Semiconductor structure and method for forming the same
By forming and thinning the first sidewall material layer on the sidewall of the semiconductor structure to form the source and drain doping layer, the problem of short channel effect is solved and the electrical performance of the semiconductor structure is improved.
Patent Information
- Application Number
- CN201910579466.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-06-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2039-06-28
AI Technical Summary
As the channel length of semiconductor devices shortens, the gate structure's ability to control the channel decreases, causing the short channel effect to become more serious and affecting the electrical performance of the semiconductor structure.
By forming a first spacer material layer on the sidewall of the semiconductor structure, etching the first spacer material layer to form a trench, and then laterally thinning the first spacer material layer to form the first spacer layer, and then etching the first spacer material layer in the trench. Form the source and drain doped layers, and use the selective epitaxial growth process to improve the quality and stress of the doped layers.
The distance between the side walls of adjacent gate structures is increased, making it easier for reactive gases to enter, improving the formation quality of source and drain doped layers, enhancing the migration rate of carriers in the channel, and improving the electrical properties of the semiconductor structure.
Smart Images

Figure CN112151449B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the same. Background Art
[0002] In semiconductor manufacturing, with the development trend of ultra-large-scale integrated circuits, the feature size of integrated circuits continues to decrease. In order to adapt to smaller feature sizes, the channel length of metal-oxide-semiconductor field-effect transistors (MOSFETs) is also shortened accordingly. However, as the channel length of the device shortens, the distance between the source region and the drain region of the device also shortens. Therefore, the control ability of the gate structure over the channel becomes worse, and it becomes increasingly difficult for the gate voltage to pinch off the channel, making the subthreshold leakage phenomenon, the so-called short-channel effects (SCE), more likely to occur.
[0003] Therefore, in order to reduce the impact of the short channel effect, semiconductor processes have gradually begun to transition from planar MOSFETs to three-dimensional transistors with higher efficiency, such as fin field effect transistors (FinFETs). In FinFETs, the gate structure can control the ultra-thin body (fin) from at least two sides. Compared with planar MOSFETs, the gate structure has a stronger control over the channel and can effectively suppress the short channel effect; and FinFETs have better compatibility with existing integrated circuit manufacturing than other devices. Summary of the invention
[0004] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, so as to optimize the performance of the semiconductor structure.
[0005] To solve the above problems, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising: providing a base, the base comprising a substrate and a gate structure located on the substrate, with the extension direction perpendicular to the gate structure as the lateral direction; forming a first sidewall material layer on the sidewall of the gate structure; after forming the first sidewall material layer, etching the substrate on both sides of the gate structure to form a groove; after forming the groove, thinning the first sidewall material layer from the lateral direction to form a first sidewall layer; forming a source-drain doping layer in the groove exposed by the first sidewall layer.
[0006] Optionally, after forming the groove and before forming the first sidewall layer, the method further includes: forming a seed layer conformally covering the groove; or, after forming the first sidewall layer and before forming the source / drain doping layer, the method further includes: forming a seed layer conformally covering the groove.
[0007] Optionally, a material of the first spacer layer is one or more of silicon nitride, silicon oxide, silicon oxynitride, silicon carbon boron nitride and silicon carbide nitride.
[0008] Optionally, the thickness of the first spacer layer is 1 nanometer to 2 nanometers.
[0009] Optionally, the first sidewall material layer is thinned by a wet etching process to form the first sidewall layer.
[0010] Optionally, the first spacer material layer is etched using a phosphoric acid solution to form the first spacer layer.
[0011] Optionally, after forming the groove and before forming the first sidewall layer, the method further includes: cleaning the groove.
[0012] Optionally, the gas used in the cleaning process includes one or more of He, NH3 and Ar.
[0013] Optionally, the material of the seed layer includes: Si.
[0014] Optionally, the seed layer is formed by a selective epitaxial growth process or a molecular beam epitaxy technique.
[0015] Optionally, in the step of forming the source / drain doping layer, the source / drain doping layer is doped with a first type of ions; in the step of forming the seed layer, the seed layer is doped with a second type of ions, and when the semiconductor structure is NMOS, the second type of ions are P-type ions, and the P-type ions include boron ions, gallium ions or indium ions; or, when the semiconductor structure is PMOS, the second type of ions are N-type ions, and the N-type ions include phosphorus ions, arsenic ions or antimony ions.
[0016] Optionally, after the source-drain doping layer is formed, a second spacer layer is formed on the side wall of the first spacer layer.
[0017] Optionally, the material of the second spacer layer is a low-K material.
[0018] Optionally, the material of the second spacer layer includes: SiON, SiBCN, SiCN, carbon-doped SiN or oxygen-doped SiN.
[0019] Optionally, after forming the groove and before forming the first sidewall layer, it also includes: forming a seed layer conformally covering the groove; in the process of etching the first sidewall material layer to form the first sidewall layer, the etching rate of the first sidewall material layer is greater than the etching rate of the seed layer.
[0020] Correspondingly, an embodiment of the present invention also provides a semiconductor structure, including: a substrate; a gate structure located on the substrate; a source-drain doped layer located in the substrate on both sides of the gate structure; a first sidewall layer located on the sidewall of the gate structure; a second sidewall layer located on the sidewall of the first sidewall layer, and the second sidewall layer is located on the source-drain doped layer.
[0021] Optionally, the thickness of the first spacer layer is 1 nanometer to 2 nanometers.
[0022] Optionally, a material of the first spacer layer is one or more of silicon nitride, silicon oxide, silicon oxynitride, silicon carbon boron nitride and silicon carbide nitride.
[0023] Optionally, the material of the second spacer layer is a low-K material.
[0024] Optionally, the material of the second spacer layer includes: SiON, SiBCN, SiCN, carbon-doped SiN or oxygen-doped SiN.
[0025] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:
[0026] The source-drain doping layer described in the embodiment of the present invention is usually formed by a selective epitaxial growth process. Compared with the case where the source-drain doping layer is formed in the groove exposed by the first sidewall material layer, in the embodiment of the present invention, the first sidewall material layer is thinned in the lateral direction to form the first sidewall layer, so that the distance between the first sidewall layers on the adjacent sidewalls of the gate structure is farther. In the process of forming the source-drain doping layer by the selective epitaxial growth method, the reaction gas can more easily enter the groove, so that the formation quality of the source-drain doping layer is good, which is conducive to improving the stress of the source-drain doping layer on the channel, so that the migration rate of carriers in the channel is higher, and the electrical performance of the semiconductor structure is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figures 1 to 3 It is a schematic structural diagram corresponding to each step in a method for forming a semiconductor structure;
[0028] Figures 4 to 11 is a schematic structural diagram corresponding to each step in a first embodiment of a method for forming a semiconductor structure according to an embodiment of the present invention;
[0029] Fig.12 and Fig.13It is a schematic structural diagram corresponding to each step in the second embodiment of the method for forming a semiconductor structure according to an embodiment of the present invention. DETAILED DESCRIPTION
[0030] As can be seen from the background technology, the devices currently formed still have the problem of poor performance. The reasons for the poor performance of the devices are now analyzed in combination with a method for forming a semiconductor structure.
[0031] Figures 1 to 3 A structural schematic diagram corresponding to each step in a method for forming a semiconductor structure is shown.
[0032] like Figure 1 As shown, a base is provided, which includes a substrate 1, a fin 2 located on the substrate 1, and a gate structure 3 spanning the fin 2, and the gate structure 3 covers part of the top wall and part of the side wall of the fin 2; a sidewall layer 6 is formed on the sidewall of the gate structure 3, and the size between the sidewall layers 6 on adjacent sidewalls of the gate structure 3 is taken as D1.
[0033] like Figure 2 As shown, the fins 2 on both sides of the gate structure 3 are etched to form grooves 4 in the fins 2 .
[0034] like Figure 3 As shown, in the groove 4 (as Figure 2 As shown in the figure, a source-drain doped layer 5 is formed.
[0035] With the development of semiconductor manufacturing technology, semiconductor process nodes are constantly decreasing. Therefore, the size of D1 in the extension direction perpendicular to the gate structure 3 is getting smaller and smaller. The source-drain doped layer 5 is usually formed by a selective epitaxial growth process. Because the size of D1 is too small, it is easy to cause the reaction gas to be difficult to enter the groove 4 during the epitaxial growth process, resulting in poor formation quality of the source-drain doped layer 5. When the semiconductor structure is working, the source-drain doped layer 5 generates less stress on the channel below the gate structure 3, and the carrier migration rate in the channel is reduced, resulting in poor electrical performance of the semiconductor structure.
[0036] In order to solve the technical problem, an embodiment of the present invention provides a method for forming a semiconductor structure, including: providing a base, the base including a substrate and a gate structure located on the substrate, with the extension direction perpendicular to the gate structure as the lateral direction; forming a first sidewall material layer on the sidewall of the gate structure; after forming the first sidewall material layer, etching the substrate on both sides of the gate structure to form a groove; after forming the groove, thinning the first sidewall material layer from the lateral direction to form a first sidewall layer; forming a source-drain doping layer in the groove exposed by the first sidewall layer.
[0037] The source-drain doping layer described in the embodiment of the present invention is usually formed by a selective epitaxial growth process. Compared with the case where the source-drain doping layer is formed in the groove exposed by the first sidewall material layer, in the embodiment of the present invention, the first sidewall material layer is thinned in the lateral direction to form the first sidewall layer, so that the distance between the first sidewall layers on the adjacent sidewalls of the gate structure is farther. In the process of forming the source-drain doping layer by the selective epitaxial growth method, the reaction gas can more easily enter the groove, so that the formation quality of the source-drain doping layer is good, which is conducive to improving the stress of the source-drain doping layer on the channel, so that the migration rate of carriers in the channel is higher, and the electrical performance of the semiconductor structure is improved.
[0038] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and easy to understand, specific embodiments of the embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0039] Figures 4 to 11 It is a schematic structural diagram corresponding to each step in the first embodiment of the method for forming a semiconductor structure according to an embodiment of the present invention.
[0040] refer to Figure 4 , providing a substrate, the substrate comprising a substrate 100 and a gate structure 102 located on the substrate 100, with the extension direction perpendicular to the gate structure 102 as the lateral direction.
[0041] The substrate provides a process foundation for the subsequent formation of semiconductor structures.
[0042] In this embodiment, the semiconductor structure formed is a fin field effect transistor (FinFET) as an example, and the substrate 100 is the substrate 100 having a fin portion 101. In other embodiments, the semiconductor structure formed may also be a planar structure, and correspondingly, the substrate is a planar substrate.
[0043] In this embodiment, the material of the substrate 100 is silicon. In other embodiments, the material of the substrate may also be germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be a silicon substrate on an insulator or a germanium substrate on an insulator. An interface layer may also be formed on the surface of the substrate 100, and the material of the interface layer may be silicon oxide, silicon nitride or silicon oxynitride.
[0044] In this embodiment, the material of the fin 101 is silicon. In other embodiments, the material of the fin may also be germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium.
[0045] The gate structure 102 is used to occupy a space for a subsequently formed metal gate structure.
[0046] In this embodiment, the gate structure 102 is a polysilicon gate structure.
[0047] Specifically, the gate structure 102 spans across the fin 101 , and the gate structure 102 covers a portion of the sidewall and top wall of the fin 101 .
[0048] In this embodiment, the gate structure 102 is a stacked structure, including a gate oxide layer 1021 that conformally covers a portion of the top surface and a portion of the sidewall of the fin 101 and a gate layer 1022 located on the gate oxide layer 1021. In other embodiments, the gate structure can also be a single-layer structure, that is, the gate structure only includes a gate layer.
[0049] In this embodiment, the material of the gate oxide layer 1021 is silicon oxide. In other embodiments, the material of the gate oxide layer may also be silicon oxynitride.
[0050] In this embodiment, the material of the gate layer 1022 is polysilicon. In other embodiments, the material of the gate layer may also be silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, silicon carbon nitride oxide, or amorphous carbon.
[0051] refer to Figure 5 , forming a first spacer material layer 103 on the sidewall of the gate structure 102 .
[0052] The first spacer material layer 103 is used to prepare for the subsequent formation of the first spacer layer. The first spacer material layer 103 protects the sidewall of the gate structure 102 during the subsequent trench formation process and is used to define the formation area of the subsequent source and drain doping layer.
[0053] The first spacer material layer 103 is made of dielectric material.
[0054] Specifically, the material of the first spacer material layer 103 is one or more of silicon nitride, silicon oxide, silicon oxynitride, silicon carbon boron nitride and silicon carbide nitride. In this embodiment, the material of the first spacer material layer 103 is silicon nitride.
[0055] The step of forming the first sidewall material layer 103 includes: conformally covering the first sidewall material film (not shown in the figure) on the gate structure 102 and the fin 101 exposed by the gate structure 102; removing the first sidewall material film on the gate structure 102 and the fin 101, and the remaining first sidewall material film located on the side wall of the gate structure 102 serves as the first sidewall material layer 103.
[0056] In this embodiment, the first sidewall material film is formed by an atomic layer deposition (ALD) process. The atomic layer deposition process includes performing multiple atomic layer deposition cycles, which is beneficial to improving the thickness uniformity of the first sidewall material film; in addition, the atomic layer deposition process has good gap filling performance and step coverage, which correspondingly improves the conformal coverage ability of the first sidewall material film. In other embodiments, other deposition processes may be used to form the first sidewall material film, such as plasma chemical vapor deposition process, etc.
[0057] It should be noted that the first spacer material layer 103 should not be too thick or too thin. Subsequently, grooves are formed in the fins 101 on both sides of the gate structure 102 and the first spacer material layer 103. If the first spacer material layer 103 is too thick, the distance d1 between the first spacer material layers 103 on the adjacent side walls of the gate structure 102 is too close, which may cause the lateral size of the grooves formed in the fins 101 on both sides of the gate structure 102 to be too small. After the source and drain doping layers are formed in the grooves, the distance between the source and drain doping layers on both sides of the gate structure 102 is far, which may cause the channel formed between the source and drain doping layers to be longer when the semiconductor structure is working, which is not conducive to improving the migration rate of carriers in the channel. If the first spacer material layer 103 is too thin, the first spacer material layer 103 may be removed in the subsequent process of forming the grooves, which may cause the gate structure 102 to be damaged. When the semiconductor structure is working, the gate structure 102 may have poor control over the channel. In this embodiment, the thickness of the first spacer material layer 103 is 6 nanometers to 12 nanometers.
[0058] refer to Figure 6 After forming the first spacer material layer 103 , the substrate 100 on both sides of the gate structure 102 is etched to form a trench 104 .
[0059] The trench 104 provides a process space for subsequently forming a source-drain doping layer.
[0060] Specifically, trenches 104 are formed in the fins 101 on both sides of the gate structure 102 .
[0061] In this embodiment, a dry etching process is used to form the groove 104. The dry etching process is an anisotropic etching process, which has good etching profile controllability, is conducive to making the morphology of the groove 104 meet the process requirements, and reduces damage to other film structures.
[0062] It should be noted that the method for forming the semiconductor structure further includes: after forming the trench 104 and before forming the first spacer layer, the method further includes: cleaning the trench 104 .
[0063] After the fin 101 is dry-etched to form the groove 104, polymer impurities remain on the bottom and sidewalls of the groove 104. The cleaning process is used to remove the polymer impurities in the groove 104, improve the purity of the subsequently formed source-drain doping layer, and also reduce the probability of dislocation of the source-drain doping layer growth, thereby improving the electrical performance of the semiconductor structure.
[0064] The process parameters of the cleaning treatment include: the gas used includes one or more of He, NH3 and Ar; the chamber pressure is 2Torr to 5Torr, the flow rate of the introduced NH3 can be between 500 and 1000sccm; the flow rate of He is between 1000 and 2000sccm.
[0065] It should also be noted that the method for forming the semiconductor structure further includes: after cleaning the groove 104 , baking the groove 104 .
[0066] The baking process is used to further remove polymer impurities attached to the sidewalls and bottom of the groove 104, improve the purity of the subsequently formed source-drain doping layer, and reduce the probability of dislocation of the growth of the source-drain doping layer.
[0067] The baking process generally uses hydrogen, which reacts with the polymer impurities in the groove 104 to form carbon monoxide or carbon dioxide.
[0068] In this embodiment, the baking process is performed at a temperature of 700° C. to 800° C.
[0069] refer to Figure 7 The method for forming the semiconductor structure further includes: after forming the trench 104 and before forming the first sidewall layer, the method further includes: forming a seed layer 105 conformally covering the trench 104 .
[0070] The seed layer 105 is used to improve the surface flatness and smoothness of the groove 104, thereby providing a good interface state and providing a process basis for the subsequent formation of source-drain doping layers, so that the source-drain doping layers have better formation quality.
[0071] In this embodiment, the material of the seed layer 105 includes Si. The material of the seed layer 105 is the same as that of the fin 101 , which reduces defects in the seed layer 105 and helps to improve the formation quality of the seed layer 105 .
[0072] In this embodiment, a selective epitaxial growth process (SEG) is used to form the seed layer 105. The film obtained by the selective epitaxial growth process has high purity and few defects, which is conducive to improving the formation quality of the seed layer 105, thereby facilitating the optimization of the electrical properties of the semiconductor structure. In other embodiments, the seed layer can also be formed by processes such as molecular beam epitaxy technology.
[0073] The process parameters for forming the seed layer 105 include: the reaction gas includes SiH 2 Cl 2 or SiH 4 .
[0074] It should be noted that the seed layer 105 should not be too thick or too thin. If the seed layer 105 is too thick, the source and drain doping layers formed subsequently will be too far away from the channel region below the gate structure 102. When the semiconductor structure is working, the source and drain doping layers exert less stress on the channel, resulting in a lower carrier migration rate in the channel. If the seed layer 105 is too thin, it is easy to cause the surface flatness and smoothness of the groove 104 to be poor, and there will be areas on the surface of the groove 104 that are not covered by the seed layer 105, resulting in poor quality of the source and drain doping layers formed subsequently. In this embodiment, the thickness of the seed layer 105 is 2 nanometers to 4 nanometers.
[0075] In addition, it should be noted that in the subsequent step of forming the source-drain doping layer, the source-drain doping layer is doped with first type ions. When the semiconductor structure is working, the first type ions are used to increase the stress of the source-drain doping layer on the channel and increase the migration rate of carriers in the channel.
[0076] In this embodiment, in the step of forming the seed layer 105 , second type ions are doped into the seed layer 105 . When the semiconductor structure is NMOS, the second type ions are P type ions.
[0077] When the semiconductor structure is working, the P-type ions make it difficult for the source depletion layer and the drain depletion layer of the source-drain doping layer to expand, thereby reducing the probability of source and drain punch-through.
[0078] Specifically, the P-type ions include boron ions, gallium ions or indium ions.
[0079] In other embodiments, when the transistor is a PMOS, the second type of ions are N-type ions. Specifically, the N-type ions include phosphorus ions, arsenic ions or antimony ions.
[0080] refer to Figure 8 After the groove 104 is formed, the first spacer material layer 103 is thinned in the lateral direction to form a first spacer layer 106 .
[0081] Compared with the case where a source-drain doped layer is formed in the groove 104 exposed by the first sidewall material layer 103, in an embodiment of the present invention, the first sidewall material layer 103 is thinned in the horizontal direction to form a first sidewall layer 106, so that the distance d2 between the first sidewall layers 106 on the adjacent side walls of the gate structure 102 is greater. In the subsequent process of forming the source-drain doped layer in the groove 104 by a selective epitaxial growth method, the reaction gas can more easily enter the groove 104, so that the formation quality of the source-drain doped layer is good, which is beneficial to increasing the stress of the source-drain doped layer on the channel, so that the migration rate of carriers in the channel is higher, and the electrical performance of the semiconductor structure is improved.
[0082] In this embodiment, a wet etching process is used to thin the first spacer material layer 103 to form the first spacer layer 106. The wet etching process is isotropic etching, and is simple to operate, low in process cost, and has a high etching rate. The wet etching process is also conducive to controlling the removal thickness of the first spacer material layer 103 to avoid damage to the gate structure 102.
[0083] It should also be noted that the etching rate of the wet etching solution on the first spacer material layer 103 is greater than the etching rate on the seed layer 105 .
[0084] Specifically, the first spacer material layer 103 is etched with a phosphoric acid solution to form the first spacer layer 106 .
[0085] It should be noted that the first sidewall layer 106 should not be too thick or too thin. If the first sidewall layer 106 is too thick, it is easy to cause the distance d2 between the first sidewall layers 106 on the adjacent sidewalls of the gate structure 102 to be too small. In the subsequent process of forming the source-drain doping layer by the selective epitaxial growth method, the reaction gas is not easy to enter the groove 104, resulting in poor formation quality of the source-drain doping layer, which is not conducive to improving the electrical performance of the semiconductor structure. If the first sidewall layer 106 is too thin, the first sidewall layer 106 is easy to expose part of the sidewall of the gate structure 102; and the material of the gate structure 102 is polycrystalline silicon. In the subsequent selective epitaxial growth process to form the source-drain doping layer, it is easy to grow redundant source-drain doping layers on the sidewalls of the gate structure 102. The redundant source-drain doping layers will cause a high capacitive coupling effect between the gate structure 102 and the contact hole plug formed subsequently, thereby resulting in poor electrical performance of the semiconductor structure. In this embodiment, the thickness of the first sidewall layer 106 is 1 nanometer to 2 nanometers.
[0086] It should be noted that, in the process of etching the first sidewall material layer 103 to form the first sidewall layer 106 , the etching rate of the seed layer 105 is relatively low. Accordingly, the surface of the seed layer 105 is relatively flat and smooth, which is beneficial to improving the formation quality of the source-drain doping layer subsequently formed in the groove 104 .
[0087] refer to Fig. 9 , a source-drain doped layer 107 is formed in the trench 104 exposed by the first spacer layer 116 .
[0088] When the semiconductor structure is working, the source-drain doped layer 107 provides stress to the channel to increase the migration rate of carriers in the channel.
[0089] In this embodiment, the source-drain doping layer 107 is formed by a selective epitaxial growth method, and in the process of forming the source-drain doping layer 107, the source-drain doping layer 107 is doped with first type ions. Doping ions can achieve the purpose of improving the carrier mobility in the channel.
[0090] In this embodiment, the semiconductor structure is used to form a PMOS (Positive Channel Metal Oxide Semiconductor) transistor, that is, the material of the source and drain doping layer 107 is silicon germanium doped with P-type ions. In this embodiment, P-type ions are doped into silicon germanium to replace the position of silicon atoms in the lattice. The more P-type ions are doped, the higher the concentration of majority carriers is, and the stronger the conductivity is. Specifically, the P-type ions include B, Ga or In.
[0091] In other embodiments, the semiconductor structure is used to form an NMOS (Negative channel Metal Oxide Semiconductor) transistor, and the material of the source and drain doping layer is silicon carbide or silicon phosphide doped with N-type ions. By doping N-type ions in silicon carbide or silicon phosphide, the N-type ions replace the position of silicon atoms in the lattice. The more N-type ions are doped, the higher the concentration of majority carriers and the stronger the conductivity. Specifically, the N-type ions include P, As or Sb.
[0092] refer to Fig.10 The method for forming the semiconductor structure further includes: after forming the source-drain doping layer 107 , forming a second spacer layer 108 on the side wall of the first spacer layer 106 .
[0093] Subsequently, an interlayer dielectric layer is formed to cover the sidewalls of the gate structure 102 and expose the top wall of the gate structure 102; in order to improve the electrical performance of the semiconductor structure, the gate structure 102 is subsequently removed to form a gate opening surrounded by the interlayer dielectric layer and the fin 101; and a metal gate structure is formed in the gate opening. The first sidewall layer 106 is too thin, and in the process of forming the gate opening, the first sidewall layer 106 is easily etched. The second sidewall layer 108 is used to protect the interlayer dielectric layer from being damaged in the process of forming the gate opening, which is conducive to controlling the spatial position of the metal gate structure formed subsequently, so that the metal gate structure is not easy to contact with the source-drain doping layer 107, thereby reducing the probability of leakage current in the semiconductor structure.
[0094] In this embodiment, the material of the second spacer 108 is a low-K material. A contact plug connected to the source-drain doping layer 107 is subsequently formed, and the second spacer 108 is used to reduce the capacitive coupling effect between the contact plug and the gate structure 102 .
[0095] Specifically, the material of the second spacer layer includes: SiON, SiBCN, SiCN, carbon-doped SiN or oxygen-doped SiN.
[0096] refer to Fig.11 The method for forming the semiconductor structure also includes: after forming the second sidewall layer 108, forming an anti-etching layer 109 that conformally covers the sidewalls of the gate structure 102 and the source-drain doping layer 107; after forming the anti-etching layer 109, forming an interlayer dielectric layer 110 that covers the sidewalls of the gate structure 102 and exposes the top wall of the gate structure 102.
[0097] In the subsequent process of forming an opening for filling the contact hole plug in the interlayer dielectric layer 110, the etching rate of the anti-etching layer 109 is lower than the etching rate of the interlayer dielectric layer 110. The anti-etching layer 109 is used to define a temporary etching stop position. Thereafter, the anti-etching layer 109 is further etched until the source-drain doped layer 107 is exposed, thereby making it easy to make the etching rates of the openings on each source-drain doped layer 107 consistent, and not easily causing problems such as over-etching or under-etching, thereby further improving the electrical performance and reliability of the semiconductor structure.
[0098] The material of the anti-etching layer 109 can be one or more of silicon nitride, silicon oxynitride, silicon carbide, silicon carbide nitride, boron nitride, silicon boron nitride and silicon boron nitride carbon. In this embodiment, the material of the anti-etching layer 109 is silicon nitride.
[0099] The interlayer dielectric layer 110 is used to electrically isolate adjacent devices.
[0100] The material of the interlayer dielectric layer 110 is a dielectric material.
[0101] Specifically, in this embodiment, the material of the interlayer dielectric layer 110 is silicon oxide. In other embodiments, the material of the interlayer dielectric layer may also be one or more of silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbonitride and silicon carbon oxynitride.
[0102] It should be noted that, in the subsequent process, the gate structure 102 is replaced with a metal gate structure, and the specific process will not be repeated here.
[0103] refer to Fig.12 and Fig.13 , is a schematic structural diagram corresponding to each step in the second embodiment of the method for forming a semiconductor structure according to an embodiment of the present invention.
[0104] The similarities between the embodiment of the present invention and the first embodiment are not repeated here. The difference between the present invention and the first embodiment is that after forming the first sidewall layer 206 and before forming the source-drain doping layer, a seed layer 205 conformally covering the groove 204 is formed.
[0105] The source-drain doping layer described in the embodiment of the present invention is usually formed by a selective epitaxial growth process. Compared with the case where the source-drain doping layer is formed in the groove 204 exposed by the first sidewall material layer (not shown in the figure), in the embodiment of the present invention, the first sidewall material layer is thinned in the lateral direction to form the first sidewall layer 206, so that the distance between the first sidewall layers 206 on the adjacent sidewalls of the gate structure 202 is farther. In the process of forming the source-drain doping layer by the selective epitaxial growth method, the reaction gas can more easily enter the groove 204, so that the formation quality of the source-drain doping layer is good, which is conducive to improving the stress of the source-drain doping layer on the channel, so that the migration rate of carriers in the channel is higher, and the electrical performance of the semiconductor structure is improved.
[0106] Moreover, in the embodiment of the present invention, compared with the situation in which the seed layer 205 is first formed and then the first side wall material layer is thinned to form the first side wall layer 206, after the first side wall layer 206 is formed, the seed layer 205 conformally covering the groove 204 is formed, thereby avoiding damage to the seed layer 205 caused by thinning the first side wall material layer. The surface of the seed layer 205 is relatively smooth and flat, which is beneficial to improving the formation quality of the source-drain doping layer.
[0107] In the embodiment of the present invention, the method for forming the seed layer 205 is the same as that of the first embodiment, and will not be described again.
[0108] Accordingly, an embodiment of the present invention further provides a semiconductor structure. Fig.11 , showing a schematic structural diagram of a first embodiment of a semiconductor structure of the present invention.
[0109] The semiconductor structure includes: a substrate 100; a gate structure 102, located on the substrate 100; a source-drain doped layer 107, located in the substrate 100 on both sides of the gate structure 102; a first spacer layer 106, located on the sidewall of the gate structure 102; a second spacer layer 108, located on the sidewall of the first spacer layer 106, and the second spacer layer 108 is located on the source-drain doped layer 107.
[0110] During the formation of the semiconductor structure, after the substrate 100 and the gate structure 102 are formed, a first spacer material layer 103 (eg, Figure 7 As shown); with the extension direction perpendicular to the gate structure 102 as the lateral direction, the first sidewall material layer 103 is thinned in the lateral direction to form a first sidewall layer 106, so that the distance between the first sidewall layers 106 on the adjacent sidewalls of the gate structure 102 is farther, so that in the process of forming the source-drain doped layer 107 by the epitaxial growth method, the reaction gas can more easily enter the groove 104, thereby improving the formation quality of the source-drain doped layer 107, and improving the migration rate of carriers in the channel, which is beneficial to improving the electrical performance of the semiconductor structure.
[0111] In this embodiment, the semiconductor structure formed is a fin field effect transistor (FinFET) as an example, and the substrate 100 is the substrate 100 having a fin portion 101. In other embodiments, the semiconductor structure formed may also be a planar structure, and correspondingly, the substrate is a planar substrate.
[0112] In this embodiment, the material of the substrate 100 is silicon. In other embodiments, the material of the substrate may also be germanium, silicon carbide, gallium arsenide or indium gallium, and the substrate may also be a silicon substrate on an insulator or a germanium substrate on an insulator. An interface layer may also be formed on the surface of the substrate 100, and the material of the interface layer may be silicon oxide, silicon nitride or silicon oxynitride.
[0113] In this embodiment, the material of the fin 101 is silicon. In other embodiments, the material of the fin may also be germanium, silicon germanium, silicon carbide, gallium arsenide or indium gallium.
[0114] The gate structure 102 is used to occupy a space for a subsequently formed metal gate structure.
[0115] In this embodiment, the gate structure 102 is a polysilicon gate structure.
[0116] In this embodiment, the gate structure 102 is a stacked structure, including a gate oxide layer 1021 that conformally covers a portion of the top surface and a portion of the sidewall of the fin 101 and a gate layer 1022 located on the gate oxide layer 1021. In other embodiments, the gate structure can also be a single-layer structure, that is, the gate structure only includes a gate layer.
[0117] In this embodiment, the material of the gate oxide layer 1021 is silicon oxide. In other embodiments, the material of the gate oxide layer may also be silicon oxynitride.
[0118] In this embodiment, the material of the gate layer 1022 is polysilicon. In other embodiments, the material of the gate layer may also be silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, silicon carbon nitride oxide, or amorphous carbon.
[0119] When the semiconductor structure is working, the source-drain doped layer 107 provides stress to the channel to increase the migration rate of carriers in the channel.
[0120] In this embodiment, the semiconductor structure is used to form a PMOS (Positive Channel Metal Oxide Semiconductor) transistor, that is, the material of the source and drain doping layer 107 is silicon germanium doped with the first type of ions. In this embodiment, P-type ions are doped into silicon germanium to replace the position of silicon atoms in the lattice. The more P-type ions are doped, the higher the concentration of majority carriers is, and the stronger the conductive performance is. Specifically, the P-type ions include B, Ga or In.
[0121] In other embodiments, the semiconductor structure is used to form an NMOS (Negative channel Metal Oxide Semiconductor) transistor, and the material of the source and drain doping layers is silicon carbide or silicon phosphide doped with the first type of ions. By doping N-type ions in silicon carbide or silicon phosphide, the N-type ions replace the position of silicon atoms in the lattice. The more N-type ions are doped, the higher the concentration of majority carriers and the stronger the conductivity. Specifically, the N-type ions include P, As or Sb.
[0122] During the formation of the semiconductor structure, a first spacer material layer 103 (eg, Figure 5 As shown in FIG. 1 , the first spacer layer 106 is formed by thinning the first spacer material layer 103. Compared with the distance d1 between the first spacer material layers 103 on the sidewalls of adjacent gate structures 102, the distance d2 between the first spacer layers 106 on the sidewalls of adjacent gate structures 102 is larger, so that more reaction gases can enter the trench 104 (as shown in FIG. 1 ) during the process of forming the source-drain doping layer 107 by the selective epitaxial growth method. Figure 6 As shown in the figure), the formation quality of the source-drain doping layer 107 is better.
[0123] The first spacer layer 106 is made of dielectric material.
[0124] Specifically, the material of the first spacer 106 is one or more of silicon nitride, silicon oxide, silicon oxynitride, silicon carbon boron nitride and silicon carbide nitride. In this embodiment, the material of the first spacer 106 is silicon nitride.
[0125] It should be noted that the first sidewall layer 106 should not be too thick or too thin. If the first sidewall layer 106 is too thick, it is easy to cause the distance d2 between the first sidewall layers 106 on the adjacent sidewalls of the gate structure 102 to be too small. In the process of forming the source-drain doped layer 107 by epitaxial growth, the reaction gas is not easy to enter the groove 104, which is not conducive to improving the migration rate of carriers in the channel, resulting in poor formation quality of the source-drain doped layer 107. If the first sidewall layer 106 is too thin, it is easy to expose the gate structure 102. The material of the gate structure 102 is polysilicon. In the process of selective epitaxial growth to form the source-drain doped layer 107, it is easy to grow redundant source-drain doped layers on the sidewalls of the gate structure 102. The redundant source-drain doped layers will increase the capacitive coupling effect between the gate structure 102 and the contact hole plug formed subsequently, thereby resulting in poor electrical performance of the semiconductor structure. In this embodiment, the thickness of the first sidewall layer 106 is 1 nanometer to 2 nanometers.
[0126] The semiconductor structure further includes an interlayer dielectric layer 110 covering the sidewalls of the gate structure 102 , and the interlayer dielectric layer 110 exposes the top of the gate structure 102 .
[0127] The interlayer dielectric layer 110 is used to electrically isolate adjacent devices.
[0128] The material of the interlayer dielectric layer 110 is a dielectric material.
[0129] Specifically, in this embodiment, the material of the interlayer dielectric layer 110 is silicon oxide. In other embodiments, the material of the interlayer dielectric layer may also be one or more of silicon nitride, silicon oxynitride, silicon oxycarbide, silicon carbonitride and silicon carbon oxynitride.
[0130] In order to improve the electrical performance of the semiconductor structure, the gate structure 102 is subsequently removed to form a gate opening (not shown in the figure) surrounded by the interlayer dielectric layer 110 and the fin 101; a metal gate structure is formed in the gate opening. The second sidewall layer 108 is used to protect the interlayer dielectric layer 110 from being damaged during the formation of the gate opening, which is conducive to controlling the spatial position of the metal gate structure, so that the metal gate structure is not easy to contact the source and drain doping layer 107, and the probability of leakage current in the semiconductor structure is reduced.
[0131] In this embodiment, the material of the second spacer 108 is a low-K material. A contact plug connected to the source-drain doping layer 107 is subsequently formed, and the second spacer 108 is used to reduce the capacitive coupling effect between the contact plug and the gate structure 102 .
[0132] Specifically, the material of the second spacer layer 108 includes: SiON, SiBCN, SiCN, carbon-doped SiN or oxygen-doped SiN.
[0133] The semiconductor structure further includes an anti-etching layer 109 located between the interlayer dielectric layer 110 and the second spacer layer 108 , and between the source / drain doping layer 107 and the interlayer dielectric layer 110 .
[0134] In the subsequent process of forming an opening for filling the contact hole plug in the interlayer dielectric layer 110, the etching rate of the anti-etching layer 109 is lower than the etching rate of the interlayer dielectric layer 110. The anti-etching layer 109 is used to define a temporary etching stop position. Thereafter, the anti-etching layer 109 is further etched until the source-drain doped layer 107 is exposed, thereby making it easy to make the etching rates of the openings on each source-drain doped layer 107 consistent, and not easily causing problems such as over-etching or under-etching, thereby further improving the electrical performance and reliability of the semiconductor structure.
[0135] The material of the anti-etching layer 109 can be one or more of silicon nitride, silicon oxynitride, silicon carbide, silicon carbide nitride, boron nitride, silicon boron nitride and silicon boron nitride carbon. In this embodiment, the material of the anti-etching layer 109 is silicon nitride.
[0136] The semiconductor structure further includes a seed layer 105 located between the source / drain doping layer 107 and the fin 101 .
[0137] The surface of the seed layer 105 has high surface flatness and smoothness, and can provide a good interface state, so that the source-drain doping layer 107 has a good formation quality.
[0138] In this embodiment, the material of the seed layer 105 includes Si. The material of the seed layer 105 is the same as that of the substrate 100 and the fin 101 , which reduces defects in the seed layer 105 and helps improve the formation quality of the seed layer 105 .
[0139] It should be noted that the seed layer 105 is doped with second type ions, and when the semiconductor structure is NMOS, the second type ions are P type ions.
[0140] When the semiconductor structure is working, the P-type ions make it difficult for the source depletion layer and the drain depletion layer of the source-drain doping layer 107 to expand, thereby reducing the probability of source and drain punch-through.
[0141] Specifically, the P-type ions include boron ions, gallium ions or indium ions.
[0142] In other embodiments, when the first-type transistor is a PMOS, the second-type ions are N-type ions. Specifically, the N-type ions include phosphorus ions, arsenic ions, or antimony ions.
[0143] The semiconductor structure can be formed by the formation method described in the above embodiment, or by other formation methods. For the specific description of the semiconductor structure described in this embodiment, reference can be made to the corresponding description in the above embodiment, and this embodiment will not be repeated here.
[0144] Although the embodiments of the present invention are disclosed above, the embodiments of the present invention are not limited thereto. Any person skilled in the art may make various changes and modifications without departing from the spirit and scope of the embodiments of the present invention. Therefore, the protection scope of the embodiments of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, the substrate comprising a substrate and a gate structure located on the substrate, with a lateral direction perpendicular to an extension direction of the gate structure; forming a first spacer material layer on the sidewall of the gate structure; After forming the first spacer material layer, etching the substrate on both sides of the gate structure to form a groove; After forming the groove, the first spacer material layer is thinned in a lateral direction to form a first spacer layer; forming a source-drain doped layer in the trench exposed by the first sidewall layer; After forming the trench and before forming the first sidewall layer, the method further includes: forming a seed layer conformally covering the trench, wherein the material of the seed layer is the same as that of the substrate, and the seed layer is formed by a selective epitaxial growth process or a molecular beam epitaxy technique; The first spacer material layer is thinned by a wet etching process to form a first spacer layer. The etching rate of the first spacer material layer by the wet etching process is greater than the etching rate of the seed layer.
2. The method for forming a semiconductor structure according to claim 1, wherein: The material of the first spacer layer is one or more of silicon nitride, silicon oxide, silicon oxynitride, silicon carbon boron nitride and silicon carbide nitride.
3. The method for forming a semiconductor structure according to claim 1, wherein: The thickness of the first spacer layer is 1 nanometer to 2 nanometers.
4. The method for forming a semiconductor structure according to claim 1, wherein: The first sidewall material layer is thinned by a wet etching process to form the first sidewall layer.
5. The method for forming a semiconductor structure according to claim 4, wherein: The first spacer material layer is etched using a phosphoric acid solution to form the first spacer layer.
6. The method for forming a semiconductor structure according to claim 1, wherein: After forming the groove and before forming the first sidewall layer, the method further includes: cleaning the groove.
7. The method for forming a semiconductor structure according to claim 6, wherein: The gas used in the cleaning process includes one or more of He, NH3 and Ar.
8. The method for forming a semiconductor structure according to claim 1, wherein: The material of the seed layer includes: Si.
9. The method for forming a semiconductor structure according to claim 1, wherein: In the step of forming the source-drain doping layer, the source-drain doping layer is doped with first type ions; In the step of forming the seed layer, second type ions are doped into the seed layer, and when the semiconductor structure is NMOS, the second type ions are P type ions, and the P type ions include boron ions, gallium ions or indium ions; or, When the semiconductor structure is a PMOS, the second type ions are N-type ions, and the N-type ions include phosphorus ions, arsenic ions, or antimony ions.
10. The method for forming a semiconductor structure according to claim 1, wherein: After the source-drain doping layer is formed, a second spacer layer is formed on the sidewall of the first spacer layer.
11. The method for forming a semiconductor structure according to claim 10, wherein: The material of the second spacer layer is a low-K material.
12. The method for forming a semiconductor structure according to claim 11, wherein: The material of the second spacer layer includes: SiON, SiBCN, SiCN, carbon-doped SiN or oxygen-doped SiN.