Semiconductor device manufacturing method

By using a buffer material sheet with a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa in the sintering and bonding process, the problem of unbonding of the sintering layer is solved, and uniformity and reliability of the sintering layer are achieved.

CN112041972BActive Publication Date: 2024-11-19NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980028570.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-04-27
Filing Date
2019-03-27
Publication Date
2024-11-19
Estimated Expiration
2039-03-27

AI Technical Summary

Technical Problem

In the sintering and bonding process, the periphery of the sintered layer of the plurality of semiconductor chips cannot be effectively bonded to the substrate, resulting in poor bonding problems, mainly due to inaccurate parallelism and attitude control of the parallel plates, resulting in uneven loads.

Method used

The buffer material sheet with a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa overlaps the sintered joint workpiece and is clamped in a heating press to absorb load differences and reduce the deviation and inclination of the parallel plates to ensure sintering. uniformity of the layer.

Benefits of technology

Through the use of the buffer material sheet, high uniformity of pressure and load in the sintering and joining process is achieved, failure of bonding is avoided, and the reliability and firmness of the sintered layer are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112041972B_ABST
    Figure CN112041972B_ABST
Patent Text Reader

Abstract

The semiconductor device manufacturing method includes a preparation step and a sintering and bonding step. In the preparation step, a sintering and bonding workpiece (X) having a stacked structure is prepared, wherein the stacked structure includes: a substrate (S), a plurality of semiconductor chips (C) arranged on one side thereof and to be bonded, and a plurality of sintering and bonding material layers (11) containing sinterable particles respectively sandwiched between each semiconductor chip (C) and the substrate (S). In the sintering and bonding step, a buffer material sheet (20) having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa is overlapped with the sintering and bonding workpiece (X) and clamped between a pair of pressurizing surfaces (Pa, Pa), and the sintering and bonding workpiece (X) is pressurized along its stacking direction between the pressurizing surfaces (Pa, Pa) and subjected to a heating process, thereby forming a sintered layer (12) from each sintering and bonding material layer (11). This semiconductor device manufacturing method is suitable for sintering and bonding a plurality of semiconductor chips to a substrate at a time under pressurized conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a semiconductor device, such as a so-called power semiconductor device. Background Art

[0002] In the manufacture of semiconductor devices, the following methods are known as methods for electrically connecting a semiconductor chip to the substrate side and bonding the chip to a substrate such as a lead frame or an insulating circuit substrate: a method of forming an Au-Si eutectic alloy layer between the substrate and the chip to achieve a bonding state; and a method of using solder or a resin containing conductive particles as bonding materials.

[0003] On the other hand, in recent years, the popularity of power semiconductor devices that are responsible for controlling the supply of electric power has increased significantly. In power semiconductor devices, in most cases, a large amount of heat is released due to the large amount of current flowing during operation. Therefore, in the manufacture of power semiconductor devices, a technique for bonding the chip to the substrate while allowing the semiconductor chip to be electrically connected to the substrate side requires a highly reliable bonding state even during high-temperature operation. Such a requirement is particularly strong in power semiconductor devices that use SiC and GaN as semiconductor materials to achieve high-temperature operation. In addition, in order to meet such requirements, a technology using a sintering bonding composition containing sinterable particles and a solvent has been proposed as a chip bonding technique accompanied by electrical connection.

[0004] In chip bonding using a sintering bonding material containing sinterable particles, first, a semiconductor chip is placed under specified temperature / load conditions relative to a predetermined chip bonding position of a substrate with the aid of a sintering bonding material. Afterwards, a sintering process is performed under specified temperature / pressure conditions in a manner such that the solvent in the sintering bonding material evaporates between the substrate and the semiconductor chip thereon and sintering is performed between the sinterable particles. Thus, a sintering layer is formed between the substrate and the semiconductor chip, the semiconductor chip is electrically connected to the substrate, and mechanical bonding is performed. Such a technology is described in, for example, the following patent documents 1 and 2.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2008 / 065728

[0008] Patent Document 2: Japanese Patent Application Publication No. 2013-039580 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] In the sintering bonding process in the semiconductor device manufacturing process in which the chip is bonded by sintering bonding, a heating and pressing machine with a pair of parallel plates for heating and pressurizing is sometimes used. In this process, specifically, the substrate and the semiconductor chip temporarily fixed by the sintering bonding material layer, that is, the workpiece is sandwiched between a pair of parallel plates open toward the stacking direction of the substrate and the semiconductor chip, and the pair of parallel plates are used to pressurize and heat. Through this process, a sintering layer is formed by the sintering bonding material layer, and the semiconductor chip is sintered and bonded to the substrate.

[0011] In addition, in the sintering bonding process in the semiconductor device manufacturing process in which chip bonding is performed by sintering bonding, sometimes multiple semiconductor chips are sintered and bonded to the substrate at the same time. However, when the sintering bonding process is performed at the same time using the above-mentioned heating and pressing machine, it is sometimes observed that the peripheral portion of the multiple sintered layers formed is not bonded to the substrate or the semiconductor chip. It can be considered that the reason for this poor bonding is that the load acting on the workpiece clamped between the parallel plates in the sintering bonding process is uneven between multiple sintering bonding material layers. The thickness of the semiconductor chip and the sintering bonding material layer in the workpiece is as small as a few μm to hundreds of μm. In the sintering bonding process performed using a heating and pressing machine equipped with a pair of parallel plates, the deviation and / or tilt of the parallel plates from the ideal parallel posture easily leads to load differences for each semiconductor chip and / or sintering bonding material layer. It can be considered that when the parallelism of the parallel plates and the accuracy of the posture control do not meet the thinness of the semiconductor chip and the sintering bonding material layer, the above-mentioned poor bonding is likely to occur.

[0012] The present invention has been conceived based on the above-mentioned situation, and an object of the present invention is to provide a method suitable for collectively sintering and bonding a plurality of semiconductor chips to a substrate in a semiconductor device manufacturing method that undergoes a sintering and bonding step of semiconductor chips under pressure.

[0013] Solutions for solving problems

[0014] The semiconductor device manufacturing method provided by the present invention includes the following preparation step and sintering and bonding step. This method is suitable for manufacturing a semiconductor device such as a power semiconductor device having a sintered bonding portion of a semiconductor chip.

[0015] In the preparation step, a sintered bonding workpiece is prepared. The sintered bonding workpiece includes: a substrate having a first surface and a second surface opposite thereto, a plurality of semiconductor chips arranged on the first surface side and to be bonded, and a plurality of sintered bonding material layers containing sinterable particles respectively sandwiched between each semiconductor chip and the substrate. For example, a sintered bonding workpiece can be prepared by crimping and temporarily fixing a semiconductor chip with a sintered bonding material layer relative to a substrate with the aid of its sintered bonding material layer. As a supply material for the sintered bonding material layer, a sheet body (sintered bonding sheet) of a composition that simultaneously contains sinterable particles and a thermally decomposable polymer binder can be used.

[0016] In the sintering and bonding process, a buffer material sheet is used, and each semiconductor chip is sintered and bonded to the substrate in the sintering and bonding workpiece. The buffer material sheet used has a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa. In the present invention, the tensile modulus of the buffer material sheet is set to a value obtained based on the following measurement, which is a measurement in a tensile test conducted on a buffer material sheet sample with a width of 10 mm × a length of 40 mm × a thickness of 100 μm under the conditions of an initial chuck distance of 10 mm, 23°C and a tensile speed of 50 mm / min. In the sintering and bonding process, the sintering and bonding workpiece is overlapped with the buffer material sheet and clamped between a pair of pressurizing surfaces in a heating and pressing machine, and the sintering and bonding workpiece is pressurized along its stacking direction between the pressurizing surfaces and subjected to a heating process, thereby forming a sintered layer from each sintering and bonding material layer in the workpiece. A pair of pressurizing surfaces is, for example, a pair of opposing surfaces of a pair of parallel plates for heating and pressing. The buffer material sheet overlaps the semiconductor chip arrangement side of the sinter-bonded workpiece or overlaps the second surface side of the substrate. By forming a sintering layer between the substrate and each semiconductor chip, each semiconductor chip is sinter-bonded to the substrate.

[0017] In the present semiconductor device manufacturing method, in its sintering bonding process, as described above, the sintering bonding workpiece is heated while being pressurized in a state where a buffer material sheet having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa overlaps with the sintering bonding workpiece and is clamped between the pressurizing surfaces of the heating press. This configuration is suitable for achieving high uniformity of the pressure and / or load acting on the sintering bonding workpiece clamped between the parallel flat plates in the sintering bonding process between multiple sintering bonding material layers. This is because: in the sintering bonding process, the buffer material sheet having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa and overlapping with the sintering bonding workpiece can play the following buffering function: substantially absorbing and reducing / eliminating the deviation and / or inclination of a pair of pressurizing surfaces from the ideal parallel posture, and substantially absorbing and reducing / eliminating the difference in height between semiconductor chips when there is a difference between the semiconductor chips from the first surface of the substrate to the top surface of the semiconductor chip.

[0018] Furthermore, a cushioning material sheet having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa has sufficient shape retention and is easy to handle in the semiconductor device manufacturing process. Such a cushioning material sheet can be easily and efficiently overlapped with the sinter-bonded workpiece in the above-mentioned sinter-bonding step in an appropriate arrangement.

[0019] As described above, the semiconductor device manufacturing method according to the present invention is suitable for collectively sintering and bonding a plurality of semiconductor chips to a substrate.

[0020] The weight loss rate of the cushioning material sheet used in the above-mentioned sintering and bonding process at 350°C in the weight loss measurement under the conditions of an atmospheric atmosphere, a reference weight temperature of 25°C and a heating rate of 10°C / minute is 0.1% or less. This configuration is suitable for making the cushioning material sheet fully exert its cushioning function in the sintering and bonding process that undergoes a high-temperature heating process. The weight loss rate of the cushioning material sheet can be measured, for example, using a differential thermal-thermogravimetric simultaneous measurement device for a cushioning material sheet sample of about 10 mg.

[0021] In the sintering and bonding process, it is preferred that the heating temperature is 200°C or higher and the pressure is 5 MPa or higher. That is, in the sintering and bonding process, the sintering and bonding workpiece is pressed between a pair of pressurized surfaces along the stacking direction thereof at a pressure of preferably 5 MPa or higher and subjected to a heating process at a temperature of preferably 200°C or higher, thereby forming a sintered layer from the sintering and bonding material layer. This configuration is suitable for forming a strong sintered layer between the substrate to be sintered and each semiconductor chip.

[0022] The sinterable particles in the sinter-bonding material layer preferably include at least one selected from the group consisting of silver particles, copper particles, silver oxide particles, and copper oxide particles. This configuration is suitable for forming a strong sintered layer between the substrate and the semiconductor chip to be sinter-bonded.

[0023] From the viewpoint of achieving highly reliable sintered bonding, the content of the sinterable particles in the sintered bonding material layer is preferably 60 to 99% by mass, more preferably 65 to 98% by mass, and even more preferably 70 to 97% by mass. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Part of the steps in a method for manufacturing a semiconductor device according to one embodiment of the present invention is shown.

[0025] Figure 2 An example of a method for producing a sintered bonded workpiece is shown.

[0026] Figure 3 Show Figure 1 A process subsequent to the process shown.

[0027] Figure 4 Show Figure 3 A process subsequent to the process shown.

[0028] Figure 5 The following shows changes in the use of the cushioning material sheet in the sintering and bonding step.

[0029] Figure 6 The following shows changes in the use of the cushioning material sheet in the sintering and bonding step.

[0030] Figure 7 The following shows changes in the use of the cushioning material sheet in the sintering and bonding step.

[0031] Figure 8 The following shows changes in the use of the cushioning material sheet in the sintering and bonding step. DETAILED DESCRIPTION

[0032] Figure 1 to Figure 4 A semiconductor device manufacturing method according to one embodiment of the present invention is described. The semiconductor device manufacturing method of this embodiment is a method for manufacturing a semiconductor device such as a power semiconductor device having a sintered bonding portion of a semiconductor chip, and includes at least the following preparation steps and sintering steps.

[0033] In the preparation step, the sintering bonding step is performed. Figure 1 The sinter-bonded workpiece X shown in the figure has a laminated structure including a substrate S, a plurality of chips C, and a plurality of sinter-bonding material layers 11 .

[0034] The substrate S has a surface Sa and a surface Sb opposite thereto. Examples of the substrate S include an insulating circuit substrate and a lead frame having copper wiring or the like on the surface. The chip mounting portion of the substrate S may be a base surface of the copper wiring, lead frame, or the like, or a plated film surface formed on the base surface. Examples of the plated film include gold plated film, silver plated film, nickel plated film, palladium plated film, and platinum plated film.

[0035] Each chip C is a semiconductor chip having a device-forming surface on one side where a semiconductor device is formed and a back surface opposite to the device-forming surface. A planar electrode (not shown) serving as an external electrode is formed on the back surface. Figure 1 The lower surface (in the middle) side is temporarily fixed to the surface Sa side of the substrate S by means of a sintering bonding material layer 11. As constituent materials for forming the chip body in the chip C, semiconductor materials for power semiconductor devices such as silicon carbide (SiC) and gallium nitride (GaN) can be cited. In addition, the thickness of the chip C is, for example, 20 to 1000 μm.

[0036] In the present embodiment, each sintering bonding material layer 11 is a layer of a composition containing a binder component and sinterable particles containing a conductive metal, and is interposed between the chip C and the substrate S for each chip C.

[0037] The sintered-bonded workpiece X having the above-described laminated structure can be produced as follows.

[0038] First, if Figure 2 As shown in (a) of FIG. 1 , a plurality of chips C and a sintering bonding sheet 10 are prepared. The plurality of chips C are each provided with a predetermined semiconductor element and fixed on the adhesive surface T1a of the chip fixing tape T1. In each chip C, a surface (on the side where the sintering bonding sheet 10 is to be attached) of the chip is provided. Figure 2 On the other side of each chip C (in the figure, the upper surface) a planar electrode (not shown) is formed as an external electrode. Figure 2 The sheet 10 for sintering and bonding is a sheet body containing at least a binder component and a sinterable particle composition containing a conductive metal, and has a release liner L on one side thereof.

[0039] Then, if Figure 2 As shown in (b), the sintering bonding sheet 10 is pasted to multiple chips C. Specifically, the sintering bonding sheet 10 is pasted to multiple chips C while being pressed from its release liner L side to the chip C side. As a pressing means, a pressure roller can be cited, for example. The pasting temperature is, for example, in the range of room temperature to 200°C. The pasting load is, for example, 0.01 to 10 MPa.

[0040] Then, if Figure 2 As shown in (c) of FIG. 1 , the release liner L is peeled off. Thus, the surface of each chip C is transferred to each location of the sinter bonding sheet 10 , and a chip C with a sinter bonding material layer 11 is obtained.

[0041] Then, if Figure 2 As shown in (d), the chip C is temporarily fixed to the substrate S. Specifically, for example, a chip mounter is used to temporarily fix the chip C with the sintering bonding material layer by pressing the sintering bonding material layer 11 to the substrate S. In this way, the sintering bonding workpiece X can be prepared.

[0042] The sinter-bonding sheet 10 used for producing the sinter-bonded workpiece X is a supply material for the sinter-bonding material, and is a sheet body of a composition containing at least a binder component and sinterable particles containing a conductive metal, as described above.

[0043] The sinterable particles in the sintered bonding sheet 10 are particles containing conductive metal elements and capable of sintering. As conductive metal elements, for example, gold, silver, copper, palladium, tin and nickel can be cited. As the constituent materials of such sinterable particles, for example, gold, silver, copper, palladium, tin, nickel and alloys of two or more metals selected from their groups can be cited. As the constituent materials of sinterable particles, metal oxides such as silver oxide, copper oxide, palladium oxide, and tin oxide can also be cited. In addition, the sinterable particles can be particles with a core-shell structure. For example, the sinterable particles can be particles of the following core-shell structure, that is, the particles of the core-shell structure have a core with copper as the main component and a shell with gold, silver, etc. as the main component and covering the core. In the present embodiment, the sinterable particles preferably include at least one selected from the group consisting of silver particles, copper particles, silver oxide particles and copper oxide particles. From the viewpoint that the formed sintered layer realizes high electrical conductivity and high thermal conductivity, as sinterable particles, silver particles and copper particles are preferably used. And, from the viewpoint of oxidation resistance, silver particles are easy to handle and are preferred. For example, in the sintering bonding of a semiconductor chip to a copper substrate with a silver plated layer, when a sintering material containing copper particles as sinterable particles is used, the sintering process needs to be performed in an inactive environment such as a nitrogen atmosphere. However, when a sintering material containing silver particles as sinterable particles is used, the sintering process can be properly performed even in an air atmosphere.

[0044] From the viewpoint of achieving a low sintering temperature for the sinterable particles and ensuring good sinterability, the average particle size of the sinterable particles used is preferably 2000nm or less, more preferably 800nm ​​or less, and more preferably 500nm or less. From the viewpoint of achieving good dispersibility for the sinterable particles in the sintering bonding sheet 10 and / or the composition used to form it, the average particle size of the sinterable particles is preferably 1nm or more, preferably 10nm or more, more preferably 50nm or more, and more preferably 100nm or more. The average particle size of the sinterable particles can be measured by observation using a scanning electron microscope (SEM).

[0045] From the viewpoint of achieving highly reliable sintered bonding, the content of the sinterable particles in the sintered bonding sheet 10 is preferably 60 to 99% by mass, more preferably 65 to 98% by mass, and even more preferably 70 to 97% by mass.

[0046] In the present embodiment, the binder component in the sintering bonding sheet 10 includes at least a thermally decomposable polymer binder and a low boiling point binder, and may further include other components such as a plasticizer. The thermally decomposable polymer binder is a binder component that can be thermally decomposed during the high-temperature heating process for sintering bonding, and is an element that helps to maintain the sheet shape of the sintering bonding sheet 10 until the heating process. In the present embodiment, from the perspective of guaranteeing the sheet shape retention function, the thermally decomposable polymer binder is a material that is solid at room temperature (23°C). Examples of such thermally decomposable polymer binders include polycarbonate resins and acrylic resins.

[0047] Examples of polycarbonate resins that are thermally decomposable polymer binders include: aliphatic polycarbonates that do not contain aromatic compounds such as benzene rings between the carbonate groups (-O-CO-O-) of the main chain and contain aliphatic chains; and aromatic polycarbonates that contain aromatic compounds between the carbonate groups (-O-CO-O-) of the main chain. Examples of aliphatic polycarbonates include polyethylene carbonate and polypropylene carbonate. Examples of aromatic polycarbonates include polycarbonates that contain a bisphenol A structure in the main chain.

[0048] Examples of acrylic resins that are heat-decomposable polymer binders include polymers of acrylic acid esters and / or methacrylic acid esters having a linear or branched alkyl group with 4 to 18 carbon atoms. In the following, "(meth)acrylic acid" means "acrylic acid" and / or "methacrylic acid", and "(meth)acrylate" means "acrylate" and / or "methacrylate". Examples of the alkyl group of (meth)acrylate used to form the acrylic resin that is a heat-decomposable polymer binder include methyl, ethyl, propyl, isopropyl, n-butyl, tert-butyl, isobutyl, amyl, isopentyl, hexyl, heptyl, cyclohexyl, 2-ethylhexyl, octyl, isooctyl, nonyl, isononyl, decyl, isodecyl, undecyl, lauryl, tridecyl, tetradecyl, stearyl, and octadecyl.

[0049] The acrylic resin of the thermally decomposable polymer binder can be a polymer containing monomer units derived from other monomers other than the above-mentioned (meth) acrylic acid ester. As such other monomers, for example, carboxyl-containing monomers, anhydride monomers, hydroxyl-containing monomers, sulfonic acid-containing monomers, and phosphoric acid-containing monomers can be cited. Specifically, as carboxyl-containing monomers, for example, acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid can be cited. As anhydride monomers, for example, maleic anhydride and itaconic anhydride can be cited. As hydroxyl-containing monomers, for example, 2-hydroxyethyl (meth) acrylic acid, 2-hydroxypropyl (meth) acrylic acid, 4-hydroxybutyl (meth) acrylic acid, 6-hydroxyhexyl (meth) acrylic acid, 8-hydroxyoctyl (meth) acrylic acid, 10-hydroxydecyl (meth) acrylic acid, 12-hydroxylauryl (meth) acrylic acid, and 4-(hydroxymethyl)cyclohexylmethyl (meth) acrylic acid can be cited. Examples of the sulfonic acid group-containing monomer include styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, (meth)acrylate sulfopropyl ester, and (meth)acryloyloxynaphthalenesulfonic acid. Examples of the phosphoric acid group-containing monomer include 2-hydroxyethylacryloyl phosphate.

[0050] The weight average molecular weight of the thermally decomposable polymer binder is preferably not less than 10000. The weight average molecular weight of the thermally decomposable polymer binder is a value measured by gel permeation chromatography (GPC) and calculated in terms of polystyrene.

[0051] From the viewpoint of appropriately exhibiting the sheet shape-retaining function, the content of the thermally decomposable polymer binder in the sinter-bonding sheet 10 is preferably 0.5 to 10% by mass, more preferably 0.8 to 8% by mass, and even more preferably 1 to 6% by mass.

[0052] The low boiling point binder in the sinter bonding sheet 10 has a viscosity of 1×10 5 Liquid or semi-liquid adhesive with a viscosity of less than Pa·s. In this viscosity measurement, parallel plates with a diameter of 20 mm were used as a jig, the gap between the plates was set to 100 μm, and the shear rate in the rotational shear was set to 1 s. -1 .

[0053] As the low boiling point binder contained in the sintering bonding material layer 11, for example, terpene alcohols, alcohols other than terpene alcohols, alkylene glycol alkyl ethers, and ethers other than alkylene glycol alkyl ethers can be cited. As terpene alcohols, for example, isobornyl cyclohexanol, citronellol, geraniol, nerol, carveol, and α-terpineol can be cited. As alcohols other than terpene alcohols, for example, amyl alcohol, hexanol, heptanol, octanol, 1-decanol, ethylene glycol, diethylene glycol, propylene glycol, butanediol, and 2,4-diethyl-1,5-pentanediol can be cited. Examples of the alkylene glycol alkyl ethers include ethylene glycol butyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol butyl ether, diethylene glycol isobutyl ether, diethylene glycol hexyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, diethylene glycol isopropyl methyl ether, triethylene glycol methyl ether, triethylene glycol dimethyl ether, triethylene glycol butyl methyl ether, propylene glycol propyl ether, dipropylene glycol methyl ether, dipropylene glycol ethyl ether, dipropylene glycol propyl ether, dipropylene glycol butyl ether, dipropylene glycol dimethyl ether, tripropylene glycol methyl ether, and tripropylene glycol dimethyl ether. As ethers other than alkylene glycol alkyl ethers, for example, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether acetate, and dipropylene glycol methyl ether acetate can be cited. As a component in the sintering bonding sheet 10, one low boiling point binder can be used, or two or more low boiling point binders can be used. As the low boiling point binder in the sintering bonding sheet 10, from the viewpoint of stability at room temperature, terpene alcohols are preferred, and isobornyl cyclohexanol is more preferred.

[0054] The thickness of the sintered bonding sheet 10 at 23° C. is preferably 5 μm or more, more preferably 10 μm or more, and preferably 300 μm or less, more preferably 200 μm or less, and more preferably 150 μm or less. The viscosity of the sintered bonding sheet 10 and / or the sintered bonding composition forming the sintered bonding sheet 10 at 70° C. is, for example, 5×10 3 ~1×10 7 Pa·s, preferably 1×10 4 ~1×10 6Pa·s.

[0055] The sintered bonding sheet 10 can be produced, for example, by mixing the above components in a solvent to prepare a varnish, applying the varnish on a separator as a substrate to form a coating film, and drying the coating film. As the solvent for preparing the varnish, an organic solvent or an alcohol solvent can be used.

[0056] In the semiconductor device manufacturing method of the present invention, after the above-mentioned preparation step, each chip C is sinter-bonded to the substrate S in the sinter-bonding workpiece X (sinter-bonding step). The details are as follows.

[0057] First, if Figure 3 (a) and Figure 3 As shown in (b), the sintered workpiece X is overlapped with the cushioning material sheet 20 and clamped between a pair of pressurizing surfaces Pa, Pa in a pair of parallel flat plates P, P for heating and pressing provided in a heating and pressing machine. Figure 3 In (b), the cushioning material sheet 20 is overlapped on the chip arrangement side of the sintered bonded workpiece X. Examples of the constituent material of the cushioning material sheet 20 include fluororesins such as tetrafluoroethylene resin (PTFE), silicone resins such as polymethylsiloxane, and carbon sheets.

[0058] The thickness of the buffer material sheet 20 used is 5 to 5000 μm. From the viewpoint of ensuring the rigidity and shape retention of the buffer material sheet 20, the thickness of the buffer material sheet 20 is preferably 10 μm or more, more preferably 20 μm or more, and more preferably 30 μm or more. From the viewpoint of suppressing the relevant cost of the buffer material sheet 20 and the manufacturing cost of the semiconductor device, the thickness of the buffer material sheet 20 is preferably 3000 μm or less, more preferably 1500 μm or less, more preferably 1000 μm or less, and more preferably 500 μm or less. In addition, the size of the top view shape of the buffer material sheet 20 may be the same as the size of the top view shape of the sintered bonded workpiece X, or may be larger than the size of the top view shape of the sintered bonded workpiece X.

[0059] The tensile modulus of the buffer material sheet 20 is 2 to 150 MPa. The tensile modulus of the buffer material sheet is set to a value obtained based on the following measurement, which is a measurement in a tensile test performed under the conditions of an initial chuck distance of 10 mm, 23° C. and a tensile speed of 50 mm / min for a buffer material sheet sample with a width of 10 mm×a length of 40 mm×a thickness of 100 μm. Specifically, the tensile modulus can be obtained by the slope of the rising straight line portion during the initial period of the measurement in the stress-strain curve obtained by this measurement. This tensile test can be implemented using, for example, a tensile testing machine (trade name "AUTOGRAPH AGS-50NX", manufactured by Shimadzu Corporation). From the viewpoint of ensuring the rigidity and shape retention of the buffer material sheet 20, the tensile modulus of the buffer material sheet 20 is preferably 5 MPa or more, more preferably 15 MPa or more, and more preferably 30 MPa or more. From the viewpoint of achieving high cushioning properties of the cushioning material sheet 20 , the tensile modulus of the cushioning material sheet 20 is preferably 150 MPa or less, more preferably 120 MPa or less, and even more preferably 100 MPa or less.

[0060] The weight loss rate of the cushioning material sheet 20 at 350°C in the weight loss measurement under the conditions of the reference weight temperature of 25°C and the heating rate of 10°C / min in the air atmosphere is 0.1% or less. The weight loss rate of the cushioning material sheet can be measured for about 10 mg of the cushioning material sheet sample using a differential thermal-thermogravimetric simultaneous measurement device. As such a device, for example, a differential thermal balance TG-DTA TG8120 manufactured by Rigaku Corporation can be cited.

[0061] In the sintering bonding process, the sintered steel is then subjected to a predetermined high temperature heating process. Figure 3 As shown in (c), a sintered layer 12 is formed by each sintered bonding material layer 11 in the sintered bonding workpiece X. Specifically, in a state where the buffer material sheet 20 is overlapped with the sintered bonding workpiece X and clamped between a pair of pressurized surfaces Pa, Pa, the sintered bonding workpiece X is pressurized along its thickness direction and / or stacking direction between the pressurized surfaces Pa, Pa and undergoes a prescribed high-temperature heating process. As a result, between the substrate S and the chip C, the low-boiling point binder in the sintered bonding material layer 11 is volatilized, the thermally decomposable polymer binder is thermally decomposed and volatilized, and the conductive metal of the sinterable particles is sintered. In this process, a sintered layer 12 is formed between the substrate S and each chip C, so that the chip C is electrically connected to the substrate S side and sintered and bonded to the substrate S and / or its surface Sa.

[0062] In this process, the heating temperature for sintering bonding is, for example, 150 to 400°C, preferably 200 to 400°C, and more preferably 250 to 350°C. The pressure applied for sintering bonding is preferably 5 MPa or more, for example, 60 MPa or less, and preferably 40 MPa or less. Such temperature and pressure conditions are suitable for forming a strong sintered layer 12 between the substrate S to be sintered and each chip C. The pressurized heating time for sintering bonding is, for example, 0.3 to 300 minutes, and preferably 0.5 to 240 minutes. In addition, from the viewpoint of preventing oxidation of the metal involved in sintering bonding, this process is preferably carried out in a nitrogen atmosphere, under reduced pressure, or under a reducing gas atmosphere.

[0063] The average thickness of the sintered layer 12 formed by this step is preferably 5 to 200 μm, more preferably 10 to 150 μm. This configuration is preferred for alleviating internal stress caused by thermal stress in the sintered layer 12 to ensure sufficient thermal shock reliability while reducing the cost associated with sintering and bonding and thus the manufacturing cost of the semiconductor device.

[0064] In the semiconductor device manufacturing method, next, Figure 4 As shown in (a), the terminal portion of the chip C (not shown) and the terminal portion of the substrate S (not shown) are electrically connected by means of a bonding wire W as needed (wire bonding process). The connection between the terminal portion of the chip C, the terminal portion of the substrate S and the bonding wire W is achieved by, for example, ultrasonic welding accompanied by heating. As the bonding wire W, for example, a gold wire, an aluminum wire or a copper wire can be used. The wire heating temperature in the wire bonding is, for example, 80 to 250°C, preferably 80 to 220°C. In addition, the heating time is several seconds to several minutes.

[0065] Then, if Figure 4 As shown in (b), a sealing resin R for protecting the chip C and the bonding wire W on the substrate S is formed (sealing process). In this process, the sealing resin R is formed, for example, by a transfer molding technique using a mold. As a constituent material of the sealing resin R, for example, an epoxy resin can be used. In this process, the heating temperature for forming the sealing resin R is, for example, 165 to 185°C, and the heating time is, for example, 60 seconds to several minutes. In the case where the sealing resin R is not fully cured in this sealing process, a post-curing process for completely curing the sealing resin R is performed after this process.

[0066] As described above, a semiconductor device including a sintered bonded portion of a semiconductor chip can be manufactured.

[0067] In the semiconductor device manufacturing method, referring to Figure 3In the sintering and bonding process described above, the sintering and bonding workpiece X is heated while being pressurized in a state where the cushioning material sheet 20 having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa is overlapped with the sintering and bonding workpiece X and clamped between the pressurizing surfaces Pa and Pa of a pair of parallel plates P and P of a heating and pressing machine. This configuration is suitable for achieving high uniformity of the pressure and / or load acting on the sintering and bonding workpiece X sandwiched between the parallel plates P and P in the sintering and bonding process among the plurality of sintering and bonding material layers 11. This is because: in the sintering and bonding process, the buffer material sheet 20 having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa and overlapping with the sintering and bonding workpiece X can exert the following buffering function: substantially absorbing and reducing / eliminating the deviation and / or inclination of a pair of pressurized surfaces Pa, Pa from the ideal parallel posture, and substantially absorbing and reducing / eliminating the difference in height from the surface Sa of the substrate S to the top surface of the chip C when there is a difference between the chips C.

[0068] Furthermore, the buffer material sheet 20 having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa has sufficient shape retention and is easy to handle in the semiconductor device manufacturing process. This buffer material sheet 20 is easy to overlap the sintered bonding workpiece X efficiently and in an appropriate configuration in the above-mentioned sintering bonding process. In addition, this buffer material sheet 20 is not prone to excessive compression deformation and sagging deformation in the above-mentioned sintering bonding process that undergoes a high-temperature pressurization process. During the high-temperature pressurization process, if the buffer material sheet is used to produce excessive compression deformation and sagging deformation such as burying the chip C on the substrate S and forming a closed space around the chip C (a space enclosed by the substrate S, the chip C and the buffer material sheet), the components volatilized and escaped from the sintering bonding material layer 11 are sometimes deposited on the substrate S. If such deposition occurs, a separate cleaning process is required to clean the deposited area, so it is not preferred. The above-mentioned buffer material sheet 20 that is not prone to excessive compression deformation and sagging deformation in the above-mentioned sintering bonding process that undergoes a high-temperature pressurization process is suitable for avoiding such problems.

[0069] As described above, the semiconductor device manufacturing method according to the present embodiment is suitable for collectively sintering and bonding a plurality of chips C to the substrate S.

[0070] As described above, the weight loss rate of the cushioning material sheet 20 at 25 to 350° C. is preferably 0.1% or less. This configuration is suitable for allowing the cushioning material sheet 20 to fully exhibit its cushioning function in the sintering bonding step that undergoes a high-temperature heating process.

[0071] In the sintering bonding step in the semiconductor device manufacturing method, sintering bonding can be performed on a plurality of sintering bonding workpieces X at the same time. Figure 5As shown in FIG. 1 , in a state where a plurality of sintered bonded workpieces X each accompanied by a plurality of chips C are overlapped with the buffer material sheet 20 and clamped between a pair of pressurizing surfaces Pa, Pa, the plurality of sintered bonded workpieces X are pressurized along the thickness direction and / or the stacking direction between the pressurizing surfaces Pa, Pa, and subjected to a predetermined high-temperature heating process. The plurality of sintered bonded workpieces X overlapped with the buffer material sheet 20 in the sintering bonding process can be, for example, Figure 6 3 rows × 3 columns are arranged in multiple rows and columns as shown in the arrangement of 3 rows × 3 columns. In this sintering and bonding process, when the thickness of the sintering and bonding workpieces X, including the thickness of the substrate S, differs between the sintering and bonding workpieces X, the buffer material sheet 20 having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa and overlapping with the plurality of sintering and bonding workpieces X can play a buffering function of substantially absorbing and reducing / eliminating the difference. By playing this buffering function, the pressure and / or load acting on the plurality of sintering and bonding workpieces X sandwiched between the parallel plates P, P in the sintering and bonding process can be made uniform between the plurality of sintering and bonding material layers 11.

[0072] In the sintering bonding step in the semiconductor device manufacturing method, Figure 7 (a) and Figure 7 As shown in (b), the buffer material sheet 20 can be overlapped on the surface Sb side of the substrate S relative to the sintered and bonded workpiece X. Based on this structure, the buffer function of the buffer material sheet 20 can also be exerted to achieve uniformity of the pressure and / or load acting on the sintered and bonded workpiece X clamped between the parallel plates P, P among the plurality of sintered and bonded material layers 11.

[0073] In the sintering bonding step in the semiconductor device manufacturing method, Figure 8 As shown in FIG. 1 , the buffer material sheet 20 can be overlapped on the chip arrangement side of the sintered bonding workpiece X with the chip arrangement side facing downward. Based on this structure, the pressure and / or load acting on the sintered bonding workpiece X clamped between the parallel plates P and P can be made uniform between the plurality of sintered bonding material layers 11 by exerting the buffer function of the buffer material sheet 20. In addition, this structure is suitable for avoiding the formation of the above-mentioned closed space that causes the components derived from the sintered bonding material layer 11 to be deposited on the substrate S.

[0074] The buffer material sheet 20 used in the semiconductor device manufacturing method may have a plurality of through holes formed therethrough in the thickness direction. This configuration is suitable for preventing the formation of the closed space in the substrate S where components derived from the sinter-bonding material layer 11 are deposited.

[0075] Example

[0076] [Production of Sheets for Sintering and Bonding]

[0077] A hybrid mixer (trade name "HM-500", manufactured by Keyence Corporation) was used in a stirring mode to mix 35.86 parts by mass of first silver particles (average particle size of 60 nm, manufactured by DOWA Electronics Materials Co., Ltd.) as sinterable particles, 23.90 parts by mass of second silver particles (average particle size of 1100 nm, manufactured by Mitsui Mining & Smelting Co., Ltd.) as sinterable particles, 0.87 parts by mass of a polycarbonate resin (trade name "QPAC40", weight average molecular weight of 150,000, solid at room temperature, manufactured by Empower Materials Inc.) as a thermally decomposable polymer binder, 3.47 parts by mass of isobornyl cyclohexanol (trade name "TERSOLVE MTPH", liquid at room temperature, manufactured by Nippon Terpene Chemicals Inc.) as a low boiling point binder, and 35.91 parts by mass of methyl ethyl ketone as a solvent to prepare a varnish. The stirring time was set to 3 minutes. Then, the obtained varnish was applied to a release film (trade name "MRA50", manufactured by Mitsubishi Resins Co., Ltd.) and dried to form a sheet of a sintering bonding composition having a thickness of 40 μm. The drying temperature was set to 110° C. and the drying time was set to 3 minutes. In this way, a sintering bonding sheet containing sinterable particles, a thermally decomposable polymer binder, and a low boiling point binder was prepared.

[0078] [Example 1]

[0079] The following steps were performed: fabrication of a silicon chip with a sinter-bonding material layer, fabrication of a sinter-bonded workpiece by provisionally fixing the chip to a copper substrate, and collective sinter-bonding of the workpiece. Furthermore, the sinter-bonded portion was observed.

[0080] [Fabrication of silicon chip with sintered bonding material layer]

[0081] First, prepare a silicon chip (5 mm square, 350 μm thick) with a planar electrode (5 mm square) on one side. The planar electrode has a stacked structure of a Ti layer (50 nm thick) on the surface of the silicon chip and an Au layer (100 nm thick) thereon. Next, use a laminator equipped with a crimping roller to stick the sintered bonding sheet to the planar electrode of the silicon chip. The pasting temperature is 70°C, the pasting load (based on the pressure of the crimping roller) is 0.3 MPa, and the speed of the crimping roller is 10 mm / second. After pasting, the portion of the sintered bonding sheet that is crimped to the planar electrode of the silicon chip remains on the electrode, and the rest of the sheet is removed to obtain a silicon chip with a 5 mm square sintered bonding material layer on one side. In this way, the necessary number of silicon chips with sintered bonding material layers are made.

[0082] [Production of sintered workpieces]

[0083] Two silicon chips with sintering material layers were temporarily fixed by pressing the sintering material layer side of the two silicon chips onto a copper plate (3 mm thick) entirely covered with an Ag film (5 μm thick) to obtain sintering workpieces.

[0084] 〔Joint sintering〕

[0085] A sintering device (trade name "HTM-3000", manufactured by Hakuto Co., Ltd.) equipped with a pair of parallel plates for heating and pressurizing is used to sinter and join multiple sintered and joined workpieces at the same time. Specifically, when multiple sintered and joined workpieces (two semiconductor chips with sintered and joined material layers are temporarily fixed) and a first buffer material sheet (trade name "900UL", manufactured by Nitto Denko Corporation) with a thickness of 30 μm superimposed thereon are clamped between a pair of pressurized surfaces in a pair of parallel plates, the sintered and joined workpieces are pressurized along their stacking direction between the pressurized surfaces and undergo a heating process, and a sintered layer is formed by each sintered and joined material layer in each sintered and joined workpiece. In this sintering and joining process, the pressure is set to 10 MPa. During the heating process, the temperature is increased from 80°C to 300°C at a heating rate of 1.5°C / second, and maintained at 300°C for 2.5 minutes. Thereafter, the temperature is cooled to 170°C by air cooling, and the temperature is cooled to 80°C by water cooling. Water cooling is performed using a water cooling mechanism installed in the parallel plates.

[0086] 〔Observation of sintered joints〕

[0087] An ultrasonic imaging device (trade name "FineSAT FS200", manufactured by Hitachi Power Solutions Co., Ltd.) was used to observe each sintered bonded portion in the sintered bonded workpiece. In each sintered bonded workpiece, no poor bonding (a state where the peripheral edge of the sintered layer was not bonded to the substrate or semiconductor chip) was observed at each sintered layer formed between each of the two silicon chips and the copper substrate. The results are recorded in Table 1.

[0088] [Example 2]

[0089] In the sintering and bonding process, a second buffer material sheet with a thickness of 100 μm (trade name "900UL", manufactured by Nitto Denko Corporation) was used instead of a first buffer material sheet with a thickness of 30 μm. In addition, the same operation as in Example 1 was performed to prepare a silicon chip with a sintering and bonding material layer until sintering and bonding were performed together, and the sintering and bonding parts were observed. In each sintering and bonding workpiece, no poor bonding (the peripheral edge of the sintering layer was not bonded to the substrate or the semiconductor chip) was observed at each sintering layer formed between the two silicon chips and the copper substrate. The results are recorded in Table 1.

[0090] [Example 3]

[0091] In the sintering and bonding process, a third buffer material sheet with a thickness of 30 μm (trade name "920UL", manufactured by Nitto Denko Corporation) was used instead of the first buffer material sheet with a thickness of 30 μm. In addition, the same operation as in Example 1 was performed to prepare a silicon chip with a sintering and bonding material layer until sintering and bonding were performed together, and the sintering and bonding parts were observed. In each sintering and bonding workpiece, no poor bonding (the peripheral edge of the sintering layer was not bonded to the substrate or the semiconductor chip) was observed at each sintering layer formed between the two silicon chips and the copper substrate. The results are recorded in Table 1.

[0092] [Comparative Example 1]

[0093] In the sintering and bonding process, the buffer material sheet was not used. Except for this, the same operation as in Example 1 was performed to prepare a silicon chip with a sintering and bonding material layer until it was sintered and bonded together, and the sintering and bonding position was observed. Poor bonding occurred at the sintering layer in the sintering and bonding workpiece (the peripheral edge of the sintering layer was not bonded to the substrate or the semiconductor chip). The results are recorded in Table 1.

[0094] [Comparative Example 2]

[0095] In the sintering step, a fourth buffer material sheet with a thickness of 30 μm was used instead of the first buffer material sheet with a thickness of 30 μm. The same operations as in Example 1 were performed to prepare a silicon chip with a sintering material layer and to perform sintering and bonding at the same time, and observe the sintering and bonding site. The fourth buffer material sheet was prepared as follows.

[0096] First, 2031 g of a predetermined polydimethylsiloxane (number average molecular weight of 11500) having silanol groups at both ends was stirred with 15.71 g of vinyltrimethoxysilane and 2.80 g of (3-glycidoxypropyl)trimethoxysilane to obtain a mixture. Next, 0.97 mL of a methanol solution of tetramethylammonium hydroxide (concentration of 10% by mass, catalyst content of 0.88 mmol) was added to the mixture as a condensation catalyst, and then stirred at 40°C for 1 hour (condensation reaction). Next, the composition obtained by the above operation was stirred at 40°C under reduced pressure (10 mmHg) for 1 hour. Thus, volatile components such as methanol in the composition were removed. Next, under normal pressure, 44.5 g of organohydrogensiloxane (manufactured by Shin-Etsu Chemical Co., Ltd., dimethylpolysiloxane-co-methylhydrogenpolysiloxane, with an average molecular weight of 2000) was added to the composition, and after stirring at 40°C for 1 hour, 0.13 g of a siloxane solution of a platinum-carbonyl complex as an addition catalyst (platinum concentration of 2% by mass) was added, and stirred at 40°C for 10 minutes (addition reaction). Thus, a thermosetting silicone resin composition was obtained. Next, polymethylsilsesquioxane microparticles (trade name "Tospearl 2000B", with an average particle size of 6.0 μm, manufactured by Momentive Performance Materials Japan) (mixing amount of 20% by mass) were mixed with the thermosetting silicone resin composition, and the composition was stirred at room temperature (25°C) for 10 minutes. After stirring, the composition was degassed at room temperature for more than 30 minutes using a vacuum dryer. The resin composition for forming a cushioning material sheet prepared in this way was applied to a polyester film (trade name "SS4C", thickness 50 μm, manufactured by NIPPA Co., Ltd.) as a release sheet, and then heated at 135° C. for 9 minutes. Thus, a semi-cured silicone resin sheet with a thickness of 30 μm was formed on the release sheet. The fourth cushioning material sheet used in Comparative Example 2 was prepared as above.

[0097] [Comparative Example 3]

[0098] In the sintering and bonding process, a fifth buffer material sheet with a thickness of 30 μm (trade name "9700UL", manufactured by Nitto Denko Corporation) was used instead of the first buffer material sheet with a thickness of 30 μm. In addition, the same operation as in Example 1 was performed to prepare a silicon chip with a sintering and bonding material layer until sintering and bonding were performed together, and the sintering and bonding parts were observed. Poor bonding occurred at the sintering layer in the sintering and bonding workpiece (the peripheral edge of the sintering layer was not bonded to the substrate or the semiconductor chip). The results are recorded in Table 1.

[0099] [Tensile modulus of cushioning material sheet]

[0100] The tensile modulus was investigated for each cushioning material sheet used in Examples 1 to 3 and Comparative Examples 1 to 3. Specifically, a tensile test was conducted on a cushioning material sheet sample sheet (width 10 mm × length 40 mm × thickness 100 μm) of the same composition using a tensile testing machine (trade name "AUTOGRAPH AGS-50NX", manufactured by Shimadzu Corporation) at an initial chuck distance of 10 mm, 23°C, and a tensile speed of 50 mm / min. Furthermore, the tensile modulus (MPa) was determined from the slope of the rising straight line portion during the initial period of the measurement in the stress-strain curve obtained by the measurement of the test. The results are recorded in Table 1.

[0101] [Heat resistance of cushioning material sheets]

[0102] Heat resistance was investigated for each cushioning material sheet used in Examples 1 to 3 and Comparative Examples 1 to 3. The results are shown in Table 1. Specifically, a sample of about 10 mg was cut out from the cushioning material sheet, and the sample was subjected to a differential thermal-thermogravimetric simultaneous measurement device (trade name "differential thermal balance TG-DTA TG8120", manufactured by Rigaku Corporation) to measure weight loss during heating. In this measurement, the temperature was raised from a reference weight temperature of 25°C to 500°C at a heating rate of 10°C / min in an atmospheric atmosphere. The weight reduction rate (%) of the sample from the weight at 25°C (reference weight) to the weight at 350°C is shown in Table 1.

[0103] [Workability during joint sintering]

[0104] The fourth cushioning material sheet used in Comparative Example 2 was too soft to be overlapped on the sintered workpiece during the sintering step. In contrast, the other cushioning material sheets did not have this problem. The results are shown in Table 1.

[0105] 〔Observation of chip damage〕

[0106] In Comparative Examples 1 and 3, cracks and chipping occurred in the sintered and bonded workpieces subjected to the batch sintering. Such cracks and chipping did not occur in Examples 1 to 3 and Comparative Example 2. The results are shown in Table 1.

[0107] [Table 1]

[0108]

[0109] As a summary of the above, the configuration and modifications of the present invention are listed below in the form of appendices.

[0110] [Appendix 1]

[0111] A method for manufacturing a semiconductor device, comprising:

[0112] A step of preparing a sintered bonding workpiece having a stacked structure, the stacked structure comprising: a substrate having a first surface and a second surface opposite thereto, a plurality of semiconductor chips to be bonded and arranged on the first surface side, and a plurality of sintered bonding material layers containing sinterable particles respectively interposed between each semiconductor chip and the substrate; and

[0113] The sintering bonding process comprises the following steps: overlapping a buffer material sheet having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa with the aforementioned sintering bonding workpiece and clamping the sheet between a pair of pressurizing surfaces, pressurizing the aforementioned sintering bonding workpiece along its stacking direction between the pair of pressurizing surfaces and subjecting the sheet to a heating process, thereby forming a sintered layer from the aforementioned sintering bonding material layer.

[0114] [Appendix 2]

[0115] The method for manufacturing a semiconductor device according to Appendix 1, wherein the thickness of the buffer material sheet is 10 μm or more, preferably 20 μm or more, and more preferably 30 μm or more.

[0116] [Appendix 3]

[0117] The method for manufacturing a semiconductor device according to Appendix 1 or 2, wherein the thickness of the buffer material sheet is 3000 μm or less, preferably 1500 μm or less, more preferably 1000 μm or less, and more preferably 500 μm or less.

[0118] [Appendix 4]

[0119] The method for manufacturing a semiconductor device according to any one of Appendices 1 to 3, wherein the tensile modulus of the buffer material sheet is 5 MPa or more, preferably 15 MPa or more, and more preferably 30 MPa or more.

[0120] [Appendix 5]

[0121] The method for manufacturing a semiconductor device according to any one of Appendixes 1 to 4, wherein the tensile modulus of the buffer material sheet is 120 MPa or less, preferably 100 MPa or less.

[0122] [Appendix 6]

[0123] A method for manufacturing a semiconductor device according to any one of Appendices 1 to 5, wherein the weight loss rate of the buffer material sheet at 350°C in a weight loss measurement under the conditions of an atmospheric atmosphere, a reference weight temperature of 25°C and a heating rate of 10°C / min is 0.1% or less.

[0124] [Appendix 7]

[0125] The method for manufacturing a semiconductor device according to any one of appendices 1 to 6, wherein the heating temperature in the sintering and bonding step is 200° C. or higher and the pressure is 5 MPa or higher.

[0126] [Appendix 8]

[0127] The method for manufacturing a semiconductor device according to any one of Appendixes 1 to 7, wherein the sinterable particles include at least one selected from the group consisting of silver particles, copper particles, silver oxide particles, and copper oxide particles.

[0128] [Appendix 9]

[0129] A method for manufacturing a semiconductor device according to any one of appendices 1 to 8, wherein the content ratio of the sinterable particles in the sintering bonding material layer is 60 to 99% by mass, preferably 65 to 98% by mass, and more preferably 70 to 97% by mass.

[0130] [Appendix 10]

[0131] The method for manufacturing a semiconductor device according to any one of Appendices 1 to 9, wherein the thickness of the sintered layer is 5 to 200 μm, preferably 10 to 150 μm.

[0132] Description of Reference Numerals

[0133] X Sintering of workpieces

[0134] S substrate

[0135] C chip (semiconductor chip)

[0136] 10 Sintering bonding sheet

[0137] 11 Sintering bonding material layer

[0138] 12 Sintering layer

[0139] 20 cushioning material sheets

[0140] Pa Pressure surface

Claims

1. A method for manufacturing a semiconductor device, comprising: A step of preparing a sintered bonding workpiece having a stacked structure, the stacked structure comprising: a substrate having a first surface and a second surface opposite thereto, a plurality of semiconductor chips arranged on the first surface side and to be bonded, and a plurality of sintered bonding material layers containing sinterable particles respectively interposed between each semiconductor chip and the substrate; as well as A sintering step, wherein a cushioning material sheet having a thickness of 5 to 5000 μm and a tensile modulus of 2 to 150 MPa is overlapped with the sintering workpiece and clamped between a pair of pressurizing surfaces, and the sintering workpiece is pressurized along a stacking direction thereof between the pair of pressurizing surfaces and subjected to a heating process, thereby forming a sintered layer from the sintering material layer, The heating temperature in the sintering bonding step is 200° C. or higher and the pressurizing pressure is 5 MPa or higher.

2. The method for manufacturing a semiconductor device according to claim 1, wherein: The cushioning material sheet has a weight loss rate of 0.1% or less at 350° C. in a weight loss measurement under conditions of an atmospheric atmosphere, a base weight temperature of 25° C., and a heating rate of 10° C. / min.

3. The method for manufacturing a semiconductor device according to claim 1 or 2, wherein: The sinterable particles include at least one selected from the group consisting of silver particles, copper particles, silver oxide particles, and copper oxide particles.

4. The method for manufacturing a semiconductor device according to claim 1 or 2, wherein: The content ratio of the sinterable particles in the sinter-bonding material layer is 60 to 99% by mass.

5. The method for manufacturing a semiconductor device according to claim 1 or 2, wherein: The thickness of the sintered layer is 5 to 200 μm.