Epoxy resin, method for producing the same, curable epoxy resin composition, cured product, prepreg, insulating sheet and laminate
By introducing an oxazolidinone ring structure into epoxy resin and optimizing the use of isocyanate compounds, the problem of insufficient dielectric properties of existing epoxy resins is solved, and the reduction of dielectric constant and dielectric loss tangent and heat resistance are achieved. Improved, suitable for highly functional printed wiring boards.
Patent Information
- Application Number
- CN202010390616.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-21
- Filing Date
- 2020-05-11
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-05-11
AI Technical Summary
Existing epoxy resins have shortcomings in improving dielectric constant and dielectric loss tangent, and the solvent solubility becomes worse after the isocyanate modification rate is increased, making it difficult to meet the needs of highly functional printed wiring substrates.
By reacting an epoxy resin with a specific structure and an isocyanate compound, an epoxy resin containing an oxazolidinone ring is formed. The molecular weight is controlled within the range of 1,000 to 20,000 to ensure good solvent solubility, and the temperature is above 100°C and below 250°C. Carry out the reaction to optimize the usage amount and structure of the isocyanate compound.
It achieves the reduction of dielectric constant and dielectric loss tangent, maintains good heat resistance and adhesion, is suitable for lamination, molding, casting and other purposes, and meets the requirements of low dielectricity and high functionality.
Smart Images

Figure CN111978511B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an epoxy resin containing an oxazolidone ring which provides a cured product having excellent low dielectric properties without deteriorating heat resistance and adhesion, a method for producing the epoxy resin, an epoxy resin composition containing the epoxy resin as an essential component, and an epoxy resin cured product, a prepreg, an insulating sheet, an adhesive sheet, a laminate, a sealing material, and a casting material obtained from the epoxy resin composition. Background Art
[0002] Epoxy resins are used in many fields such as coatings, civil engineering adhesives, casting, electrical and electronic materials, and film materials because of their excellent adhesion, flexibility, heat resistance, chemical resistance, insulation, and curing reactivity.
[0003] As one of the uses of printed wiring substrates, portable devices or infrastructure devices such as base stations that maintain them have been in need of high functionality as the amount of information has increased dramatically in recent years. In portable devices, high-layer or fine wiring is being carried out for the purpose of miniaturization. In order to make the substrate thinner, a material with a lower dielectric constant is required. Due to the reduction of the bonding surface due to fine wiring, a material with higher adhesion is required. In the substrate facing the base station, in order to suppress the attenuation of the signal caused by high frequency, a material with a lower dielectric loss tangent is required.
[0004] Although the properties such as low dielectric constant and low dielectric loss tangent are derived from the structure of epoxy resin as the base resin of the printed wiring board, new epoxy resins or modification technologies thereof are required to a great extent.
[0005] Regarding the low dielectric constant of epoxy resin, patent document 1 discloses a diglycidyl ether of 4,4'-[1,3-phenylene bis(1-methylethylidene)]bis[2,6-dimethyl]phenol. In addition, patent document 2 discloses an epoxy resin obtained by reacting an epoxy resin having an alcoholic hydroxyl equivalent of less than 1.0meq. / g with an isocyanate compound having two or more isocyanate groups in the molecule, and discloses that the epoxy resin polymerized by an oxazolidinone ring has a low dielectric constant, a low dielectric loss tangent, and a high glass transition temperature. However, generally speaking, if the isocyanate modification rate is increased, the solvent solubility deteriorates and cannot be used for printed wiring board purposes, so its modification rate has a limit. As a resin with better solvent solubility than existing isocyanate-modified epoxy resins, Patent Document 3 discloses an epoxy resin obtained by reacting an epoxy resin having a specific structure with an isocyanate compound having two or more isocyanate groups in the molecule, but it does not fully meet the recent demand for highly functional dielectric properties.
[0006] [Prior art literature]
[0007] [Patent Document]
[0008] [Patent Document 1] Japanese Patent Application Laid-Open No. 5-293929
[0009] [Patent Document 2] Japanese Patent Application Laid-Open No. 9-278867
[0010] [Patent Document 3] Japanese Patent Application Publication No. 2016-169362 Summary of the invention
[0011] [Problems to be solved by the invention]
[0012] Therefore, the problem to be solved by the present invention is to provide an epoxy resin having low dielectric properties, excellent heat resistance and adhesion and useful in lamination, molding, casting, bonding and the like, an epoxy resin composition containing the epoxy resin as an essential component and its cured product.
[0013] [Technical means to solve the problem]
[0014] In order to solve the above-mentioned problems, the inventors have made great efforts to study materials with low dielectric constant and low dielectric loss tangent. As a result, they found that the epoxy resin containing oxazolidone ring obtained by reacting an epoxy resin with a specific structure with an isocyanate compound has good solvent solubility when the raw epoxy resin is highly modified by the isocyanate compound, and exhibits a low dielectric constant and low dielectric loss tangent that have not been seen before, thereby completing the present invention.
[0015] That is, the present invention is an oxazolidone ring-containing epoxy resin having at least one divalent group represented by the following formula (a) and at least one oxazolidone ring structure in one molecule, and having a weight average molecular weight (Mw) of 1,000 to 20,000 as measured by gel permeation chromatography (GPC).
[0016] [Chemistry 1]
[0017]
[0018] In formula (a), X represents -CH2-, -CH(CH3)-, -C(CH3)2-, -C2H4-, -C(CF3)2-, -S-, -SS-, -SO2-, -O-, -CO-, -CO-O-, -CH2-O-CH2-, phenylene, phenylenebis(methylene) group, phenylmethylene, diphenylmethylene, 9H-fluorene-9-indenyl or any one of the diradicals of a polycyclic aliphatic ring. R 1 Each independently represents a hydrocarbon group having 1 to 11 carbon atoms or a hydrocarbonoxy group having 1 to 11 carbon atoms, and R 2Each independently represents a hydrogen atom, a hydrocarbon group having 1 to 11 carbon atoms, or a hydrocarbonoxy group having 1 to 11 carbon atoms. When X has a benzene ring, the benzene ring may have a 1 Same substituents.
[0019] The oxazolidinone ring-containing epoxy resin may have a structure represented by the following formula (1) or formula (2).
[0020] [Chemistry 2]
[0021]
[0022] [Chemistry 3]
[0023]
[0024] In formula (1) and formula (2), W represents a divalent group represented by formula (a). Z represents a divalent group, and 5 mol% to 100 mol% of Z is a divalent group represented by formula (a). Y represents a residue obtained by removing an isocyanate group from a diisocyanate compound. G represents a glycidyl group. n represents the number of repetitions, and the average value is 1 to 5.
[0025] The present invention is also a method for producing an oxazolidone ring-containing epoxy resin, comprising reacting an epoxy resin (a) containing 50% by mass or more of an epoxy resin (a1) represented by the following formula (3) with an isocyanate compound (b) in the presence of a catalyst at a reaction temperature in the range of 100° C. to 250° C.
[0026] [Chemistry 4]
[0027]
[0028] In formula (3), W represents a divalent group represented by the following formula (a), and G represents a glycidyl group. m represents the number of repetitions, and the average value is 0 to 5.
[0029] [Chemistry 5]
[0030]
[0031] In formula (a), X represents -CH2-, -CH(CH3)-, -C(CH3)2-, -C2H4-, -C(CF3)2-, -S-, -SS-, -SO2-, -O-, -CO-, -CO-O-, -CH2-O-CH2-, phenylene, phenylenebis(methylene) group, phenylmethylene, diphenylmethylene, 9H-fluorene-9-indenyl or any one of the diradicals of a polycyclic aliphatic ring. R 1 Each independently represents a hydrocarbon group having 1 to 11 carbon atoms or a hydrocarbonoxy group having 1 to 11 carbon atoms, and R 2Each independently represents a hydrogen atom, a hydrocarbon group having 1 to 11 carbon atoms, or a hydrocarbonoxy group having 1 to 11 carbon atoms. When X is a group having a benzene ring, the benzene ring may have a 1 Same substituents.
[0032] It is preferred that the amount of the isocyanate group in the isocyanate compound (b) is in the range of 0.02 mol or more and less than 0.7 mol per 1 mol of the epoxy group in the epoxy resin (a).
[0033] The epoxy equivalent of the epoxy resin (a) is preferably 180 g / eq. to 400 g / eq.
[0034] In addition, the present invention is an oxazolidone ring-containing epoxy resin (A2), which comprises 5% to 55% by mass of the oxazolidone ring-containing epoxy resin; and an epoxy resin having a divalent group represented by the formula (a) and not containing an oxazolidone ring.
[0035] Furthermore, the present invention is an oxazolidone ring-containing epoxy resin (A2), which is obtained from an epoxy resin (a) containing 50% by mass or more of the epoxy resin (a1) represented by the formula (3) and an isocyanate compound (b), and has an epoxy equivalent of 200 g / eq. to 1600 g / eq.
[0036] In addition, the present invention provides an epoxy resin composition comprising the epoxy resin containing an oxazolidone ring and a hardener.
[0037] Preferably, the active hydrogen group of the curing agent is 0.2 mol to 1.5 mol per 1 mol of epoxy groups of all epoxy resins in the epoxy resin composition.
[0038] Furthermore, the present invention is a prepreg, an insulating sheet or a laminated board using the epoxy resin composition. In addition, the present invention is a laminated board using the prepreg or the insulating sheet. Furthermore, the present invention is a cured product obtained by curing the epoxy resin composition.
[0039] [Effects of the Invention]
[0040] The epoxy resin containing an oxazolidone ring of the present invention and the resin composition containing the same have good heat resistance and adhesion and exhibit low dielectric constant and dielectric loss tangent. Therefore, they have good properties in laminates and electronic circuit boards requiring low dielectric properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 This is the GPC chart of the epoxy resin containing an oxazolidinone ring of Example 1.
[0042] Figure 2This is an infrared radiation (IR) chart of the epoxy resin containing an oxazolidinone ring in Example 1. DETAILED DESCRIPTION
[0043] Hereinafter, embodiments of the present invention will be described in detail.
[0044] The oxazolidinone ring-containing epoxy resin of the present invention has at least one divalent group represented by the formula (a) and at least one oxazolidinone ring structure in one molecule, and Mw is 1000 to 20000. Here, Mw is determined by GPC measurement, and the GPC measurement conditions are determined according to the conditions described in the Examples.
[0045] In formula (a), the substituent R 1 are essential, and each independently represents a hydrocarbon group having 1 to 11 carbon atoms or a hydrocarbonoxy group having 1 to 11 carbon atoms. 2 Each independently represents a hydrogen atom, a hydrocarbon group having 1 to 11 carbon atoms, or a hydrocarbonoxy group having 1 to 11 carbon atoms.
[0046] Examples of the hydrocarbon group having 1 to 11 carbon atoms include an alkyl group having 1 to 8 carbon atoms, an aryl group having 6 to 10 carbon atoms, and an aralkyl group having 7 to 11 carbon atoms. Examples of the hydrocarbonoxy group having 1 to 11 carbon atoms include an alkoxy group having 1 to 8 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, and an aralkyloxy group having 7 to 11 carbon atoms. Preferably, it is an alkyl group having 1 to 8 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an aryloxy group having 6 to 10 carbon atoms, and more preferably, it is an alkyl group having 1 to 8 carbon atoms or an aryl group having 6 to 10 carbon atoms.
[0047] The alkyl or alkoxy group having 1 to 8 carbon atoms may be linear, branched or cyclic, and examples thereof include methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, methylbutyl, dimethylbutyl, methylhexyl, dimethylpentyl, ethylpentyl, trimethylbutyl, isooctyl, ethylhexyl, cyclohexyl, cycloheptyl, cyclooctyl, methylcyclohexyl, dimethylcyclohexyl, ethylcyclohexyl, methylcycloheptyl, methoxy, ethoxy, n-propoxy , n-butoxy, n-pentyloxy, n-hexyloxy, n-heptyloxy, n-octyloxy, isopropoxy, isobutoxy, sec-butoxy, tert-butoxy, isopentyloxy, neopentyloxy, tert-pentyloxy, methylbutoxy, dimethylbutoxy, methylhexyloxy, dimethylpentyloxy, ethylpentyloxy, trimethylbutoxy, isooctyloxy, ethylhexyloxy, isohexyloxy, cyclopentyloxy, cyclohexyloxy, cycloheptyloxy, cyclooctyloxy, methylcyclohexyloxy, dimethylcyclohexyloxy, ethylcyclohexyloxy, methylcycloheptyloxy and the like.
[0048] Examples of the aryl group or aryloxy group having 6 to 10 carbon atoms include phenyl, tolyl, ethylphenyl, xylyl, propylphenyl, trimethylphenyl, naphthyl, indanyl, phenoxy, tolyloxy, ethylphenoxy, xylyloxy, propylphenoxy, trimethylphenoxy, and naphthyloxy.
[0049] Examples of the aralkyl group or aralkyloxy group having 7 to 11 carbon atoms include benzyl, methylbenzyl, dimethylbenzyl, trimethylbenzyl, phenethyl, 1-phenylethyl, 2-phenylisopropyl, naphthylmethyl, benzyloxy, methylbenzyloxy, dimethylbenzyloxy, trimethylbenzyloxy, phenethyloxy, 1-phenylethyloxy, 2-phenylisopropyloxy, and naphthylmethyloxy.
[0050] R 1 The substitution position of may be any of the ortho, meta, and para positions relative to the carbon atom bonded to X, and is preferably the ortho or meta position.
[0051] In formula (a), R 2 are independently a hydrogen atom or 1 The same substituents as R 2 Different, R 1 There is no hydrogen atom, so the two benzene rings of formula (a) need to be substituted by at least two substituents R 1 replace.
[0052] In formula (a), X represents -CH2-, -CH(CH3)-, -C(CH3)2-, -C2H4-, -C(CF3)2-, -S-, -SS-, -SO2-, -O-, -CO-, -CO-O-, -CH2-O-CH2-, phenylene, phenylenebis(methylene) group, phenylmethylene, diphenylmethylene, 9H-fluorene-9-indenyl or any one of the diradicals of a polycyclic aliphatic ring. Furthermore, when X has a benzene ring, the benzene ring may have a ring with R 1 Same substituents.
[0053] The diyl group of the polycyclic aliphatic ring may be any diyl group having a structure of two or more aliphatic rings. Examples thereof include bicyclo[4.4.0]decyldiyl, bicyclohexyldiyl, spirobicyclohexanediyl, adamantanediyl, adamantanebis(methylene)diyl, bicyclo[2.2.1]heptanediyl, tricyclo[5.2.1.0 2,6 ]decanediyl (tetrahydrodicyclopentadienediyl), 4,9:5,8-dimethylbridgedodecahydro-1H-cyclopenta[b]naphthalenediyl (tetrahydrotricyclopentadienediyl), decahydro-1,4:5,8-dimethylbridgedai naphthalenenediyl, etc.
[0054] In formula (a), each benzene ring needs to have two or more substituents, and the more substituents there are, the better the solvent solubility. In addition, the total number of carbon atoms in the substituents has an effect on the dielectric properties, and the more substituents there are, the more effective it is in reducing the dielectric properties. Therefore, it is preferred that the number of substituents is two or more and the number of carbon atoms in each substituent is 3 or more. Preferred R 1 is methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, cyclohexyl, phenyl, benzyl, 1-phenylethyl, preferably R 2 It is a hydrogen atom, a methyl group, a cyclohexyl group, a phenyl group, or a 1-phenylethyl group.
[0055] As X, from the viewpoint of solvent solubility and heat resistance, preferably -S-, -SS-, -SO2-, -O-, -CO-, -CO-O-, -CH2-O-CH2-, -C(CF3)2-, tetrahydrodicyclopentadiene diyl, tetrahydrotricyclopentadiene diyl, more preferably -S-, -SS-, -SO2-, -O-, -CO-, -CO-O-, -CH2-O-CH2-, -C(CF3)2-, tetrahydrodicyclopentadiene diyl, further preferably -O-, -S-, -SO2-, tetrahydrodicyclopentadiene diyl. The mobility of these structures is controlled, so the heat resistance is improved, and the polarized structure is adopted, so it is believed that the solvent solubility becomes good.
[0056] In formula (a), the bonding position of X to two benzene rings may be any of 2,2', 2,3', 2,4', 3,3', 3,4', and 4,4', and is preferably 4,4'.
[0057] Formula (a) is preferably a structure represented by the following formula (1a) to formula (1i).
[0058] [Chemistry 6]
[0059]
[0060] A preferred structure having a divalent group represented by the formula (a) and an oxazolidinone ring structure in one molecule is the structure represented by the formula (1), and a more preferred structure is the structure represented by the formula (2).
[0061] In formula (1), W is a divalent group represented by formula (a). Y is a residue obtained by removing two isocyanate groups from a polyisocyanate compound, and represents a divalent or higher functional group that may have a substituent, preferably a structure represented by the following formula (2a) to formula (2k). When Y is a group generated from a trifunctional or higher polyisocyanate compound, as a substituent, it may have a group containing an oxazolidinone ring, a group containing a carbamate bond, etc.
[0062] [Chemistry 7]
[0063]
[0064] The oxazolidinone ring epoxy resin of the present invention may be an oxazolidinone ring-containing epoxy resin represented by the above formula (1), formula (2), etc.
[0065] The oxazolidone ring-containing epoxy resin of the present invention can be advantageously obtained by the manufacturing method of the oxazolidone ring-containing epoxy resin of the present invention described later, but is usually obtained in the form of an oxazolidone ring-containing epoxy resin containing a byproduct. Here, the byproduct can be interpreted as the meaning of containing unreacted products. The oxazolidone ring epoxy resin of the present invention includes an oxazolidone ring-containing epoxy resin containing the byproduct.
[0066] When it is necessary to distinguish between the oxazolidone ring-containing epoxy resin A1 which is a single oxazolidone ring-containing epoxy resin and the oxazolidone ring-containing epoxy resin A2 which contains a byproduct, A1 and A2 are indicated as described above.
[0067] A suitable oxazolidone ring-containing epoxy resin A2 of the present invention is an oxazolidone ring-containing epoxy resin comprising 5 to 55% by mass of the oxazolidone ring-containing epoxy resin A1 and an epoxy resin B, wherein the epoxy resin B has a divalent group of the formula (a) and does not contain an oxazolidone ring.
[0068] Here, the epoxy resin B corresponds to the byproduct. When an oxazolidone ring-containing epoxy resin is obtained from an epoxy resin and a polyisocyanate, the byproduct includes unreacted epoxy resin, epoxy resin having a urethane structure, and the like.
[0069] The oxazolidone ring-containing epoxy resin of the present invention can be obtained from an epoxy resin (a) containing 50% by mass or more of the epoxy resin (a1) represented by the formula (3) and an isocyanate compound (b), and has an epoxy equivalent (g / eq.) of 200 to 1600.
[0070] The oxazolidinone ring-containing epoxy resin is generally an oxazolidinone ring-containing epoxy resin A2 containing a byproduct. The oxazolidinone ring-containing epoxy resin A1 may be isolated therefrom, but in many applications, this is not necessary and the oxazolidinone ring-containing epoxy resin A1 may be used without isolation.
[0071] In the case of separating or concentrating the epoxy resin A1 containing an oxazolidone ring from the epoxy resin A2 containing an oxazolidone ring, an existing separation method can be used. For example, the epoxy resin A2 is heated under high vacuum, thereby evaporating and separating the unreacted epoxy resin, and a method for obtaining a separated or concentrated epoxy resin containing an oxazolidone ring in the form of a residual component, or a method for obtaining a separated or concentrated epoxy resin containing an oxazolidone ring by chromatography, etc. However, any method is difficult to industrialize and is not practical, so it is preferably used in the state of the epoxy resin A2 containing an oxazolidone ring.
[0072] The content of the structure represented by formula (1) in the epoxy resin A2 containing oxazolidone ring of the present invention is preferably 5 mass %~65 mass %, more preferably 10 mass %~65 mass %, and further preferably 15 mass %~60 mass %. If the content is few, there is a worry that the effect of reducing dielectric constant and dielectric loss tangent is not shown. In addition, if the content is many, adverse effects such as solvent solubility deterioration or resin viscosity increase are produced, or at the temperature of reflow soldering, elastic coefficient is reduced, and there is a worry in use. Furthermore, the reason why the content is not close to 100 mass % is: as mentioned above, comprising byproducts such as raw epoxy resin (a) without oxazolidone ring structure.
[0073] In formula (2), Z represents a divalent group which may have a substituent, and 5 mol% to 100 mol% of all Z are divalent groups represented by formula (a). Y has the same meaning as Y in formula (1). G represents a glycidyl group. n represents the number of repetitions, and its average value is 1 to 5, which can be calculated based on the epoxy equivalent of the epoxy resin containing an oxazolidinone ring and the structures of Z and Y.
[0074] When used in the form of an oxazolidinone ring-containing epoxy resin A1, the effect of the present invention is exhibited if the formula (a) is present in Z in an amount of 5 mol% or more. However, when used in the form of an oxazolidinone ring-containing epoxy resin A2, the formula (a) is preferably present in Z in an amount of 50 mol% or more, more preferably 70 mol% or more.
[0075] Hereinafter, a method for producing the oxazolidone ring-containing epoxy resin of the present invention will be described, together with a description of the oxazolidone ring-containing epoxy resin of the present invention.
[0076] In the method for producing an oxazolidone ring-containing epoxy resin of the present invention, an epoxy resin (a) containing 50% by mass or more of the epoxy resin (a1) represented by the formula (3) is reacted with an isocyanate compound (b) in the presence of a catalyst at a reaction temperature in the range of 100° C. to 250° C.
[0077] In the formula (3), W has the same meaning as W in the formula (1), G represents a glycidyl group, and m represents the number of repetitions, the average value of which is 0 to 5.
[0078] In the production method, an oxazolidone ring-containing epoxy resin A2 can be advantageously produced. The oxazolidone ring-containing epoxy resin obtained by the production method includes an oxazolidone ring-containing epoxy resin having a structure represented by the formula (1) as a target product, and a raw material epoxy resin represented by the formula (3) as a byproduct or an epoxy resin having a urethane bond formed by an OH group of the raw material epoxy resin represented by the formula (3) and a polyisocyanate compound.
[0079] The content of the structure represented by formula (1) can be obtained by quantitative NMR, etc. When quantitative nuclear magnetic resonance (NMR) is used for measurement, the raw materials (epoxy resin, isocyanate compound) used are first inferred based on structure factor analysis, and a standard substance for calibration curve is synthesized from the inferred raw materials. The raw material epoxy resin in the above case is preferably 0 in formula (3). The method of making m 0 can be a method known in the art. For example, there is a method as follows: after reacting with 10 to 20 times the molar amount of epichlorohydrin relative to the raw material phenol compound, the obtained epoxy resin is subjected to reduced pressure distillation to separate only the m=0 component as a distillate component. The epoxy resin of the m=0 component obtained in the above manner is reacted with an isocyanate compound, and only the n=1 component of formula (2) is separated from the obtained epoxy resin containing an oxazolidinone ring as a standard substance for calibration curve. In the calibration curve, even a small amount is acceptable, so it is efficient to use GPC fractionation. Quantification can be performed by preparing a calibration curve using the standard substances obtained in the above manner.
[0080] The epoxy resin containing an oxazolidinone ring preferably has a wavelength of 1745 cm-1 derived from the stretching vibration of the carbonyl group of the oxazolidinone ring in an analysis using infrared absorption spectroscopy. -1 ~1760cm -1 The maximum value of the peak contained in is taken as absorbance Ox, and the peak value of the stretching vibration of the carbonyl group derived from the carbamate bond structure at 1730 cm -1 ~1740cm -1 When the maximum value of the peak value contained in is set as absorbance Ur, the absorbance ratio Ox / Ur is greater than 1.35. If the absorbance ratio Ox / Ur is greater than 1.35, the urethane bond can be basically ignored, so if the types or charging amounts of the raw material epoxy resin and isocyanate compound are known, the generation amount of the oxazolidinone ring structure can also be calculated.
[0081] The weight average molecular weight Mw of the epoxy resin A1 containing oxazolidinone rings of the present invention measured by GPC is in the range of 1000 to 20000, preferably in the range of 1200 to 18000 or less, more preferably 1300 to 16000, and further preferably 1400 to 14000. If Mw is low, there is concern about deterioration of adhesion. In addition, there is concern that the content of oxazolidinone rings decreases and the dielectric constant increases. In addition, if Mw is high, the content of oxazolidinone rings is more than the required amount, resulting in adverse effects such as deterioration of solvent solubility or increase in resin viscosity, or at the temperature of reflow soldering, the elastic modulus decreases, and there is concern about use.
[0082] The epoxy equivalent (g / eq.) of the epoxy resin A1 containing oxazolidone ring is preferably 500~2500, more preferably 600~2000, and further preferably 650~1500. If the epoxy equivalent is low, there is a worry that the molecular length shortens and the adhesion deteriorates. In addition, because the hydroxyl concentration in the hardener increases, there is a worry that the dielectric constant and the dielectric loss tangent increase. If the epoxy equivalent is high, the molecular length grows to more than the required length, resulting in adverse effects such as solvent solubility deterioration or resin viscosity increase, or at the temperature of reflow soldering, the elastic coefficient decreases, and there is a worry in use.
[0083] The softening point of the epoxy resin A1 containing an oxazolidone ring varies according to the structure of X or Y of formula (1), or the epoxy equivalent. When the epoxy resin A1 containing an oxazolidone ring is used alone in a prepreg or a film material, it is preferably 90°C to 150°C, more preferably 90°C to 160°C, and further preferably 90°C to 140°C. In the case described, there is no concern that the softening point is too low, so the lower limit does not need to be particularly noted. If the softening point is high, the resin viscosity becomes high, the impregnation in the prepreg deteriorates, or the solvent solubility deteriorates, or the dilution solvent does not volatilize during heating and drying and remains in the resin, so there is concern that voids are generated when making a laminate, etc., which becomes a problem in use.
[0084] In the production method of the present invention, the isocyanate group of the isocyanate compound (b) reacts with the epoxy group of the epoxy resin (a) to form an oxazolidone ring, and reacts with the alcoholic hydroxyl group contained in the epoxy resin (a) to form a urethane bond.
[0085] If the concentration of the urethane bond contained in the epoxy resin containing an oxazolidone ring increases, there is a concern that the heat resistance of the epoxy resin cured product obtained by curing the epoxy resin composition will be reduced. The absorbance ratio Ox / Ur is preferably 1.35 or more, and more preferably 2.0 or more. When the absorbance ratio Ox / Ur is less than 1.35, there is a concern that the heat resistance of the cured product of the epoxy resin composition containing it will be reduced.
[0086] The epoxy equivalent of the epoxy resin A2 containing oxazolidone ring of the present invention is preferably 200-1600, more preferably 250-1400, and further preferably 275-1300, and particularly preferably 275-1200. If the epoxy equivalent is low, the content of the oxazolidone ring decreases, and the hydroxyl concentration in the hardened material increases, so there is a concern that the dielectric constant and the dielectric loss tangent increase. In addition, if the epoxy equivalent is high, the content of the oxazolidone ring is more than the required amount, the solvent solubility deteriorates or the resin viscosity increases, or at the temperature of the reflow soldering, the elastic coefficient decreases, and there is a concern in use.
[0087] In addition, the softening point of the epoxy resin A2 containing an oxazolidone ring is preferably 50°C to 150°C, more preferably 65°C to 135°C, and further preferably 70 to 110°C when used in a prepreg or a film material. If the softening point is low, when the resin varnish is impregnated into the glass cloth and then heated and dried in an oven, there is a concern that the amount of resin attached will decrease due to the low viscosity. If the softening point is high, the resin viscosity becomes high, the impregnation property in the prepreg is deteriorated, the solvent solubility is deteriorated, or the dilution solvent does not volatilize during heating and drying and remains in the resin, so there is a concern that voids will be generated when a laminate is made, which will become a problem in use.
[0088] In the epoxy resin containing an oxazolidinone ring, in addition to the structure of formula (a), it may also contain a skeleton derived from biphenol, bisphenol Z, 4,4'-(3,3,5-trimethylcyclohexylene)diphenol or phenol novolac, and may also have a structure similar to R on its aromatic ring. 1 The same substituents are used as substituents. 2 All are hydrogen atoms, and R 1 A structure in which one or more of the atoms is a hydrogen atom.
[0089] The epoxy resin (a) used in the manufacturing method of the epoxy resin containing the oxazolidone ring of the present invention contains the epoxy resin (a1) represented by the formula (3) of more than 50 mass %. The content is more preferably more than 65 mass %, and further preferably more than 80 mass %, and particularly preferably more than 90 mass %. The most effective formulation for showing the effect of the present invention is to use epoxy resin (a1) (100 mass %) alone.
[0090] In formula (3), m is a repetition number, and its average value (number average) is 0 to 5, preferably in the range of 0 to 3, more preferably in the range of 0 to 1, and further preferably in the range of 0 to 0.5. Moreover, the repetition number (integer) is sometimes 6 or more, but is generally preferably in the range of integers of 0 to 5. It can be a single compound with a repetition number of any integer from 0 to 5, or it can be a mixture of multiple integers in which m is 0 to 5. In the epoxidation of a conventional polyhydroxy resin using epihalohydrin or the like, since it is obtained in the form of a mixture, if it is a mixture, it has the advantage of being able to be used directly.
[0091] The epoxy equivalent of the epoxy resin (a) is preferably 180 to 400, more preferably 200 to 350. Similarly, the epoxy equivalent of the epoxy resin (a1) is also preferably 180 to 400, more preferably 200 to 350. In addition, when multiple epoxy resins are used in combination, the epoxy equivalent can be obtained by measuring after mixing. In addition, when the epoxy equivalents of each are known, they can also be obtained by calculation.
[0092] The alcoholic hydroxyl contained in the epoxy resin (a) reacts with isocyanate to form a carbamate bond, thereby reducing the heat resistance of the epoxy resin cured product formed by curing the epoxy resin composition. Therefore, the alcoholic hydroxyl equivalent of the epoxy resin (a) is preferably more than 1000, more preferably more than 3000, and further preferably more than 5000. In the case of using a variety of epoxy resins, it can be obtained by measuring after mixing. In addition, when the respective alcoholic hydroxyl equivalents are known, it can be obtained by calculation.
[0093] In addition, the alcoholic hydroxyl group of epoxy resin (a) is an alcoholic hydroxyl group generated by the reaction of phenolic compound and epihalohydrin. In the case where epihalohydrin is epichlorohydrin, these alcoholic hydroxyl groups are alcoholic hydroxyl groups (α) of 2-chloro-3-hydroxypropyl generated by the addition of phenolic compound to the α position of epichlorohydrin, alcoholic hydroxyl groups (β) of 1-chloromethyl-2-hydroxyethyl generated by the addition of phenolic compound to the β position of epichlorohydrin, secondary alcoholic hydroxyl groups (γ) generated by the addition of phenolic compound to epoxy resin, and α-diols (δ) generated by the hydrolysis of epoxy groups of epoxy resin. The alcoholic hydroxyl group in the present invention refers to all of (α), (β), (γ) and (δ), so the measurement object of the alcoholic hydroxyl group equivalent is all of (α), (β), (γ) and (δ).
[0094] In the reduction of secondary alcoholic hydroxyl group (γ), the repetition number (integer) in formula (3) is preferably small. Therefore, the repetition number is preferably 0 to 3, more preferably 0 to 2, and further preferably 0 to 1. In the case of compounds comprising more than 6, the alcoholic hydroxyl group in epoxy resin (a) becomes more, and it reacts with isocyanate to generate carbamate bonds, so that the glass transition point of the cured product is reduced, so it is not preferred. In addition, the hydroxyl concentration in the cured product increases, so the dielectric constant and dielectric loss tangent of the cured product can be increased, so it is also not preferred. When m is 0, the alcoholic hydroxyl group disappears, and the alcoholic hydroxyl group equivalent becomes infinite in theory, so there is no need to particularly specify its upper limit value.
[0095] The epoxy resin (a1) can be obtained by a known method such as a method of reacting a phenol compound represented by the following formula (4) with an epihalohydrin in the presence of a base such as sodium hydroxide, or a method of allyl-etherifying the phenol compound represented by the formula (4) with an allyl etherified product and then oxidizing the allyl group with an oxidizing agent such as a peroxide to perform epoxidation.
[0096] [Chemistry 8]
[0097]
[0098] In formula (4), R 1 , R 2 and X are respectively 1 , R 2 and X have the same meaning.
[0099] As the epoxy resin (a1) represented by formula (3), the epoxy resin obtained by the phenolic compounds represented by the above formula (4) and epihalohydrin can be listed. For example, 2-(1,1-dimethylethyl)-4[[2-(1,1-dimethylethyl)-4-hydroxy-6-methylphenyl]thio]-5-methylphenol, 2,2',6,6'-tetramethyl-4,4'-sulfonyldiphenol, 4,4'-dihydroxy-3,3',5,5'-tetramethyldiphenylmethane, 2,2-bis(3,5-di-tert-butyl-4-hydroxyphenol)propane, 4,4'-dihydroxy-3,3',5,5'-tetramethyldiphenyl ether, 4,4'-dihydroxy-3,3',5,5'-tetramethylbenzophenone, etc. can be listed, but it is not limited to these, and can be used alone or in combination of two or more.
[0100] As the epoxy resin (a) used in the manufacturing method of the present invention, as long as the effect of the present invention is not impaired, an epoxy resin (a2) other than the epoxy resin (a1) less than 50% by mass can be used in combination. It can be understood that the epoxy resin (a2) does not have the structure represented by formula (3). The most effective formulation for showing the effect of the present invention is to use epoxy resin (a1) (100% by mass) alone. In addition, if the amount of epoxy resin (a1) used is less than 50% by mass, there is a concern that the effect of the present invention cannot be shown. The purpose of using the epoxy resin (a2) that can be used in combination is, for example, to impart other characteristics such as further improving solvent solubility. Therefore, it is preferred that the amount of epoxy resin (a2) used is as little as possible. The amount of epoxy resin (a2) that can be used in combination is preferably less than 35% by mass, more preferably less than 20% by mass, and further preferably less than 10% by mass.
[0101] The alcoholic hydroxyl group contained in the epoxy resin (a2) also reacts with isocyanate to form a urethane bond, so there is a concern that the heat resistance of the cured product will be reduced. Therefore, as the epoxy resin (a), it is necessary to use an epoxy resin (a2) having an alcoholic hydroxyl group equivalent within the preferred alcoholic hydroxyl group equivalent range.
[0102] The epoxy equivalent of the epoxy resin (a2) is not particularly limited, but is preferably 100 to 300, more preferably 170 to 300.
[0103] As the epoxy resin (a2) that can be used, an unsubstituted type or a monosubstituted type bisphenol type can be used. For example, bisphenol A type epoxy resins [such as Epotohto YD-127, Epotohto YD-128, Epotohto YD-8125, Epotohto YD-825GS (the above are Nippon Steel Chemical Materials (NIPPONSTEEL) Chemical & Material Co., Ltd.), etc.], bisphenol F type epoxy resins [for example, Epotohto YDF-170, Epotohto YDF-1500, Epotohto YDF-8170, Epotohto YDF-870GS (all manufactured by Nippon Steel Chemical Materials Co., Ltd.)], diphenyl sulfide type epoxy resins [for example, YSLV-50TE (manufactured by Nippon Steel Chemical Materials Co., Ltd.)], diphenyl ether type epoxy resins [for example, YSLV-80DE (manufactured by Nippon Steel Chemical Materials Co., Ltd.)], bisphenol S type epoxy resins [for example, TX-0710 (manufactured by Nippon Steel Chemical Materials Co., Ltd.), Epiclon EXA-1515 (manufactured by Dainippon Chemical Industries, Ltd.)], bisphenol fluorene type epoxy resins [for example, ZX-1201 (manufactured by Nippon Steel Chemical Materials Co., Ltd.)], dimethyl bisphenol F type epoxy resins, etc. In addition, biphenol type epoxy resins [e.g., YX-4000 (manufactured by Mitsubishi Chemical Co., Ltd.), ZX-1251 (manufactured by Nippon Steel Chemical Materials Co., Ltd.), etc.], hydroquinone type epoxy resins [e.g., Epotohto YDC-1312, ZX-1027 (manufactured by Nippon Steel Chemical Materials Co., Ltd.), etc.], resorcinol type epoxy resins [e.g., Epotohto ZX-1684 (manufactured by Nippon Steel Chemical Materials Co., Ltd.), DENACOL EX-201 (manufactured by Nagase Chemicals Co., Ltd.), etc.], chemteX Co., Ltd.), etc.], naphthalene diol type epoxy resins [e.g. ZX-1355 (manufactured by Nippon Steel Chemical Materials Co., Ltd.), Epiclon HP-4032D (manufactured by DIC Corporation)], phenol novolac type epoxy resins [e.g. Epotohto YDPN-638 (manufactured by Nippon Steel Chemical Materials Co., Ltd.), jER152, jER154 (manufactured by Mitsubishi Chemical Co., Ltd.), Epiclon N-740, Epiclon N-770, Epiclon N-775 (manufactured by DIC Corporation)], etc.],Cresol novolac type epoxy resins [e.g., Epotohto YDCN-700 series (manufactured by Nippon Steel Chemical Materials Co., Ltd.), Epiclon N-660, Epiclon N-665, Epiclon N-670, Epiclon N-673, Epiclon N-695 (manufactured by DIC Corporation), EOCN-1020, EOCN-102S, EOCN-104S (manufactured by Nippon Kayaku Co., Ltd.), etc.], alkyl novolac type epoxy resins [e.g., Epotohto ZX- 1071T, Epotohto ZX-1270, Epotohto ZX-1342 (manufactured by Nippon Steel Chemicals Co., Ltd.), etc.], aromatic modified phenol novolac type epoxy resins [e.g., Epotohto ZX-1247, GK-5855, Epotohto TX-1210, Epotohto YDAN-1000 (manufactured by Nippon Steel Chemicals Co., Ltd.), etc.], bisphenol novolac type epoxy resins, naphthol novolac type epoxy resins [e.g., Epotohto ZX-1142L (manufactured by Nippon Steel Chemicals Co., Ltd.), etc.], β - naphthol aralkyl type epoxy resins [e.g. ESN-155, ESN-185V, ESN-175 (manufactured by Nippon Steel Chemicals Co., Ltd.)], naphthalene diol aralkyl type epoxy resins [e.g. ESN-300 series ESN-355, ESN-375 (manufactured by Nippon Steel Chemicals Co., Ltd.)], α-naphthol aralkyl type epoxy resins [e.g. ESN-400 series ESN-475V, ESN-485 (manufactured by Nippon Steel Chemicals Co., Ltd.)], biphenyl aralkylphenol type epoxy resins [e.g. NC-3000, NC-3000H (manufactured by Nippon Kayaku Co., Ltd.)], trihydroxyphenylmethane type epoxy resins [ For example, EPPN-501, EPPN-502 (both manufactured by Nippon Kayaku Co., Ltd.) etc.], tetrahydroxyphenylethane type epoxy resins [for example, YDG-414 (manufactured by Nippon Steel Chemicals Co., Ltd.) etc.], dicyclopentadiene type epoxy resins [for example, Epiclon HP7200, Epiclon HP-7200H (manufactured by DIC Corporation) etc.], alkanediol type epoxy resins [Epotohto PG-207, Epotohto PG-207GS (manufactured by Nippon Steel Chemicals Co., Ltd.), SR-16H, SR-16HL, SR-PG,SR-4PG, SR-SBA, SR-EGM, SR-8EGS (all manufactured by Sakamoto Pharmaceutical Co., Ltd.), etc.], aliphatic cyclic epoxy resins [SunTohto ST-3000, Epotohto ZX-1658, Epotohto ZX-1658GS, FX-318 (all manufactured by Nippon Steel Chemical Materials Co., Ltd.), HBPA-DGE (manufactured by Maruzen Petrochemical Co., Ltd.), etc.], etc.], polyglycidyl ether compounds or diamino Diphenylmethane type epoxy resins [e.g., Epotohto YH-434, Epotohto YH-434GS (both manufactured by Nippon Steel Chemical Materials Co., Ltd.), ELM434 (manufactured by Sumitomo Chemical Co., Ltd.), Araldite MY720, Araldite MY721, Araldite MY9512, Araldite MY9663 (manufactured by Huntsman Advanced Chemicals Co., Ltd.) Advanced Chemicals) etc.], m-xylene diamine type epoxy resins [e.g., TETRADX (manufactured by Mitsubishi Gas Chemical Co., Ltd.) etc.], 1,3-bisaminomethylcyclohexane type epoxy resins [e.g., TETRAD-C (manufactured by Mitsubishi Gas Chemical Co., Ltd.) etc.], isocyanurate type epoxy resins [e.g., TEPIC-P (manufactured by Nissan Chemical Industries, Ltd.) etc.], aniline type epoxy resins [e.g., GAN, GOT (manufactured by Nippon Kayaku Co., Ltd.) etc.], hydantoin type epoxy resins [e.g., Y238 (manufactured by Huntsman Advanced Chemicals Co., Ltd.) etc.], aminophenol type epoxy resins [e.g., ELM120, ELM100 (manufactured by Sumitomo Chemical Co., Ltd.) and jER630 (manufactured by Mitsubishi Chemical Co., Ltd.), Araldite MY0510, Araldite MY0600, Araldite MY0610 (all manufactured by Huntsman Advanced Chemicals Co., Ltd.), etc.] or polyglycidylamine compounds or dimer acid type epoxy resins [e.g. Epotohto YD-171 (manufactured by Nippon Steel Chemical Materials Co., Ltd.), jER871 (manufactured by Mitsubishi Chemical Co., Ltd.), etc.], hexahydrophthalic acid type epoxy resins [e.g. SR-HHPA (manufactured by Sakamoto Pharmaceutical Industries Co., Ltd.), etc.] or polyglycidyl ester compounds, aliphatic cyclic epoxy resins [e.g. Celloxide 2021, Celloxide 2021A, Celloxide 2021P,Celloxide 3000 (manufactured by Daicel Chemical Industries, Ltd.), DCPD-EP, MCPD-EP, TCPD-EP (manufactured by Maruzen Petrochemical Co., Ltd.), etc.], but not limited to these, these epoxy resins may be used alone or in combination of two or more.
[0104] Among the epoxy resins (a2) that can be used in combination, epoxy resins containing aliphatic substituents or bisphenol A type or F type epoxy resins having fluorine atoms in the molecule are preferred for the purpose of further reducing the dielectric constant and dielectric loss tangent; polyfunctional phenol novolac type epoxy resins or cresol novolac type epoxy resins are preferred for the purpose of further improving heat resistance; bisphenol S type epoxy resins or bisphenol fluorene type epoxy resins are preferred for the purpose of further improving heat resistance by increasing the refractive index; biphenol type epoxy resins, diphenyl ether type epoxy resins, or benzophenone type epoxy resins are preferred for the purpose of improving high thermal conductivity; and bisphenol A type epoxy resins, bisphenol F type epoxy resins, or bisphenol E type epoxy resins are preferred for the purpose of reducing viscosity, but are not limited to these.
[0105] When manufacturing the epoxy resin containing oxazolidone ring of the present invention, an isocyanate compound (b) is used together with the epoxy resin (a). The desired epoxy resin containing oxazolidone ring can be obtained by the reaction of the epoxy resin (a) and the isocyanate compound (b). The isocyanate compound (b) can be any isocyanate compound having an average of 1.8 or more isocyanate groups (-N=C=O) in one molecule, that is, a polyfunctional isocyanate compound having substantially two or more functions, and known and commonly used isocyanate compounds can be used. A small amount of monofunctional isocyanate compounds may also be included, but they become terminal groups, so they are effective in the purpose of reducing the degree of polymerization, but the degree of polymerization does not become higher.
[0106] Specific examples thereof include 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 3,5-toluene diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, m-xylene diisocyanate, p-xylene diisocyanate, tetramethylxylene diisocyanate, 1,4-naphthalene diisocyanate, 1,5-naphthalene diisocyanate, 2,6-naphthalene diisocyanate, 2,7-naphthalene diisocyanate, 1,4-naphthalene diisocyanate, 1,5-naphthalene diisocyanate, 2,6-naphthalene diisocyanate, 2,7-naphthalene diisocyanate, 1,4-naphthalene diisocyanate, 1,5-naphthalene diisocyanate, 2,6-naphthalene diisocyanate, 2,7-naphthalene diisocyanate, 1,4-naphthalene diisocyanate, 1,5-naphthalene diisocyanate, 2,2'-diphenylmethane ... m-phenylene diisocyanate, p-phenylene diisocyanate, biphenyl-4,4'-diisocyanate, 3,3'-dimethylbiphenyl-4,4'-diisocyanate, 2,3'-dimethoxybiphenyl-4,4'-diisocyanate, diphenylmethane-4,4'-diisocyanate, 3,3'-dimethoxydiphenylmethane-4,4'-diisocyanate, 4,4'-dimethoxydiphenylmethane-3,3'-diisocyanate, diphenyl sulfite-4,4'-diisocyanate, diphenyl sulfone-4,4'-diisocyanate, bicyclo[2.2.1]heptane-2,5-diylbismethylene diisocyanate, bicyclo[2.2.1] heptane-2,6-diylbismethylene diisocyanate, isophorone diisocyanate, 4,4'-methylenebiscyclohexyl diisocyanate, lysine diisocyanate, 1,1-bis(isocyanate methyl)cyclohexane, 1,2-bis(isocyanate methyl)cyclohexane, 1,3-bis(isocyanate methyl)cyclohexane, 1,4-bis(isocyanate methyl)cyclohexane, 1,3-cyclohexylene diisocyanate, 1,4-cyclohexylene diisocyanate, 4-methyl-1,3-cyclohexylene diisocyanate, 2-methyl-1,3-cyclohexylene diisocyanate, 1-Methylbenzene-2,4-diisocyanate, 1-Methylbenzene-2,5-diisocyanate, 1-Methylbenzene-2,6-diisocyanate, 1-Methylbenzene-3,5-diisocyanate, Hexamethylene diisocyanate, 2,2,4-Trimethylhexamethylene diisocyanate, 2,4,4-Trimethylhexamethylene diisocyanate, Methane diisocyanate, Ethane-1,2-diisocyanate, Propane-1,3-diisocyanate, Butane-1,1-diisocyanate, Butane-1,2-diisocyanate, Butane-1,4-diisocyanate, 2-Butene-1,4-diisocyanate diisocyanate compounds such as esters, 2-methylbutene-1,4-diisocyanate, 2-methylbutane-1,4-diisocyanate, pentane-1,5-diisocyanate, 2,2-dimethylpentane-1,5-diisocyanate, hexane-1,6-diisocyanate, heptane-1,7-diisocyanate, octane-1,8-diisocyanate, nonane-1,9-diisocyanate, decane-1,10-diisocyanate, dimethylsilane diisocyanate, diphenylsilane diisocyanate, or triphenylmethane triisocyanate, 1,3,6-hexamethylene triisocyanate , 1,8-diisocyanato-4-isocyanatomethyloctane, dicycloheptane triisocyanate, tris(isocyanatophenyl)thiophosphate, lysine ester triisocyanate, undecane triisocyanate, tris(4-phenylisocyanatothiophosphate)-3,3',4,4'-diphenylmethane tetraisocyanate, polymethylene polyphenyl isocyanate and other polyfunctional isocyanate compounds, or dimers or trimers of the isocyanate compounds, or blocked isocyanates masked with blocking agents such as alcohols or phenols, or biscarbamate compounds, but are not limited to these. These isocyanate compounds may be used alone or in combination of two or more. .
[0107] Among these isocyanate compounds, difunctional isocyanate compounds or trifunctional isocyanate compounds are preferred, and difunctional isocyanate compounds are further preferred. If the number of functional groups of the isocyanate compound is large, there is a concern that the storage stability is reduced; if the number of functional groups of the isocyanate compound is small, there is a concern that the heat resistance or dielectric properties are not improved.
[0108] Particularly preferred isocyanate compounds (b) are selected from 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 3,5-toluene diisocyanate, 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, m-xylene diisocyanate, p-xylene diisocyanate, tetramethylxylene diisocyanate, 1,4-naphthalene diisocyanate, 1,5-naphthalene diisocyanate, 2,6-naphthalene diisocyanate, 2,7-naphthalene diisocyanate, 3,3'-dimethylbiphenyl-4,4'-diisocyanate, m-phenylene diisocyanate, One or more of the group consisting of diisocyanate, p-phenylene diisocyanate, cyclohexane-1,4-diyl diisocyanate, cyclohexane-1,3-diyl dimethylene diisocyanate, cyclohexane-1,4-diyl dimethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, 4,4'-methylenebiscyclohexyl diisocyanate, bicyclo[2.2.1]heptane-2,5-diyl dimethylene diisocyanate, bicyclo[2.2.1]heptane-2,6-diyl dimethylene diisocyanate and isophorone diisocyanate.
[0109] The reaction of epoxy resin (a) and isocyanate compound (b) can be carried out using a known method. Specific reaction methods include: (1) melting epoxy resin (a), removing moisture from epoxy resin by flushing with dry gas or setting the system to decompression, and then adding isocyanate compound (b) and catalyst to react; and (2) premixing epoxy resin (a) with catalyst, removing moisture from epoxy resin by flushing with dry gas or setting the system to decompression, and then adding isocyanate compound (b) to react. The amount of water in the system at this time is preferably 0.5% by mass or less, more preferably 0.1% by mass or less, and further preferably 0.05% by mass or less. In addition, in any method, in the case where the resin viscosity is high and difficult to stir, if necessary, a non-reactive solvent can also be used.
[0110] The reaction mechanism for forming an oxazolidinone ring is represented by the following reaction formula (5). The epoxy resin (a) and the isocyanate compound (b) react with the epoxy group of the epoxy resin (a) and the isocyanate group of the isocyanate compound (b) by adding a catalyst to form an oxazolidinone ring. In addition, Y in formula (1) is the residue of the isocyanate compound (b) in the reaction.
[0111] [Chemistry 9]
[0112]
[0113] When the epoxy resin (a) contains an alcoholic hydroxyl group, as shown in the following reaction formula (6), the isocyanate group of the isocyanate compound (b) and the alcoholic hydroxyl group undergo an addition reaction to form a urethane bond.
[0114] [Chemistry 10]
[0115]
[0116] In addition, the epoxy equivalent of the oxazolidone ring-containing epoxy resin can be predicted based on the amount of raw materials charged and according to the following calculation formula (7). The preferred epoxy equivalent of the oxazolidone ring-containing epoxy resin A2 of the present invention is 200 to 1600. The epoxy equivalent can be adjusted to the above range by adjusting the NCO concentration of the isocyanate compound (b) used.
[0117] [Formula 1]
[0118]
[0119] No: Epoxy equivalent of epoxy resin containing oxazolidinone ring (g / eq.)
[0120] Ne: Epoxy equivalent weight of epoxy resin (a) (g / eq.)
[0121] Ni: equivalent weight of isocyanate group of isocyanate compound (b) (g / eq.)
[0122] Me: loading amount of epoxy resin (a) (g)
[0123] Mi: Charge amount of isocyanate compound (b) (g)
[0124] For example, when the epoxy equivalent of the epoxy resin (a) is 218 and the equivalent of the isocyanate group of the isocyanate compound (b) is 125, the epoxy equivalent of the epoxy resin A2 containing an oxazolidone ring is charged in a range of 200 g / eq. to 550 g / eq., and according to calculation formula (7), the charging ratio Me / Mi of the epoxy resin (a) to the isocyanate compound (b) is greater than 3.3.
[0125] It is preferred that the isocyanate group of the isocyanate compound (b) is used in an amount within a range of 0.02 mol or more and less than 0.7 mol per 1 mol of the epoxy group of the epoxy resin (a).
[0126] In other words, the molar ratio of the isocyanate group of the isocyanate compound (b) to 1 mol of the epoxy group of the epoxy resin (a) is in the range of [(b) / (a)] = 0.02 to 0.70. The oxazolidone ring-containing epoxy resin of the present invention is excellent in solvent solubility even if it is obtained by highly modifying the raw epoxy resin with an isocyanate compound, so the molar ratio [(b) / (a)] is more preferably 0.10 to 0.65, and further preferably 0.30 to 0.60.
[0127] The reaction of the epoxy resin (a) and the isocyanate compound (b) is preferably carried out by adding a catalyst. The catalyst addition temperature is preferably in the range of room temperature to 150°C, more preferably in the range of room temperature to 100°C.
[0128] The reaction temperature is preferably 100°C to 250°C, more preferably 100°C to 200°C, and further preferably 120°C to 160°C. If the reaction temperature is low, the formation of the oxazolidinone ring cannot be fully carried out, and the isocyanurate ring is formed by the trimerization reaction of the isocyanate group. In addition, if the reaction temperature is high, local high molecular weight is produced, and the generation of insoluble gel components becomes more. Therefore, it is preferred to adjust the addition rate of the isocyanate compound (b) to maintain the reaction temperature at a suitable temperature. By appropriately controlling the reaction conditions, the oxazolidinone ring can be roughly quantitatively generated by the epoxy group of the epoxy resin (a) and the isocyanate group of the isocyanate compound (b).
[0129] The reaction time is preferably in the range of 15 minutes to 10 hours after completion of the addition of the isocyanate compound (b), more preferably 30 minutes to 8 hours, and still more preferably 1 hour to 5 hours.
[0130] As the catalyst used in the reaction, if it is a basic catalyst, the type is not particularly limited. Specifically, lithium compounds such as lithium chloride and butoxylithium, boron trifluoride complex salts, quaternary ammonium salts such as tetramethylammonium chloride, tetramethylammonium bromide, tetraethylammonium bromide, tetrabutylammonium bromide, tetramethylammonium iodide, tetraethylammonium iodide, and tetrabutylammonium iodide, dimethylaminoethanol, triethylamine, tributylamine, benzyldimethylamine, N-methylmorpholine, N,N'-dimethylpiperazine, 1,4-diethylpiperazine, phosphines such as triphenylphosphine and tri(2,6-dimethoxyphenyl)phosphine, amyltriphenylphosphonium bromide, diallylphosphine, etc. can be listed. Phosphonium salts such as diphenylphosphonium bromide, ethyltriphenylphosphonium chloride, ethyltriphenylphosphonium bromide, ethyltriphenylphosphonium iodide, butyltriphenylphosphonium chloride, butyltriphenylphosphonium bromide, butyltriphenylphosphonium iodide, tetrabutylphosphonium acetate·acetic acid complex, tetrabutylphosphonium acetate, tetrabutylphosphonium chloride, tetrabutylphosphonium bromide, and tetrabutylphosphonium iodide, a combination of triphenyl antimony and iodine, imidazoles such as 2-phenylimidazole, 2-methylimidazole, and 2-ethyl-4-methylimidazole, etc., but are not limited to these, and these catalysts may be used alone or in combination of two or more. In addition, they may be divided and used several times.
[0131] Among these catalysts, quaternary ammonium salts, tertiary amines, phosphines or phosphonium salts are preferred, and tetramethylammonium iodide is more preferred in terms of reaction activity and reaction selectivity. If the catalyst has low reaction activity, there is a concern that the reaction time becomes long and productivity decreases; if the catalyst has low reaction selectivity, there is a concern that the polymerization reaction between epoxy groups cannot obtain the target property.
[0132] The usage amount of catalyst is not particularly limited, and relative to the total mass of epoxy resin (a) and isocyanate compound (b), the usage amount of the catalyst is 0.0001 mass %~5 mass %, preferably 0.0005 mass %~1 mass %, more preferably 0.001 mass %~0.5 mass %, and then preferably 0.002 mass %~0.2 mass %. If the amount of catalyst is large, the self-polymerization reaction of epoxy group is carried out according to the situation, so the resin viscosity becomes high. In addition, the self-polymerization reaction of isocyanate is promoted and the generation of oxazolidone ring is suppressed. And then, there is the following worry: in the generated resin, it remains as impurities, in various uses, particularly in the case of the material used as laminate or sealing material, causing insulation reduction or moisture resistance reduction.
[0133] In addition, when the epoxy resin (a) and the isocyanate compound (b) are reacted, the molecular weight (epoxy equivalent) and the like can be adjusted by further using various epoxy resin modifiers within a range that does not affect the effects of the present invention. The amount that can be used is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and further preferably 10 parts by mass or less relative to 100 parts by mass of the epoxy resin (a).
[0134] Specific examples of epoxy resin modifiers that can be used include bisphenol A, dimethylbisphenol A, tetramethylbisphenol A, tetrabutylbisphenol A, bisphenol F, dimethylbisphenol F, tetramethylbisphenol F, bisphenol S, dimethylbisphenol S, tetramethylbisphenol S, bisphenol B, bisphenol C, bisphenol E, bisphenol P, bisphenol AF, bisphenol AP, bisphenol fluorene, biscresol fluorene, bisphenol Z, tetramethylbisphenol Z, bisphenol TMC, hydroquinone, methyl hydroquinone, Dimethylhydroquinone, dibutylhydroquinone, resorcinol, methylresorcinol, biphenol, tetramethylbiphenol, dihydroxynaphthalene, dihydroxydiphenyl ether, dihydroxybenzophenone, dihydroxydiphenyl sulfide, dihydroxystilbenes, phenol novolac resin, cresol novolac resin, bisphenol A novolac resin, dicyclopentadiene phenol resin, phenol aralkyl resin, naphthol novolac resin, styrenated phenol novolac resin, terpene Various phenols such as phenol resins and heavy oil-modified phenol resins, or polyphenol resins obtained by condensation reactions of various phenols with various aldehydes such as hydroxybenzaldehyde, crotonaldehyde, and glyoxal, or amine compounds such as aniline, phenylenediamine, toluidine, xylidine, diethyltoluenediamine, diaminodiphenylmethane, diaminodiphenylethane, diaminodiphenylpropane, diaminodiphenylketone, diaminodiphenyl sulfide, diaminodiphenyl sulfone, bis(aminophenyl)fluorene, diaminodiethyldimethyldiphenylmethane, diaminodiphenyl ether, diaminobenzanilide, diaminobiphenyl, dimethyldiaminobiphenyl, biphenyltetramine, bisaminophenylanthracene, bisaminophenoxybenzene, bisaminophenoxyphenyl ether, bisaminophenoxybiphenyl, bisaminophenoxyphenyl sulfone, bisaminophenoxyphenylpropane, and diaminonaphthalene, but are not limited to these. These epoxy resin modifiers may be used alone or in combination of two or more.
[0135] In addition, as described above, when the epoxy resin (a) and the isocyanate compound (b) are reacted, a non-reactive solvent may be used as needed. Specifically, hydrocarbons such as hexane, heptane, octane, decane, dimethylbutane, pentene, cyclohexane, methylcyclohexane, benzene, toluene, xylene, ethylbenzene, or ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, or ethers such as ethyl ether, isopropyl ether, butyl ether, diisoamyl ether, methyl phenyl ether, ethyl phenyl ether, pentyl phenyl ether, ethyl benzyl ether, dioxane, methylfuran, tetrahydrofuran, diethylene glycol dimethyl ether, ethylene glycol diethyl ether, and methyl ethyl carbitol, or methyl cellosolve acetate, cellosolve acetate, butyl Cellosolve acetate, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, diethyl oxalate and other esters, or N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide and other amides, or γ-butyrolactone and other lactones, or dimethyl sulfoxides, or tetramethylurea and other ureas, or dichloromethane, 1,2-dichloroethane, 1,4-dichlorobutane, chlorobenzene, o-dichlorobenzene and other halogenated hydrocarbons, but not limited to these, these non-reactive solvents can be used alone, or two or more can be used in combination. The amount of these solvents used is preferably 1 to 900 parts by mass, more preferably 5 to 100 parts by mass, relative to 100 parts by mass of the epoxy resin (a).
[0136] The oxazolidinone ring-containing epoxy resin of the present invention is obtained by the above-mentioned production method. Advantageously, the oxazolidinone ring-containing epoxy resin A2 is obtained.
[0137] Epoxy resin A1 containing oxazolidone ring, epoxy resin A2 containing oxazolidone ring can be used without allocating other epoxy resins, and other epoxy resin A3 can be allocated as needed. And, the content of the structure represented by formula (1) in epoxy resin A2 containing oxazolidone ring or epoxy resin mixture with other epoxy resin A3 is preferably 5 mass %~55 mass %, more preferably 10 mass %~45 mass %, and then preferably 15 mass %~35 mass %. If the content is few, there is the worry that the effect of reducing dielectric constant and dielectric loss tangent is not shown. In addition, if the content is many, there is the worry that the adverse effects such as solvent solubility deterioration or resin viscosity increase due to the improvement effect of dielectric properties become more. In addition, because the epoxy equivalent becomes high, the cross-linking density of the hardened material obtained becomes low, so there is the worry that the elastic coefficient decreases at the temperature of reflow soldering, etc., which becomes a big problem in use.
[0138] Next, the curable epoxy resin composition of the present invention will be described.
[0139] The curable epoxy resin composition of the present invention comprises the oxazolidone ring-containing epoxy resin of the present invention and a curing agent.
[0140] The hardener is not particularly limited as long as it is a hardener for hardening epoxy resins, and hardeners for epoxy resins such as phenolic hardeners, acid anhydride hardeners, amine hardeners, hydrazide hardeners, active ester hardeners, and phosphorus-containing hardeners described later can be used. These hardeners can be used alone or in combination of two or more. Among these hardeners, dicyandiamide, phenolic hardeners, or active ester hardeners are preferred, and phenolic hardeners or active ester hardeners are more preferred.
[0141] In the curable epoxy resin composition, the amount of the curing agent used is such that the active hydrogen group of the curing agent becomes 0.2 mol to 1.5 mol relative to 1 mol of the epoxy group of all epoxy resins including the epoxy resin containing an oxazolidone ring. In the case where the active hydrogen group is less than 0.2 mol or exceeds 1.5 mol relative to 1 mol of the epoxy group, there is a concern that the curing becomes incomplete and good curing properties cannot be obtained. The preferred range is 0.3 mol to 1.5 mol, the more preferred range is 0.5 mol to 1.5 mol, and the further preferred range is 0.8 mol to 1.2 mol. For example, when a phenolic curing agent, an amine curing agent, or an active ester curing agent is used, approximately equimolar active hydrogen groups are prepared relative to the epoxy group, and when an anhydride curing agent is used, 0.5 mol to 1.2 mol, preferably 0.6 mol to 1.0 mol of anhydride groups are prepared relative to 1 mol of the epoxy group. Here, the epoxy resin includes the oxazolidone ring-containing epoxy resin A1, the oxazolidone ring-containing epoxy resin A2, and the other epoxy resin A3, and includes a compound having an epoxy group such as a phosphorus-containing epoxy resin. In addition, the hardener includes a phosphorus-containing hardener.
[0142] The active hydrogen group described in the present invention is a functional group having active hydrogen that is reactive with an epoxy group (including a functional group having potential active hydrogen that generates active hydrogen due to hydrolysis, etc., or a functional group that exhibits an equivalent curing effect). Specifically, an acid anhydride group, a carboxyl group, an amino group, or a phenolic hydroxyl group can be cited. Furthermore, regarding the active hydrogen group, a carboxyl group (-COOH) or a phenolic hydroxyl group (-OH) is calculated as 1 mole, and an amino group (NH2) is calculated as 2 moles. In addition, when the active hydrogen group is not clear, the active hydrogen equivalent can be obtained by measurement. For example, by reacting a monoepoxy resin with a known epoxy equivalent such as phenyl glycidyl ether with a curing agent with an unknown active hydrogen equivalent, the amount of the monoepoxy resin consumed can be measured to obtain the active hydrogen equivalent of the curing agent used.
[0143] Specific examples of the phenolic curing agent include bisphenols such as bisphenol A, bisphenol F, bisphenol C, bisphenol K, bisphenol Z, bisphenol S, tetramethylbisphenol A, tetramethylbisphenol F, tetramethylbisphenol S, tetramethylbisphenol Z, dihydroxydiphenyl sulfide, and 4,4'-thiobis(3-methyl-6-tert-butylphenol); or dihydroxybenzenes such as catechol, resorcinol, methylresorcinol, hydroquinone, monomethylhydroquinone, dimethylhydroquinone, trimethylhydroquinone, mono-tert-butylhydroquinone, and di-tert-butylhydroquinone; or hydroxynaphthalenes such as dihydroxynaphthalene, dihydroxymethylnaphthalene, and trihydroxynaphthalene; or phenol novolac resins [e.g., Shonol BRG-55 7 (manufactured by AICA Industries, Ltd.), etc.], cresol novolac resins [e.g. DC-5 (manufactured by Nippon Steel Chemical Materials Co., Ltd.), etc.], trihydroxyphenylmethane type novolac resins [e.g. Resitop TPM-100 (manufactured by Qun Rong Chemical Industry Co., Ltd.), etc.], naphthol novolac resins and / or condensates of naphthols and aldehydes, or naphthol aralkyl resins [e.g. SN-160, SN-395, SN-485 (manufactured by Nippon Steel Chemical Materials Co., Ltd.), etc.], phenols and / or naphthols and benzenedimethanol and / or dichloromethylbenzene (xylylene glycol) chloride), or condensates of phenols and / or naphthols with isopropenyl acetophenone, or reaction products of phenols and / or naphthols with dicyclopentadiene, or condensates of phenols and / or naphthols with biphenyl condensing agents, etc., aminotriazine-modified phenol resins (polyphenol compounds formed by linking phenol nuclei with melamine, benzoguanamine, etc.), or phenol compounds formed by ring substitution of these phenol compounds with substituents such as alkyl, alkoxy, aryl, etc., but are not limited to these.
[0144] As raw materials of these phenolic compounds, phenols include phenol, cresol, xylenol, butylphenol, octylphenol, pentylphenol, nonylphenol, butylmethylphenol, trimethylphenol, phenylphenol, etc. Naphthols include 1-naphthol and 2-naphthol. In addition, although strictly speaking, they are not naphthols, naphthalene diols such as 1,4-naphthalene diol, 1,5-naphthalene diol, 2,6-naphthalene diol, and 2,7-naphthalene diol are also included in naphthols. Aldehydes include formaldehyde, acetaldehyde, propionaldehyde, butyraldehyde, valeraldehyde, hexanal, benzaldehyde, chloral, bromoaldehyde, glyoxal, malondialdehyde, succinaldehyde, glutaraldehyde, adipaldehyde, heptanedialdehyde, decanedial, acrolein, crotonaldehyde, salicylaldehyde, o-phthalaldehyde, hydroxybenzaldehyde, etc. Examples of the biphenyl-based condensing agent include bis(hydroxymethyl)biphenyl, bis(methoxymethyl)biphenyl, bis(ethoxymethyl)biphenyl, and bis(chloromethyl)biphenyl.
[0145] In addition, benzoxazine compounds that open their rings to become phenol compounds when heated are also effective as curing agents. Specifically, bisphenol F-type or bisphenol S-type benzoxazine compounds [such as BF-BXZ, BS-BXZ (these are manufactured by Konishi Chemical Industries, Ltd.)] and the like can be cited, but are not limited to these.
[0146] Specific examples of the acid anhydride curing agent include tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, pyromellitic dianhydride, phthalic anhydride, trimellitic anhydride, methylnadic anhydride, and maleic anhydride, but are not limited thereto.
[0147] Specific examples of the amine curing agent include diethylenetriamine, triethylenetetramine, m-xylene diamine, isophoronediamine, diaminodiphenylmethane, diaminodiphenyl sulfone, diaminodiphenyl ether, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, dicyandiamide, and amine compounds such as polyamide amines which are condensates of acids such as dimer acid and polyamines, but are not limited to these.
[0148] Examples of active ester curing agents include reaction products of polyfunctional phenol compounds and aromatic carboxylic acids as described in Japanese Patent No. 5152445, and commercially available products include Epiclon HPC-8000-65T (manufactured by DIC Corporation), but are not limited to these.
[0149] Specific examples of other curing agents include phosphine compounds such as triphenylphosphine, phosphonium salts such as tetraphenylphosphonium bromide, imidazoles such as 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, and 1-cyanoethyl-2-methylimidazole, imidazole salts that are salts of imidazoles with trimellitic acid, isocyanuric acid, boric acid, and the like, quaternary ammonium salts such as trimethylammonium chloride, diazabicyclic compounds, salts of diazabicyclic compounds with phenols or phenol novolac resins, complex compounds of boron trifluoride with amines or ether compounds, aromatic phosphonium, or iodonium salts, but are not limited to these.
[0150] In addition, as described above, the other epoxy resin A3 can be used in combination as needed within the range that does not damage the physical properties of the epoxy resin composition. The so-called range that does not damage the physical properties of the epoxy resin composition refers to the range of the structure represented by formula (1) containing 5% to 55% by mass in all epoxy resins. Furthermore, as other epoxy resins A3, existing well-known epoxy resins can be used. The target properties vary depending on the application, so it is impossible to determine in general. As a standard for the amount used, it is preferably 0% to 95% by mass in all epoxy resins, more preferably 0% to 80% by mass, and further preferably 0% to 50% by mass.
[0151] The other epoxy resin A3 is preferably a multifunctional epoxy resin having two or more functions, and can be selected according to the purpose. For example, in order to impart flame retardancy, it is preferably used in combination with a phosphorus-containing epoxy resin described later, and in order to further improve heat resistance, it is preferably used in combination with a trifunctional epoxy resin or the like.
[0152] Examples of the other epoxy resin A3 include the bisphenol A type epoxy resin, bisphenol F type epoxy resin, tetramethyl bisphenol F type epoxy resin, biphenyl type epoxy resin, hydroquinone type epoxy resin, bisphenol fluorene type epoxy resin, naphthylene type epoxy resin, bisphenol S type epoxy resin, diphenyl sulfide type epoxy resin, resorcinol type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, alkyl novolac type epoxy resin, styrenated phenol novolac type epoxy resin, bisphenol novolac type epoxy resin, naphthol novolac type epoxy resin, β-naphthol aralkyl type epoxy resin, naphthalene diol aralkyl type epoxy resin, α-naphthol aralkyl Polyglycidyl ether compounds such as diaminodiphenylmethane epoxy resin, meta-xylene diamine epoxy resin, 1,3-bisaminomethylcyclohexane epoxy resin, isocyanurate epoxy resin, aniline epoxy resin, hydantoin epoxy resin, aminophenol epoxy resin, etc., polyglycidyl amine compounds such as dimer acid epoxy resin, hexahydrophthalic acid epoxy resin, etc., or alicyclic epoxy compounds. In addition, examples include urethane-modified epoxy resins [e.g., AER4152 (manufactured by Asahi Kasei Electronic Materials Co., Ltd.)], oxazolidone ring-containing epoxy resins other than the epoxy resin (A1), epoxy-modified polybutadiene rubber derivatives [e.g., PB-3600 (manufactured by Daicel Chemical Industries, Ltd.)], CTBN-modified epoxy resins [e.g., Epotohto YR-102, Epotohto YR-450 (manufactured by Nippon Steel Chemical Materials Co., Ltd.)], phosphorus-containing epoxy resins described later, etc., but are not limited to these, and these epoxy resins may be used alone or in combination of two or more.
[0153] In the curable epoxy resin composition, a curing accelerator may be used as needed. Examples of the curing accelerator include, but are not limited to, imidazole derivatives, tertiary amines, phosphorus compounds such as phosphines, metal compounds, Lewis acids, and amine complex salts. These curing accelerators may be used alone or in combination of two or more.
[0154] As imidazole derivatives, there are no particular limitations as long as they are compounds having an imidazole skeleton. Examples include imidazole compounds substituted with an alkyl group such as 2-ethylimidazole, 2-ethyl-4-methylimidazole, bis-2-ethyl-4-methylimidazole, 1-methyl-2-ethylimidazole, 2-isopropylimidazole, 2,4-dimethylimidazole, and 2-heptadecylimidazole, or imidazole compounds substituted with a hydrocarbon group containing a ring structure such as an aryl group or an aralkyl group such as 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-ethylimidazole, 1-benzyl-2-phenylimidazole, benzimidazole, and 2-ethyl-4-methyl-1-(2'-cyanoethyl)imidazole.
[0155] Examples of tertiary amines include 2-dimethylaminopyridine, 4-dimethylaminopyridine, 2-(dimethylaminomethyl)phenol, 1,8-diaza-bicyclo[5.4.0]-7-undecene (DBU), etc. Examples of phosphines include triphenylphosphine, tricyclohexylphosphine, triphenylphosphinetriphenylborane, etc. Examples of metal compounds include tin octylate, etc.
[0156] Among these curing accelerators, when used as a build-up material or a circuit substrate, 2-dimethylaminopyridine, 4-dimethylaminopyridine or imidazoles are preferred in terms of excellent heat resistance, dielectric properties, solder resistance, etc. In addition, when used as a semiconductor sealing material, triphenylphosphine or DBU is preferred in terms of excellent curability, heat resistance, electrical properties, moisture resistance reliability, etc.
[0157] The amount of the curing accelerator can be appropriately selected according to the purpose of use. For 100 parts by mass of the epoxy resin component in the epoxy resin composition, 0.02 parts by mass to 15 parts by mass are used as needed. Preferably, it is 0.1 parts by mass to 10 parts by mass, more preferably 0.5 parts by mass to 8 parts by mass, and further preferably 0.5 parts by mass to 5 parts by mass. By using a curing accelerator, the curing temperature can be lowered or the curing time can be shortened.
[0158] In the curable epoxy resin composition, in order to improve the flame retardancy of the obtained cured product, various conventionally known flame retardants can be used. As usable flame retardants, for example, halogen flame retardants, phosphorus flame retardants (phosphorus compounds as flame retardants), nitrogen flame retardants, silicone flame retardants, inorganic flame retardants, organic metal salt flame retardants, etc. can be cited. From the perspective of the environment, halogen-free flame retardants are preferred, and phosphorus flame retardants are particularly preferred. These flame retardants are not particularly limited when used, and can be used alone, or multiple flame retardants of the same series can be used, and flame retardants of different series can also be used in combination.
[0159] In particular, in epoxy resin compositions that further include phosphorus compounds as flame retardants, phosphorus compounds are divided into two types: additive phosphorus flame retardants (phosphorus-containing additives) and reactive phosphorus compounds, and reactive phosphorus compounds are further divided into phosphorus-containing epoxy resins and phosphorus-containing curing agents. When comparing additive phosphorus flame retardants with reactive phosphorus compounds, reactive phosphorus compounds have a greater flame retardant effect in terms of not oozing out during curing and having good compatibility, and it is preferred to use reactive phosphorus compounds.
[0160] The phosphorus-containing additive may be any of an inorganic phosphorus compound and an organic phosphorus compound. Examples of the inorganic phosphorus compound include ammonium phosphates such as red phosphorus, monoammonium phosphate, diammonium phosphate, triammonium phosphate, and ammonium polyphosphate, and nitrogen-containing inorganic phosphorus compounds such as phosphoramide, but are not limited to these.
[0161] In addition, red phosphorus is preferably subjected to surface treatment for the purpose of preventing hydrolysis, etc. Examples of the surface treatment method include (1) a method of coating with an inorganic compound such as magnesium hydroxide, aluminum hydroxide, zinc hydroxide, titanium hydroxide, bismuth oxide, bismuth hydroxide, bismuth nitrate, or a mixture thereof; (2) a method of coating with a mixture of an inorganic compound such as magnesium hydroxide, aluminum hydroxide, zinc hydroxide, titanium hydroxide, and a thermosetting resin such as a phenol resin; (3) a method of double coating with a thermosetting resin such as a phenol resin on a film of an inorganic compound such as magnesium hydroxide, aluminum hydroxide, zinc hydroxide, titanium hydroxide, etc., but the present invention is not limited to these.
[0162] Examples of the organophosphorus compounds include phosphate compounds [e.g., methyl phosphate, ethyl phosphate, isopropyl phosphate, dibutyl phosphate, monobutyl phosphate, butoxyethyl phosphate, 2-ethylhexyl phosphate, bis(2-ethylhexyl) phosphate, monoisodecyl phosphate, lauryl phosphate, tridecyl phosphate, oleyl phosphate, tetradecyl phosphate, stearyl phosphate, isostearyl phosphate, butyl pyrophosphate, ethylene glycol phosphate, (2-hydroxyethyl) methacrylate phosphate, etc.], condensed phosphates [e.g., PX-200 (Dahachi Chemical Industry Co., Ltd.) Co., Ltd.)], phosphonic acid compounds, phosphinic acid compounds, phosphine oxide compounds [e.g., diphenylphosphine oxide, triphenylphosphine oxide, etc.], phosphorane compounds [e.g., triphenyl(9H-fluorene-9-ylidene)phosphorane, etc.], or nitrogen-containing organophosphorus compounds [e.g., SPS-100, SPB-100, SPE-100 (all manufactured by Otsuka Chemical Co., Ltd.)], or phosphinic acid metal salts [e.g., EXOLIT OP1230, EXOLIT OP124 0, EXOLIT OP930, EXOLIT OP935 (all manufactured by Clariant), etc.], in addition, phosphorus compounds having an active hydrogen group directly bonded to a phosphorus atom [such as 9,10-dihydro-9-oxa-10-phosphophananthrene-10-oxide (hereinafter referred to as DOPO), diphenylphosphine oxide, etc.] or phosphorus-containing phenolic compounds [such as 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphophananthrene-10-oxide (hereinafter referred to as The present invention also includes organophosphorus compounds such as 1,4-dihydroxy-2-naphthyl-10H-9-oxa-10-phosphophananthrene-10-oxide (hereinafter referred to as DOPO-NQ), diphenylphosphinylhydroquinone, diphenylphosphinyl-1,4-dioxynaphthalene, 1,4-cyclooctylphosphinyl-1,4-phenylene glycol, 1,5-cyclooctylphosphinyl-1,4-phenylene glycol, etc., or derivatives obtained by reacting these organophosphorus compounds with compounds such as epoxy resins or phenol resins, but is not limited to these.
[0163] The reactive phosphorus compound used in the phosphorus-containing epoxy resin or the phosphorus-containing hardener is preferably a phosphorus compound having an active hydrogen group directly bonded to a phosphorus atom or a phosphorus-containing phenol, and specific examples thereof include DOPO, DOPO-HQ, and DOPO-NQ.
[0164] Examples of the phosphorus-containing epoxy resin include Epotohto FX-305, Epotohto FX-289B, TX-1320A, and Epotohto TX-1328 (all manufactured by Nippon Steel Chemical Materials Co., Ltd.), but are not limited thereto.
[0165] The epoxy equivalent of the phosphorus-containing epoxy resin is preferably 200 to 800, more preferably 300 to 780, and still more preferably 400 to 760. The phosphorus content of the phosphorus-containing epoxy resin is preferably 0.5 to 6% by mass, more preferably 2 to 5.5% by mass, and still more preferably 3 to 5% by mass.
[0166] As the phosphorus-containing curing agent, in addition to the above-mentioned phosphorus-containing phenols, phosphorus-containing phenol compounds can be obtained by, for example, reacting DOPO with aldehydes and phenol compounds using the production method disclosed in Japanese Patent Publication No. 2008-501063 or Japanese Patent No. 4548547. In addition, phosphorus-containing active ester compounds can be obtained from phosphorus-containing phenol compounds by further reacting with aromatic carboxylic acids using the production method disclosed in Japanese Patent Publication No. 2013-185002. In addition, phosphorus-containing benzoxazine compounds can be obtained by the production method disclosed in Japanese Patent Publication No. WO2008 / 010429.
[0167] The phosphorus content of the phosphorus-containing hardener is preferably 0.5 to 12% by mass, more preferably 2 to 11% by mass, and still more preferably 4 to 10% by mass.
[0168] The amount of phosphorus compound can be suitably selected according to the type of phosphorus compound, the composition of epoxy resin composition, and the degree of desired flame retardancy. In the case where the phosphorus compound is a reactive phosphorus compound, i.e., a phosphorus-containing epoxy resin or a phosphorus-containing hardener, relative to the solid components (non-volatile components) in all curable epoxy resin compositions equipped with epoxy resins, hardeners, flame retardants and other fillers or additives, the phosphorus content is preferably 0.2 mass % or more and 6 mass % or less, more preferably 0.4 mass % or more and 4 mass % or less, and further preferably 0.5 mass % or more and 3.5 mass % or less, and particularly preferably 0.6 mass % or more and 3 mass % or less. If the phosphorus content is small, there is a concern that it is difficult to ensure flame retardancy; if the phosphorus content is too much, there is a concern that heat resistance is adversely affected.
[0169] Here, the phosphorus-containing epoxy resin may be regarded as a phosphorus compound or an epoxy resin. Similarly, the phosphorus-containing hardener may be regarded as a phosphorus compound or both of them are equivalent to the hardener. Therefore, when a phosphorus-containing hardener is used, there is a case where it is not necessary to use other hardeners or phosphorus compounds. Similarly, when a phosphorus-containing epoxy resin is used, there is a case where it is not necessary to use other epoxy resins or phosphorus compounds.
[0170] Regarding the amount of the phosphorus compound added as an additive phosphorus flame retardant, in 100 parts by mass of the solid content (non-volatile content) in the curable epoxy resin composition, when red phosphorus is used, it is preferably mixed in the range of 0.1 to 2 parts by mass, and when an organic phosphorus compound is used, it is also preferably mixed in the range of 0.1 to 10 parts by mass, and particularly preferably mixed in the range of 0.5 to 6 parts by mass.
[0171] When a phosphorus compound is used as a flame retardant, for example, hydrotalcite, magnesium hydroxide, a boron compound, zirconium oxide, calcium carbonate, zinc molybdate, etc. may be used in combination as a flame retardant auxiliary.
[0172] In the present invention, it is preferred to use these phosphorus compounds as flame retardants, but flame retardants described below may be used in combination with the phosphorus compounds or in place of the phosphorus compounds.
[0173] As nitrogen flame retardants, for example, triazine compounds, cyanuric acid compounds, isocyanuric acid compounds, phenothiazine, etc. can be cited, preferably triazine compounds, cyanuric acid compounds, isocyanuric acid compounds. As triazine compounds, for example, melamine, acetoguanamine, benzoguanamine, dicyanocyanamide [2,4,6-tris (cyanoamino) -1,3,5-triazine], melam [4,4'-iminobis (1,3,5-triazine-2,6-diamine)], ethylene dimelamine, polyphosphate melamine, triguanamine, etc. can be cited. In addition, for example, sulfated aminotriazine compounds such as guanidinomelamine, melem sulfate, and melam sulfate can be cited, aminotriazine-modified phenol resins [such as LA-7052 (manufactured by DIC Corporation)] and aminotriazine-modified phenol resins modified with tung oil, isomerized linseed oil, etc. can be cited, but it is not limited to these. Examples of the cyanuric acid compound include cyanuric acid and melamine cyanurate, but are not limited to these.
[0174] The amount of the nitrogen flame retardant can be appropriately selected according to the type of the nitrogen flame retardant, other components of the epoxy resin composition, and the desired degree of flame retardancy. For example, it is preferably mixed in the range of 0.05 to 10 parts by mass, and particularly preferably in the range of 0.1 to 5 parts by mass, based on 100 parts by mass of the solid content (non-volatile component) in the curable epoxy resin composition. In addition, when using a nitrogen flame retardant, a metal hydroxide, a molybdenum compound, etc. may also be used in combination.
[0175] As the silicone-based flame retardant, any organic compound containing a silicon atom can be used without particular limitation, and examples thereof include silicone oil, silicone rubber, silicone resin, and the like, but the present invention is not limited to these.
[0176] The amount of the silicone flame retardant can be appropriately selected according to the type of silicone flame retardant, other components of the epoxy resin composition, and the desired degree of flame retardancy, for example, preferably in the range of 0.05 to 20 parts by mass based on 100 parts by mass of the solid content (non-volatile component) in the curable epoxy resin composition. In addition, when using a silicone flame retardant, a molybdenum compound, aluminum oxide, etc. may also be used in combination.
[0177] As inorganic flame retardants, for example, metal hydroxides, metal oxides, metal carbonate compounds, metal powders, boron compounds, low melting point glass, etc. can be listed, but they are not limited to these. As metal hydroxides, for example, aluminum hydroxide, magnesium hydroxide, dolomite, hydrotalcite, boehmite, calcium hydroxide, barium hydroxide, zirconium hydroxide, etc. can be listed, but they are not limited to these. As metal oxides, for example, zinc molybdate, molybdenum trioxide, zinc stannate, tin oxide, aluminum oxide, iron oxide, titanium oxide, manganese oxide, zirconium oxide, zinc oxide, molybdenum oxide, cobalt oxide, bismuth oxide, chromium oxide, nickel oxide, copper oxide, tungsten oxide, etc. can be listed, but they are not limited to these. As metal carbonate compounds, for example, zinc carbonate, magnesium carbonate, calcium carbonate, barium carbonate, basic magnesium carbonate, aluminum carbonate, iron carbonate, cobalt carbonate, titanium carbonate, etc. can be listed, but they are not limited to these. As metal powders, for example, aluminum, iron, titanium, manganese, zinc, molybdenum, cobalt, bismuth, chromium, nickel, copper, tungsten, tin, etc. can be listed, but they are not limited to these. Boron compounds include, but are not limited to, zinc borate, zinc metaborate, barium metaborate, boric acid, borax, etc. Low-melting-point glass includes, but is not limited to, hydrated glass, SiO2-MgO-H2O, PbO-B2O3, ZnO-P2O5-MgO, P2O5-B2O3-PbO-MgO, P-Sn-OF, PbO-V2O5-TeO2, Al2O3-H2O, lead borosilicate, and other glassy compounds.
[0178] The amount of the inorganic flame retardant can be appropriately selected according to the type of the inorganic flame retardant, other components of the epoxy resin composition, and the desired degree of flame retardancy. For example, it is preferably mixed in the range of 0.05 to 20 parts by mass, and particularly preferably in the range of 0.5 to 15 parts by mass, based on 100 parts by mass of the solid content (non-volatile content) in the total epoxy resin composition containing epoxy resin, hardener, flame retardant and other fillers or additives.
[0179] Examples of the organic metal salt flame retardant include ferrocene, acetylacetone metal complexes, organic metal carbonyl compounds, organic cobalt salt compounds, organic sulfonic acid metal salts, and compounds in which a metal atom is ionically or coordinately bonded to an aromatic compound or a heterocyclic compound, but are not limited thereto.
[0180] The amount of the organic metal salt flame retardant can be appropriately selected according to the type of the organic metal salt flame retardant, other components of the epoxy resin composition, and the desired degree of flame retardancy. For example, it is preferably mixed in the range of 0.005 to 10 parts by mass based on 100 parts by mass of the solid content (non-volatile content) in the total epoxy resin composition including epoxy resin, hardener, flame retardant and other fillers or additives.
[0181] As halogen flame retardants, bromine compounds or chlorine compounds can be cited, and chlorine compounds are not preferred in terms of toxicity. As bromine compounds, for example, p-dibromobenzene, pentabromodiphenyl ether, octabromodiphenyl ether, tetradecabromo-p-diphenoxybenzene, decabromodiphenyl ether, tetrabromobisphenol A, hexabromocyclododecane, hexabromobenzene, 2,2'-ethylenebis(4,5,6,7-tetrabromoisoindoline-1,3-dione [for example, SAYTEX BT-93 (manufactured by Albemarle)], ethane-1,2-bis(pentabromophenyl) [for example, SAYTEX 8010 (manufactured by Albemarle)], or brominated epoxy oligomers [for example, SR-T1000, SR-T2000 (manufactured by Sakamoto Pharmaceutical Industries)], etc. can be cited, but are not limited to these.
[0182] The amount of halogen flame retardant can be appropriately selected according to the type of halogen flame retardant, other components of epoxy resin composition, and the desired degree of flame retardancy, for example, relative to the solid components (non-volatile components) in all epoxy resin compositions mixed with epoxy resin, hardener, flame retardant and other fillers or additives, the halogen content is preferably 5% by mass or more and 15% by mass or less. Alternatively, in the case of using halogen flame retardant as flame retardant, as flame retardant aid, for example, antimony compounds such as antimony trioxide, antimony tetroxide, antimony pentoxide, tin compounds such as tin oxide and tin hydroxide, molybdenum compounds such as molybdenum oxide and ammonium molybdate, zirconium compounds such as zirconium oxide and zirconium hydroxide, boron compounds such as zinc borate and barium metaborate, silicon compounds such as silicone oil, silane coupling agent, high molecular weight silicone, chlorinated polyethylene, etc. can also be used in combination.
[0183] In addition, the curable epoxy resin composition of the present invention may be formulated with fillers, thermoplastic resins, thermosetting resins other than epoxy resins, silane coupling agents, antioxidants, mold release agents, defoamers, emulsifiers, thixotropy imparting agents, lubricants, pigments and other additives as needed. Furthermore, an organic solvent or a reactive diluent may be formulated for viscosity adjustment.
[0184] As filler, for example, inorganic fillers such as fused silica, crystalline silica, aluminum oxide, silicon nitride, boron nitride, aluminum hydroxide, calcium hydroxide, magnesium hydroxide, boehmite, talc, mica, clay, calcium carbonate, magnesium carbonate, barium carbonate, zinc oxide, titanium oxide, magnesium oxide, magnesium silicate, calcium silicate, zirconium silicate, barium sulfate, carbon, or fibrous fillers such as carbon fiber, glass fiber, aluminum oxide fiber, silicon dioxide aluminum oxide fiber, silicon carbide fiber, polyester fiber, cellulose fiber, aromatic polyamide fiber, ceramic fiber, or microparticle rubber, etc. can be listed. Among these fillers, preferably, those that are not decomposed or dissolved by acidifying compounds such as aqueous solutions of permanganate used in the surface roughening treatment of the hardened material, particularly fused silica or crystalline silica are easy to obtain fine particles, so it is preferred. In addition, in the case where the amount of the filler is particularly large, it is preferred to use fused silica. Fused silica can use any of crushed and spherical shapes. In order to improve the amount of fused silica and suppress the rise in the melt viscosity of the molding material, it is more preferred to mainly use spherical fused silica. And then, in order to improve the amount of spherical silica, it is preferably to appropriately adjust the particle size distribution of spherical silica. Moreover, the filler can also be treated with silane coupling agents or organic acids such as stearic acid. Generally speaking, the reason for using the filler can be cited as the impact resistance improvement effect of the hardened material or the low linear expansion of the hardened material. In addition, when using metal hydroxides such as aluminum hydroxide, boehmite, and magnesium hydroxide, it plays a role as a flame retardant aid, and has the effect of improving flame retardancy. When used in the use of conductive pastes, conductive fillers such as silver powder or copper powder can be used.
[0185] In the case of considering the low linear expansion or flame retardancy of the hardened material, the amount of filler is preferably high. Relative to the solid content (non-volatile component) in the epoxy resin composition, it is preferably 1% by mass to 90% by mass, more preferably 10% by mass to 85% by mass, and then preferably 40% by mass to 80% by mass, and particularly preferably 50% by mass to 70% by mass. If the amount of allocation is large, there is a concern that the adhesiveness required for the laminated board is reduced, and then there is a concern that the hardened material becomes brittle and cannot obtain sufficient mechanical properties. In addition, if the amount of allocation is small, there is the following concern: improving the impact resistance of the hardened material is not the allocation effect of the filler.
[0186] The average particle size of the inorganic filler is preferably 0.05 μm to 1.5 μm, more preferably 0.1 μm to 1 μm. If the average particle size of the inorganic filler is within the above range, the fluidity of the epoxy resin composition is well maintained. The average particle size can be measured using a particle size distribution measuring device.
[0187] In particular, when the curable epoxy resin composition is formed into a sheet or film, it is effective to mix a thermoplastic resin. Examples of the thermoplastic resin include phenoxy resin, polyurethane resin, polyester resin, polyethylene resin, polypropylene resin, polystyrene resin, acrylonitrile-butadiene-styrene (ABS) resin, acrylonitrile-styrene (AS) resin, vinyl chloride resin, polyvinyl acetate resin, polymethyl methacrylate resin, polycarbonate resin, polyacetal resin, cyclic polyolefin resin, polyamide resin, thermoplastic polyimide resin, polyamideimide resin, polytetrafluoroethylene resin, polyetherimide resin, polyphenylene ether resin, modified polyphenylene ether resin, polyethersulfone resin, polysulfone resin, polyetheretherketone resin, polyphenylene sulfide resin, and polyethylene formaldehyde resin, but are not limited thereto. In terms of compatibility with epoxy resin, phenoxy resin is preferred, and in terms of low dielectric properties, polyphenylene ether resin or modified polyphenylene ether resin is preferred.
[0188] As other additives, for example, thermosetting resins other than epoxy resins such as phenol resins, melamine resins, urea resins, unsaturated polyester resins, alkyd resins, diallyl phthalate resins, and thermosetting polyimides, or organic pigments such as quinacridone, azo, and phthalocyanine, or inorganic pigments such as titanium oxide, metallic foil pigments, and rust-proof pigments, or ultraviolet light absorbers such as hindered amine, benzotriazole, and benzophenone, or antioxidants such as hindered phenol, phosphorus, sulfur, and hydrazide, or coupling agents such as silane and titanium, or mold release agents such as stearic acid, palmitic acid, zinc stearate, and calcium stearate, leveling agents, rheology control agents, pigment dispersants, shrinkage inhibitors, and defoaming agents, etc. The amount of these other additives is preferably in the range of 0.01% by mass to 20% by mass relative to the solid content (non-volatile content) in the epoxy resin composition. In addition, an organic solvent or a reactive diluent may be used for adjusting the viscosity.
[0189] Examples of the organic solvent include amides such as N,N-dimethylformamide and N,N-dimethylacetamide, ethers such as ethylene glycol monomethyl ether, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone, alcohols such as methanol, ethanol, 1-methoxy-2-propanol, benzyl alcohol, butyl diethylene glycol, and pine oil, acetates such as butyl acetate, cellosolve acetate, ethyl diethylene glycol acetate, propylene glycol monomethyl ether acetate, and carbitol acetate, carbitols such as cellosolve and butyl carbitol, aromatic hydrocarbons such as benzene, toluene, and xylene, dimethyl sulfoxide, acetonitrile, and N-methylpyrrolidone, but are not limited to these.
[0190] Examples of the reactive diluent include monofunctional glycidyl ethers such as allyl glycidyl ether, 2-ethylhexyl glycidyl ether, and phenyl glycidyl ether; difunctional glycidyl ethers such as resorcinol glycidyl ether, neopentyl glycol glycidyl ether, and 1,6-hexanediol diglycidyl ether; and polyfunctional glycidyl ethers such as glycerol polyglycidyl ether, trimethylolpropane polyglycidyl ether, and pentaerythritol polyglycidyl ether, but are not limited thereto.
[0191] These solvents or reactive diluents are preferably used alone or mixed with a plurality of non-volatile components of 90% by mass or less, and the appropriate type or amount used can be appropriately selected according to the application. For example, in the use of printed wiring boards, polar solvents having a boiling point of 160°C or less such as methyl ethyl ketone, acetone, 1-methoxy-2-propanol are preferably used, and the amount used is preferably 40% to 80% by mass based on the non-volatile component. In addition, in the use of adhesive films, for example, ketones, acetates, carbitols, aromatic hydrocarbons, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc. are preferably used, and the amount used is preferably 30% to 60% by mass based on the non-volatile component.
[0192] The curable epoxy resin composition of the present invention can be cured by the same method as the known epoxy resin composition to obtain the cured product of the present invention. As a method for obtaining the cured product, the same method as the known epoxy resin composition can be used, and casting, injection, perfusion, dipping, drip coating, transfer molding, compression molding, etc. can be appropriately used, or it can be made into a resin sheet, a copper foil with a resin, a prepreg, etc., and then stacked and heated and pressurized to cure, thereby making a laminated board. At this time, the curing temperature is usually in the range of 100°C to 300°C, and the curing time is usually about 10 minutes to 5 hours.
[0193] The curable epoxy resin composition of the present invention can be obtained by uniformly mixing the above-mentioned components. The epoxy resin composition prepared with the epoxy resin, the curing agent, and various additives as needed can be easily made into a cured product by the same method as the conventionally known method. Examples of the cured product include laminates, castings, molded products, adhesive layers, insulating layers, films, and other shaped cured products.
[0194] As the purposes of using curable epoxy resin composition, circuit substrate insulating materials such as printed wiring board material, flexible wiring board resin composition, build-up substrate interlayer insulating materials, semiconductor sealing materials, conductive paste, conductive film, build-up adhesive film, resin casting material, adhesive, etc. can be listed. In these various uses, printed wiring board material, circuit substrate insulating material, build-up adhesive film purposes, can be used as passive parts such as capacitors or active parts such as integrated circuits (integrated circuit, IC) chips embedded in the substrate so-called electronic parts built-in substrate insulating materials. In these uses, with regard to the characteristics such as high flame retardancy, high heat resistance, low dielectric properties and solvent solubility, it is preferably used for printed wiring board material, flexible wiring board resin composition, build-up substrate interlayer insulating materials and circuit substrate (laminated board) materials and semiconductor sealing materials.
[0195] When the curable epoxy resin composition is formed into a plate such as a laminate, the filler used is preferably a fibrous filler in terms of dimensional stability, bending strength, etc., and more preferably a glass cloth obtained by weaving glass fibers into a mesh.
[0196] By impregnating a curable epoxy resin composition in a fibrous reinforcing substrate, the prepreg of the present invention used in a printed wiring board, etc. can be made. As a fibrous reinforcing substrate, inorganic fibers such as glass, or woven or non-woven fabrics of organic fibers such as polyester resins, polyamine resins, polyacrylic resins, polyimide resins, and aromatic polyamide resins can be used, but it is not limited thereto. As a method for manufacturing a prepreg from an epoxy resin composition, there is no particular limitation, for example, it can be obtained by the following method: a varnish-like epoxy resin composition containing the organic solvent is made into a resin varnish adjusted to an appropriate viscosity by blending an organic solvent, and after the resin varnish is impregnated in the fibrous substrate, it is heated and dried to semi-harden the resin component (B stage). As a heating temperature, it is preferably 50°C to 200°C, and more preferably 100°C to 170°C, depending on the type of organic solvent used. The heating time is adjusted according to the type of organic solvent used or the curability of the prepreg, preferably 1 minute to 40 minutes, and more preferably 3 minutes to 20 minutes. At this time, the mass ratio of the epoxy resin composition to the reinforcing substrate used is not particularly limited, but is usually preferably adjusted so that the resin component in the prepreg is 20% by mass to 80% by mass.
[0197] The curable epoxy resin composition of the present invention can be formed into a sheet or film and used. In the case described, it is possible to use a known method to form a sheet or film. As a method for manufacturing an adhesive sheet, it is not particularly limited, for example, it can be obtained in the following manner: on a supporting base film that is not dissolved in the resin varnish, a coating machine such as a reverse roll coater, a notch wheel coater, a die coater, etc. is used to apply the resin varnish, and then heat and dry to make the resin component B staged. In addition, other supporting base films are overlapped as protective films on the coating surface (adhesive layer) as needed, and dried to obtain an adhesive sheet with a peeling layer on both sides of the adhesive layer. As a supporting base film, metal foils such as copper foil, polyolefin films such as polyethylene films and polypropylene films, polyester films such as polyethylene terephthalate films, polycarbonate films, silicone films, polyimide films, etc., are listed, and these supporting base films are preferably polyethylene terephthalate films with excellent dimensional accuracy and excellent cost without defects such as broken. In addition, it is preferred that the metal foil, especially the copper foil, which is easy to multilayer the laminated board is used. The thickness of the supporting base film is not particularly limited, and it is preferably 10μm to 150μm, and more preferably 25μm to 50μm, in terms of having strength as a support and being difficult to produce poor lamination. The thickness of the protective film is not particularly limited, and is usually 5μm to 50μm. Furthermore, in order to easily peel off the formed adhesive sheet, it is preferably surface treated with a release agent in advance. In addition, the thickness of the coated resin varnish is preferably 5μm to 200μm, and more preferably 5μm to 100μm, based on the thickness after drying. As the heating temperature, it is preferably 50°C to 200°C, and more preferably 100°C to 170°C, depending on the type of organic solvent used. The heating time is adjusted according to the type of organic solvent used or the curability of the prepreg, and is preferably 1 minute to 40 minutes, and more preferably 3 minutes to 20 minutes. The adhesive sheet obtained in the above manner is usually an insulating adhesive sheet with insulating properties, but a conductive adhesive sheet can also be obtained by mixing a conductive metal or metal-coated microparticles in an epoxy resin composition. Furthermore, the supporting base film is peeled off after being laminated on a circuit substrate or after being heat-cured to form an insulating layer. If the supporting base film is peeled off after the adhesive sheet is heat-cured, dust can be prevented from being attached during the curing step. Here, the insulating adhesive sheet is also an insulating sheet of the present invention.
[0198] The method for manufacturing the laminate of the present invention using the prepreg or insulating adhesive sheet of the present invention is described. For example, in the case of forming a laminate using a prepreg, one or more prepregs are stacked, and a metal foil is arranged on one side or both sides to form a laminate, and the laminate is pressurized and heated, thereby hardening and integrating the prepreg to obtain a laminate. Here, as a metal foil, copper, aluminum, brass, nickel, etc., can be used alone, alloy, or composite metal foil. As a condition for heating and pressurizing the laminate, it is sufficient to heat and pressurize as long as it is appropriately adjusted under the condition that the epoxy resin composition is cured, but if the pressure of the pressurization is too low, there are residual bubbles inside the laminate obtained, and the electrical properties are reduced. Therefore, it is ideal to pressurize under conditions that meet the moldability. The heating temperature is preferably 160°C to 250°C, and more preferably 170°C to 220°C. The pressurization pressure is preferably 0.5MPa to 10MPa, and more preferably 1MPa to 5MPa. The heating and pressing time is preferably 10 minutes to 4 hours, more preferably 40 minutes to 3 hours. Furthermore, the single-layer laminate obtained in the above manner can be used as an inner layer material to make a multilayer board. In the above case, the laminate is firstly subjected to circuit formation by an additive method or a subtractive method, and the surface of the formed circuit is treated with an acid solution to perform a blackening treatment to obtain an inner layer material. On the circuit forming surface of one side or both sides of the inner layer material, an insulating layer is formed by using a prepreg or an insulating adhesive sheet, and a conductor layer is formed on the surface of the insulating layer to form a multilayer board.
[0199] When an insulating layer is formed by using an insulating adhesive sheet, an insulating adhesive sheet is arranged on the circuit forming surface of multiple inner layer materials to form a laminate. Alternatively, an insulating adhesive sheet is arranged between the circuit forming surface of the inner layer material and the metal foil to form a laminate. Then, the laminate is heated and pressurized to be integrally formed, thereby forming a hardened insulating adhesive sheet as an insulating layer, and forming a multilayer of the inner layer material. Alternatively, a hardened insulating adhesive sheet is formed between the inner layer material and the metal foil as a conductor layer as an insulating layer. Here, as the metal foil, the same metal foil used in the laminate used as the inner layer material can be used. In addition, the heating and pressurizing molding can be carried out under the same conditions as the molding of the inner layer material.
[0200] In addition, when the insulating layer is formed using the prepreg, one or more prepregs are arranged on the circuit forming surface of the inner layer material, and a metal foil is arranged on its outer side to form a laminate. Then, the laminate is heated and pressurized to be integrally formed, thereby forming a hardened material of the prepreg as an insulating layer, and forming a metal foil on its outer side as a conductor layer. Here, as the metal foil, the same metal foil used in the laminate used as the inner layer material can be used. In addition, the heating and pressing molding can be carried out under the same conditions as the molding of the inner layer material. On the surface of the multilayer laminate formed in the manner described, the formation of the via or the formation of the circuit is implemented by the additive method or the subtractive method, and a printed wiring board can be molded. In addition, the printed wiring board is used as the inner layer material, and the method is repeatedly performed, thereby further forming a multilayer multilayer board.
[0201] In addition, when a curable epoxy resin composition is applied to a laminate to form an insulating layer, the curable epoxy resin composition is applied to a thickness of preferably 5 μm to 100 μm, and then heated and dried at 100°C to 200°C, preferably 150°C to 200°C, for 1 minute to 120 minutes, preferably 30 minutes to 90 minutes to form a sheet. It is usually formed by a method called casting. It is ideal to form the thickness after drying to 5 μm to 150 μm, preferably 5 μm to 80 μm. Furthermore, in order to obtain sufficient film thickness and to prevent uneven coating or stripes, the viscosity of the curable epoxy resin composition is preferably in the range of 10 mPa·s to 40000 mPa·s at 25°C, and more preferably 200 mPa·s to 30000 mPa·s. On the surface of the multilayer laminate formed in the above manner, the formation of vias or the formation of circuits is further implemented by an additive method or a subtractive method to form a printed wiring board. Furthermore, by using the printed wiring board as an inner layer material and repeating the above-mentioned process, a multi-layer laminate can be formed.
[0202] The sealing material obtained by using the curable epoxy resin composition of the present invention includes tape-shaped semiconductor chips, potting liquid seals, bottom filling, semiconductor interlayer insulation films, etc., and can be appropriately used in these. For example, as semiconductor package molding, there can be cited: casting the epoxy resin composition, or molding the epoxy resin composition using a transfer molding machine, an injection molding machine, etc., and then heating it at 50°C to 200°C for 2 hours to 10 hours to obtain a molded product.
[0203] In order to prepare the curable epoxy resin composition as a semiconductor sealing material, it can be cited that the curable epoxy resin composition is pre-mixed with inorganic fillers and other formulations as needed, or additives such as coupling agents and release agents, and then fully melt-mixed using an extruder, a kneader, a roller, etc. until it becomes uniform. At this time, as an inorganic filler, silica is generally used. In the case, it is preferred to prepare an inorganic filler in a ratio of 70% to 95% by mass in the curable epoxy resin composition. In the case where the curable epoxy resin composition obtained in the manner is used as a tape-shaped sealing material, it can be cited that it is heated to make a semi-cured sheet, and after the sealing tape is made, the sealing tape is placed on a semiconductor chip, heated to 100°C to 150°C to soften it and form it, and it is completely cured at 170°C to 250°C. In addition, when used as a pouring type liquid sealing material, the obtained curable epoxy resin composition is dissolved in a solvent as needed, applied to a semiconductor chip or an electronic component, and it can be directly cured.
[0204] In addition, the curable epoxy resin composition of the present invention can also be used as a resist ink. In this case, a method can be cited in which a vinyl monomer having an ethylenically unsaturated double bond and a cationic polymerization catalyst as a curing agent are mixed in the epoxy resin composition, and then a pigment, talc and a filler are added to prepare a resist ink composition, and then the composition is applied to a printed substrate by screen printing to prepare a cured resist ink. The curing temperature at this time is preferably in the temperature range of about 20°C to 250°C.
[0205] [Example]
[0206] The present invention is described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples. Unless otherwise specified, "part" means part by mass, and "%" means mass %. The measurement method was measured according to the following method.
[0207] The unit of equivalent is g / eq.
[0208] · Epoxy equivalent: in accordance with Japanese Industrial Standards (JIS) K7236.
[0209] Solvent solubility: The state when diluted with methyl ethyl ketone to 50% of the nonvolatile content was visually determined. The case of complete dissolution and transparency was rated as ○, the case of white turbidity or separation was rated as ×, and the case of slight turbidity was rated as △.
[0210] Copper foil peel strength and interlayer adhesive force: The test was conducted in accordance with JIS C6481. The interlayer adhesive force was measured by peeling between the seventh layer and the eighth layer.
[0211] Glass transition temperature: expressed by DSC·Tgm (the middle temperature of the variation curve with respect to the tangent line between the glass state and the rubber state) measured at a temperature increase of 20°C / min using a differential scanning calorimeter (manufactured by Hitachi High-Technologies Co., Ltd., EXSTAR6000 DSC6200) in accordance with IPC-TM-650 2.4.25.c.
[0212] Relative dielectric constant and dielectric loss tangent: According to IPC-TM-650 2.5.5.9, the dielectric constant and dielectric loss tangent at a frequency of 1 GHz were obtained by a capacitance method using a material analyzer (manufactured by AGILENT Technologies) and evaluated.
[0213] ·GPC and molecular weight: A device including a column (TSKgel G4000HXL, TSKgel G3000HXL, TSKgel G2000HXL, manufactured by Tosoh Corporation) in series in a body (HLC-8220GPC manufactured by Tosoh Corporation) was used, and the column temperature was set to 40°C. In addition, tetrahydrofuran was used as an eluent, and the flow rate was set to 1 mL / min, and an RI (differential refractometer) detector was used as a detector. The weight average molecular weight converted based on the calibration curve obtained from standard monodisperse polystyrene (A-500, A-1000, A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40, F-80, F-128 manufactured by Tosoh Corporation) was used for data processing. GPC-8020 Model II Version 4.10 manufactured by Tosoh Corporation was used. As the measurement sample, 0.1 g of the sample was dissolved in 10 mL of tetrahydrofuran (THF), and the solution was filtered using 100 μL of a microfilter.
[0214] IR: measured at a wave number of 650 cm using a Fourier transform infrared spectrophotometer (PerkinElmer Precisely manufactured, Spectrum One FT-IR Spectrometer 1760X) using the attenuated total reflection method (ATR (Attenuated Total Reflection) method). -1 ~4000cm -1 The absorbance.
[0215] Synthesis example 1
[0216] In a glass separable flask, 100 parts of 4,4'-thiobis(6-tert-butyl-3-methylphenol) (TBBC, hydroxyl equivalent 179), 310 parts of epichlorohydrin, and 3 parts of ion exchange water were placed, and the temperature was raised to 50°C while stirring. After uniform dissolution, 4.6 parts of 49% sodium hydroxide aqueous solution were added and reacted for 3 hours. Secondly, after heating to 64°C, the pressure was reduced to the extent that water reflux was produced, and 41 parts of 49% sodium hydroxide aqueous solution were added dropwise for 3 hours. During the addition, the refluxed distilled water and epichlorohydrin were separated by a separation tank, and the epichlorohydrin was returned to the reaction container, and the water was removed from the system to react. After the reaction was completed, the temperature was raised to 70°C for dehydration, and the temperature was set to 135°C to recover the remaining epichlorohydrin. The pressure was restored to normal pressure, and 197 parts of toluene were added for dissolution. 109 parts of ion exchange water were added, stirred and allowed to stand to dissolve the by-produced salt in the water and remove it. Next, 5.8 parts of 49% sodium hydroxide aqueous solution were added, and the reaction was stirred at 80°C for 90 minutes to perform a purification reaction. Methyl isobutyl ketone (MIBK) was added, and the ionic impurities were removed by washing several times. The solvent was recovered to obtain the epoxy resin (a-1) in which W of the formula (3) was represented by the following formula (8). The epoxy equivalent of the obtained epoxy resin (a-1) was 245, and m was 0.04.
[0217] [Chemistry 11]
[0218]
[0219] Synthesis example 2
[0220] The same operation was performed using the same apparatus as in Synthesis Example 1 except that 100 parts of TBBC in Synthesis Example 1 was replaced with 105 parts of 4,4'-(tetrahydrodicyclopentadienediyl)bis(2,6-dimethylphenol) (hydroxyl equivalent 188), thereby obtaining an epoxy resin (a-2) in which W of the formula (3) is represented by the following formula (9). The epoxy equivalent of the obtained epoxy resin (a-2) was 261, and m was 0.07.
[0221] [Chemistry 12]
[0222]
[0223] Synthesis example 3
[0224] Except that 100 parts of TBBC in Synthesis Example 1 were replaced with 85 parts of 2,2',6,6'-tetramethyl-4,4'-sulfonyldiphenol (hydroxyl equivalent 153), the same operation was performed using the same apparatus as Synthesis Example 1 to obtain an epoxy resin (a-3) in which W of the formula (3) is represented by the following formula (10). The epoxy equivalent of the obtained epoxy resin (a-3) was 230, and m was 0.11.
[0225] [Chemistry 13]
[0226]
[0227] Comparative Synthesis Example 1
[0228] Except that 100 parts of TBBC in Synthesis Example 1 were replaced with 87 parts of 4,4'-(3,3,5-trimethylcyclohexylene)diphenol (BisP-TMC, manufactured by Honshu Chemical Industry Co., Ltd., hydroxyl equivalent 155), the same operation was performed using the same apparatus as Synthesis Example 1 to obtain an epoxy resin (a-5) in which W of the formula (3) is represented by the following formula (12). The epoxy equivalent of the obtained epoxy resin (a-5) is 219, and m is 0.04.
[0229] [Chemistry 14]
[0230]
[0231] The explanations of the abbreviations used in the Examples and Comparative Examples are as follows.
[0232] [Epoxy resin]
[0233] (a-1): Epoxy resin obtained in Synthesis Example 1
[0234] (a-2): Epoxy resin obtained in Synthesis Example 2
[0235] (a-3): Epoxy resin obtained in Synthesis Example 3
[0236] (a-4): Bisphenol A type liquid epoxy resin (manufactured by Nippon Steel Chemical Materials Co., Ltd., Epotohto YD-128, epoxy equivalent 186, m=0.11)
[0237] (a-5): Epoxy resin obtained in Comparative Synthesis Example 1
[0238] [Isocyanate]
[0239] (b-1): diphenylmethane diisocyanate (manufactured by Mitsui Chemicals, Cosmonate PH, NCO concentration 34%)
[0240] (b-2): A mixture of 2,4-toluene diisocyanate (80%) and 2,6-toluene diisocyanate (20%) (manufactured by Mitsui Chemicals, Cosmonate T-80, NO concentration 48%)
[0241] [catalyst]
[0242] TBAB: Tetrabutylammonium Bromide (manufactured by Tokyo Chemical Industry Co., Ltd., reagent)
[0243] [Hardener]
[0244] (d-1): Phenol novolac resin (manufactured by AICA Industrial Co., Ltd., Shonol BRG-557, softening point 80°C, phenolic hydroxyl equivalent 105)
[0245] [Hardening accelerator]
[0246] 2E4MZ: 2-ethyl-4-methylimidazole (produced by Shikoku Chemical Industry Co., Ltd., Curezol 2E4MZ)
[0247] Example 1
[0248] In the same apparatus as in Synthesis Example 1, 100 parts of (a-1) as an epoxy resin and 0.06 parts of TBAB as a catalyst were placed, and the temperature was raised while nitrogen was added. The temperature was maintained at 120°C for 30 minutes to remove the moisture in the system, and it was confirmed that the moisture content in the raw materials in the system was 0.1% or less. Next, 30 parts of xylene were added, and while the reaction temperature was maintained at 130°C to 140°C, 15.3 parts of (b-1) as an isocyanate compound (the molar ratio of the isocyanate group of the isocyanate compound (b) to 1 mol of the epoxy group of the epoxy resin (a) [(b) / (a)] = 0.40) was heated to 60°C and added dropwise over 3 hours. After the addition was completed, the same temperature was maintained while stirring was continued for 180 minutes to obtain an epoxy resin (resin 1) containing an oxazolidone ring. The results of measuring the epoxy equivalent, softening point, solvent solubility, and absorbance ratio of the obtained oxazolidone ring-containing epoxy resin are shown in Table 1. Figure 1 The GPC diagram is shown in Figure 2 The IR diagram is shown in FIG.
[0249] Furthermore, the resin 1 was fractionated by GPC to remove the raw material epoxy resin (a-1) to obtain an oxazolidone ring-containing epoxy resin (resin 1D). Table 2 shows the results of measuring the epoxy equivalent and molecular weight of the resin 1D.
[0250] exist Figure 1 Among them, the component corresponding to the oxazolidone ring-containing epoxy resin 1D is the peak group (a), the remaining raw material epoxy resin (a-1) is the peak (c), and the n=1 component of the oxazolidone ring-containing epoxy resin 1D represented by formula (2) is the peak (b).
[0251] Example 2 to Example 5, Comparative Example 1 to Comparative Example 2
[0252] According to the charge amount (parts) of each raw material shown in Table 1, the same method as in Example 1 was used to synthesize an epoxy resin containing an oxazolidone ring. In addition, the reaction temperature was maintained in the temperature range of ±5°C of the reaction temperature shown in Table 1, and the reaction solvent used was the type shown in Table 1 in the required number of parts. The isocyanate compound was added dropwise at the addition time shown in Table 1. The epoxy equivalent and solvent solubility of the obtained epoxy resin containing an oxazolidone ring were measured in the same manner as in Example 1, and the results are shown in Table 1.
[0253] The oxazolidone ring-containing epoxy resin obtained in Example 1 is referred to as Resin 1, and the same is hereinafter referred to as Resins 2 to 5. The oxazolidone ring-containing epoxy resin obtained in Comparative Example 1 is referred to as Resin H1, and the same is hereinafter referred to as Resin H2.
[0254] [Table 1]
[0255]
[0256] Furthermore, similarly to Example 1, each of the obtained resins 2 to 5, resin H1, and resin H2 was fractionated by GPC, and the raw material epoxy resins (a-1) to (a-5) were removed to obtain epoxy resins containing oxazolidone rings (resins 2D to 5D, resin H1D, and resin H2D). The results of measuring the epoxy equivalent and molecular weight of each of the obtained resins are shown in Table 2. The solvent solubility is the same as that in Table 1.
[0257] [Table 2]
[0258]
[0259] Example 6
[0260] 100 parts of Resin 1 as an epoxy resin, 23.8 parts of (d-1) as a hardener, and 0.16 parts of 2E4MZ as a hardening accelerator were prepared and dissolved in a mixed solvent prepared from methyl ethyl ketone (MEK) and propylene glycol monomethyl ether to obtain an epoxy resin composition varnish.
[0261] The obtained epoxy resin composition varnish was impregnated into glass cloth (WEA2116, 0.1 mm thick, manufactured by Nitto Bosei Co., Ltd.). The impregnated glass cloth a was dried in a hot air circulation oven at 150°C for 10 minutes to obtain a prepreg. 8 pieces of the obtained prepreg were overlapped with copper foil (3EC-III, 35 μm thick, manufactured by Mitsui Mining and Smelting Co., Ltd.) on top and bottom, and vacuum pressed at 2 MPa under the temperature conditions of 130°C × 15 minutes + 190°C × 80 minutes to obtain a 1 mm thick laminate. The measurement results of the glass transition temperature (Tg) of the laminate, the copper foil peel strength and the interlayer adhesion are shown in Table 3.
[0262] In addition, the obtained prepreg was untied and made into a powdered prepreg powder that passed 100 meshes using a sieve. The obtained prepreg powder was placed in a fluororesin mold and vacuum pressed at 2MPa under the temperature conditions of 130°C×15 minutes+190°C×80 minutes to obtain a 50mm square×2mm thick test piece. The results of the relative dielectric constant and dielectric loss tangent of the test piece are shown in Table 3.
[0263] Embodiment 7 to Embodiment 10
[0264] The epoxy resin composition varnish was obtained in the same manner as in Example 6 by mixing the formulation amounts (parts) of Table 3, and a laminate and a test piece were obtained. The same test as in Example 6 was performed, and the results are shown in Table 3.
[0265] Comparative Example 3 to Comparative Example 4
[0266] The epoxy resin composition varnish was obtained by mixing the mixture in the amount (parts) of the formula in Table 3, and then a laminate and a test piece were obtained in the same manner as in Example 6. The same test as in Example 6 was performed, and the results are shown in Table 3. Among them, when the prepreg was prepared in Comparative Example 4 using the resin H2, the prepreg could not be formed due to poor impregnation, so the test was not performed. "×" in the table means that the test was not performed.
[0267] [Table 3]
[0268]
[0269] [Industrial Applicability]
[0270] The epoxy resin composition using the oxazolidone ring-containing epoxy resin of the present invention and its cured product are excellent in heat resistance, adhesion and dielectric properties, and can be used as an epoxy resin composition for various high-functional material applications such as epoxy resin cured products, prepregs, insulating sheets, adhesive sheets, laminates, sealing materials, and casting materials. It can also be used as an epoxy resin composition for various high-functional material applications such as electronic circuit board materials that meet the recent demand for high functionality.
Claims
1. An epoxy resin containing an oxazolidinone ring, characterized in that: The compound has at least one divalent group represented by the following formula (a) and at least one oxazolidinone ring structure in one molecule, and has a weight average molecular weight of 1,000 to 20,000 as measured by gel permeation chromatography; In the formula, X represents any one of -C(CF3)2-, -S-, -SS-, -SO2-, -O-, -CH2-O-CH2-, tetrahydrodicyclopentadienediyl or tetrahydrotricyclopentadienediyl; R 1 Each independently represents a hydrocarbon group having 1 to 11 carbon atoms or a hydrocarbonoxy group having 1 to 11 carbon atoms, and R 2 Each independently represents a hydrogen atom, a hydrocarbon group having 1 to 11 carbon atoms, or a hydrocarbonoxy group having 1 to 11 carbon atoms; furthermore, when X is a group having a benzene ring, the benzene ring may have a 1 Same substituents.
2. The epoxy resin containing an oxazolidinone ring according to claim 1, which has a structure represented by the following formula (1); In the formula, W represents a divalent group represented by the above formula (a), and Y represents a residue obtained by removing two isocyanate groups from a polyisocyanate compound.
3. The oxazolidinone ring-containing epoxy resin according to claim 1 or 2, which has a structure represented by the following formula (2); In the formula, Z represents a divalent group, 5 mol% to 100 mol% of Z is the divalent group represented by the formula (a); Y represents a residue obtained by removing an isocyanate group from a diisocyanate compound; G represents a glycidyl group; and n represents the number of repetitions, with an average value of 1 to 5.
4. An oxazolidone ring-containing epoxy resin, comprising 5% to 55% by mass of the oxazolidone ring-containing epoxy resin according to any one of claims 1 to 3; and an epoxy resin having a divalent group represented by the formula (a) and not containing an oxazolidone ring.
5. An epoxy resin containing an oxazolidinone ring, characterized in that: Obtained from an epoxy resin (a) containing 50% by mass or more of an epoxy resin (a1) represented by the following formula (3) and an isocyanate compound (b), and having an epoxy equivalent of 200 g / eq. to 1600 g / eq.; In the formula, W represents a divalent group represented by the following formula (a), G represents a glycidyl group; m represents the number of repetitions, the average value of which is 0 to 5. In the formula, X represents any one of -C(CF3)2-, -S-, -SS-, -SO2-, -O-, -CH2-O-CH2-, tetrahydrodicyclopentadienediyl or tetrahydrotricyclopentadienediyl; R 1 Each independently represents a hydrocarbon group having 1 to 11 carbon atoms or a hydrocarbonoxy group having 1 to 11 carbon atoms, and R 2 Each independently represents a hydrogen atom, a hydrocarbon group having 1 to 11 carbon atoms, or a hydrocarbonoxy group having 1 to 11 carbon atoms; furthermore, when X has a benzene ring, the benzene ring may have a 1 Same substituents.
6. A method for producing an epoxy resin containing an oxazolidinone ring, characterized in that: An epoxy resin (a) containing 50% by mass or more of an epoxy resin (a1) represented by the following formula (3) is reacted with an isocyanate compound (b) in the presence of a catalyst at a reaction temperature in the range of 100° C. to 250° C.; In the formula, W represents a divalent group represented by the following formula (a), G represents a glycidyl group; m represents the number of repetitions, the average value of which is 0 to 5. In the formula, X represents any one of -C(CF3)2-, -S-, -SS-, -SO2-, -O-, -CH2-O-CH2-, tetrahydrodicyclopentadienediyl or tetrahydrotricyclopentadienediyl; R 1 Each independently represents a hydrocarbon group having 1 to 11 carbon atoms or a hydrocarbonoxy group having 1 to 11 carbon atoms, and R 2 Each independently represents a hydrogen atom, a hydrocarbon group having 1 to 11 carbon atoms, or a hydrocarbonoxy group having 1 to 11 carbon atoms; furthermore, when X has a benzene ring, the benzene ring may have a 1 Same substituents.
7. The method for producing an epoxy resin containing an oxazolidinone ring according to claim 6, wherein: The isocyanate group of the isocyanate compound (b) is used in an amount within a range of 0.02 mol or more and less than 0.7 mol per 1 mol of the epoxy group of the epoxy resin (a).
8. The method for producing an oxazolidinone ring-containing epoxy resin according to claim 6 or 7, wherein: The epoxy equivalent of the epoxy resin (a) is 180 g / eq. to 400 g / eq.
9. A curable epoxy resin composition, characterized in that: A method comprising: comprising an epoxy resin containing an oxazolidinone ring as claimed in any one of claims 1 to 5 and a hardener.
10. The curable epoxy resin composition according to claim 9, wherein The active hydrogen groups of the curing agent are 0.2 mol to 1.5 mol per 1 mol of epoxy groups of all epoxy resins in the epoxy resin composition.
11. A prepreg, characterized in that: The curable epoxy resin composition according to claim 9 or 10 is used.
12. An insulating sheet, characterized in that: The curable epoxy resin composition according to claim 9 or 10 is used.
13. A laminated plate, characterized in that: The curable epoxy resin composition according to claim 9 or 10 is used.
14. A cured product obtained by curing the curable epoxy resin composition according to claim 9 or 10.