portions 31. The protrusions 41 and the receiving portions 31 can be formed by a simple operation of compressing the electrode assembly 10 in the stacking direction, and the protrusions 41 and the receiving portions 31 engage with each other. Therefore, it is possible to avoid the complication of the manufacturing process caused by the operation of setting the protrusions 41 on the separator 4 or the operation of setting the receiving portions 31 on the positive electrode active material layer 3p.

[0115] In addition, by pressing the separator 4 including the nonwoven fabric onto the positive electrode active material layer 3p including many active material particles, the fibers 42 of the separator 4 can be pressed into the gaps between the positive electrode active material particles 32p to form the mesh-like protrusions 41 and the accommodation portions 31. As a result, the separator 4 can be more firmly held on the positive electrode active material layer 3p, and the formation of a gap between the separator 4 and the positive electrode active material layer 3p can be more effectively suppressed.

[0116] The positive electrode active material layer 3p of this example contains positive electrode active material particles 32p with a cumulative 50% particle size of 15 μm based on volume. In addition, the average pore size of the separator 4 is 10 μm, and the average fiber diameter is 5 μm. Therefore, the cumulative 50% particle size D [μm] of the positive electrode active material particles 32p based on volume, the average pore size A [μm] of the separator 4, and the average fiber diameter B [μm] of the separator 4 satisfy the relationship of the following formula (1).

[0117] 0.2<D / (A+B)<1.5…(1)

[0118] If the foil electrodes 11 and separators 4 of this example are alternately stacked, the average spacing between the fibers 42 exposed on the surface of the separator 4, i.e., the sum of the average pore diameter A and the average fiber diameter B, and the average spacing between the positive electrode active material particles 32p exposed on the surface of the positive electrode active material layer 3p, i.e., the cumulative 50% particle diameter D of the positive electrode active material particles 32p, will be of the same magnitude. Figure 4 As shown in the example in FIG. 2 , the gaps between the positive electrode active material particles 32 p and the intervals between the fibers 42 of the separator 4 are easily matched.

[0119] Therefore, by compressing the electrode assembly 10, the fibers 42 exposed on the surface of the separator 4 can more easily enter the gaps between the positive electrode active material particles 32p, and the fibers 42 can be more easily pressed into the gaps. As a result, the separator 4 can be more firmly held on the positive electrode active material layer 3p, and the formation of a gap between the separator 4 and the positive electrode active material layer 3p can be more effectively suppressed.

[0120] Furthermore, the average fiber diameter of the separator 4 in this example is smaller than the cumulative 50% particle diameter D of the positive electrode active material particles 32p. Figure 4 As shown, the fibers 42 of the separator 4 easily enter the gaps between the positive electrode active material particles 32p existing on the surface of the positive electrode active material layer 3p. Therefore, by compressing the electrode assembly 10, a part of the fibers 42 of the separator 4 can be more easily pressed into the gaps between the positive electrode active material particles 32p existing on the surface of the positive electrode active material layer 3p. As a result, the separator 4 can be more firmly held on the positive electrode active material layer 3p, and the formation of a gap between the separator 4 and the positive electrode active material layer 3p can be more effectively suppressed.

[0121] In addition, the positive electrode active material layer 3p of this example contains carboxymethyl cellulose. The positive electrode active material layer 3p containing carboxymethyl cellulose is easily softened by being impregnated with the electrolyte compared to before being impregnated with the electrolyte. Therefore, by compressing the electrode assembly 10 after impregnating the positive electrode active material layer 3p with the electrolyte, the fibers 42 of the separator 4 can be more easily pressed into the gaps between the positive electrode active material particles 32p. As a result, the separator 4 can be more firmly held in the positive electrode active material layer 3p, and the formation of a gap between the separator 4 and the positive electrode active material layer 3p can be more effectively suppressed.

[0122] The negative electrode active material layer 3n of this example has a higher apparent density than the positive electrode active material layer 3p, and is therefore harder than the positive electrode active material layer 3p. Therefore, when the electrode assembly 10 is compressed in the stacking direction in the compression step, the separator 4 can be supported by the negative electrode active material layer 3n, and the load when the separator 4 is pressed against the positive electrode active material layer 3p can be further increased. As a result, the protrusion 41 and the housing 31 can be formed more easily.

[0123] As described above, according to the alkaline storage battery 1 of this example, it is possible to suppress the formation of a gap between the active material layer 3 and the separator 4 and to quickly supply the electrolyte from the separator 4 to the active material layer 3 .

[0124] Example 2

[0125] This example is an example of a spacer 402 having a protrusion 43 formed in advance. In addition, among the reference numerals used in this example, the same reference numerals as those in the previous examples indicate the same components as those in the previous examples unless otherwise specified.

[0126] The separator 402 in this example is a non-woven fabric including polyolefin fibers. Figure 5 As shown, the spacer 402 has a plurality of protrusions 43 in a columnar shape.

[0127] The manufacturing method of the alkaline storage battery 102 using the separator 402 of this example is the same as that of Example 1. That is, first, a stacking step is performed in which the foil electrodes 11 and the separators 402 are alternately stacked and the foil electrodes 11 and the separators 402 are impregnated with an electrolyte. Figure 6 As shown, the electrode assembly 14 is fabricated by alternately stacking the foil electrodes 11 and the separators 402 so that the protrusions 43 of the separators 402 come into contact with the positive electrode active material layers 3 p .

[0128] Thereafter, a compression step is performed to compress the electrode assembly 14 in the stacking direction. Figure 7As shown, the protrusion 43 can be pressed into the positive electrode active material layer 3p. As a result, the housing 33 can be formed in the positive electrode active material layer 3p, and the protrusion 43 of the separator 402 can be engaged with the housing 33 while entering the housing 33.

[0129] In the alkaline storage battery 102 of this example, the protrusion 43 of the separator 402 is engaged with the receiving portion 33 of the positive electrode active material layer 3p, so that the formation of a gap between the separator 402 and the positive electrode active material layer 3p can be suppressed. In addition, the alkaline storage battery 102 of this example does not need to provide other layers such as adhesive layers between the separator 402 and the positive electrode active material layer 3p. Therefore, the electrolyte can be quickly supplied from the separator 402 to the active material layer 3.

[0130] Experimental example

[0131] This example is an example of an alkaline storage battery 1 in which the cumulative 50% particle size of the positive electrode active material particles 32p, the average pore size of the separator 4, and the average fiber diameter are variously changed. In this example, alkaline storage batteries 1 (test bodies A1 to A5) having the cumulative 50% particle size of the positive electrode active material particles 32p, the average pore size of the separator 4, and the average fiber diameter shown in Table 1 were prepared.

[0132] These test bodies were charged at a charging rate of 1C in an environment of 45°C, and the charging was terminated 1 hour after the start of charging, that is, when the SOC (State of Charge) reached 100%. Then, the internal pressure of each single cell C in the test body was measured in this state. The maximum value of the internal pressure of the single cell C in each test body is shown in Table 1.

[0133] [Table 1]

[0134]

[0135] As shown in Table 1, the cumulative 50% particle size D [μm] of the positive electrode active material particles 32p based on volume in the test pieces A1 to A3, the average pore size A [μm] of the separator 4, and the average fiber diameter B [μm] of the separator 4 satisfy the relationship of the following formula (1).

[0136] 0.2<D / (A+B)<1.5…(1)

[0137] Therefore, the maximum value of the internal pressure of the single cell C at the end of charging in these test bodies is smaller than that of the test bodies A4 and A5 that do not satisfy the relationship of the above formula (1). From these results, it can be understood that when the cumulative 50% particle size D [μm] of the positive electrode active material particles 32p based on volume, the average pore size A [μm] of the separator 4, and the average fiber diameter B [μm] of the separator 4 satisfy the relationship of the above formula (1), the separator 4 is more firmly held in the positive electrode active material layer 3p, so that the increase in the internal pressure of the single cell C can be suppressed.

[0138] The specific aspects of the alkaline storage battery and the method for producing the same according to the present invention are not limited to those of the above-described Embodiments 1 and 2, and the configurations can be appropriately changed within a range that does not impair the gist of the present invention.

[0139] Description of Reference Numerals

[0140] 1. 102 Alkaline storage battery

[0141] 11 Foil Electrode

[0142] 2 metal foil

[0143] 3 Active material layer

[0144] 31, 33 Accommodation

[0145] 4. 402 Isolation

[0146] 41, 43 protrusions.

Claims

1. An alkaline storage battery, It is characterized in that have: A plurality of foil electrodes including a metal foil and an active material layer disposed on one or both surfaces of the metal foil, and disposed such that the active material layers face each other; as well as A separator is disposed between the active material layers. The separator is a nonwoven fabric having a plurality of fibers as protrusions protruding toward the active material layer. The active material layer includes a plurality of active material particles bonded to each other and gaps formed between the active material particles as receiving portions for receiving the protrusions of the spacers. The fibers are engaged in the gap. The cumulative 50% particle size D [μm] of the active material particles based on volume, the average pore size A [μm] of the separator, and the average fiber diameter B [μm] of the separator satisfy the relationship of the following formula (1): 0.2<D / (A+B)<1.5…(1).

2. The alkaline storage battery according to claim 1, in, The average fiber diameter B [μm] of the separator is smaller than the cumulative 50% particle diameter D [μm] of the active material particles based on volume.

3. The alkaline storage battery according to claim 2, in, The cumulative 50% particle size D of the active material particles based on volume is 3 to 50 [μm].

4. The alkaline storage battery according to claim 2 or 3, in, The average fiber diameter B [μm] of the above-mentioned separator is 2 to 10 μm.

5. The alkaline storage battery according to any one of claims 1 to 4, in, The average pore diameter A [μm] of the above-mentioned separator is 10 to 25 μm.

6. The alkaline storage battery according to any one of claims 1 to 5, in, The active material layer contains carboxymethyl cellulose.

7. The alkaline storage battery according to any one of claims 1 to 6, in, The foil electrode is a bipolar electrode including a positive electrode active material layer as the active material layer disposed on one surface of the metal foil and a negative electrode active material layer as the active material layer disposed on the other surface of the metal foil.

8. A method for manufacturing an alkaline storage battery, the method for manufacturing an alkaline storage battery according to any one of claims 1 to 7, It is characterized in that have: a lamination step of alternately laminating the foil electrodes and the separators to produce an electrode assembly, and impregnating the foil electrodes and the separators with an electrolyte; and The compression step compresses the electrode assembly in a stacking direction thereof, thereby pressing a portion of the separator into the active material layer and causing the protrusion to engage with the receiving portion.