Binder composition for non-aqueous secondary battery electrode, slurry composition for non-aqueous secondary battery electrode and method for producing the same, electrode for non-aqueous secondary battery and non-aqueous secondary battery

By using a binder composition composed of a specific polymer, the problem of insufficient adhesion of the electrode composite material layer of lithium-ion secondary batteries is solved, the rate and cycle characteristics of the battery are improved, and higher solid content concentration and peeling are achieved Strength, improves battery performance.

CN112136236BActive Publication Date: 2024-10-18ZEON CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN201980033370.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-06-18
Publication Date
2024-10-18
Estimated Expiration
2039-06-18

AI Technical Summary

Technical Problem

The existing technology still has room for improvement in improving the rate characteristics and cycle characteristics of lithium-ion secondary batteries. In particular, the adhesiveness is insufficient in improving the solid content concentration of the slurry composition and the peeling strength of the electrode composite material layer.

Method used

A binder composition for non-aqueous secondary battery electrodes containing three polymers of specific composition and properties is used. Polymer A contains (meth)acrylate monomer units, and polymer B has a high iodine value and is easy to dissolve. Polymer C contains more than 70% of nitrile group-containing monomer units and exists in an organic solvent. The combination of these polymers improves the solid content concentration and peel strength of the adhesive composition.

Benefits of technology

The battery characteristics of secondary battery electrodes are significantly improved, including rate characteristics and cycle characteristics, the peel strength and solid content concentration of the electrode composite material layer are enhanced, and the overall performance of the battery is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002784324870000371
    Figure BDA0002784324870000371
Patent Text Reader

Abstract

The present invention provides a binder composition for non-aqueous secondary battery electrodes, comprising a polymer A, a polymer B, a polymer C and an organic solvent, wherein the polymer A comprises a (meth)acrylate monomer unit, the polymer B has an iodine value of 5 g / 100 g or more and 100 g / 100 g or less, and the polymer C comprises a nitrile group-containing monomer unit in a ratio of 70% by mass or more and 98% by mass or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a binder composition for non-aqueous secondary battery electrodes, a slurry composition for non-aqueous secondary battery electrodes and a method for producing the same, an electrode for a non-aqueous secondary battery, and a non-aqueous secondary battery. Background Art

[0002] Non-aqueous secondary batteries such as lithium-ion secondary batteries are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are therefore used in a wide range of applications. Therefore, in recent years, in order to further improve the performance of non-aqueous secondary batteries, research has been conducted on improving battery components such as electrodes.

[0003] Here, the electrode for a non-aqueous secondary battery such as a lithium ion secondary battery (hereinafter sometimes simply referred to as a "secondary battery") generally has a current collector and an electrode composite material layer (a positive electrode composite material layer or a negative electrode composite material layer) formed on the current collector. In addition, the electrode composite material layer is formed by, for example, applying a slurry composition including an electrode active material and a binder composition containing a binding material on the current collector and drying the applied slurry composition.

[0004] Therefore, in recent years, attempts have been made to improve the slurry composition for forming the electrode composite material layer in order to further improve the performance of secondary batteries.

[0005] For example, Patent Document 1 proposes a method comprising a substrate having a BET specific surface area of ​​400 m 2 / g or more conductive material and a specific binding material for a lithium ion secondary battery positive electrode slurry composition. The positive electrode slurry composition of Patent Document 1 is characterized in that as a binding material, it contains (1) a fluorine-containing polymer X, (2) a polymer Y containing 10 to 50% by mass or less of a nitrile group-containing monomer unit, and (3) a polymer Z containing 50 to 90% by mass or less of a (meth) alkyl acrylate monomer unit, and the polymer X accounts for 50 to 95% by mass of the total binding material. The positive electrode slurry composition can not only improve the cycle characteristics and rate characteristics of the lithium ion secondary battery, but also has excellent viscosity stability.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent document 1: International Publication No. 2015 / 064099. Summary of the invention

[0009] Problem that the invention aims to solve

[0010] In recent years, for secondary batteries, it is necessary to further improve battery characteristics such as rate characteristics and cycle characteristics (hereinafter sometimes referred to as "battery characteristics"). It is also necessary to prepare a binder composition for a secondary battery with excellent battery characteristics, and to fully increase the solid content concentration when preparing a slurry composition. In addition, in the electrode formed using the binder composition, it is also very important that the electrode composite material layer and the current collector can show sufficient bonding strength (that is, it is possible to fully improve the peel strength).

[0011] However, in the above-mentioned existing binder compositions that have been used to prepare slurry compositions, there is still room for improvement in terms of sufficiently increasing the solid content concentration of the slurry composition at a sufficiently high level, sufficiently improving the adhesion between the electrode composite material layer and the current collector in the obtained electrode, and improving battery characteristics.

[0012] Therefore, an object of the present invention is to provide a non-aqueous secondary battery electrode binder composition that can sufficiently increase the solid content concentration of the obtained slurry composition and the peel strength of the obtained electrode composite layer, and can improve the battery characteristics of a secondary battery having the obtained electrode.

[0013] Another object of the present invention is to provide a non-aqueous secondary battery electrode slurry composition having a sufficiently high solid content concentration and capable of sufficiently improving the peel strength of the obtained electrode composite material layer and thus improving the battery characteristics of the obtained secondary battery, and a method for producing the same.

[0014] Furthermore, an object of the present invention is to provide an electrode for a non-aqueous secondary battery capable of sufficiently improving the battery characteristics of the non-aqueous secondary battery, and a non-aqueous secondary battery having excellent battery characteristics such as rate characteristics and cycle characteristics.

[0015] Solutions for solving problems

[0016] The present inventors have conducted intensive research to solve the above problems. Then, the present inventors found that if a non-aqueous secondary battery electrode binder composition to which three polymers satisfying specific compositions or properties are added is used as a binder, the above problems can be solved advantageously, thereby completing the present invention.

[0017] That is, the purpose of the present invention is to advantageously solve the above-mentioned problems. The non-aqueous secondary battery electrode binder composition of the present invention is characterized in that it contains polymer A, polymer B, polymer C and an organic solvent, the polymer A is a granular polymer containing a (meth) acrylate monomer unit, the polymer B is an easily soluble polymer having an iodine value of 5g / 100g or more and 100g / 100g or less, and the polymer C is an easily soluble polymer containing a nitrile group-containing monomer unit at a ratio of 70% by mass or more and 98% by mass or less when the total of all monomer units constituting the polymer C is 100% by mass. In this way, according to the binder composition containing the above polymers A to C, the solid content concentration of the slurry composition and the peel strength of the obtained electrode composite material layer can be fully increased, and the battery characteristics of the secondary battery having the obtained electrode can be improved.

[0018] Here, "(meth)acrylic acid" in this specification refers to acrylic acid or methacrylic acid. In addition, the types of monomer units contained in a certain polymer and the "ratio of monomer units" in a certain polymer can be expressed as 1 H-NMR or other nuclear magnetic resonance (NMR) methods for identification or measurement. In addition, "comprising monomer units" means "containing repeating units from the monomer in the polymer obtained using the monomer". In addition, whether a certain polymer is "easily soluble" can be determined by the method described in the examples. Furthermore, the "iodine value" of polymer B can be measured by the method described in the examples.

[0019] Here, the non-aqueous secondary battery electrode binder composition of the present invention preferably further comprises an ethylenically unsaturated acid monomer unit in the above-mentioned polymer A. If the polymer A further comprises an ethylenically unsaturated acid monomer unit, the polymer A can exert a more excellent bonding force, and the peel strength of the electrode composite material layer formed by the non-aqueous secondary battery electrode slurry composition comprising the binder composition can be further improved.

[0020] In addition, the non-aqueous secondary battery electrode binder composition of the present invention preferably has a weight average molecular weight of the polymer B of 5000 or more and 500000 or less. By making the weight average molecular weight of polymer B within the above range, the dispersibility of the conductive material and the like in the non-aqueous secondary battery electrode slurry composition containing the binder composition can be improved. Furthermore, the peel strength of the electrode composite material layer obtained using the slurry composition can be further improved. Moreover, the battery characteristics such as the cycle characteristics of the secondary battery having the electrode can be further improved.

[0021] In addition, the "weight average molecular weight" of the polymer B can be measured by the method described in the examples.

[0022] In addition, in the non-aqueous secondary battery electrode binder composition of the present invention, when the total content of the above-mentioned polymer A, the above-mentioned polymer B and the above-mentioned polymer C is 100% by mass, it is preferred that the content a of the above-mentioned polymer A is 5% by mass or more and 60% by mass or less, the content b of the above-mentioned polymer B is 0.1% by mass or more and 50% by mass or less, and the content c of the above-mentioned polymer C is 20% by mass or more and 94% by mass or less. By making the content of polymers A to C respectively within the above range, the dispersibility of the conductive material and the like in the slurry composition for non-aqueous secondary battery electrodes containing the binder composition can be improved. Furthermore, the peel strength of the electrode composite material layer obtained using the slurry composition can be further improved. Moreover, the battery characteristics such as the cycle characteristics of the secondary battery having the electrode can be further improved.

[0023] In addition, the non-aqueous secondary battery electrode binder composition of the present invention preferably has the above-mentioned content a and the above-mentioned content c satisfying the relationship: 10≤a / (a+c)×100≤50. By adjusting the addition amount of polymer A and polymer C in a manner that the content a and the content c satisfy the above-mentioned relationship, the peel strength of the electrode composite material layer obtained using the non-aqueous secondary battery electrode slurry composition containing the binder composition can be further improved. Moreover, the battery characteristics such as the cycle characteristics of the secondary battery having the electrode can be further improved.

[0024] In addition, in the non-aqueous secondary battery electrode binder composition of the present invention, the above-mentioned polymers A to C are preferably the following polymers: in the case of preparing a N-methyl-2-pyrrolidone mixed solution containing the above-mentioned polymer A at the above-mentioned content a, the above-mentioned polymer B at the above-mentioned content b, and the above-mentioned polymer C at the above-mentioned content c as a solid component, the ratio of the amount of insoluble components in the mixed solution satisfies 30% by mass or more and 80% by mass or less. If the amount of insoluble components of the mixture of polymers A to C in N-methyl-2-pyrrolidone is within the above range, the peel strength of the electrode composite material layer obtained using the non-aqueous secondary battery electrode slurry composition containing the binder composition can be further improved. Moreover, the battery characteristics such as the cycle characteristics of the secondary battery having the obtained electrode can be further improved.

[0025] In addition, the above-mentioned "ratio of the amount of insoluble components" can be measured by the method described in Examples.

[0026] In addition, the object of the present invention is to advantageously solve the above-mentioned problems, and the non-aqueous secondary battery electrode slurry composition of the present invention is characterized in that it comprises any of the above-mentioned non-aqueous secondary battery electrode binder compositions, electrode active materials and conductive materials, and the above-mentioned conductive materials contain carbon nanotubes. If, like this, the above-mentioned non-aqueous secondary battery electrode binder composition comprising polymer A, electrode active materials and conductive materials containing carbon nanotubes are added, then the electrode active materials and the carbon nanotubes as conductive materials in the slurry composition can be well dispersed. Therefore, the solid content concentration of the slurry composition can be fully improved. And then according to the slurry composition, the peel strength of the obtained electrode composite material layer can be fully improved, and then the battery characteristics of the obtained secondary battery can be improved.

[0027] In addition, the object of the present invention is to advantageously solve the above-mentioned problems. The method for producing a slurry composition for non-aqueous secondary battery electrodes of the present invention is characterized in that it comprises the following steps: a premixing step of mixing at least the carbon nanotubes, the polymer B and the organic solvent to obtain a premix; and a main mixing step of mixing the premix with at least the polymer A and the polymer C. By performing the main mixing step after mixing the carbon nanotubes and the polymer B in the premixing step, the dispersibility of the carbon nanotubes in the slurry composition can be further improved. Therefore, according to the method for producing the slurry composition of the present invention, the slurry composition for non-aqueous secondary battery electrodes of the present invention containing carbon nanotubes can be effectively prepared.

[0028] In addition, the object of the present invention is to advantageously solve the above-mentioned problems, and the non-aqueous secondary battery electrode of the present invention is characterized in that it has an electrode composite material layer formed using the above-mentioned non-aqueous secondary battery electrode slurry composition. The peel strength of the electrode composite material layer formed using the above-mentioned non-aqueous secondary battery electrode slurry composition is high. Moreover, according to the non-aqueous secondary battery electrode having the electrode composite material layer, the battery characteristics of the secondary battery can be fully improved.

[0029] Furthermore, the object of the present invention is to advantageously solve the above-mentioned problems, and the non-aqueous secondary battery of the present invention is characterized in that it has the above-mentioned electrode for non-aqueous secondary battery. If the above-mentioned electrode for non-aqueous secondary battery is used in this way, a non-aqueous secondary battery with excellent battery characteristics such as rate characteristics and cycle characteristics can be provided.

[0030] Effects of the Invention

[0031] According to the present invention, a nonaqueous secondary battery electrode binder composition can be provided which can sufficiently increase the solid content concentration of the obtained slurry composition and the peel strength of the obtained electrode composite layer and can improve the battery characteristics of a secondary battery having the obtained electrode.

[0032] Furthermore, the present invention can provide a nonaqueous secondary battery electrode slurry composition having a sufficiently high solid content concentration and capable of sufficiently improving the peel strength of the obtained electrode composite material layer and thus improving the battery characteristics of the obtained secondary battery, and a method for producing the same.

[0033] Furthermore, according to the present invention, it is possible to provide a nonaqueous secondary battery electrode capable of sufficiently improving the battery characteristics of the nonaqueous secondary battery, and a nonaqueous secondary battery having excellent battery characteristics such as rate characteristics and cycle characteristics. DETAILED DESCRIPTION

[0034] Hereinafter, embodiments of the present invention will be described in detail.

[0035] Here, the non-aqueous secondary battery electrode binder composition of the present invention can be used when preparing a slurry composition for non-aqueous secondary battery electrodes. In addition, the non-aqueous secondary battery electrode slurry composition prepared using the non-aqueous secondary battery electrode binder composition of the present invention can be used when forming an electrode of a non-aqueous secondary battery such as a lithium ion secondary battery. In addition, the non-aqueous secondary battery electrode slurry composition of the present invention can be effectively manufactured by the manufacturing method of the slurry composition of the present invention. Furthermore, the non-aqueous secondary battery of the present invention is characterized in that a non-aqueous secondary battery electrode formed using the non-aqueous secondary battery electrode slurry composition of the present invention is used.

[0036] Furthermore, the binder composition for nonaqueous secondary battery electrodes and the slurry composition for nonaqueous secondary battery electrodes of the present invention can be particularly preferably used when forming a positive electrode of a nonaqueous secondary battery.

[0037] (Binder composition for secondary battery electrodes)

[0038] The non-aqueous secondary battery electrode binder composition of the present invention is a non-aqueous secondary battery electrode binder composition comprising polymer A, polymer B, polymer C and an organic solvent. Moreover, it is characterized in that polymer A is a granular polymer containing a (meth) acrylate monomer unit, polymer B is an easily soluble polymer having an iodine value of 5 g / 100 g or more and 100 g / 100 g or less, and polymer C contains a nitrile-containing monomer unit at a ratio of 70% by mass or more and 98% by mass or less when the total of all monomer units constituting the polymer C is 100% by mass. Furthermore, in the non-aqueous secondary battery electrode binder composition of the present invention, as a binder, in addition to the above-mentioned polymers A to C, any other binder may be contained.

[0039] Here, the non-aqueous secondary battery electrode binder composition of the present invention (hereinafter referred to as "binder composition"). Since it contains polymers A to C that satisfy the above-mentioned composition and properties, the solid content concentration of the obtained slurry composition and the peel strength of the obtained electrode composite material layer can be fully improved. Furthermore, according to the binder composition of the present invention, the battery characteristics of the secondary battery having the obtained electrode can be improved. The reason is not clear, but it is speculated as follows.

[0040] First, polymer A as a granular polymer can play the following role: effectively bond the bonded components such as electrode active materials to each other by point bonding in the electrode composite material layer. Therefore, polymer A can help to improve the peel strength of the formed electrode composite material layer. In addition, polymer B can play the following role: when preparing the slurry composition, it is adsorbed on the surface of the carbon nanotube (hereinafter sometimes abbreviated as "CNT") contained in the slurry composition as a conductive material to improve the dispersibility of the CNT in the slurry composition. If CNT is well dispersed in the slurry composition, other solid components will also be well dispersed in the slurry composition as a result. And, if the dispersibility of the solid component is high, the solid component concentration of the slurry composition can be increased. Then, polymer C can play the following role: when preparing the slurry composition, the slurry composition is given appropriate viscosity, and when the slurry composition is used to form an electrode composite material layer, the electrode active material is coated in the electrode composite material layer in the form of a film, and the degradation of the electrode active material accompanied by repeated charge and discharge is suppressed. Therefore, by polymer C, the cycle characteristics of the secondary battery can be improved. Thus, the binder composition of the present invention can sufficiently increase the solid content concentration of the obtained slurry composition and the peel strength of the obtained electrode composite layer by containing polymers A to C, and as a result, when used to produce a secondary battery, the battery characteristics of the obtained secondary battery can be improved.

[0041] <Polymer A>

[0042] Polymer A is a component that keeps the components contained in the electrode composite layer from being separated from the electrode composite layer (i.e., acting as a binder) in an electrode manufactured by forming an electrode composite layer on a current collector using a slurry composition containing a binder composition. Moreover, polymer A is a component that exists in a granular state in an organic solvent. Whether polymer A is "granular" in an organic solvent can be confirmed by the method described in the embodiment.

[0043] [Composition of polymer A]

[0044] The polymer A needs to contain a (meth)acrylic acid ester monomer unit as a repeating unit. Furthermore, the polymer A preferably contains an ethylenically unsaturated acid monomer unit as a repeating unit, and may also contain a crosslinkable monomer unit and other monomer units other than the above.

[0045] [(Meth)acrylate monomer unit]

[0046] The (meth)acrylate monomer unit is a repeating unit derived from a (meth)acrylate monomer. If the polymer A contains the (meth)acrylate monomer unit, the peel strength of the obtained electrode composite material layer can be improved, and the rate characteristics of the obtained secondary battery can be improved.

[0047] Examples of the (meth)acrylic acid ester monomer include alkyl (meth)acrylate monomers having 1 ethylenically unsaturated bond. Examples of the alkyl (meth)acrylate monomer include alkyl (meth)acrylate monomers having a linear alkyl group and alkyl (meth)acrylate monomers having a branched alkyl group. For example, as (meth) acrylic acid ester monomers, there can be mentioned: methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, tert-butyl acrylate, pentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, stearyl acrylate and other alkyl acrylates; methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate and other alkyl methacrylates, etc. Among these, from the viewpoint of imparting appropriate affinity to the electrolyte to the obtained electrode composite material layer, preferably the alkyl (meth) acrylic acid ester whose alkyl group is a linear alkyl group, more preferably butyl acrylate and methyl methacrylate. In addition, these may be used alone or in combination of two or more.

[0048] Moreover, the content ratio of the (meth) acrylate monomer unit in polymer A is preferably 30.0% by mass or more, more preferably 40.0% by mass or more, preferably 98.0% by mass or less, and more preferably 95.0% by mass or less, when all repeating units contained in polymer A are 100.0% by mass. By making the content ratio of the (meth) acrylate monomer unit in polymer A within the above range, the obtained electrode composite material layer can be given a moderate affinity with the electrolyte, and the rate characteristics of the secondary battery having the electrode composite material layer can be improved.

[0049] [Ethylenically unsaturated acid monomer unit]

[0050] The ethylenically unsaturated acid monomer unit is a repeating unit from an ethylenically unsaturated acid monomer. Moreover, polymer A can exert excellent bonding strength because it contains ethylenically unsaturated acid monomer units. Therefore, the electrode composite material layer formed using the slurry composition comprising the binder composition of the present invention can exert more excellent peel strength. In addition, in this specification, "ethylenically unsaturated acid monomer unit" refers to a monomer unit comprising an ethylenically unsaturated bond and an acidic group.

[0051] Here, examples of the ethylenically unsaturated acid monomer capable of forming the ethylenically unsaturated acid monomer unit include monomers having a carboxylic acid group, a sulfonic acid group, and a phosphoric acid group in addition to an ethylenically unsaturated bond.

[0052] Examples of the carboxylic acid group-containing monomer include monocarboxylic acids and derivatives thereof, dicarboxylic acids and anhydrides thereof, and derivatives thereof.

[0053] Examples of the monocarboxylic acid include acrylic acid, methacrylic acid, and crotonic acid.

[0054] Examples of the monocarboxylic acid derivative include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, and α-chloro-β-E-methoxyacrylic acid.

[0055] Examples of the dicarboxylic acid include maleic acid, fumaric acid, and itaconic acid.

[0056] Examples of the dicarboxylic acid derivatives include maleic acid monoesters such as methylmaleic acid, dimethylmaleic acid, phenylmaleic acid, chloromaleic acid, dichloromaleic acid, and fluoromaleic acid; and nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, and fluoroalkyl maleate.

[0057] Examples of the anhydride of dicarboxylic acid include maleic anhydride, acrylic anhydride, methylmaleic anhydride, and dimethylmaleic anhydride.

[0058] Furthermore, as the carboxylic acid group-containing monomer, an acid anhydride that generates a carboxyl group by hydrolysis can also be used.

[0059] Examples of the sulfonic acid group-containing monomer include styrene sulfonic acid, vinyl sulfonic acid, methyl vinyl sulfonic acid, (meth)allyl sulfonic acid, 3-allyloxy-2-hydroxypropanesulfonic acid, and 2-acrylamido-2-methylpropanesulfonic acid.

[0060] In addition, in the present invention, "(meth)allyl group" means an allyl group and / or a methallyl group.

[0061] Furthermore, examples of the phosphoric acid group-containing monomer include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate.

[0062] In addition, in the present invention, "(meth)acryloyl" means acryloyl and / or methacryloyl.

[0063] These ethylenically unsaturated acid monomers can be used alone or in combination of two or more. And, among these ethylenically unsaturated acid monomers, from the viewpoint of further improving the peel strength of the obtained electrode composite material layer, preferably acrylic acid, methacrylic acid, itaconic acid, maleic acid and fumaric acid, more preferably acrylic acid and methacrylic acid.

[0064] Moreover, when all repeating units in polymer A are set to 100.0 mass %, the content ratio of the ethylenically unsaturated acid monomer unit in polymer A is preferably more than 1.0 mass %, more preferably more than 1.5 mass %, more preferably more than 2.0 mass %, more preferably more than 3.0 mass %, preferably less than 10.0 mass %, more preferably less than 8.0 mass %, more preferably less than 6.0 mass %, more preferably less than 5.0 mass %. By making the content ratio of the ethylenically unsaturated acid monomer unit more than the above lower limit, the peel strength of the electrode composite material layer formed using the slurry composition comprising the binder composition can be improved. In particular, by making the content ratio of the ethylenically unsaturated acid monomer unit less than the above upper limit, the flexibility of polymer A can be improved, thereby, the peel strength of the electrode composite material layer obtained can be further improved. And then, by making the flexibility of polymer A high, it is possible to easily densify the electrode density when pressing the electrode composite material layer.

[0065] [Crosslinking monomer unit]

[0066] The crosslinkable monomer unit is a repeating unit from a crosslinkable monomer. A crosslinkable monomer is a monomer that can form a crosslinked structure when polymerized. Moreover, if polymer A contains a crosslinkable monomer unit, the peel strength of the obtained electrode composite material layer can be further improved. As an example of a crosslinkable monomer, a monomer having two or more reactive groups per molecule can be cited.

[0067] More specifically, as the crosslinkable monomer, a polyfunctional ethylenically unsaturated carboxylic acid ester monomer having two or more ethylenically unsaturated bonds can be mentioned.

[0068] Examples of the difunctional ethylenically unsaturated carboxylic acid ester monomer having two ethylenically unsaturated bonds in the molecule include allyl acrylate, allyl methacrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, 2-hydroxy-3-acryloxypropyl methacrylate, polyethylene glycol diacrylate, ethoxylated propoxylated bisphenol A diacrylate, ethoxylated bisphenol A diacrylate, 9,9-bis[4-(2-acryloxyethoxy)phenyl]fluorene, propoxylated bisphenol A diacrylate, tricyclodecane dimethanol diacrylate, 1,10-decanediol diacrylate, 1,6-hexanediol diacrylate, Alkynes, 1,9-nonanediol diacrylate, polypropylene glycol diacrylate, polypropylene glycol dimethacrylate, polytetramethylene glycol diacrylate, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, ethoxylated bisphenol A dimethacrylate, tricyclodecane dimethanol dimethacrylate, 1,10-decanediol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,9-nonanediol dimethacrylate, neopentyl glycol dimethacrylate, ethoxylated polypropylene glycol dimethacrylate and glycerol dimethacrylate, etc.

[0069] Examples of the trifunctional ethylenically unsaturated carboxylic acid ester monomer having three ethylenically unsaturated bonds in the molecule include ethoxylated isocyanuric acid triacrylate, ε-caprolactone-modified tri(2-acryloyloxyethyl)isocyanurate, ethoxylated glycerol triacrylate, pentaerythritol triacrylate, trimethylolpropane triacrylate, and trimethylolpropane trimethacrylate.

[0070] Examples of the tetrafunctional or higher-functional ethylenically unsaturated carboxylic acid ester monomer having four or more ethylenically unsaturated bonds in the molecule include ditrimethylolpropane tetraacrylate, ethoxylated pentaerythritol tetraacrylate, pentaerythritol tetraacrylate, dipentaerythritol polyacrylate, and dipentaerythritol hexaacrylate.

[0071] Among these, from the viewpoint of improving the peel strength and flexibility of the obtained electrode composite material layer, preferred are allyl methacrylate (2-functional), ethylene glycol dimethacrylate (2-functional), trimethylolpropane triacrylate (3-functional) and ethoxylated pentaerythritol tetraacrylate (4-functional).

[0072] Moreover, the content ratio of the crosslinking monomer unit in polymer A is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, more preferably 0.1% by mass or more, preferably 5.0% by mass or less, more preferably 2.0% by mass or less, and more preferably 1.5% by mass or less when all repeating units contained in polymer A are 100.0% by mass. By making the content ratio of the crosslinking monomer unit in polymer A above the above lower limit, the peel strength of the obtained electrode composite material layer can be further improved. In addition, by making the content ratio of the crosslinking monomer unit in polymer A below the above upper limit, the flexibility of the obtained electrode composite material layer can be improved, thereby, the peel strength of the obtained electrode composite material layer can be further improved.

[0073] [Other monomer units]

[0074] Furthermore, polymer A may also include other monomer units from other monomers that can be copolymerized with the above-mentioned various monomers. As other monomers that can form such other monomer units, known monomers that can be used to manufacture the adhesive component in the electrode binder composition of the non-aqueous secondary battery can be used. More specifically, for example, as other monomers, aromatic vinyl monomers described in detail in the project of <Polymer B>, and nitrile-containing monomers and basic group-containing monomers described in detail in the project of <Polymer C> can be cited. These can be used alone or in combination of two or more.

[0075] Furthermore, the content ratio of other monomer units in the polymer A is preferably 50.0 mass % or less, and may be 0.0 mass %, when all repeating units in the polymer A are taken as 100.0 mass %.

[0076] [NMP insoluble content]

[0077] Here, the amount of insoluble components when polymer A is mixed with N-methyl-2-pyrrolidone at a concentration of 8% by mass is preferably 70% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more, and can be 100% by mass, that is, polymer A is insoluble in N-methyl-2-pyrrolidone (hereinafter sometimes abbreviated as "NMP".). If the amount of NMP insoluble components is above the above lower limit, the battery characteristics of the secondary battery with the electrode composite material layer obtained can be further improved. In addition, the amount of insoluble components of NMP can be controlled by adjusting the addition amount of the crosslinking monomer in the monomer composition for preparing polymer A. The amount of NMP insoluble components of polymer A can be measured by the method described in the embodiment.

[0078] [Method for preparing polymer A]

[0079] The preparation method of the above-mentioned polymer A is not particularly limited. The polymerization method when preparing the polymer A is not particularly limited, and any method of solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. can be used. In addition, as the polymerization reaction, any reaction of ion polymerization, free radical polymerization, living free radical polymerization, etc. can be used. Moreover, the emulsifier, dispersant, polymerization initiator, chain transfer agent, etc. that can be used for the polymer can use those commonly used.

[0080] <Polymer B>

[0081] Polymer B is a component as described below: when preparing a slurry composition, it plays a role in improving the dispersibility of conductive materials such as CNT in the slurry composition, and as a result, the solid content concentration of the slurry composition can be increased. In addition, polymer B is a component that can act as a binder material in the electrode composite material layer together with polymer A. In addition, polymer B is a component that is easily soluble in an organic solvent constituting the binder composition.

[0082] The iodine value of polymer B needs to be more than 5g / 100g and less than 100g / 100g, preferably more than 10g / 100g, more preferably more than 20g / 100g. If the iodine value of polymer B is more than the above-mentioned lower limit, then in the case of preparing a slurry composition, the dispersibility of conductive materials such as CNT can be fully improved, the conductivity of the obtained electrode composite layer can be improved, and the battery characteristics (particularly rate characteristics) of the secondary battery with the electrode composite layer can be improved. In addition, if the iodine value of polymer B is below the above-mentioned upper limit, the electrode composite layer formed can be suppressed from excessively swelling the electrolyte, improving battery characteristics (particularly rate characteristics).

[0083] Moreover, the weight average molecular weight of polymer B is preferably more than 5000, more preferably more than 15000, more preferably more than 30000, preferably less than 500000, more preferably less than 400000, more preferably less than 300000. If the weight average molecular weight of polymer B is more than the above lower limit, then in the case of preparing a slurry composition, it is possible to suppress the sedimentation of conductive materials such as CNT and electrode active materials. As a result, the peel strength of the obtained electrode composite material layer can be improved. In addition, if the weight average molecular weight of polymer B is less than the above upper limit, then in the case of preparing a slurry composition, it is possible to suppress the viscosity from increasing and the dispersibility from decreasing, and it is easy to increase the solid content concentration of the slurry composition. Thus, it is possible to improve the rate characteristics and cycle characteristics of the secondary battery obtained.

[0084] The composition of polymer B is not particularly limited as long as it can satisfy the above-mentioned iodine value range, and can be any composition. Among them, polymer B preferably contains aromatic vinyl monomer units, nitrile group-containing monomer units, ethylenically unsaturated acid monomer units, and linear alkylene structural units having 4 or more carbon atoms.

[0085] As monomers that can be used to form aromatic vinyl monomer units, aromatic vinyl monomers such as styrene, α-methylstyrene, butoxystyrene, vinyltoluene, and vinylnaphthalene can be cited. In addition, aromatic vinyl monomers do not contain acidic groups. These can be used alone or in combination with more than two kinds. Among them, from the viewpoint of good copolymerizability, styrene is preferred. The proportion of the aromatic vinyl monomer unit of polymer B is preferably 30% by mass or more, more preferably 35% by mass or more, more preferably 40% by mass or more, preferably 55% by mass or less, more preferably 50% by mass or less, and more preferably 45% by mass or less when all repeating units (total of structural units and monomer units) of polymer B are set to 100% by mass.

[0086] In addition, as a monomer that can be used to form a nitrile-containing monomer unit, an α, β-ethylenically unsaturated nitrile monomer can be cited. Specifically, as an α, β-ethylenically unsaturated nitrile monomer, for example, acrylonitrile; α-halogenated acrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkyl acrylonitriles such as methacrylonitrile and α-ethylacrylonitrile, etc. These can be used alone or in combination of two or more. Among these, from the viewpoint of increasing the bonding force that can be exerted by polymer B, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is more preferred. These can be used alone or in combination of two or more. The content ratio of the nitrile-containing monomer unit of polymer B is preferably 10% by mass or more, more preferably 13% by mass or more, more preferably 18% by mass or more, preferably 40% by mass or less, more preferably 33% by mass or less, and more preferably 28% by mass or less, when all repeating units are set to 100% by mass.

[0087] In addition, as a monomer that can be used to form an ethylenically unsaturated acid monomer unit, the same monomers as the various monomers listed in the item [ethylenically unsaturated acid monomer unit] of the above-mentioned <Polymer A> can be used. Among them, acrylic acid and methacrylic acid are preferred, and methacrylic acid is more preferred, especially from the aspect of being able to efficiently capture transition metal ions that are sometimes dissolved from the positive electrode active material. The content ratio of the ethylenically unsaturated acid monomer unit of the easily soluble polymer B1 is preferably 0.1% by mass or more, more preferably 1% by mass or more, preferably 10% by mass or less, and more preferably 6% by mass or less, when all repeating units are set to 100% by mass.

[0088] Here, the linear alkylene structural unit having 4 or more carbon atoms refers to a linear alkylene structural unit having 4 or more carbon atoms (hereinafter also simply referred to as "alkylene structural unit") consisting only of the general formula: n H 2n -[wherein n is an integer of 4 or more] is a repeating unit composed of a linear alkylene structure having 4 or more carbon atoms. The method for introducing the linear alkylene structure unit having 4 or more carbon atoms into the polymer B is not particularly limited, and examples thereof include the following method (1) or (2):

[0089] (1) a method of preparing a polymer from a monomer composition containing a conjugated diene monomer, and hydrogenating the polymer to convert the conjugated diene monomer unit into a linear alkylene structural unit having 4 or more carbon atoms;

[0090] (2) A method for producing a polymer from a monomer composition containing a 1-olefin monomer having 4 or more carbon atoms, such as 1-butene and 1-hexene. These conjugated diene monomers and 1-olefin monomers can be used alone or in combination of two or more.

[0091] Among these, the method (1) is preferred because it is easy to produce a polymer.

[0092] In addition, as conjugated diene monomers that can be used in the method of (1) above, for example, conjugated diene compounds having carbon atoms of 4 or more, such as 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, and 1,3-pentadiene, can be cited. These can be used alone or in combination of two or more. Among them, 1,3-butadiene is preferred. That is, the straight-chain alkylene structural unit having carbon atoms of 4 or more is preferably a structural unit (conjugated diene hydride unit) obtained by hydrogenating the conjugated diene monomer unit, and more preferably a structural unit (1,3-butadiene hydride unit) obtained by hydrogenating the 1,3-butadiene unit. Moreover, the selective hydrogenation of the conjugated diene monomer unit can be carried out using known methods such as oil layer hydrogenation method and water layer hydrogenation method.

[0093] The polymer B can be prepared, for example, by polymerizing a monomer composition containing the above-mentioned monomers to obtain a copolymer and then hydrogenating (adding hydrogen) the obtained copolymer as necessary, and is not particularly limited.

[0094] Moreover, the content ratio of the straight-chain alkylene structural unit having 4 or more carbon atoms in the polymer B is preferably 15 mass% or more, more preferably 20 mass% or more, further preferably 25 mass% or more, preferably 50 mass% or less, more preferably 45 mass% or less, further preferably 40 mass% or less, when all repeating units are set to 100 mass%.

[0095] In addition, when the linear alkylene structural units having 4 or more carbon atoms contained in the polymer B are formed by a method of preparing a polymer from a monomer composition containing a conjugated diene monomer and hydrogenating the polymer, the total content ratio of the linear alkylene structural units having 4 or more carbon atoms contained in the polymer B and the conjugated diene monomer units remaining in the polymer B without being hydrogenated preferably satisfies the above range.

[0096] <Polymer C>

[0097] Polymer C is a component that can impart appropriate viscosity to the slurry composition when preparing the slurry composition. In addition, polymer C is a component that can function as a binder in the electrode composite material layer together with polymers A and B. In addition, polymer C is a component that is easily soluble in an organic solvent constituting the binder composition.

[0098] As described above, when all repeating units contained in polymer C are set to 100% by mass, polymer C needs to include nitrile-containing monomer units in a ratio of 70.0% by mass or more and 98.0% by mass or less. Furthermore, polymer C preferably includes nitrile-containing monomer units of more than 80.0% by mass, more preferably includes nitrile-containing monomer units of more than 80.0% by mass, preferably includes nitrile-containing monomer units of less than 98.0% by mass, and more preferably includes nitrile-containing monomer units of less than 95.0% by mass. If the ratio of nitrile-containing monomer units in polymer C is above the above lower limit, polymer C is easily adsorbed on electrode active materials in the case of preparing slurry compositions, and electrode active materials can be well coated in the form of thin films. Thus, the cycle characteristics of the secondary battery obtained can be improved. In addition, if the ratio of nitrile-containing monomer units in polymer C is below the above upper limit, the solubility of polymer C in organic solvents can be suppressed to become excessively low, polymer C is suppressed from precipitating in slurry compositions, and the solid content concentration of slurry compositions is well improved. As a result, the electrode active material and the conductive material can be contained in the slurry composition at a high concentration, and the rate characteristics and cycle characteristics of the obtained secondary battery can be improved.

[0099] As the nitrile-containing monomer that can be used to form the nitrile-containing monomer unit, the monomers identical to the various monomers listed in the item of <polymer B> can be cited. These can be used alone or in combination of two or more. Among these, as the nitrile-containing monomer, acrylonitrile and methacrylonitrile are preferred. These can be used alone or in combination of two or more.

[0100] In addition, the polymer C may contain other monomer units such as a basic group-containing monomer unit, an ethylenically unsaturated acid monomer unit, and a (meth)acrylic acid ester monomer unit in addition to the nitrile group monomer unit.

[0101] Here, the basic group-containing monomer unit can be formed using a basic group-containing monomer. As a basic group-containing monomer, it is not particularly limited, and amino monomers such as dimethylaminoethyl (methyl) acrylate, diethylaminoethyl (methyl) acrylate, aminoethyl vinyl ether, dimethylaminoethyl vinyl ether can be cited; and amide-containing monomers such as N-vinylacetamide, (methyl) acrylamide, N-methylol (methyl) acrylamide, dimethyl (methyl) acrylamide, diethyl (methyl) acrylamide, N-methoxymethyl (methyl) acrylamide, dimethylaminopropyl (methyl) acrylamide, etc. The containing ratio of the basic group-containing monomer unit in polymer C is preferably 0.5% by mass or more, more preferably 1.0% by mass or more, preferably 5% by mass or less, and more preferably 1.5% by mass or less when all repeating units are set to 100% by mass.

[0102] In addition, ethylenically unsaturated acid monomer units and (methyl) acrylic acid ester monomer units can be formed using monomers identical to the various monomers listed in the items of [ethylenically unsaturated acid monomer units] and [(methyl) acrylic acid ester monomer units] of the above-mentioned <polymer A>, respectively. And, the proportion of the ethylenically unsaturated acid monomer units in polymer C, for example, when all repeating units are set to 100% by mass, is preferably more than 0.1% by mass, more preferably more than 1% by mass, preferably less than 10% by mass, more preferably less than 5% by mass. In addition, the proportion of the (methyl) acrylic acid ester monomer units in polymer C, when all repeating units are set to 100% by mass, is preferably more than 1% by mass, more preferably less than 20% by mass, preferably more than 1% by mass, more preferably less than 10% by mass.

[0103] The polymer C can be produced by, for example, a known method as described in the section [Production method of polymer A], and is not particularly limited.

[0104] <Content ratio of polymers A to C>

[0105] Here, the content of the polymers A to C satisfying the above-mentioned properties and / or composition conditions in the adhesive composition is preferably within the following ranges, respectively, when the total content of the polymers A to C is 100% by mass.

[0106] First, the content a of the above-mentioned polymer A is preferably more than 5% by mass, more preferably more than 10% by mass, preferably less than 60% by mass, more preferably less than 50% by mass, further preferably less than 40% by mass, and particularly preferably less than 30% by mass. If the content a of polymer A is more than the above-mentioned lower limit, the peel strength of the electrode composite material layer formed using the binder composition can be fully improved. In addition, if the content a of polymer A is less than the above-mentioned upper limit, the sedimentation of polymer A can be suppressed in the case of preparing a slurry composition, so that the peel strength of the obtained electrode composite material layer can be suppressed to reduce. Moreover, the battery characteristics of the secondary battery obtained can be improved.

[0107] In addition, the content b of the above-mentioned polymer B is preferably more than 0.1% by mass, more preferably more than 1% by mass, preferably less than 50% by mass, more preferably less than 30% by mass, further preferably less than 25% by mass, and particularly preferably less than 20% by mass. If the content b of polymer B is more than the above-mentioned lower limit, then in the case of preparing a slurry composition, the dispersibility of CNT as a conductive material can be improved, and the solid content concentration of the slurry composition can be improved. As a result, the initial capacity and rate characteristics of the secondary battery obtained can be improved. In addition, if the content b of polymer B is less than the above-mentioned upper limit, then in the case of preparing a slurry composition, it is possible to suppress the sedimentation that is easy to occur. As a result, the peel strength of the electrode composite material layer obtained can be improved, and the battery characteristics of the secondary battery obtained can be improved.

[0108] Furthermore, the content c of the above-mentioned polymer C is preferably more than 20% by mass, more preferably more than 30% by mass, more preferably more than 35% by mass, more preferably more than 40% by mass, preferably less than 94% by mass. If the content c of polymer C is more than the above-mentioned lower limit, then in the case of preparing a slurry composition, it is possible to suppress the easy generation of sedimentation. As a result, the peel strength of the obtained electrode composite material layer can be improved, and the battery characteristics of the obtained secondary battery can be improved. In addition, if the content c of polymer C is below the above-mentioned upper limit, the solid content concentration of the slurry composition can be increased.

[0109] <Relationship between content ratios a to c>

[0110] For the content a of polymer A and the content b of polymer B, the value of the ratio (%) of polymer A to the total content of polymers A and B represented by the formula: a / (a+b)×100 preferably satisfies 20≤a / (a+b)×100≤90, and more preferably satisfies 25≤a / (a+b)×100≤90. If the value of the above formula: a / (a+b)×100 is 20 or more, the peel strength of the obtained electrode composite material layer can be further improved. In addition, if the value of the above formula: a / (a+b)×100 is 90 or less, the solid content concentration can be fully increased when preparing a slurry composition. As a result, the rate characteristics of the obtained secondary battery can be further improved.

[0111] In addition, for the content a of polymer A and the content c of polymer C, the value of the ratio (%) of polymer A to the total content of polymers A and C represented by the formula: a / (a+c)×100 preferably satisfies 10≤a / (a+c)×100≤50, more preferably satisfies 10≤a / (a+c)×100≤40, and further preferably satisfies 10≤a / (a+c)×100≤35. If the value of the above formula: a / (a+c)×100 is 10 or more, the bonded components can be point-bonded to each other with sufficient frequency by polymer A, and the peel strength of the obtained electrode composite material layer can be further improved. In addition, if the value of the above formula: a / (a+c)×100 is 50 or less, the electrode active material can be coated in a thin film by polymer C, and the cycle characteristics of the obtained secondary battery can be further improved.

[0112] <NMP Solubility of Polymers A to C>

[0113] The polymers A to C are preferably the following polymers: in the case of preparing a N-methyl-2-pyrrolidone mixed solution containing polymer A at a content rate a, polymer B at a content rate b, and polymer C at a content rate c with a solid content concentration of 8% by mass, the ratio of the amount of insoluble components in the mixed solution satisfies 30% by mass or more and 80% by mass or less. Moreover, the ratio of the amount of insoluble components of polymers A to C is more preferably 35% by mass or more and 75% by mass or less. If the ratio of the amount of insoluble components is 30% by mass or more, the peel strength of the obtained electrode composite material layer can be further improved. In addition, if the ratio of the amount of insoluble components is 80% by mass or less, in the case of preparing a slurry composition, the viscosity of the slurry composition can be suppressed from becoming too high, and the solid content concentration in the slurry composition can be fully increased. As a result, the rate characteristics and cycle characteristics of the obtained secondary battery can be improved.

[0114] <Other adhesive materials>

[0115] The adhesive composition of the present invention may also contain other adhesive materials different from these in addition to the above-mentioned polymers A to C. As such adhesive materials, fluorine-based polymer adhesive materials such as polyvinylidene fluoride, polyvinyl acetate-based adhesive materials, polyacrylic acid-based adhesive materials, polyvinyl alcohol-based adhesive materials, etc. may be cited. In addition, when the adhesive composition of the present invention contains other adhesive materials, the content ratio of the other adhesive materials is preferably less than 50% by mass, more preferably less than 40% by mass, further preferably less than 30% by mass, and may also be 0% by mass, i.e., the adhesive composition of the present invention may contain only the above-mentioned polymers A to C as adhesive materials.

[0116] <Organic Solvents>

[0117] In addition, examples of the organic solvent of the adhesive composition of the present invention include alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, tert-butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, and neopentyl alcohol; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; diethyl ether, dimethicone, and dimethicone; Ethers such as alkanes and tetrahydrofuran, amide-based polar organic solvents such as N,N-dimethylformamide and N-methyl-2-pyrrolidone (NMP), aromatic hydrocarbons such as toluene, xylene, chlorobenzene, o-dichlorobenzene, and p-dichlorobenzene, etc. These may be used alone or in combination of two or more.

[0118] Among them, NMP is preferred as the organic solvent.

[0119] <Other ingredients>

[0120] The binder composition of the present invention may also contain reinforcing materials, leveling agents, viscosity modifiers, electrolyte additives and other components in addition to the above-mentioned components. As long as these do not affect the battery reaction, there is no particular restriction, and known components can be used, such as the components described in International Publication No. 2012 / 115096. In addition, these components can be used alone, or two or more can be used in combination in any proportion.

[0121] <Preparation of Adhesive Composition>

[0122] Moreover, the binder composition of the present invention can be prepared by mixing the above-described polymers A to C as binder materials, an organic solvent, and any other components by known methods. Specifically, the binder composition can be prepared by mixing the above components using a mixer such as a ball mill, sand mill, bead mill, pigment disperser, grinder, ultrasonic disperser, homogenizer, planetary mixer, Filmix, etc. In addition, the solid content concentration of the binder composition is not particularly limited and can be, for example, 5% by mass or more and 60% by mass or less.

[0123] (Slurry composition for non-aqueous secondary battery electrode)

[0124] The slurry composition for non-aqueous secondary battery electrode of the present invention contains an electrode active material, a conductive material containing carbon nanotubes, and the above-described binder composition, and optionally further contains other components. That is, the slurry composition of the present invention contains an electrode active material, carbon nanotubes, the above-described polymers A to C, and an organic solvent, and optionally further contains other components. Moreover, since the slurry composition of the present invention contains the above-described binder composition, an electrode composite material layer having a sufficiently high solid content concentration and high peel strength can be formed. Therefore, according to the slurry composition of the present invention, a secondary battery can exhibit excellent battery characteristics.

[0125] In addition, as an example below, the case where the slurry composition for secondary battery electrode is a slurry composition for positive electrode of a lithium ion secondary battery will be described, but the present invention is not limited to the following example.

[0126] <Electrode active material>

[0127] The electrode active material is a material that conducts electrons in the electrode of a secondary battery. Moreover, as the positive electrode active material for a lithium ion secondary battery, a material that can absorb and release lithium is usually used.

[0128] Specifically, as the positive electrode active material for a lithium ion secondary battery, there is no particular limitation, and examples include lithium-containing cobalt oxide (LiCoO2), lithium manganate (LiMn2O4), lithium-containing nickel oxide (LiNiO2), lithium-containing composite oxide of Co-Ni-Mn (Li(CoMnNi)O2), lithium-containing composite oxide of Ni-Mn-Al, lithium-containing composite oxide of Ni-Co-Al, olivine-type lithium iron phosphate (LiFePO4), olivine-type lithium manganese phosphate (LiMnPO4), Li2MnO3-LiNiO2-based solid solution, Li 1+x Mn 2-x O4 (0 < X < 2) represents a lithium-rich spinel compound, Li[Ni 0.17 Li 0.2 Co 0.07 Mn0.56 ]O2、LiNi 0.5 Mn 1.5 O4 and other known positive electrode active materials.

[0129] In addition, the particle size of the positive electrode active material is not particularly limited and can be the same as the positive electrode active material used in the past. In addition, the content ratio of the positive electrode active material in the slurry composition can be, for example, 90% by mass or more and 99% by mass or less when the total solid content in the slurry composition is 100% by mass.

[0130] <Conductive Materials>

[0131] The conductive material is a material for ensuring electrical contact between electrode active materials. Moreover, the slurry composition of the present invention preferably contains fibrous carbon material CNT as a conductive material. This is because the CNT can be well dispersed in the slurry composition by the binder composition of the present invention, so the dispersibility of other solid components such as the electrode active material in the slurry composition can be improved. As CNT, single-layer or multi-layer carbon nanotubes (multi-layer carbon nanotubes include stacked cups) can be cited. Moreover, the specific surface area of ​​CNT is preferably 50m 2 / g or more, more preferably 70m 2 / g or more, more preferably 100m 2 / g or more, preferably 400 m 2 / g or less, more preferably 350m 2 / g or less, more preferably 300m 2 / g or less. If the specific surface area of ​​CNT is within the above range, good dispersibility of CNT in the slurry composition can be ensured, and the viscosity of the slurry composition can be stabilized. In addition, in the present invention, "specific surface area" refers to the nitrogen adsorption specific surface area measured using the BET method.

[0132] Furthermore, as a conductive material other than CNT, carbon black (for example, acetylene black, Ketjen black (registered trademark), furnace black, etc.), carbon nanohorns, ground carbon fibers obtained by sintering and crushing polymer fibers, single-layer or multi-layer graphene, non-woven fabrics formed by polymer fibers, sintered and obtained, and other conductive carbon materials such as carbon non-woven fabric sheets; various metal fibers or foils, etc. These can be used alone or in combination of two or more. In addition, the particle size of the conductive material is not particularly limited and can be the same as the conductive material used all the time. In addition, the content ratio of the conductive material in the slurry composition can be, for example, 0.1% by mass or more and 3% by mass or less when the total solid content in the slurry composition is 100% by mass.

[0133] <Binder Composition>

[0134] As the binder composition, the above-mentioned binder composition for non-aqueous secondary battery electrodes of the present invention is used. In addition, the content of the binder composition in the slurry composition can be, for example, 0.1% by mass or more and 5% by mass or less when the total solid content in the slurry composition is 100% by mass.

[0135] <Other ingredients>

[0136] The other components that can be added to the slurry composition are not particularly limited, and examples thereof include the same components as those that can be added to the binder composition of the present invention. In addition, the other components may be used alone or in combination of two or more in any ratio.

[0137] <Method for producing slurry composition>

[0138] The above-mentioned slurry composition can be manufactured by dissolving or dispersing the above-mentioned components in an organic solvent. More specifically, the above-mentioned method for manufacturing the slurry composition of the present invention preferably includes a premixing step of mixing at least CNT (conductive material), the above-mentioned polymer B and an organic solvent to obtain a premix; and a main mixing step of mixing the obtained premix with at least polymer A and polymer C. In this way, after mixing CNT and polymer B in the premixing step, the main mixing step is implemented, thereby further improving the dispersibility of CNT in the slurry composition.

[0139] [Pre-mixing process]

[0140] In the premixing process, at least CNT, polymer B and organic solvent are mixed to obtain a premix. As a mixing method, there is no particular limitation, and a mixing method using a ball mill, a sand mill, a bead mill, a pigment disperser, a grinder, an ultrasonic disperser, a homogenizer, a planetary mixer, a Filmix and other mixers can be cited. In addition, the stirring conditions in the premixing process are preferably stirring conditions that can produce a stronger stirring force than the stirring conditions in the subsequent main mixing process. This is because by stirring and mixing CNT and polymer B with a strong stirring force in the premixing process, CNT can be effectively suppressed from agglomerating in the slurry composition. When performing the premixing process, other polymers other than polymer B can also be added. In the case of adding other polymers other than polymer B (i.e., polymers A and C and other polymers) in the premixing process, it is preferred that the addition amount of the other polymers is less than 1 / 2 of the total addition amount (mass basis). By making polymer B pre-adsorbed on CNT before adding other polymers, the dispersibility of CNT in the obtained slurry composition can be effectively improved. Furthermore, when a component other than CNT is added as a conductive material, the component may be added in this step.

[0141] Examples of the organic solvent include the same organic solvents as those that can be added to the adhesive composition of the present invention. In addition, as the organic solvent used in this step, an organic solvent contained in the adhesive composition can also be used.

[0142] In addition, the ratio of CNT to polymer B in the premixing process is, for example, relative to 1.0 parts by mass of CNT, preferably polymer B (solid content conversion amount) is 0.01 parts by mass or more and 0.5 parts by mass or less. By making the ratio of CNT to polymer B in the premixing process within the above range, it is possible to further well balance the increase in the solid content concentration of the slurry composition and the increase in the rate characteristics of the secondary battery obtained.

[0143] [Main mixing process]

[0144] In the main mixing process, the premix obtained in the above-mentioned premixing process is mixed with at least polymers A and C. In addition, in this process, in addition to polymers A and C, electrode active materials and any other components mentioned above can also be added. In addition, in order to optimize the mixing conditions, an organic solvent can also be added in this process. Of course, it is also possible not to add electrode active materials in this process, but to add them in the later stage of this process.

[0145] The total amount of various components added in the method for producing the slurry composition is as described in detail in the items (Binder composition for non-aqueous secondary battery electrodes) and (Slurry composition for non-aqueous secondary battery electrodes).

[0146] (Electrode for non-aqueous secondary batteries)

[0147] The electrode for a non-aqueous secondary battery of the present invention has a current collector and an electrode composite material layer formed on the current collector. Moreover, the electrode composite material layer is formed using the above-mentioned slurry composition. That is, the electrode composite material layer contains at least an electrode active material, carbon nanotubes, and a polymer from polymers A to C, and optionally contains other components. In addition, the components contained in the electrode composite material layer are the components contained in the above-mentioned slurry composition, and the preferred existence ratio of these components is the same as the preferred existence ratio of the components in the slurry composition. In addition, the above-mentioned "polymer from polymer A" can maintain a particle shape in the electrode composite material layer, or it can be in other shapes without maintaining a particle shape. In addition, the polymer from polymer B is preferably present in a manner adjacent to CNT. Furthermore, the polymer from polymer C is preferably present in a manner that covers at least a portion of the surface of a solid component such as an electrode active material.

[0148] Furthermore, the non-aqueous secondary battery electrode of the present invention is formed using a slurry composition containing the binder composition of the present invention, and thus has high peel strength. Therefore, if the electrode is used, a secondary battery having excellent battery characteristics such as rate characteristics and cycle characteristics can be obtained.

[0149] <Method for producing electrode>

[0150] In addition, the electrode for the non-aqueous secondary battery of the present invention can be manufactured by, for example, the following steps: a step of applying the above-mentioned slurry composition on a current collector (coating step), and a step of drying the slurry composition applied on the current collector to form an electrode composite material layer on the current collector (drying step).

[0151] [Coating process]

[0152] As a method for applying the above-mentioned slurry composition on the current collector, it is not particularly limited, and a known method can be used. Specifically, as a coating method, a doctor blade method, an immersion method, a reverse roll coating method, a direct roll coating method, a gravure printing method, an extrusion method, a brush coating method, etc. can be used. At this time, the slurry composition can be applied only on one side of the current collector, or it can be applied on both sides. The thickness of the slurry film on the current collector before drying after coating can be appropriately set according to the thickness of the electrode composite material layer obtained by drying.

[0153] Here, as the current collector for coating the slurry composition, a material having conductivity and electrochemical durability can be used. Specifically, as the current collector, a current collector formed of, for example, iron, copper, aluminum, nickel, stainless steel, titanium, tantalum, gold, platinum, etc. can be used. In addition, the above-mentioned materials can be used alone or in combination of two or more in any ratio.

[0154] [Drying process]

[0155] The method for drying the slurry composition on the current collector is not particularly limited, and a known method can be used, such as a drying method using warm air, hot air, or low-humidity air, a vacuum drying method, or a drying method using irradiation of infrared rays, electron beams, etc. By drying the slurry composition on the current collector in this way, an electrode composite material layer can be formed on the current collector to obtain an electrode for a secondary battery having a current collector and an electrode composite material layer.

[0156] In addition, after the drying step, the electrode composite material layer can be subjected to pressure treatment using metal molding or roller pressing. By pressure treatment, the adhesion of the electrode composite material layer to the current collector can be improved. In addition, in the case where the electrode composite material layer includes a curable polymer, it is preferred that the above polymer is cured after forming the electrode composite material layer.

[0157] (Non-aqueous secondary battery)

[0158] The non-aqueous secondary battery of the present invention has the electrode for the non-aqueous secondary battery of the present invention. More specifically, the non-aqueous secondary battery of the present invention has a positive electrode, a negative electrode, an electrolyte, and a separator, and the electrode for the non-aqueous secondary battery of the present invention is used as at least one of the positive electrode and the negative electrode. Moreover, the non-aqueous secondary battery of the present invention has excellent battery characteristics such as rate characteristics and cycle characteristics because it has the electrode for the non-aqueous secondary battery of the present invention.

[0159] The nonaqueous secondary battery of the present invention preferably uses the nonaqueous secondary battery electrode of the present invention as a positive electrode. In addition, the following describes a case where the secondary battery is a lithium ion secondary battery as an example, but the present invention is not limited to the following example.

[0160] <Electrode>

[0161] Here, as an electrode other than the above-mentioned electrode for non-aqueous secondary batteries that can be used in the non-aqueous secondary battery of the present invention, there is no particular limitation, and known electrodes that can be used to manufacture non-aqueous secondary batteries can be used. Specifically, as an electrode other than the above-mentioned electrode for non-aqueous secondary batteries, an electrode formed by forming an electrode composite material layer on a current collector using a known manufacturing method can be used.

[0162] <Electrolyte>

[0163] As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent can generally be used. As the supporting electrolyte of a lithium ion secondary battery, for example, a lithium salt can be used. As the lithium salt, for example: LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. can be cited. Among them, since they are easily soluble in solvents and show a high degree of dissociation, LiPF6, LiClO4, CF3SO3Li are preferred, and LiPF6 is particularly preferred. In addition, one electrolyte can be used alone, or two or more electrolytes can be used in combination in any ratio. Generally, there is a tendency that the higher the degree of dissociation of the supporting electrolyte, the higher the lithium ion conductivity, so the lithium ion conductivity can be adjusted according to the type of supporting electrolyte.

[0164] As the organic solvent used in the electrolyte, as long as it is an organic solvent that can dissolve the supporting electrolyte, it is not particularly limited, and carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), ethyl methyl carbonate (EMC) can be preferably used; esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as cyclopentane and dimethyl sulfoxide, etc. In addition, a mixed solution of these solvents can also be used. Among them, due to the high dielectric constant and wide stable potential region, carbonates are preferably used, and a mixture of ethylene carbonate and diethyl carbonate is further preferably used.

[0165] In addition, the concentration of the electrolyte in the electrolytic solution can be appropriately adjusted. In addition, a known additive such as vinylene carbonate can be added to the electrolytic solution.

[0166] <Spacer>

[0167] As a separator, there is no particular limitation, and for example, the separators described in Japanese Patent Publication No. 2012-204303 can be used. Among these, from the aspect of being able to make the overall film thickness of the separator thinner, thereby being able to increase the ratio of the electrode active material in the secondary battery and increase the capacity per unit volume, a microporous membrane formed of a polyolefin resin (polyethylene, polypropylene, polybutylene, polyvinyl chloride) is preferred.

[0168] <Method for producing non-aqueous secondary battery>

[0169] The non-aqueous secondary battery of the present invention can be manufactured by, for example, the following method: overlapping the positive electrode and the negative electrode through a spacer, winding and folding the battery according to the shape of the battery as needed, and placing the battery container, injecting electrolyte into the battery container, and sealing. In order to prevent the internal pressure of the secondary battery from rising, overcharging and discharging, etc., fuses, PTC elements and other overcurrent protection elements, porous metal mesh, guide plates, etc. can be provided as needed. The shape of the secondary battery can be, for example, any of coin-shaped, button-shaped, sheet-shaped, cylindrical, square, flat, etc.

[0170] Example

[0171] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these Examples. In the following description, "%" and "part" indicating an amount are based on mass unless otherwise specified.

[0172] In a polymer produced by copolymerizing multiple types of monomers, the proportion of a monomer unit formed by polymerizing a certain monomer in the above polymer is usually consistent with the ratio (feed ratio) of the certain monomer in all monomers used to polymerize the polymer unless otherwise specified.

[0173] In addition, in the examples and comparative examples, the NMP solubility of polymer A, the NMP solubility of polymers B and C, the iodine value and weight average molecular weight of polymer B, the ratio of the NMP insoluble components of the mixture of polymers A to C, and the solid content concentration of the slurry composition are measured or confirmed as described below. In addition, in the examples and comparative examples, the peel strength of the electrode composite material layer and the initial capacity, rate characteristics, and cycle characteristics of the secondary battery are evaluated as described below.

[0174] <NMP Solubility of Polymer A>

[0175] The polymer A prepared in the examples and comparative examples was vacuum dried for 24 hours at 25°C to obtain a dry polymer (mass: W1g). The obtained dry polymer was placed in NMP at 60°C for 72 hours and filtered with 200 mesh to separate the insoluble components. After washing the insoluble components with methanol, it was dried for 24 hours at 25°C to obtain a dry insoluble component (mass: W2g). The amount of NMP insoluble components of polymer A was calculated based on the above W1 and W2 (=W2 / W1×100 (mass %)). Then, for polymer A prepared in all the examples and comparative examples, it was confirmed that the amount of NMP insoluble components was 70% by mass or more.

[0176] <NMP Solubility of Polymers B and C>

[0177] The solubility of polymers B and C in NMP was confirmed by the following procedure.

[0178] 25 g of a composition containing a polymer in N-methyl-2-pyrrolidone (NMP) prepared in the examples and comparative examples was added dropwise to 1 L of methanol to precipitate the polymer. The precipitated polymer was vacuum dried at 25°C for 24 hours to obtain a dry polymer (mass: W1g). The obtained dry polymer was placed in NMP at 60°C for 72 hours and filtered with 200 mesh to separate the insoluble components. After washing the insoluble components with methanol, it was dried at 25°C for 24 hours to obtain a dry insoluble component (mass: W2g). The amount of NMP insoluble components of the polymer was calculated based on the above W1 and W2 (=W2 / W1×100 (mass %)). Then, for polymers B and C prepared in all the examples and comparative examples, it was confirmed that the amount of NMP insoluble components was less than 50% by mass.

[0179] <Iodine value of polymer B>

[0180] 100 g of the aqueous dispersion of polymer B prepared in Examples and Comparative Examples (before solvent substitution with NMP) was coagulated in 1 liter of methanol and then vacuum dried at 60° C. for 12 hours. The iodine value of the obtained dried easily soluble polymer B was measured in accordance with JIS K6235 (2006).

[0181] <Weight Average Molecular Weight of Polymer B>

[0182] The weight average molecular weight of the polymer B prepared in the examples and comparative examples was measured by gel permeation chromatography (GPC). Specifically, a calibration curve was prepared using a polystyrene standard substance, and the weight average molecular weight was calculated as a standard substance conversion value. In addition, the measurement conditions are as follows.

[0183] <<Measurement Conditions>>

[0184] Measuring device

[0185] Column: TSKgelα-M×2 columns ( (Tosoh Corporation)

[0186] Measurement conditions

[0187] Eluent: dimethylformamide (50 mM lithium bromide, 10 mM phosphoric acid)

[0188] Sulfuric acid: 0.5mL / min.

[0189] Sample concentration: about 0.5g / L (solid content concentration)

[0190] Injection volume: 200 μL

[0191] Column temperature: 40°C

[0192] Detector: Differential refractive index detector RI (HLC-8320GPC RI detector manufactured by Tosoh Corporation)

[0193] Detector conditions: RI: Pol(+), Res(1.0s)

[0194] Molecular weight marker: Standard polystyrene kit PSt Quick K manufactured by Tosoh

[0195] <Ratio of NMP-insoluble component in the mixture of polymers A to C>

[0196] In an environment of temperature 25°C, polymers A to C prepared or prepared in the examples and comparative examples were added to the NMP solvent at the mixing ratio described in the examples, and the solid content concentration was 8%, and 100 g of a (polymer A to C)-NMP mixed solution was prepared. The prepared mixed solution was filtered through a metal mesh of 80 mesh, and the filtrate was weighed to calculate the ratio (mass %) of the mass of the insoluble components to the total solid content added.

[0197] <Solid Content Concentration of Slurry Composition>

[0198] The same process as the <Preparation of the positive electrode slurry composition> process in the examples and comparative examples was performed. In the main mixing process, N-methylpyrrolidone (NMP) was added to adjust the slurry viscosity so that the slurry viscosity was 3500 mPa·s when measured at 23° C. using a B-type viscometer (rotation speed: 60 rpm). The solid content concentration of the obtained positive electrode slurry composition was evaluated according to the following criteria.

[0199] A: More than 78%

[0200] B: 75% or more and less than 78%

[0201] C: 72% or more and less than 75%

[0202] D: less than 72%

[0203] <Peel Strength of Electrode Composite Layer>

[0204] The positive electrode for lithium ion secondary battery made in the embodiment and comparative example is cut into a rectangle with a length of 100mm and a width of 10mm as a test piece, and the surface with the positive electrode composite material layer is made downward, and a transparent tape (based on the transparent tape of JIS Z1522) is pasted on the surface of the positive electrode composite material layer, and one end of the current collector is stretched in the vertical direction, and the stress during the tensile peeling at a speed of 100mm / minute is measured (in addition, the transparent tape is fixed on the test bench). 3 measurements are carried out, and the average value is obtained as the peel strength, and it is evaluated according to the following benchmarks. The larger the value of the peel strength, the more firmly the positive electrode composite material layer and the current collector are in close contact, and the higher the peel strength of the electrode (positive electrode) composite material layer.

[0205] A: Peel strength is 30N / m or more

[0206] B: Peel strength is 25 N / m or more and less than 30 N / m

[0207] C: Peel strength is 20 N / m or more and less than 25 N / m

[0208] D: Peel strength less than 20N / m

[0209] <Initial Capacity of Secondary Battery>

[0210] After injecting the electrolyte into the lithium-ion secondary battery prepared in the embodiment and the comparative example, it was left to stand at a temperature of 25°C for 5 hours. Next, it was charged at a temperature of 25°C and a constant current method of 0.2C until the battery voltage was 3.65V, and then an aging treatment was performed at a temperature of 60°C for 12 hours. Then, it was discharged at a temperature of 25°C and a constant current method of 0.2C until the battery voltage was 3.00V. After that, CC-CV charging was performed at a constant current of 0.2C (upper limit battery voltage 4.20V), and CC discharge was performed at a constant current of 0.2C until the battery voltage was 3.00V. The 0.2C charge and discharge was repeated 3 times. The third discharge capacity was taken as the initial capacity, and the value of initial capacity / theoretical capacity was evaluated by the following benchmark. The larger the value, the higher the initial discharge capacity.

[0211] A: Initial capacity / theoretical capacity is 0.78 or more

[0212] B: Initial capacity / theoretical capacity is greater than 0.75 and less than 0.78

[0213] C: Initial capacity / theoretical capacity is 0.73 or more and less than 0.75

[0214] D: Initial capacity / theoretical capacity is less than 0.73

[0215] <Rate Characteristics of Secondary Batteries>

[0216] After injecting the electrolyte into the lithium-ion secondary battery prepared in the embodiment and the comparative example, it was left to stand at a temperature of 25°C for 5 hours. Next, it was charged at a temperature of 25°C and 0.2C with a constant current method until the battery voltage reached 3.65V, and then aged at a temperature of 60°C for 12 hours. Then, it was discharged at a temperature of 25°C and 0.2C with a constant current method until the battery voltage reached 3.00V. After that, CC-CV charging was performed at a constant current of 0.2C (upper limit battery voltage 4.20V), and CC discharge was performed at a constant current of 0.2C until the battery voltage reached 3.00V. This 0.2C charge and discharge was repeated 3 times.

[0217] Next, at a temperature of 25°C, a constant current charge and discharge of 0.2C is performed at a battery voltage between 4.20-3.00V, and the discharge capacity at this time is defined as C0. Then, CC-CV charging is performed at a constant current of 0.2C in the same manner, and CC discharge is performed at a constant current of 2.0C to 3.00V at a temperature of 25°C, and the discharge capacity at this time is defined as C1. Then, the ratio (percentage, capacity retention rate) of the discharge capacity (C1) at 2.0C represented by (C1 / C0)×100(%) to the discharge capacity (C0) at 0.2C is calculated as the rate characteristic, and evaluated according to the following criteria. The larger the value of the capacity retention rate, the less the decrease in discharge capacity at high current, and the lower the internal impedance (that is, the better the rate characteristic).

[0218] A: Capacity maintenance rate is more than 75%

[0219] B: Capacity maintenance rate is 73% or more and less than 75%

[0220] C: Capacity maintenance rate is 70% or more and less than 73%

[0221] D: Capacity maintenance rate and less than 70%

[0222] <Cycle characteristics of secondary batteries>

[0223] After the lithium ion secondary battery prepared in the embodiment and the comparative example is injected with the electrolyte, it is left to stand at a temperature of 25°C for 5 hours. Next, it is charged at a temperature of 25°C and 0.2C with a constant current method until the battery voltage is 3.65V, and then an aging treatment is performed at a temperature of 60°C for 12 hours. Then, it is discharged at a temperature of 25°C and 0.2C with a constant current method until the battery voltage is 3.00V. After that, CC-CV charging is performed at a constant current of 0.2C (upper limit battery voltage 4.20V), and CC discharge is performed at a constant current of 0.2C until the battery voltage is 3.00V. Repeat the 0.2C charge and discharge 3 times. Then, in an environment of a temperature of 25°C, 100 cycles of charge and discharge operations are performed with a battery voltage of 4.20-3.00V and a charge and discharge rate of 1.0C. At this time, the discharge capacity of the first cycle is defined as X1, and the discharge capacity of the 100th cycle is defined as X2. Using the discharge capacity X1 and the discharge capacity X2, the capacity retention rate represented by (X2 / X1)×100 (%) (the ratio of the discharge capacity at the 100th cycle to the discharge capacity at the 1st cycle) was calculated as the cycle characteristics, and the evaluation was performed according to the following criteria. The larger the value of the capacity retention rate, the better the cycle characteristics.

[0224] A: Capacity maintenance rate is more than 93%

[0225] B: Capacity maintenance rate is 90% or more and less than 93%

[0226] C: Capacity maintenance rate is 87% or more and less than 90%

[0227] D: Capacity maintenance rate is less than 87%

[0228] (Example 1)

[0229] <Preparation of Polymer A>

[0230] 100 parts of ion exchange water were added to a 1L flask with a rubber stopper and a stirrer, the gas phase was replaced with nitrogen, and after heating to 80°C, 0.3 parts of ammonium persulfate (APS) as a polymerization initiator was dissolved in 5.7 parts of ion exchange water and added to the flask.

[0231] On the other hand, 40 parts of ion exchange water, 0.18 parts of sodium polyoxyethylene alkyl ether sulfate (Kao Corporation, "LATEMUL E-118B") as an emulsifier, and 39.1 parts of n-butyl acrylate (BA) as a (meth)acrylate monomer, 55.1 parts of methyl methacrylate (MMA), 5.0 parts of methacrylic acid (MAA) as an ethylenically unsaturated acid monomer, and 0.8 parts of allyl methacrylate (AMA) as a crosslinking monomer were mixed in another container to obtain a monomer composition. The monomer composition was continuously added to the above-mentioned 1L flask with a rubber stopper over 1 hour to perform polymerization. During the addition, the reaction was carried out at 80°C. After the addition was completed, the reaction was further stirred at 80°C for 1 hour to terminate the reaction.

[0232] Next, an appropriate amount of NMP was added to the obtained aqueous dispersion of polymer A to obtain a mixture, and then, water and excess NMP were removed from the mixture by vacuum distillation at 90°C to obtain an NMP dispersion of polymer A (solid content concentration: 8%).

[0233] The obtained NMP dispersion of polymer A was dried at 120°C for 1 hour to prepare a film with a thickness of 0.2 mm to 0.5 mm. The polymer A was confirmed to be in a granular form by scanning electron microscopy (SEM), thereby confirming that the granular polymer A was dispersed in the dispersion medium (NMP).

[0234] <Preparation of Polymer B1-1>

[0235] In an autoclave with a stirrer, 240 parts of ion exchange water, 25 parts of sodium alkylbenzene sulfonate as an emulsifier, 24 parts of acrylonitrile as a nitrile-containing monomer, 43 parts of styrene as an aromatic vinyl monomer, and 4 parts of methacrylic acid as an ethylenically unsaturated acid monomer were added in sequence, and after replacing the interior with nitrogen, 29 parts of 1,3-butadiene as a conjugated diene monomer were pressed in, and 0.25 parts of ammonium persulfate as a polymerization initiator were added, and a polymerization reaction was carried out at a reaction temperature of 40°C to obtain a copolymer containing a nitrile-containing monomer unit, an aromatic vinyl monomer unit, an ethylenically unsaturated acid monomer unit, and a conjugated diene monomer unit. The iodine value of the obtained copolymer (polymer before hydrogenation) was measured as described above, and the result was 140g / 100g. In addition, the polymerization conversion rate was 85%.

[0236] Ion exchange water is added to the polymer before hydrogenation to obtain 400mL (total solid content 48g) of the solution with total solid content concentration adjusted to 12% by mass. The solution is put into an autoclave with a stirrer of volume 1L, nitrogen is passed through for 10 minutes, after removing the dissolved oxygen in the solution, 50mg of palladium acetate as a hydrogenation catalyst is dissolved in 180mL of ion exchange water to which 4 times of moles of nitric acid have been added relative to palladium (Pd), and added. After replacing the system twice with hydrogen, the contents of the autoclave are heated to 50°C in the state of pressurizing with hydrogen until the gauge pressure is 3MPa, so that it is subjected to a 6-hour hydrogenation reaction (hydrogenation reaction of the first stage).

[0237] Next, the autoclave was returned to atmospheric pressure, and 25 mg of palladium acetate as a hydrogenation catalyst was dissolved in 60 mL of water to which 4 times the mole of nitric acid was added relative to Pd, and then added. After the system was replaced twice with hydrogen, the contents of the autoclave were heated to 50° C. while being pressurized with hydrogen until the gauge pressure was 3 MPa, and a hydrogenation reaction was carried out for 6 hours (hydrogenation reaction in the second stage).

[0238] Thereafter, the contents were returned to room temperature, the system was placed in a nitrogen atmosphere, and then concentrated using a rotary evaporator until the solid content concentration became 40%, thereby obtaining an aqueous dispersion of polymer B1-1 as polymer B.

[0239] To 100 parts of the aqueous dispersion of the polymer B1-1 obtained above, 320 parts of N-methylpyrrolidone (hereinafter referred to as "NMP") as a solvent were added, and water was evaporated under reduced pressure to obtain an NMP dispersion of the polymer B1-1.

[0240] The weight average molecular weight and iodine value of polymer B1-1 were measured according to the above-mentioned methods.

[0241] <Preparation of Polymer C1>

[0242] In a reactor A equipped with a mechanical stirrer and a condenser, 85 parts of ion exchange water and 0.2 parts of sodium dodecylbenzene sulfonate were added under a nitrogen atmosphere. While the contents were stirred, they were heated to 55° C., and 0.3 parts of a 5.0% aqueous solution of potassium persulfate were added to the reactor A. Next, in a container B different from the above reactor A, 94.0 parts of acrylonitrile as a nitrile group-containing monomer, 1.0 parts of acrylamide as a basic group-containing monomer, 2.0 parts of acrylic acid as an ethylenically unsaturated acid monomer, 3.0 parts of n-butyl acrylate as a (meth)acrylate monomer, 0.6 parts of sodium dodecylbenzene sulfonate, 0.035 parts of tert-dodecyl mercaptan, 0.4 parts of polyoxyethylene lauryl ether, and 80 parts of ion exchange water were added under a nitrogen atmosphere, and the mixture was stirred and emulsified to prepare a monomer mixed solution. Then, the monomer mixture was added to the reactor A at a constant speed over 5 hours while being stirred and emulsified, and reacted until the polymerization conversion rate reached 95%, thereby obtaining an aqueous dispersion of a polyacrylonitrile (PAN) copolymer (polymer C1) mainly containing acrylonitrile units (94% by mass). Next, an appropriate amount of NMP was added to the obtained aqueous dispersion of polymer C1 to obtain a mixture. Then, reduced pressure distillation was performed at 90° C. to remove water and excess NMP from the mixture, thereby obtaining an NMP solution of polymer C1 (solid content concentration: 8%).

[0243] <Preparation of slurry composition for secondary battery positive electrode>

[0244] [Pre-mixing process]

[0245] One portion of CNT (specific surface area measured by BET method: 150 m 2 / g) and 0.06 parts of polymer B1-1 in terms of solid content, and further NMP as an organic solvent was added so that the solid content concentration was 4% by mass, and stirred and mixed at a temperature of 25±3° C. and a rotation speed of 3000 rpm for 10 minutes to obtain a premix.

[0246] [Main mixing process]

[0247] To the premix obtained in the above step, 97 parts of Co-Ni-Mn lithium composite oxide active material NMC532 (LiNi 5 / 10 Co 2 / 10 Mn 3 / 10O2), 0.38 parts (equivalent amount of solid content) of polymer A and 1.56 parts (equivalent amount of solid content) of polymer C were stirred and mixed at a temperature of 25±3°C and a rotation speed of 50 rpm to obtain a slurry composition for a positive electrode. The viscosity of the slurry composition for a positive electrode was measured using a B-type viscometer at 60 rpm (rotor M4) and 25±3°C, and the viscosity was 3600 mPa·s.

[0248] <Manufacturing of positive electrode>

[0249] The positive electrode slurry composition obtained by the above method was coated with a notch wheel coater at a coating amount of 20±0.5 mg / cm 2 The 20 μm thick aluminum foil was coated on the current collector.

[0250] The slurry composition on the aluminum foil was dried by conveying it in an oven at 100°C for 2 minutes at a speed of 200 mm / min and further in an oven at 130°C for 2 minutes to obtain a positive electrode material having a positive electrode composite material layer formed on the current collector.

[0251] Thereafter, the positive electrode composite material layer side of the prepared positive electrode raw material was roll-pressed at a temperature of 25±3°C and a linear pressure of 14 t (tons) to obtain a positive electrode composite material layer density of 3.50 g / cm 3 For the obtained positive electrode, the peel strength of the positive electrode composite material layer was evaluated according to the above method. The results are shown in Table 1.

[0252] <Preparation of Negative Electrode Binder Composition>

[0253] In a 5MPa pressure-resistant container with a stirrer, 65 parts of styrene, 35 parts of 1,3-butadiene, 2 parts of itaconic acid, 1 part of 2-hydroxyethyl acrylate, 0.3 parts of tert-dodecyl mercaptan as a molecular weight regulator, 5 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion exchange water, and 1 part of potassium persulfate as a polymerization initiator were added, stirred thoroughly, and heated to 55°C to initiate polymerization. When the monomer consumption reaches 95.0%, the reaction is terminated by cooling. A 5% sodium hydroxide aqueous solution is added to the aqueous dispersion containing the polymer obtained in this way, and the pH is adjusted to 8. Then, the unreacted monomers are removed by heating and reduced pressure distillation. Then, by cooling until the temperature is below 30°C, an aqueous dispersion containing a negative electrode binder is obtained.

[0254] <Preparation of Negative Electrode Slurry Composition>

[0255] In a planetary mixer, 48.75 parts of artificial graphite (theoretical capacity: 360 mAh / g) as a negative electrode active material, 48.75 parts of natural graphite (theoretical capacity: 360 mAh / g), and 1 part of carboxymethyl cellulose as a thickener in terms of solid content were added. Furthermore, the mixture was diluted with ion exchange water to a solid content concentration of 60%, and then kneaded at a speed of 45 rpm for 60 minutes. Then, 1.5 parts of the above-obtained negative electrode binder composition in terms of solid content were added and kneaded at a speed of 40 rpm for 40 minutes. Then, ion exchange water was added so that the viscosity was 3000 ± 500 mPa·s (measured by a B-type viscometer at 25°C and 60 rpm), thereby preparing a negative electrode slurry composition.

[0256] <Manufacturing of negative electrode>

[0257] The negative electrode slurry composition was coated with a notch wheel coater in an amount of 11±0.5 mg / cm 2 The copper foil coated with the negative electrode slurry composition was then conveyed in an oven at 80°C for 2 minutes at a speed of 400 mm / min, and then in an oven at 110°C for 2 minutes, thereby drying the slurry composition on the copper foil to obtain a negative electrode raw material having a negative electrode composite material layer formed on the current collector.

[0258] Then, the negative electrode composite material layer side of the prepared negative electrode raw material was roll-pressed at a temperature of 25±3°C and a linear pressure of 11 t (tons) to obtain a negative electrode composite material layer with a density of 1.60 g / cm 3 of the negative electrode.

[0259] <Preparation of Separator for Secondary Battery>

[0260] A single-layer polypropylene spacer (manufactured by Celgard, “#2500”) was used.

[0261] <Production of non-aqueous secondary batteries>

[0262] Using the above-mentioned negative electrode, positive electrode and separator, a single-layer laminated battery (initial design discharge capacity equivalent to 40 mAh) is made and placed in an aluminum packaging material. Then, a 1.0M LiPF6 solution (solvent: a mixed solvent of ethylene carbonate (EC) / diethyl carbonate (DEC) = 3 / 7 (volume ratio), containing additives: 2% by volume (solvent ratio) of vinylene carbonate) is filled as an electrolyte. Furthermore, in order to seal the opening of the aluminum packaging material, a heat seal at a temperature of 150°C is performed to seal the aluminum packaging material to manufacture a lithium-ion secondary battery.

[0263] The initial capacity, rate characteristics, and cycle characteristics of the lithium ion secondary battery were evaluated according to the above-mentioned methods. The results are shown in Table 1.

[0264] (Examples 2-3)

[0265] When preparing polymer B, the hydrogenation reaction conditions were changed so that the iodine value became the value shown in Table 1, respectively, to obtain polymer B1-2 (Example 2) or polymer B1-3 (Example 3). Except for this aspect, various operations, measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0266] (Example 4)

[0267] The various operations, measurements, and evaluations were performed in the same manner as in Example 1 except that the polymer B2 prepared as described below was used as the polymer B. The results are shown in Table 1.

[0268] <Preparation of Polymer B2>

[0269] In an autoclave with a stirrer, 240 parts of ion exchange water, 25 parts of sodium alkylbenzene sulfonate as an emulsifier, 40 parts of acrylonitrile as a nitrile-containing monomer, and 4 parts of methacrylic acid as an ethylenically unsaturated acid monomer were added in sequence, and after replacing the interior with nitrogen, 56 parts of 1,3-butadiene as a conjugated diene monomer were pressed in, and 0.25 parts of ammonium persulfate as a polymerization initiator were added. The polymerization reaction was carried out at a reaction temperature of 40°C to obtain a copolymer containing a nitrile-containing monomer unit, an ethylenically unsaturated acid monomer unit, and a conjugated diene monomer unit. The iodine value of the obtained copolymer (polymer before hydrogenation) was measured according to the above method, and the result was 270g / 100g. In addition, the polymerization conversion rate was 85%.

[0270] Ion exchange water is added to the polymer before hydrogenation to obtain 400mL (total solid content 48g) of the solution with total solid content concentration adjusted to 12% by mass. The solution is put into an autoclave with a stirrer of volume 1L, nitrogen is passed through for 10 minutes, after removing the dissolved oxygen in the solution, 50mg of palladium acetate as a hydrogenation catalyst is dissolved in 180mL of ion exchange water to which 4 times of moles of nitric acid have been added relative to palladium (Pd), and added. After replacing the system twice with hydrogen, the contents of the autoclave are heated to 50°C in the state of pressurizing with hydrogen until the gauge pressure is 3MPa, so that it is subjected to a 6-hour hydrogenation reaction (hydrogenation reaction of the first stage).

[0271] Next, the autoclave was returned to atmospheric pressure, and 25 mg of palladium acetate as a hydrogenation catalyst was further dissolved in 60 mL of water to which 4 times the mole of nitric acid was added relative to Pd. After the system was replaced twice with hydrogen, the contents of the autoclave were heated to 50° C. while being pressurized with hydrogen until the gauge pressure was 3 MPa, and a hydrogenation reaction was carried out for 6 hours (second stage hydrogenation reaction).

[0272] Then, the contents were returned to room temperature, the system was placed in a nitrogen atmosphere, and then concentrated using a rotary evaporator until the solid content concentration became 40%, thereby obtaining an aqueous dispersion of polymer B2 as polymer B.

[0273] 320 parts of NMP as a solvent were added to 100 parts of the aqueous dispersion of the polymer B2 obtained above, and water was evaporated under reduced pressure to obtain an NMP dispersion of the polymer B2.

[0274] The weight average molecular weight and iodine value of polymer B2 were measured according to the above methods.

[0275] (Example 5)

[0276] The various operations, measurements, and evaluations were performed in the same manner as in Example 1 except that the polymer C2 prepared as described below was added as the polymer C. The results are shown in Table 1.

[0277] <Preparation of Polymer C2>

[0278] The same method as in Example 1 was used to obtain an aqueous dispersion of a polyacrylonitrile (PAN) copolymer (polymer C2) having an acrylonitrile unit content of 72% by mass, except that the amount of acrylamide added to the reactor B was changed to 2 parts, the amount of acrylic acid added was changed to 8 parts, and the amount of n-butyl acrylate added was changed to 18 parts. Then, the same method as in Example 1 was used to replace the solvent with NMP to obtain an NMP solution of polymer C2 (solid content concentration: 8%).

[0279] (Example 6)

[0280] When preparing the slurry composition for secondary battery positive electrode, the various operations, measurements and evaluations were performed in the same manner as in Example 1 except that the addition amounts of the polymers A to C were changed as shown in Table 1. The results are shown in Table 1.

[0281] (Comparative Examples 1 to 3)

[0282] When preparing the secondary battery positive electrode slurry composition, none of the polymers A to C was added and the addition amounts of the remaining polymers were changed as shown in Table 1. Various operations, measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0283] (Comparative Example 4)

[0284] When preparing polymer B1, the hydrogenation reaction conditions were changed so that the iodine value would be the value shown in Table 1 to obtain polymer B1-4. Various operations, measurements and evaluations were performed in the same manner as in Example 1 except that polymer B1-4 was used. The results are shown in Table 1.

[0285] (Comparative Example 5)

[0286] When preparing the slurry composition for secondary battery positive electrodes, the polymer C3 prepared as described below was added as the polymer C. Except for using the polymer C3, various operations, measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0287] <Production of Polymer C3>

[0288] The same procedure as in Example 1 was followed except that the amount of acrylonitrile added to the reactor B was changed to 50 parts, the amount of acrylamide added was changed to 10 parts, the amount of acrylic acid added was changed to 20 parts, and the amount of n-butyl acrylate added was changed to 20 parts, thereby obtaining an aqueous dispersion of a copolymer (polymer C3) having an acrylonitrile unit content of 50% by mass. Then, the same procedure as in Example 1 was followed except that the solvent was replaced with NMP to obtain an NMP solution of polymer C3 (solid content concentration: 8%).

[0289] In addition, in Table 1 shown below,

[0290] "MMA" means methyl methacrylate,

[0291] "BA" stands for n-butyl acrylate,

[0292] "MAA" means methacrylic acid,

[0293] "AMA" stands for allyl methacrylate,

[0294] "ST" stands for styrene,

[0295] "AN" stands for acrylonitrile,

[0296] "H-BD" represents 1,3-butadiene hydride unit,

[0297] "CNT" means carbon nanotube.

[0298] [Table 1]

[0299]

[0300] As can be seen from Table 1, in Examples 1 to 7 using a binder composition containing specified polymers A to C, the solid content concentration of the slurry composition and the peel strength of the electrode composite material layer can be fully improved. In addition, it can also be seen that in these embodiments, the battery characteristics of the secondary battery can be improved. In addition, as can be seen from Table 1, in Comparative Examples 1 to 5 lacking any one of polymers A to C, it is not possible to simultaneously increase the solid content concentration of the slurry composition and the peel strength of the electrode composite material layer and improve the battery characteristics of the secondary battery.

[0301] Industrial Applicability

[0302] According to the present invention, a nonaqueous secondary battery electrode binder composition can be provided which can sufficiently increase the solid content concentration of the obtained slurry composition and the peel strength of the obtained electrode composite layer and can improve the battery characteristics of a secondary battery having the obtained electrode.

[0303] Furthermore, the present invention can provide a nonaqueous secondary battery electrode slurry composition having a sufficiently high solid content concentration and capable of sufficiently improving the peel strength of the obtained electrode composite material layer and thus improving the battery characteristics of the obtained secondary battery, and a method for producing the same.

[0304] Furthermore, according to the present invention, it is possible to provide a nonaqueous secondary battery electrode capable of sufficiently improving the battery characteristics of a nonaqueous secondary battery, and a nonaqueous secondary battery having excellent battery characteristics such as rate characteristics and cycle characteristics.

Claims

1. A non-aqueous secondary battery electrode binder composition comprising a polymer A, a polymer B, a polymer C and an organic solvent, The polymer A is a granular polymer containing (meth)acrylate monomer units, The polymer B is a readily soluble polymer having an iodine value of 5 g / 100 g or more and 100 g / 100 g or less, and The polymer C is a readily soluble polymer containing nitrile group-containing monomer units in a ratio of 70% by mass or more and 98% by mass or less, when the total of all monomer units constituting the polymer C is 100% by mass, When the total content of the polymers A to C is 100% by mass, the content of the polymer B is 25% by mass or less, The amount of NMP-insoluble components in the readily soluble polymer is 50% by mass or less.

2. The binder composition for non-aqueous secondary battery electrodes according to claim 1, wherein The polymer A further comprises ethylenically unsaturated acid monomer units.

3. The binder composition for non-aqueous secondary battery electrodes according to claim 1 or 2, wherein The weight average molecular weight of the polymer B is 5,000 or more and 500,000 or less.

4. The binder composition for non-aqueous secondary battery electrodes according to claim 1, wherein When the total content of the polymer A, the polymer B and the polymer C is 100% by mass, The content a of the polymer A is 5% by mass or more and 60% by mass or less, The content b of the polymer B is 0.1 mass % or more and 25 mass % or less, The content c of the polymer C is 20 mass % or more and 94 mass % or less.

5. The binder composition for non-aqueous secondary battery electrodes according to claim 4, wherein The content rate a and the content rate c satisfy the relationship: 10≤a / (a+c)×100≤50.

6. The binder composition for non-aqueous secondary battery electrodes according to claim 4 or 5, wherein The polymers A to C are the following polymers: When preparing a mixed liquid of N-methyl-2-pyrrolidone having a solid content concentration of 8% by mass and containing the polymer A at the content a, the polymer B at the content b, and the polymer C at the content c as solid components, the ratio of the insoluble components in the mixed liquid satisfies 30% by mass or more and 80% by mass or less.

7. A slurry composition for non-aqueous secondary battery electrodes, comprising the binder composition for non-aqueous secondary battery electrodes according to any one of claims 1 to 6, an electrode active material and a conductive material, The conductive material contains carbon nanotubes.

8. A method for producing a slurry composition for a non-aqueous secondary battery electrode, which is the method for producing a slurry composition for a non-aqueous secondary battery electrode according to claim 7, The process includes the following steps: a premixing step of mixing at least the carbon nanotubes, the polymer B and the organic solvent to obtain a premix, and In the main mixing step, the premix is ​​mixed with at least the polymer A and the polymer C. 9 . A non-aqueous secondary battery electrode, comprising an electrode composite material layer formed using the slurry composition for a non-aqueous secondary battery electrode according to claim 7 . 10 . A non-aqueous secondary battery comprising the non-aqueous secondary battery electrode according to claim 9 .

Citation Information

Patent Citations

  • Electrode for secondary battery, binder for secondary battery electrode, manufacturing method and secondary battery

    JP2012204303A

  • Slurry composition for positive electrode for lithium ion rechargeable battery, positive electrode for lithium ion rechargeable battery, and lithium ion rechargeable battery

    WO2015064099A1

  • Slurry composition for electrode, electrode and secondary battery

    JP2004185826A

  • Electrode binder composition for nonaqueous electrolyte battery, electrode for nonaqueous electrolyte battery, and nonaqueous electrolyte battery

    US20130280606A1

  • Conductive material dispersed liquid and lithium secondary battery manufactured using same

    WO2017074124A1