Organic film forming composition, semiconductor device manufacturing substrate, organic film forming method, pattern forming method, and polymer
By using a combination of polymers with triple bond substituents and high boiling point solvents, an organic film is formed that is stably solidified in a passive gas under high temperature conditions, solving the problems of heat resistance and landfilling/flatness of organic films in the prior art. Solve the problem of insufficient chemical properties and improve the manufacturing efficiency and yield of semiconductor devices.
Patent Information
- Application Number
- CN202010637312.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-07-03
AI Technical Summary
The existing technology is difficult to form a stable organic film in a passive gas under high temperature conditions, and has low heat resistance and insufficient filling/planarization characteristics, which affects the manufacturing yield of semiconductor devices.
A polymer with a triple bond substituent is used as the organic film-forming composition. Through a partial structure that can be cured in both air and inert gas, a high boiling point solvent and a surfactant are combined to form a composition with high heat resistance and landfillability. /Organic film with flattening properties.
It achieves the formation of a stable organic film in a passive gas under high temperature conditions, improves the yield of semiconductor device manufacturing and the accuracy of pattern transfer, and avoids film thickness changes and poor filling caused by thermal decomposition.
Smart Images

Figure CN112180686B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an organic film-forming composition used in a semiconductor device manufacturing step, a semiconductor device manufacturing substrate using the composition, an organic film forming method, a pattern forming method using a multilayer resist method, and a polymer suitable for the composition. Background Art
[0002] In the past, the high integration and high speed of semiconductor devices were achieved by miniaturizing the pattern size obtained by shortening the wavelength of the light source in the photolithography technology (optical lithography) using light exposure as a general technology. In order to form such a fine circuit pattern on the semiconductor device substrate (processed substrate), a method of processing the processed substrate by dry etching using a photoresist film formed with a pattern as an etching mask is usually used. However, in reality, there is no dry etching method that can obtain complete etching selectivity between the photoresist film and the processed substrate, so in recent years, substrate processing by a multilayer resist method has been widely used. This method is to insert an intermediate film with different etching selectivity from the photoresist film (hereinafter referred to as the resist upper film) between the resist upper film and the processed substrate, and after the resist upper film obtains a pattern, the resist upper film pattern is used as a dry etching mask, and the pattern is transferred to the intermediate film by dry etching, and then the intermediate film is used as a dry etching mask, and the pattern is transferred to the processed substrate by dry etching.
[0003] One of the multilayer resist methods is a three-layer resist method that can be implemented using a general resist composition used in a single-layer resist method. This method forms an organic film (hereinafter referred to as an organic film) by coating and calcining an organic film material composed of a composition containing an organic resin on a processed substrate, and then forms a silicon-containing film (hereinafter referred to as a silicon-containing resist intermediate film) by coating and calcining a resist intermediate film material composed of a composition containing a silicon-containing resin, and then forms a general organic photoresist film thereon. After the resist upper film is patterned, if dry etching is performed by fluorine-based gas plasma, the organic resist upper film can obtain a good etching selectivity relative to the silicon intermediate film, so the resist upper film pattern can be transferred to the silicon intermediate film. According to this method, even if a resist upper layer film that does not have sufficient film thickness for directly processing a substrate to be processed or a resist upper layer film that does not have sufficient dry etching resistance for processing a substrate to be processed is used, the pattern can still be easily transferred to the silicon intermediate film because the film thickness of the silicon intermediate film is generally equal to or less than that of the resist upper layer film. Then, the silicon intermediate film with the transferred pattern is used as a dry etching mask, and the pattern is transferred to the organic film by dry etching using oxygen or hydrogen gas plasma, so that the pattern can be transferred to the organic film that has sufficient dry etching resistance for processing the substrate. The pattern of the organic film that has been pattern-transferred can be transferred to the substrate by dry etching using fluorine gas or chlorine gas.
[0004] On the other hand, the miniaturization in the manufacturing process of semiconductor devices is gradually approaching the essential limit of the wavelength of the light source used for optical lithography. Therefore, in recent years, the high integration of semiconductor devices that do not rely on miniaturization has been explored. As one of the methods, semiconductor devices with complex structures such as multi-gate structures have been explored, and some have been put into practical use. When forming such a structure by a multilayer resist method, the following organic film materials can be used: the film can be used to fill in tiny patterns such as holes, grooves, fins, etc. formed on the processed substrate without leaving gaps, or the film can be used to fill in the height difference, or the pattern-dense parts and the pattern-free areas and flatten them (planarization). By using such an organic film material to form a flat organic film surface on a substrate with a height difference, the film thickness variation of the silicon intermediate film and the resist upper film formed thereon can be suppressed, and the focus tolerance of optical lithography or the tolerance reduction in the subsequent processing steps of the processed substrate can be suppressed. As a result, semiconductor devices can be manufactured with good yield. On the other hand, in order to fill the gaps or patterns on the processed substrate, the thickness of the upper resist film in the single-layer resist method becomes thicker, which leads to pattern collapse after exposure and development, or degradation of the pattern shape due to reflection from the substrate during exposure. The pattern formation tolerance during exposure becomes narrower, making it difficult to manufacture semiconductor devices with good yield.
[0005] In addition, as a method for increasing the speed of next-generation semiconductor devices, the use of new materials with high electron mobility such as strained silicon or gallium arsenic, or precision materials such as ultra-thin film polysilicon controlled in angstroms has begun to be explored. However, in a substrate to be processed using such new precision materials, when a flattening film is formed using an organic film material such as the above, for example, under film formation conditions in air at 300°C or above, there is a possibility that the material will be corroded by oxygen in the air, and the performance of the semiconductor device cannot be achieved as designed, and the yield that can be achieved in industrial production cannot be achieved. Therefore, in order to avoid the reduction in yield caused by corrosion of the substrate caused by air under such high temperature conditions, an organic film material that can be formed in a passive gas is desired.
[0006] In the past, it is known that condensation resins obtained by using carbonyl compounds such as ketones or aldehydes and aromatic alcohols as condensing agents for phenolic and naphthol compounds are used as organic film forming materials for multilayer resist methods. For example, bisphenol fluorene novolac resins described in Patent Document 1, bisphenol compounds and novolac resins thereof described in Patent Document 2, novolac resins of adamantane phenol compounds described in Patent Document 3, and bisnaphthol compounds and novolac resins thereof described in Patent Document 4 can be exemplified. Such materials form a film having solvent resistance for the coating film material used in the next step by utilizing the curing action of crosslinking by a hydroxymethyl compound as a crosslinking agent or oxidation of an aromatic ring at the α position by the action of oxygen in the air and the subsequent condensation, so that a cured film cannot be formed in an inert gas, and the film thickness variation, the degradation of the embedding characteristics, or the planarization characteristics caused by thermal decomposition under high temperature conditions cannot be suppressed.
[0007] In addition, materials using triple bonds as intermolecular crosslinking groups of curable resins are known. For example, Patent Documents 5 to 10 are known. These materials form a cured film having solvent resistance by utilizing not only the aforementioned crosslinking from methylol groups but also the crosslinking due to the polymerization of triple bonds. However, these organic film-forming materials are insufficient in terms of the embedding properties and planarization properties of the pattern formed on the substrate.
[0008] In addition, as examples of materials containing nitrogen-containing polymers, there are known copolymer resins containing heterocycles (Patent Documents 11 and 12), carbazole resins (Patent Documents 13 and 14), novolacs having secondary amino groups (Patent Document 15), diarylamine novolacs (Patent Document 16), indolecarbazole novolacs (Patent Document 17), etc. However, these materials are not examples of substituents having triple bonds on nitrogen atoms, and are not known for the formation of cured films in inert gases, the variation in film thickness due to thermal decomposition under high temperature conditions, the filling characteristics, or the planarization characteristics.
[0009] In addition, with respect to nitrogen-containing compounds, there are also examples of intermediate film materials using monomolecular compounds as shown in Patent Documents 18 and 19. However, since monomolecular compounds are used, there are problems with the coating properties on substrates with complex shapes, problems caused by low-molecular sublimates during baking, and many other properties such as heat resistance and etching resistance of the organic film after curing.
[0010] [Patent Document 1] Japanese Patent Application Publication No. 2005-128509
[0011] [Patent Document 2] Japanese Patent Application Publication No. 2006-293298
[0012] [Patent Document 3] Japanese Patent Application Publication No. 2006-285095
[0013] [Patent Document 4] Japanese Patent Application Publication No. 2010-122656
[0014] [Patent Document 5] Japanese Patent Application Publication No. 2010-181605
[0015] [Patent Document 6] International Publication No. 2014-208324 Pamphlet
[0016] [Patent Document 7] Japanese Patent Application Publication No. 2012-215842
[0017] [Patent Document 8] Japanese Patent Application Publication No. 2016-044272
[0018] [Patent Document 9] Japanese Patent Application Publication No. 2016-060886
[0019] [Patent Document 10] Japanese Patent Application Publication No. 2017-119671
[0020] [Patent Document 11] Japanese Patent Application Publication No. 2013-137334
[0021] [Patent Document 12] International Publication No. 2018-212116 Pamphlet
[0022] [Patent Document 13] International Publication No. 2010-147155 Pamphlet
[0023] [Patent Document 14] International Publication No. 2013-005797 Pamphlet
[0024] [Patent Document 15] International Publication No. 2015-098594 Pamphlet
[0025] [Patent Document 16] International Publication No. 2013-047516 Pamphlet
[0026] [Patent Document 17] International Publication No. 2017-094780 Pamphlet
[0027] [Patent Document 18] International Publication No. 2016-147989 Pamphlet
[0028] [Patent Document 19] International Publication No. 2018-164267 Pamphlet Summary of the invention
[0029] Problem that the invention aims to solve
[0030] The present invention is made in view of the above situation, and aims to provide a polymer capable of forming an organic film, and a composition for forming an organic film containing the polymer; the organic film is cured under film forming conditions not only in air but also in an inert gas, and has excellent heat resistance, or the embedding and planarization characteristics of the pattern formed on the substrate, and has less sublimation products and good film forming properties on the substrate. In addition, the present invention also provides a substrate for manufacturing a semiconductor device, a method for forming an organic film, and a method for forming a pattern using the above composition.
[0031] Solutions for solving problems
[0032] In order to achieve the above-mentioned problem, the present invention provides an organic film-forming composition comprising:
[0033] A polymer having a partial structure represented by the following general formula (1) as a repeating unit, and
[0034] Organic solvents.
[0035] [Chemistry 1]
[0036]
[0037] In the above general formula (1), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, and W 1 W is any one of the following general formulas (2), (4), and (6), and two or more kinds of W may be used in combination. 1 , W 2It is a divalent organic group having 6 to 80 carbon atoms and having at least one aromatic ring.
[0038] [Chemistry 2]
[0039]
[0040] In the above general formula (2), AR3, AR4, and AR5 are benzene rings or naphthalene rings which may have substituents, and AR3 and AR4 or AR4 and AR5 may form a bridged structure with aromatic rings via carbon atoms bonded to hydrogen atoms on the aromatic rings. Y is a substituent represented by the following general formula (3).
[0041] [Chemistry 3]
[0042]
[0043] R 3 is a single bond or a divalent organic group having 20 or less carbon atoms, R 4 It is hydrogen or a monovalent organic group having 20 or less carbon atoms.
[0044] [Chemistry 4]
[0045]
[0046] In the above general formula (4), AR6 and AR7 are benzene rings or naphthalene rings which may also have substituents, n1 is 0 or 1, and when n1=0, AR6 and AR7 do not form a bridged structure between the aromatic rings via Z, and when n1=1, AR6 and AR7 form a bridged structure via Z, and Z is a single bond or any one of the following general formulas (5). Y is a substituent represented by the above general formula (3).
[0047] [Chemistry 5]
[0048]
[0049] [Chemistry 6]
[0050]
[0051] AR8 in the above general formula (6) is a benzene ring, a naphthalene ring, anthracene ring, a phenanthrene ring, or a pyrene ring, Y is a substituent represented by the above general formula (3), and n2 and n3 are integers satisfying the relationship of 0≤n2≤4, 0≤n3≤4, and 1≤n2+n3≤4.
[0052] Such an organic film-forming composition can form an organic film that cures under film-forming conditions not only in air but also in an inert gas, has high heat resistance, excellent film-forming properties, and has high filling / planarizing properties.
[0053] W in the above general formula (1) 2 The divalent organic group represented by is preferably any of the following.
[0054] [Chemistry 7]
[0055]
[0056] By importing such a partial structure into W 2 In the present invention, it becomes a polymer suitable for forming an organic film having improved heat resistance and excellent etching resistance and distortion resistance.
[0057] The polymer preferably has a weight average molecular weight of 1,000 to 5,000.
[0058] If the organic film-forming composition contains a polymer having an Mw within such a range, it is possible to suppress outgassing during baking without impairing solubility in an organic solvent.
[0059] The organic solvent is preferably a mixture of one or more organic solvents having a boiling point of less than 180 degrees and one or more organic solvents having a boiling point of 180 degrees or more.
[0060] Such an organic film-forming composition can provide the polymer with thermal fluidity of the film due to the addition of a high-boiling-point solvent, thereby achieving high-level filling / planarization properties.
[0061] The organic film-forming composition preferably further contains one or more of a surfactant and a plasticizer.
[0062] If the organic film-forming composition contains such a component, it can be an organic film-forming composition having more excellent coating properties and filling / planarization characteristics.
[0063] Furthermore, the present invention provides a substrate for manufacturing a semiconductor device, on which an organic film is formed by curing the above-mentioned organic film-forming composition.
[0064] The organic film formed from the organic film-forming composition of the present invention has high filling / planarization properties at the same time, and has no microscopic voids due to poor filling and no unevenness on the surface of the organic film due to insufficient planarization. The semiconductor device substrate of the present invention planarized using the organic film has a wider process latitude range during patterning, and semiconductor devices can be manufactured with good yield.
[0065] The present invention provides a method for forming an organic film, which is suitable for the manufacturing steps of a semiconductor device, and comprises the following steps: spin-coating the aforementioned organic film-forming composition on a substrate to be processed; and subjecting the substrate to be processed coated with the organic film-forming composition to a heat treatment at a temperature of 50° C. to 600° C. in a range of 10 seconds to 7200 seconds in an inert gas environment to obtain a cured film.
[0066] In addition, the present invention provides a method for forming an organic film, which is a method for forming an organic film suitable for the manufacturing steps of a semiconductor device, comprising the following steps: spin-coating the aforementioned organic film-forming composition on a processed substrate; heat-treating the processed substrate coated with the aforementioned organic film-forming composition in air at a temperature of 50°C to 250°C within a range of 5 seconds to 600 seconds to form a coating film; and applying heat treatment in an inert gas environment at a temperature of 200°C to 600°C within a range of 10 seconds to 7200 seconds to obtain a cured film.
[0067] The organic film formed by the organic film forming method of the present invention and suitable for the manufacturing steps of semiconductor devices has high heat resistance and high-level filling / planarization characteristics, and if used in the manufacturing steps of semiconductor devices, the yield of semiconductor devices will become good.
[0068] At this time, the oxygen concentration in the inert gas is preferably set to 1% or less.
[0069] The organic film-forming composition of the present invention does not generate sublimates even when heated in such an inert gas atmosphere, and is sufficiently cured, thereby forming an organic film having excellent adhesion to a substrate.
[0070] The substrate to be processed preferably has a structure or a height difference of 30 nm or more.
[0071] The method for forming an organic film of the present invention is particularly effective when forming a flat organic film on such a substrate to be processed.
[0072] The present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the aforementioned organic film forming composition, forming a silicon-containing resist intermediate film on the aforementioned organic film using a silicon-containing resist intermediate film material, forming a resist upper film on the aforementioned silicon-containing resist intermediate film using a photoresist composition, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film with the circuit pattern formed thereon as a mask and transferring the pattern to the aforementioned silicon-containing resist intermediate film by etching, using the aforementioned silicon-containing resist intermediate film with the pattern transferred thereon as a mask and transferring the pattern to the aforementioned organic film by etching, and using the aforementioned organic film with the pattern transferred thereon as a mask and forming the pattern on the aforementioned workpiece by etching.
[0073] The present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the aforementioned organic film forming composition, forming a silicon-containing resist intermediate film on the aforementioned organic film using a silicon-containing resist intermediate film material, forming an organic anti-reflective film (BARC) on the aforementioned silicon-containing resist intermediate film, forming a resist upper film using a photoresist composition on the aforementioned BARC, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film with the circuit pattern formed as a mask and sequentially transferring the pattern of the BARC and the aforementioned silicon-containing resist intermediate film by etching, using the aforementioned silicon-containing resist intermediate film with the pattern transferred as a mask and transferring the pattern of the organic film by etching, and using the aforementioned organic film with the pattern transferred as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.
[0074] The present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the aforementioned organic film forming composition, forming an inorganic hard mask selected from silicon oxide film, silicon nitride film, silicon oxide nitride film, titanium oxide film, and titanium nitride film on the aforementioned organic film, forming a resist upper film on the aforementioned inorganic hard mask using a photoresist composition, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film with the circuit pattern formed thereon as a mask and performing pattern transfer to the aforementioned inorganic hard mask by etching, using the aforementioned inorganic hard mask with the pattern formed thereon as a mask and performing pattern transfer to the aforementioned organic film by etching, and using the aforementioned organic film with the pattern formed thereon as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.
[0075] The present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the aforementioned organic film forming composition, forming an inorganic hard mask selected from silicon oxide film, silicon nitride film, silicon oxide nitride film, titanium oxide film, and titanium nitride film on the aforementioned organic film, forming a BARC on the aforementioned inorganic hard mask, forming a resist upper film on the aforementioned BARC using a photoresist composition, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film formed with the circuit pattern as a mask and sequentially transferring the pattern of the BARC and the aforementioned inorganic hard mask by etching, using the aforementioned inorganic hard mask formed with the pattern as a mask and transferring the pattern of the aforementioned organic film by etching, and using the aforementioned organic film formed with the pattern as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.
[0076] The organic film-forming composition of the present invention can be preferably used in various pattern forming methods such as a three-layer resist process using a silicon-containing resist interlayer or an inorganic hard mask, or a four-layer resist process using an organic antireflection film in addition to these. In the manufacturing process of a semiconductor device, if a circuit pattern is formed by such a pattern forming method of the present invention, the semiconductor device can be manufactured with good yield.
[0077] At this time, it is preferable to form the inorganic hard mask by a CVD method or an ALD method.
[0078] The pattern forming method of the present invention can form an inorganic hard mask using such a method, for example.
[0079] The method of forming the circuit pattern on the resist upper layer film preferably uses optical lithography with a wavelength of 10 nm to 300 nm, direct writing by electron beam, nanoimprinting, or a combination thereof.
[0080] In the pattern forming method of the present invention, the developing method preferably uses alkali development or development using an organic solvent.
[0081] The pattern forming method of the present invention can preferably use such a circuit pattern forming method and a developing method.
[0082] The aforementioned object to be processed is preferably a semiconductor device substrate, or a semiconductor device substrate on which any one of a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film and a metal oxide nitride film is formed.
[0083] As the metal, preferably used is silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
[0084] According to the pattern forming method of the present invention, the above-mentioned object to be processed can be processed to form a pattern.
[0085] The present invention also provides a polymer having a partial structure represented by the following general formula (1) as a repeating unit.
[0086] [Chemistry 8]
[0087]
[0088] In the above general formula (1), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, and W 1 W is any one of the following general formulas (2), (4), and (6), and two or more kinds of W may be used in combination. 1 , W 2 It is a divalent organic group having 6 to 80 carbon atoms and having at least one aromatic ring.
[0089] [Chemistry 9]
[0090]
[0091] In the above general formula (2), AR3, AR4, and AR5 are benzene rings or naphthalene rings which may have substituents, and AR3 and AR4 or AR4 and AR5 may form a bridged structure with aromatic rings via carbon atoms bonded to hydrogen atoms on the aromatic rings. Y is a substituent represented by the following general formula (3).
[0092] [Chemistry 10]
[0093]
[0094] R 3 is a single bond or a divalent organic group having 20 or less carbon atoms, R 4 It is hydrogen or a monovalent organic group having 20 or less carbon atoms.
[0095] [Chemistry 11]
[0096]
[0097] In the above general formula (4), AR6 and AR7 are benzene rings or naphthalene rings which may also have substituents, n1 is 0 or 1, and when n1=0, AR6 and AR7 do not form a bridged structure between the aromatic rings via Z, and when n1=1, AR6 and AR7 form a bridged structure via Z, and Z is a single bond or any one of the following general formulas (5). Y is a substituent represented by the above general formula (3).
[0098] [Chemistry 12]
[0099]
[0100] [Chemistry 13]
[0101]
[0102] AR8 in the above general formula (6) is a benzene ring, a naphthalene ring, anthracene ring, a phenanthrene ring, or a pyrene ring, Y is a substituent represented by the above general formula (3), and n2 and n3 are integers satisfying the relationship of 0≤n2≤4, 0≤n3≤4, and 1≤n2+n3≤4.
[0103] If such a polymer is used, it can be introduced into W 1 The polymer forms an organic film that solidifies under film-forming conditions not only in air but also in inert gas by the action of a substituent having a triple bond at the 10-15 site, and has high heat resistance, excellent film-forming properties, and high filling / flattening properties. In addition, the steric hindrance caused by the cardole structure contained in the repeating unit prevents crystallization, thereby improving film-forming properties, while imparting heat resistance and etching resistance without impairing thermal fluidity.
[0104] W in the above general formula (1) 2 The divalent organic group represented by is preferably any of the following.
[0105] [Chemistry 14]
[0106]
[0107] Such a polymer is effective in forming an organic film having both etching resistance and distortion resistance. In addition, excellent filling / planarization characteristics can be exhibited by suppressing film shrinkage during curing.
[0108] Effects of the Invention
[0109] As described above, the polymer of the present invention is an effective polymer for forming an organic film; the organic film is introduced into W 1The substituent with a triple bond in the partial structure represented by the present invention can solidify even when forming a film in a passive gas to prevent corrosion of the substrate, and has a high degree of filling and flattening properties. In addition, the composition for forming an organic film containing the polymer is a material for forming an organic film having excellent filling / flattening properties, coating properties, and multiple properties such as heat resistance and etching resistance. Therefore, it is very effective as an organic film material in a multilayer resist method such as a two-layer resist method, a three-layer resist method using a silicon-containing resist intermediate film, a four-layer resist method using a silicon-containing resist intermediate film and an organic anti-reflection film, or as a flattening material for manufacturing semiconductor devices. In addition, the organic film formed by the organic film forming composition of the present invention has excellent heat resistance, so even when a CVD hard mask is formed on the aforementioned organic film, there is no film thickness variation caused by thermal decomposition, and it is suitable for pattern formation. BRIEF DESCRIPTION OF THE DRAWINGS
[0110] Figure 1 It is an explanatory diagram of the planarization characteristics in the present invention.
[0111] Figure 2 This is an explanatory diagram of one example of a pattern forming method using the three-layer resist method of the present invention.
[0112] Figure 3 It is an explanatory diagram of the landfill characteristic evaluation method in the example.
[0113] Figure 4 It is an explanatory diagram of the planarization characteristic evaluation method in the example. DETAILED DESCRIPTION
[0114] As described above, it is required to develop an organic film forming material which will not produce sublimates even under film forming conditions in a passive gas, for example, above 300°C, in order to prevent corrosion of the substrate, and which is capable of forming an organic film having not only excellent filling and planarizing properties of the pattern formed on the substrate but also good dry etching resistance during substrate processing, and which will not cause changes in the film thickness of the organic film due to thermal decomposition even when a CVD hard mask is formed on the organic film, and a compound which is effective in a pattern forming method using the above-mentioned material.
[0115] Usually, when forming an organic film, a compound useful in forming the organic film is dissolved in an organic solvent to form a composition, which is then applied to a substrate having a structure, wiring, etc. of a semiconductor device, and calcined to form the organic film. When the composition is first applied, a coating film having a shape along the height difference structure on the substrate is formed, but when the coating film is calcined, the organic solvent is almost evaporated until solidification, and the organic film is formed using the compound remaining on the substrate. The inventors of the present invention have thought that if the compound remaining on the substrate at this time has sufficient thermal fluidity, the height difference shape when it is just applied can be flattened by thermal flow to form a flat film.
[0116] The present inventors have further studied and found that if the polymer is represented by the following general formula (1), it will become a specific organic film-forming composition, thereby completing the present invention; the organic film-forming composition is introduced into W 1 The effect of the substituent having a triple bond in the partial structure represented is that it has the same thermal curing property as the known underlying film material not only in air but also in inert gas, and does not produce by-products during the curing reaction of the triple bond as a cross-linking group. In addition, due to good thermal fluidity, it has a high degree of filling / planarization characteristics, and at the same time has good dry etching resistance and heat resistance without changes in the coating film thickness caused by thermal decomposition even when forming a CVD hard mask.
[0117] That is, the present invention is an organic film-forming composition comprising:
[0118] A polymer having a partial structure represented by the following general formula (1) as a repeating unit, and
[0119] Organic solvents.
[0120] [Chemistry 15]
[0121]
[0122] In the above general formula (1), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, and W 1 W is any one of the following general formulas (2), (4), and (6), and two or more kinds of W may be used in combination. 1 , W 2 It is a divalent organic group having 6 to 80 carbon atoms and having at least one aromatic ring.
[0123] [Chemistry 16]
[0124]
[0125] In the above general formula (2), AR3, AR4, and AR5 are benzene rings or naphthalene rings which may have substituents, and AR3 and AR4 or AR4 and AR5 may form a bridged structure with aromatic rings via carbon atoms bonded to hydrogen atoms on the aromatic rings. Y is a substituent represented by the following general formula (3).
[0126] [Chemistry 17]
[0127]
[0128] R 3 is a single bond or a divalent organic group having 20 or less carbon atoms, R 4 It is hydrogen or a monovalent organic group having 20 or less carbon atoms.
[0129] [Chemistry 18]
[0130]
[0131] In the above general formula (4), AR6 and AR7 are benzene rings or naphthalene rings which may also have substituents, n1 is 0 or 1, and when n1=0, AR6 and AR7 do not form a bridged structure between the aromatic rings via Z, and when n1=1, AR6 and AR7 form a bridged structure via Z, and Z is a single bond or any one of the following general formulas (5). Y is a substituent represented by the above general formula (3).
[0132] [Chemistry 19]
[0133]
[0134] [Chemistry 20]
[0135]
[0136] AR8 in the above general formula (6) is a benzene ring, a naphthalene ring, anthracene ring, a phenanthrene ring, or a pyrene ring, Y is a substituent represented by the above general formula (3), and n2 and n3 are integers satisfying the relationship of 0≤n2≤4, 0≤n3≤4, and 1≤n2+n3≤4.
[0137] Furthermore, the present invention is a polymer having a partial structure represented by the following general formula (1) as a repeating unit.
[0138] [Chemistry 21]
[0139]
[0140] In the above general formula (1), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, and W 1 W is any one of the following general formulas (2), (4), and (6), and two or more kinds of W may be used in combination. 1 , W 2It is a divalent organic group having 6 to 80 carbon atoms and having at least one aromatic ring.
[0141] [Chemistry 22]
[0142]
[0143] In the above general formula (2), AR3, AR4, and AR5 are benzene rings or naphthalene rings which may have substituents, and AR3 and AR4 or AR4 and AR5 may form a bridged structure with aromatic rings via carbon atoms bonded to hydrogen atoms on the aromatic rings. Y is a substituent represented by the following general formula (3).
[0144] [Chemistry 23]
[0145]
[0146] R 3 is a single bond or a divalent organic group having 20 or less carbon atoms, R 4 It is hydrogen or a monovalent organic group having 20 or less carbon atoms.
[0147] [Chemistry 24]
[0148]
[0149] In the above general formula (4), AR6 and AR7 are benzene rings or naphthalene rings which may also have substituents, n1 is 0 or 1, and when n1=0, AR6 and AR7 do not form a bridged structure between the aromatic rings via Z, and when n1=1, AR6 and AR7 form a bridged structure via Z, and Z is a single bond or any one of the following general formulas (5). Y is a substituent represented by the above general formula (3).
[0150] [Chemistry 25]
[0151]
[0152] [Chemistry 26]
[0153]
[0154] AR8 in the above general formula (6) is a benzene ring, a naphthalene ring, anthracene ring, a phenanthrene ring, or a pyrene ring, Y is a substituent represented by the above general formula (3), and n2 and n3 are integers satisfying the relationship of 0≤n2≤4, 0≤n3≤4, and 1≤n2+n3≤4.
[0155] Hereinafter, the present invention will be described in detail, but the present invention is not limited thereto.
[0156] [polymer]
[0157] The organic film-forming composition of the present invention contains a polymer having a partial structure represented by the following general formula (1) as a repeating unit.
[0158] [Chemistry 27]
[0159]
[0160] In the above general formula (1), AR1 and AR2 are benzene rings or naphthalene rings which may have substituents, and W 1 W is any one of the following general formulas (2), (4), and (6), and two or more kinds of W may be used in combination. 1 , W 2 It is a divalent organic group having 6 to 80 carbon atoms and having at least one aromatic ring.
[0161] [Chemistry 28]
[0162]
[0163] In the above general formula (2), AR3, AR4, and AR5 are benzene rings or naphthalene rings which may have substituents, and AR3 and AR4 or AR4 and AR5 may form a bridged structure with aromatic rings via carbon atoms bonded to hydrogen atoms on the aromatic rings. Y is a substituent represented by the following general formula (3).
[0164] [Chemistry 29]
[0165]
[0166] R 3 is a single bond or a divalent organic group having 20 or less carbon atoms, R 4 It is hydrogen or a monovalent organic group having 20 or less carbon atoms.
[0167] [Chemistry 30]
[0168]
[0169] In the above general formula (4), AR6 and AR7 are benzene rings or naphthalene rings which may also have substituents, n1 is 0 or 1, and when n1=0, AR6 and AR7 do not form a bridged structure between the aromatic rings via Z, and when n1=1, AR6 and AR7 form a bridged structure via Z, and Z is a single bond or any one of the following general formulas (5). Y is a substituent represented by the above general formula (3).
[0170] [Chemistry 31]
[0171]
[0172] [Chemistry 32]
[0173]
[0174] AR8 in the above general formula (6) is a benzene ring, a naphthalene ring, anthracene ring, a phenanthrene ring, or a pyrene ring, Y is a substituent represented by the above general formula (3), and n2 and n3 are integers satisfying the relationship of 0≤n2≤4, 0≤n3≤4, and 1≤n2+n3≤4.
[0175] The partial structure represented by the general formula (2) can be specifically exemplified as follows. The aromatic rings thereof may also have substituents, and examples of the substituents include hydroxyl, trifluoromethyl, alkyl having 1 to 10 carbon atoms, alkynyl and alkenyl having 3 to 10 carbon atoms, alkyloxy having 1 to 10 carbon atoms, alkynyloxy having 3 to 10 carbon atoms, alkenyloxy, aryl having 6 to 10 carbon atoms, thiol, nitro, halogen, nitrile, sulfonic acid, alkoxycarbonyl having 1 to 10 carbon atoms, alkanoyloxy having 1 to 10 carbon atoms, etc. Among them, indenofluorene is more preferred from the viewpoint of imparting heat resistance and etching resistance.
[0176] [Chemistry 33]
[0177]
[0178] In addition, the substituent Y represented by the general formula (3) can be specifically exemplified as follows. In the following formula, * represents the bonding site to the N atom in the formula (2). Among them, considering the ease of intermediate synthesis and the ease of obtaining industrial raw materials, propargyl and butynyl are preferred.
[0179] [Chemistry 34]
[0180]
[0181] The partial structure represented by the general formula (4) can be specifically exemplified as follows. The aromatic rings thereof may also have substituents, and examples of the substituents include hydroxyl, trifluoromethyl, alkyl having 1 to 10 carbon atoms, alkynyl and alkenyl having 3 to 10 carbon atoms, alkyloxy having 1 to 10 carbon atoms, alkynyloxy having 3 to 10 carbon atoms, alkenyloxy, aryl having 6 to 10 carbon atoms, thiol, nitro, halogen, nitrile, sulfonic acid, alkoxycarbonyl having 1 to 10 carbon atoms, alkanoyloxy having 1 to 10 carbon atoms, and the like. Among them, those having phenylnaphthylamine and carbazole as partial structures are more preferred from the viewpoints of the availability of industrial raw materials, heat resistance, and solvent solubility. Y in the following formula is the same as that described above.
[0182] [Chemistry 35]
[0183]
[0184] The partial structure represented by the general formula (6) can be specifically exemplified as follows. The aromatic rings thereof may also have a substituent, and examples of the substituent include a hydroxyl group, a trifluoromethyl group, an alkyl group having 1 to 10 carbon atoms, an alkyloxy group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, a thiol group, a nitro group, a halogen group, a nitrile group, a sulfonic acid group, an alkoxycarbonyl group having 1 to 10 carbon atoms, and an alkanoyloxy group having 1 to 10 carbon atoms. Among them, from the viewpoint of the ease of obtaining the raw materials and the heat resistance, the partial structure having a naphthalene ring is preferred.
[0185] [Chemistry 36]
[0186]
[0187] [Chemistry 37]
[0188]
[0189] In addition, W in the polymer represented by the above general formula (1) 2 The divalent organic group represented by is preferably any of the following.
[0190] [Chemistry 38]
[0191]
[0192] The above general formula (1) may be exemplified by the following structural formulas, and the aromatic rings thereof may have substituents. The substituents may be exemplified by hydroxyl, trifluoromethyl, alkyl having 1 to 10 carbon atoms, alkynyl having 3 to 10 carbon atoms, alkenyl, alkyloxy having 1 to 10 carbon atoms, alkynyloxy having 3 to 10 carbon atoms, alkenyloxy, aryl having 6 to 10 carbon atoms, thiol, nitro, halogen, nitrile, sulfonic acid, alkoxycarbonyl having 1 to 10 carbon atoms, alkanoyloxy having 1 to 10 carbon atoms, etc. In the following formula, n4 is an integer of 1 to 10.
[0193] [Chemistry 39]
[0194]
[0195] [Chemistry 40]
[0196]
[0197] Furthermore, the Mw (weight average molecular weight) of the polymer is preferably 1,000 to 5,000, and more preferably 1,000 to 4,000.
[0198] If it is such a molecular weight, solubility in organic solvents can be ensured, and sublimates generated during baking can be suppressed. In addition, the polymer has good thermal fluidity, so when it is deployed in a composition, it can not only well fill the fine structure formed on the substrate, but also form an organic film with a flat substrate as a whole.
[0199] Furthermore, the polymer of the present invention may have any partial structure represented by the following general formula as a repeating unit. The polymer of the present invention can increase the carbon density and impart excellent distortion resistance and etching resistance by having these partial structures.
[0200] [Chemistry 41]
[0201]
[0202] [Production method 1 of polymer]
[0203] The polymer of the present invention can be synthesized by polycondensation using a tertiary alcohol or alkyl ether compound as shown below. 1 or W 2 A tertiary alcohol or alkyl ether as a linking group, or two or more thereof, can be appropriately selected and combined according to the required properties. 1 , W 2 As mentioned above, R represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.
[0204] [Chemistry 42]
[0205]
[0206] The polymer can be obtained usually in an organic solvent in the presence of an acid catalyst at room temperature or under cooling or heating as required. The acid catalyst used can be: inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, and heteropoly acid; organic acids such as oxalic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid; and Lewis acids such as aluminum trichloride, ethoxyaluminum, isopropoxyaluminum, boron trifluoride, boron trichloride, boron tribromide, tin tetrachloride, tin tetrabromide, dibutyltin dichloride, dimethoxydibutyltin, dibutyltin oxide, titanium tetrachloride, titanium tetrabromide, methoxytitanium (IV), ethoxytitanium (IV), isopropoxytitanium (IV), and titanium (IV) oxide.
[0207] The solvent used is not particularly limited, and examples thereof include: alcohols such as methanol, ethanol, isopropanol, butanol, ethylene glycol, propylene glycol, diethylene glycol, glycerol, ethylene glycol monomethyl ether, and propylene glycol monomethyl ether; ethers such as diethyl ether, dibutyl ether, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, and 1,4-dioxane; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, and trichloroethylene; hydrocarbons such as hexane, heptane, benzene, toluene, xylene, and cumene; nitriles such as acetonitrile; ketones such as acetone, methyl ethyl ketone, and isobutyl methyl ketone; esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate; and aprotic polar solvents such as dimethyl sulfoxide, N,N-dimethylformamide, and hexamethylphosphoric acid triamide. These solvents can be used alone or in combination of two or more.
[0208] As for the reaction method, there is a method using the aforementioned AR1, AR2 and W 1 A method in which a compound and an aldehyde, a tertiary alcohol, etc. are used as monomers, and an acid catalyst is fed at once; a method in which the monomer is dispersed or dissolved, and then the catalyst is added at once or in portions, or a method in which the catalyst is diluted with a solvent and then added dropwise; a method in which the catalyst is dispersed or dissolved, and then the monomer is added at once or in portions, or a method in which the catalyst is diluted with a solvent and then added dropwise. After the reaction is completed, in order to remove the catalyst used in the reaction, the catalyst can be diluted with an organic solvent, and then liquid separation and washing can be performed to recover the target product.
[0209] In addition, in these reactions, copolymerization and condensation can also be carried out using compounds that are different from the above-mentioned monomers. Examples of copolymerization and condensation compounds are as follows. They can also have substituents such as vinyl, allyl, propargyl, aryl, and allyloxy groups on their aromatic rings. Considering the viewpoint of imparting etching resistance and solvent solubility, compounds having a naphthalene ring, a fluorene structure, and a carbazole structure are preferred, and they can be added simultaneously or separately when implementing the polycondensation using the above-mentioned method and copolymerization and condensation are carried out.
[0210] [Chemistry 43]
[0211]
[0212] [Chemistry 44]
[0213]
[0214] [Chemistry 45]
[0215]
[0216] The organic solvent used in the liquid separation cleaning is not particularly limited as long as it is an organic solvent that can dissolve the target and separate into two layers when mixed with water. Examples thereof include: hydrocarbons such as hexane, heptane, benzene, toluene, and xylene; esters such as ethyl acetate, n-butyl acetate, and propylene glycol methyl ether acetate; ketones such as methyl ethyl ketone, methyl amyl ketone, cyclohexanone, and methyl isobutyl ketone; ethers such as diethyl ether, diisopropyl ether, methyl tert-butyl ether, and ethyl cyclopentyl methyl ether; chlorine-based solvents such as dichloromethane, chloroform, dichloroethane, and trichloroethylene; and mixtures thereof. The cleaning water used at this time can be what is generally called deionized water or ultrapure water. The number of cleaning times may be one or more, but since the corresponding cleaning effect cannot be obtained by cleaning more than 10 times, it is preferably about 1 to 5 times.
[0217] In order to remove the acidic components in the reaction system during the liquid separation and washing, an alkaline aqueous solution may be used for washing. Specific examples of the alkali include alkali metal hydroxides, alkali metal carbonates, alkaline earth metal hydroxides, alkaline earth metal carbonates, ammonia, and organic ammonium.
[0218] In addition, in order to remove metal impurities or alkaline components in the reaction system during liquid separation and cleaning, an acidic aqueous solution can also be used for cleaning. Specifically, the acid includes inorganic acids such as hydrochloric acid, hydrobromic acid, sulfuric acid, nitric acid, phosphoric acid, and heteropoly acids; and organic acids such as oxalic acid, fumaric acid, maleic acid, trifluoroacetic acid, methanesulfonic acid, benzenesulfonic acid, p-toluenesulfonic acid, and trifluoromethanesulfonic acid.
[0219] The liquid separation cleaning using the alkaline aqueous solution and the acidic aqueous solution may be performed alone or in combination. Liquid separation cleaning using the alkaline aqueous solution and the acidic aqueous solution in sequence is more preferred from the viewpoint of removing metal impurities.
[0220] After the aforementioned liquid separation cleaning using alkaline aqueous solution or acidic aqueous solution, cleaning with neutral water may be continued. The cleaning frequency may be performed once or more, preferably about 1 to 5 times. Neutral water may be the aforementioned deionized water, ultrapure water, etc. The cleaning frequency may be performed once or more, but if the frequency is less, the alkaline component or acidic component may not be removed. Since the corresponding cleaning effect may not be obtained even after cleaning for more than 10 times, it is preferably about 1 to 5 times.
[0221] In addition, the reaction product after the liquid separation operation can also be concentrated to dryness or crystallized under reduced pressure or normal pressure, and recovered in the form of powder, but in order to improve the operability when preparing the organic film-forming composition, it can also be made into a solution state of appropriate concentration in advance. The concentration at this time is preferably 0.1 to 50% by mass, and more preferably 0.5 to 30% by mass. If it is such a concentration, the viscosity is not easy to increase, so it can prevent the operability from being damaged. In addition, it is more economical because the amount of solvent is not too large.
[0222] The solvent at this time is not particularly limited as long as it is a solvent that can dissolve the polymer. Specific examples include: ketones such as cyclohexanone and methyl-2-pentyl ketone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, and 1-ethoxy-2-propanol; ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, and diethylene glycol dimethyl ether; esters such as propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, tert-butyl acetate, tert-butyl propionate, and propylene glycol mono-tert-butyl ether acetate. These can be used alone or in combination of two or more.
[0223] [Method 2 for producing polymer (another method)]
[0224] In addition, a polymer having a partial structure represented by (2) or (4) can also be obtained by the following method: using a compound having a hydrogen atom as a substituent on nitrogen and a tertiary alcohol or alkyl ether compound shown below, and obtaining an intermediate by polycondensation in the same manner as in the above-mentioned polymer production method 1 (Step 1), and then converting the hydrogen atom on nitrogen to Y (Step 2). AR1, AR2, AR3, AR4, AR5, AR6, AR7, W 2 , R, Y are the same as above.
[0225] [Chemistry 46]
[0226]
[0227] Step 2 is not particularly limited if it is a reaction that can introduce the structure of Y onto the nitrogen atom, and examples thereof include N-alkylation reaction using a halide or toluenesulfonate or mesylate of Y with a base catalyst as in the above formula, coupling reaction using a transition metal catalyst, etc. In the above formula, X is a halogen, a toluenesulfonyl group, or a mesylate group.
[0228] The base catalyst used in the substitution reaction can be listed as follows: inorganic base compounds such as sodium bicarbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, potassium phosphate, etc.; organic amine compounds such as triethylamine, pyridine, N-methylmorpholine, etc., which can be used alone or in combination of two or more. In addition, when using a transition metal catalyst, copper catalysts such as copper powder, copper chloride, copper bromide, copper iodide, copper acetate, copper hydroxide, copper nitrate, etc. can be used; palladium catalysts such as tris (dibenzylideneacetone) dipalladium, tetrakis (triphenylphosphine) palladium, etc., can also be combined with the above-mentioned base catalysts.
[0229] The solvent used in the other method is not particularly limited as long as it is a solvent inactive to the above-mentioned reaction. Examples thereof include: ether solvents such as diethyl ether, tetrahydrofuran, and dioxane; aromatic solvents such as benzene, toluene, and xylene; acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, water, etc., which can be used alone or in combination.
[0230] The reaction method and the method for recovering the compound can be recovered by the same method as in the method 1 for producing the polymer.
[0231] In addition, among the polymers having a partial structure represented by the general formula (6), a polymer having OY as a substituent can also be obtained by the following method: using a compound having a hydroxyl group as a substituent and a tertiary alcohol or an alkyl ether compound as shown below, and using polycondensation in the same way as the above-mentioned polymer production methods 1 and 2 to obtain an intermediate (Step 1), and then introducing Y into the hydroxyl group by a substitution reaction (Step 2).
[0232] [Chemistry 47]
[0233]
[0234] Step 2 is not particularly limited as long as it is a reaction that can introduce Y, and examples thereof include substitution reaction using a halide, toluenesulfonate, or mesylate of Y with a base catalyst. X in the above formula represents a halogen, toluenesulfonyl group, or mesylate group.
[0235] Examples of the base catalyst used in the above-mentioned substitution reaction include inorganic base compounds such as sodium bicarbonate, sodium carbonate, potassium carbonate, calcium carbonate, cesium carbonate, sodium hydroxide, potassium hydroxide, sodium hydride, potassium phosphate, etc.; organic amine compounds such as triethylamine, pyridine, N-methylmorpholine, etc., and they can be used alone or in combination of two or more.
[0236] The solvent used at this time is not particularly limited as long as it is a solvent inactive to the above-mentioned reaction. Examples thereof include: ether solvents such as diethyl ether, tetrahydrofuran, and dioxane; aromatic solvents such as benzene, toluene, and xylene; acetonitrile, dimethyl sulfoxide, N,N-dimethylformamide, N-methylpyrrolidone, water, etc., which can be used alone or in combination.
[0237] The reaction method and the method for recovering the compound can be recovered by the same methods as in the methods 1 and 2 for producing the polymer.
[0238] In the preparation of the above polymer, two or more YX, or halides different from YX, or toluenesulfonates and mesylate salts may be combined to match the required performance. Compounds containing side chain structures that contribute to the improvement of planarization characteristics and rigid aromatic ring structures that contribute to etching resistance and heat resistance may be combined in any proportion. An organic film-forming composition using a polymer obtained using these compounds can achieve both high-level filling / planarization characteristics and etching resistance.
[0239] As described above, the polymer of the present invention can provide an organic film-forming composition having both heat resistance of 400° C. or higher and high-level filling / planarization properties.
[0240] In the present invention, the flattening property refers to the ability to flatten the surface of a substrate. If the composition for forming an organic film containing the polymer of the present invention is, for example, Figure 1 As shown, by applying the organic film-forming composition 3' onto the substrate 1 and heating it to form the organic film 3, the height difference of the substrate 1 of 100 nm can be reduced to less than 30 nm. Figure 1 The illustrated stepped shapes are typical examples of stepped shapes in a substrate for manufacturing a semiconductor device, and the stepped shapes of a substrate that can be planarized using the organic film-forming composition containing the polymer of the present invention are of course not limited thereto.
[0241] [Organic film-forming composition]
[0242] The present invention also provides an organic film-forming composition, which is a composition for forming an organic film, comprising (A) the polymer of the present invention and (B) an organic solvent. In the organic film-forming composition of the present invention, the polymer of the present invention may be used alone or in combination of two or more.
[0243] The organic solvent that can be used in the organic film-forming composition of the present invention is not particularly limited as long as it is an organic solvent that can dissolve the constituent components contained in the materials such as the aforementioned polymer, acid generator, crosslinking agent, other additives, etc. Specifically, a solvent having a boiling point lower than 180° C. such as the solvents described in paragraphs (0091) to (0092) of Japanese Patent Application Laid-Open No. 2007-199653 can be used. Among them, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, 2-heptanone, cyclopentanone, cyclohexanone, and a mixture of two or more thereof are preferably used.
[0244] Such an organic film-forming composition can be applied by spin coating, and since it contains the polymer of the present invention as described above, it can provide an organic film-forming composition having both heat resistance of 400° C. or higher and high filling / planarization properties.
[0245] In the composition for forming an organic film of the present invention, as for the organic solvent, a high boiling point solvent having a boiling point of 180°C or higher (a mixture of a solvent having a boiling point of less than 180°C and a solvent having a boiling point of 180°C or higher) may be added to the solvent having a boiling point of less than 180°C. As for the high boiling point organic solvent, there is no particular limitation on hydrocarbons, alcohols, ketones, esters, ethers, chlorine-based solvents, etc., as long as the high boiling point organic solvent is an organic solvent that can dissolve the polymer of the present invention. Specific examples thereof include 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, 1-undecanol, ethylene glycol, 1,2-propylene glycol, 1,3-butanediol, 2,4-pentanediol, 2-methyl-2,4-pentanediol, 2,5-hexanediol, 2,4-heptanedi ... 1,3-hexanediol, diethylene glycol, dipropylene glycol, triethylene glycol, tripropylene glycol, glycerol, n-nonyl acetate, ethylene glycol monohexyl ether, ethylene glycol mono-2-ethylhexyl ether, ethylene glycol monophenyl ether, ethylene glycol monobenzyl ether, diethylene glycol monoethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoisobutyl ether, diethylene glycol monohexyl ether, diethylene glycol monophenyl ether, diethylene glycol monobenzyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl methyl ether, triethylene glycol dimethyl ether , triethylene glycol monomethyl ether, triethylene glycol n-butyl ether, triethylene glycol butyl methyl ether, triethylene glycol diacetate, tetraethylene glycol dimethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, tripropylene glycol mono-n-propyl ether, tripropylene glycol mono-n-butyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, triacetin, Propylene glycol diacetate, dipropylene glycol monomethyl ether acetate, dipropylene glycol methyl n-propyl ether, dipropylene glycol methyl ether acetate, 1,4-butanediol diacetate, 1,3-butanediol diacetate, 1,6-hexanediol diacetate, triethylene glycol diacetate, γ-butyrolactone, dihexyl malonate, diethyl succinate, dipropyl succinate, dibutyl succinate, dihexyl succinate, dimethyl adipate, diethyl adipate, dibutyl adipate, etc., which can be used alone or in combination.
[0246] The boiling point of the high boiling point solvent is appropriately selected according to the temperature at which the organic film forming composition is heat treated. The boiling point of the added high boiling point solvent is preferably 180°C to 300°C, more preferably 200°C to 300°C. If it is such a boiling point, there is no concern that the solvent volatilizes too quickly during baking (heat treatment) due to a too low boiling point, so sufficient thermal fluidity can be obtained. In addition, if it is such a boiling point, since the boiling point is high, there will be no situation where the solvent remains in the film after baking without volatilization, so there is no concern that the film properties such as etching resistance will be adversely affected.
[0247] In addition, when the high boiling point solvent is used, the amount of the high boiling point solvent is preferably set to 1 to 30 parts by mass relative to 100 parts by mass of the solvent having a boiling point lower than 180° C. If such an amount is used, there is no concern that the amount is too small to provide sufficient thermal fluidity during baking, or that the amount is too large to remain in the film and cause deterioration of film properties such as etching resistance.
[0248] According to such an organic film-forming composition, by providing thermal fluidity by adding a high-boiling-point solvent to the polymer of the present invention, an organic film-forming composition having both high-level filling and planarizing properties can be provided.
[0249] In order to further promote the curing reaction, (C) an acid generator may be added to the organic film-forming composition of the present invention. The acid generator includes an acid generator that generates acid by thermal decomposition and an acid generator that generates acid by light irradiation, and any of them may be added. Specifically, the materials described in paragraphs (0061) to (0085) of Japanese Patent Application Publication No. 2007-199653 may be added, but the present invention is not limited thereto.
[0250] The acid generator may be used alone or in combination of two or more. The amount of the acid generator added is preferably 0.05 to 50 parts by mass, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the polymer of the present invention.
[0251] To improve the coating property in spin coating, a surfactant (D) may be added to the organic film-forming composition of the present invention. As the surfactant, for example, the surfactants described in (0142) to (0147) of JP-A-2009-269953 may be used.
[0252] In addition, in order to improve the curability and further inhibit the mutual mixing with the upper film, (E) a crosslinking agent may be added to the organic film-forming composition of the present invention. As for the crosslinking agent, there is no particular limitation, and various known crosslinking agents can be widely used. For example, melamine crosslinking agents, glycoluril crosslinking agents, benzoguanamine crosslinking agents, urea crosslinking agents, β-hydroxyalkylamide crosslinking agents, isocyanurate crosslinking agents, aziridine crosslinking agents, oxazoline crosslinking agents, and epoxy crosslinking agents can be illustrated.
[0253] Specifically, for melamine-based crosslinking agents, hexamethoxymethylated melamine, hexabutoxymethylated melamine, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. Specifically, for glycoluril-based crosslinking agents, tetramethoxymethylated glycoluril, tetrabutoxymethylated glycoluril, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. Specifically, for benzoguanamine-based crosslinking agents, tetramethoxymethylated benzoguanamine, tetrabutoxymethylated benzoguanamine, their alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. Specifically, for urea-based crosslinking agents, dimethoxymethylated dimethoxyethylene urea, its alkoxy and / or hydroxyl substitutions, and their partial self-condensation products can be exemplified. Specifically, for β-hydroxyalkylamide-based crosslinking agents, N,N,N',N'-tetrakis(2-hydroxyethyl)adipamide can be exemplified. Specific examples of isocyanurate crosslinking agents include triglycidyl isocyanurate and triallyl isocyanurate. Specific examples of aziridine crosslinking agents include 4,4'-bis(ethyleneiminocarbonylamino)diphenylmethane and 2,2-bishydroxymethylbutanol-tris[3-(1-aziridinyl)propionate]. Specific examples of oxazoline crosslinking agents include 2,2'-isopropylidenebis(4-benzyl-2-oxazoline), 2,2'-isopropylidenebis(4-phenyl-2-oxazoline), 2,2'-methylenebis-4,5-diphenyl-2-oxazoline, 2,2'-methylenebis-4-phenyl-2-oxazoline, 2,2'-methylenebis-4-tert-butyl-2-oxazoline, 2,2'-bis(2-oxazoline), 1,3-phenylenebis(2-oxazoline), 1,4-phenylenebis(2-oxazoline), and 2-isopropenyloxazoline copolymers. Specific examples of epoxy crosslinking agents include diglycidyl ether, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, 1,4-cyclohexanedimethanol diglycidyl ether, poly(glycidyl methacrylate), trimethylolethane triglycidyl ether, trimethylolpropane triglycidyl ether, and pentaerythritol tetraglycidyl ether.
[0254] In addition, in order to further improve the planarization / burying characteristics, a plasticizer (F) may be added to the organic film-forming composition of the present invention. There is no particular limitation on the plasticizer, and various known plasticizers can be widely used. Examples thereof include low molecular weight compounds such as phthalates, adipic acid esters, phosphates, trimellitic acid esters, and citrates, polyethers, polyesters, and polymers such as polyacetal polymers described in Japanese Patent Application Laid-Open No. 2013-253227.
[0255] In addition, in the composition for forming an organic film of the present invention, as an additive for imparting a filling / planarizing property similarly to a plasticizer, it is preferable to use, for example, a liquid additive having a polyethylene glycol or polypropylene glycol structure, or a pyrolyzable polymer having a weight loss rate of 40% by mass or more between 30° C. and 250° C. and a weight average molecular weight of 300 to 200,000. The pyrolyzable polymer preferably contains a repeating unit having an acetal structure represented by the following general formula (DP1) or (DP1a).
[0256] [Chemistry 48]
[0257]
[0258] In the formula, R 6 Y is a hydrogen atom or an optionally substituted saturated or unsaturated monovalent organic group having 1 to 30 carbon atoms. 1 It is a saturated or unsaturated divalent organic group having 2 to 30 carbon atoms.
[0259] [Chemistry 49]
[0260]
[0261] In the formula, R 6a Y is an alkyl group having 1 to 4 carbon atoms. a It is a saturated or unsaturated divalent hydrocarbon group having 4 to 10 carbon atoms, and may have an ether bond. n represents the average number of repeating units, and is 3 to 500.
[0262] As described above, the organic film-forming composition of the present invention has heat resistance of 400°C or more and high-level filling / planarization characteristics. Therefore, the organic film-forming composition of the present invention is very effective as an organic film material for multilayer resist methods such as a two-layer resist method, a three-layer resist method using a silicon-containing resist intermediate film or a silicon-containing inorganic hard mask, and a four-layer resist method using a silicon-containing resist intermediate film or a silicon-containing inorganic hard mask and an organic antireflection film. In addition, the organic film-forming composition of the present invention does not produce by-products even when forming a film in an inert gas, and has excellent filling / planarization characteristics, so it can also be preferably used as a planarization material in a semiconductor device manufacturing step other than the multilayer resist method.
[0263] [Substrates for semiconductor device manufacturing]
[0264] Furthermore, the present invention provides a substrate for manufacturing a semiconductor device, on which an organic film is formed by curing the above-mentioned organic film-forming composition.
[0265] The organic film formed from the composition for forming an organic film of the present invention has high filling / planarization properties, so there are no microscopic voids due to poor filling or unevenness on the surface of the organic film due to insufficient planarization. The semiconductor device substrate formed by planarizing the organic film has a wide process latitude range during patterning, and semiconductor devices can be manufactured with good yield.
[0266] [Method for forming organic film]
[0267] The heating film forming step for forming the organic film can use one-stage baking, two-stage baking or multi-stage baking of three or more stages, and one-stage baking or two-stage baking is more economically preferred. The film formation using one-stage baking is carried out, for example, at a temperature of 50°C or more and 600°C or less, and in the range of 5 to 7200 seconds, preferably at a temperature of 150°C or more and 500°C or less, and in the range of 10 to 3600 seconds. By performing heat treatment under such conditions, the flattening and cross-linking reactions obtained by heat flow can be promoted. In the multilayer resist method, there is a case where a coated silicon intermediate film and a CVD hard mask are formed on the obtained film. When using a coated silicon intermediate film, it is preferably formed at a temperature higher than the film forming temperature of the silicon intermediate film. Usually, the silicon intermediate film is formed at a temperature of 100°C or more and 400°C or less, preferably at a temperature of 150°C or more and 350°C or less. When the organic film is formed at a temperature higher than this temperature, dissolution of the organic film by the composition for forming a silicon interlayer film can be prevented, and an organic film that is not mixed with the composition can be formed.
[0268] When a CVD hard mask is used, the organic film is preferably formed at a temperature higher than the temperature at which the CVD hard mask is formed. The temperature at which the CVD hard mask is formed may be 150° C. or higher and 500° C. or lower, for example.
[0269] On the other hand, in the film formation using two-stage baking, for the first-stage baking, considering the influence of substrate corrosion caused by oxygen in the air, the upper limit of the processing temperature in the air is, for example, below 250°C, preferably below 200°C and above 50°C, and implemented in the range of 5 to 600 seconds. As for the baking temperature of the second stage, it is preferably higher than the baking temperature of the first stage, below 600°C, preferably below 500°C and above 200°C, and implemented in the range of 10 to 7200 seconds. In the multilayer resist method, there is a case where a coated silicon intermediate film and a CVD hard mask are formed on the obtained film. When using a coated silicon intermediate film, it is preferably formed at a temperature higher than the film formation temperature of the silicon intermediate film. Usually, the silicon intermediate film is formed at a temperature of 100°C to 400°C, preferably 150°C to 350°C. When the organic film is formed at a temperature higher than this temperature, dissolution of the organic film by the composition for forming a silicon interlayer film can be prevented, and an organic film that is not mixed with the composition can be formed.
[0270] When a CVD hard mask is used in the two-step baking, the organic film is preferably formed at a temperature higher than the temperature at which the CVD hard mask is formed. The temperature at which the CVD hard mask is formed may be 150° C. or higher and 500° C. or lower.
[0271] In addition, the present invention provides a method for forming an organic film, which is a method for forming an organic film that functions as an organic film used in the manufacturing step of a semiconductor device. In order to prevent corrosion of the processed substrate, the processed substrate is heat-treated in an environment with an oxygen concentration of less than 1% to form a cured film.
[0272] In the method for forming the organic film, for example, the organic film-forming composition of the present invention is first spin-coated on the substrate to be processed. After spin-coating, the two-stage baking is first baked in air at a temperature of 50° C. to 250° C., and then the second stage of baking is preferably performed in an environment with an oxygen concentration of 1% or less. In the case of one-stage baking, the first stage of baking in air at the beginning can be skipped. In addition, as for the environment during baking, inert gases such as nitrogen, argon, and helium can be exemplified. If it is the organic film-forming composition of the present invention, even if it is calcined in such an inert gas environment, sublimates are not generated and a fully solidified organic film can be formed.
[0273] In addition, the method for forming an organic film of the present invention can use a substrate to be processed that has a structure or a height difference of 30 nm or more. As described above, the composition for forming an organic film of the present invention has excellent filling / flattening properties, so even if the substrate to be processed has a structure or a height difference (concave and convex) of 30 nm or more, a flat cured film can still be formed. That is, the method for forming an organic film of the present invention is particularly effective when forming a flat organic film on such a substrate to be processed.
[0274] The thickness of the organic film to be formed can be appropriately selected, and is preferably set to 30 to 20,000 nm, and more preferably set to 50 to 15,000 nm.
[0275] The above-mentioned method for forming an organic film can be applied to both the case of forming an organic film for an organic film and the case of forming an organic film for a planarizing film using the organic film-forming composition of the present invention.
[0276] The present invention provides a method for forming an organic film, which is a method for forming an organic film suitable for the manufacturing steps of a semiconductor device, and is characterized in that: the aforementioned organic film-forming composition is spin-coated on a substrate to be processed, and the substrate to be processed coated with the aforementioned organic film-forming composition is heat-treated in an inert gas environment at a temperature of 50°C to 600°C for a period of 10 seconds to 7200 seconds to obtain a cured film.
[0277] In addition, the present invention provides a method for forming an organic film, which is a method for forming an organic film suitable for the manufacturing step of a semiconductor device, and is characterized in that: the aforementioned organic film-forming composition is spin-coated on a substrate to be processed, and the substrate to be processed coated with the aforementioned organic film-forming composition is heat-treated in air at a temperature of 50°C to 250°C for 5 seconds to 600 seconds, preferably in the range of 10 to 600 seconds to form a coating film, and then heat-treated in an inert gas environment at a temperature of 200°C to 600°C, preferably at a temperature of 250°C or more, for 10 seconds to 7200 seconds to obtain a cured film.
[0278] The organic film formed by the organic film forming method of the present invention and suitable for the manufacturing steps of semiconductor devices has high heat resistance and high-level filling / planarization characteristics. If used in the manufacturing steps of semiconductor devices, the yield of semiconductor devices will be improved.
[0279] In the method for forming the organic film, first, the organic film forming composition of the present invention is spin-coated (spin-coated) on the substrate to be processed. By using the spin coating method, good filling characteristics can be obtained. After spin coating, baking (heat treatment) is performed to promote the flattening and cross-linking reaction obtained by heat flow. In addition, by utilizing this baking, the solvent in the organic film forming composition can be evaporated, so when forming a resist upper film or a silicon-containing resist intermediate film on the organic film, mutual mixing can also be prevented.
[0280] [Pattern Formation Method]
[0281] <Three-layer resist method using a resist interlayer film containing silicon>
[0282] The present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the organic film forming composition of the present invention, forming a silicon-containing resist intermediate film on the organic film using a silicon-containing resist intermediate film material, forming a resist upper film on the silicon-containing resist intermediate film using a photoresist composition, forming a circuit pattern on the resist upper film, using the resist upper film with the circuit pattern formed thereon as a mask and transferring the pattern to the silicon-containing resist intermediate film by etching, using the silicon-containing resist intermediate film with the pattern transferred thereon as a mask and transferring the pattern to the organic film by etching, and using the organic film with the pattern transferred thereon as a mask and forming the pattern on the workpiece by etching.
[0283] As the object to be processed, it is preferred to use a semiconductor device substrate, or a substrate on which a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film are formed. More specifically, Si, α-Si, p-Si, SiO 2 , SiN, SiON, W, TiN, Al and other substrates, or those in which the aforementioned metal films are formed on the aforementioned substrates as the processed layers, etc., but are not particularly limited thereto.
[0284] For the processed layer, Si, SiO 2 , SiON, SiN, p-Si, α-Si, W, W-Si, Al, Cu, Al-Si and other Low-k films and barrier films thereof can be formed to a thickness of 50 to 10,000 nm, and in particular, can be formed to a thickness of 100 to 5,000 nm. In addition, when forming a film of the processed layer, different materials can be used for the substrate and the processed layer.
[0285] In addition, the metal constituting the workpiece is preferably silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
[0286] In addition, as the object to be processed, it is preferable to use a substrate to be processed having a structure with a height of 30 nm or more or a height difference.
[0287] When an organic film is formed on a workpiece using the composition for forming an organic film of the present invention, the above-mentioned method for forming an organic film of the present invention may be used.
[0288] Then, a resist interlayer film material containing silicon atoms is used on the organic film to form a resist interlayer film (silicon-containing resist interlayer film). As for the silicon-containing resist interlayer film material, a polysiloxane-based interlayer film material is preferred. By making the silicon-containing resist interlayer film have an anti-reflection effect, reflection can be suppressed. Especially for 193nm exposure, if a material containing a large amount of aromatic groups and having a high etching selectivity with the substrate is used as the material for forming the organic film, the k value will become higher and the substrate reflection will become higher, but for the silicon-containing resist interlayer film, by making it have an absorption that can become an appropriate k value, reflection can be suppressed and the substrate reflection can be adjusted to less than 0.5%. As for the silicon-containing resist intermediate film with anti-reflective effect, if it is for 248nm and 157nm exposure, it is preferred to use a pendant structure or a polysiloxane structure having anthracene, and if it is for 193nm exposure, it is preferred to use a pendant structure or a polysiloxane structure having a phenyl group or a light-absorbing group containing a silicon-silicon bond, and cross-linking polysiloxane with acid or heat.
[0289] Then, a resist upper film is formed on the silicon-containing resist intermediate film using a resist upper film material composed of a photoresist composition. As for the resist upper film material, it can be either positive or negative, and the same photoresist composition as commonly used can be used. After spin coating the resist upper film material, it is preferably pre-baked at 60 to 180° C. for 10 to 300 seconds. Thereafter, exposure is performed according to the usual method, and then post-exposure baking (PEB) and development are performed to obtain a resist upper film pattern. In addition, the thickness of the resist upper film is not particularly limited, preferably 30 to 500 nm, and particularly preferably 50 to 400 nm.
[0290] Then, a circuit pattern (resist upper film pattern) is formed on the resist upper film. The circuit pattern is preferably formed by photolithography using light with a wavelength of 10 nm to 300 nm, direct writing by electron beam, nanoimprinting, or a combination thereof.
[0291] In addition, as for the exposure light, high-energy rays with a wavelength of 300 nm or less can be listed, and specifically, far ultraviolet rays, KrF excimer laser (248 nm), ArF excimer laser (193 nm), F2 laser (157 nm), Kr2 laser (146 nm), Ar2 laser (126 nm), 3 to 20 nm soft X-rays (EUV), electron beams (EB), ion beams, X-rays, etc. In addition, nanoimprinting or a combination thereof can be used.
[0292] In the formation of the circuit pattern, it is preferred to develop the circuit pattern using an alkali developer or an organic solvent.
[0293] Then, the resist upper film having the circuit pattern formed thereon is used as a mask and the pattern is transferred to the silicon-containing resist intermediate film by etching. The etching of the silicon-containing resist intermediate film performed using the resist upper film pattern as a mask is preferably performed using a fluorocarbon-based gas, thereby forming a silicon-containing resist intermediate film pattern.
[0294] Then, the silicon-containing resist intermediate film with the transferred pattern is used as a mask to transfer the pattern to the organic film by etching. The silicon-containing resist intermediate film exhibits higher etching resistance to oxygen or hydrogen than organic matter, so the etching of the organic film performed using the silicon-containing resist intermediate film pattern as a mask is preferably performed using an etching gas mainly composed of oxygen or hydrogen. Thus, an organic film pattern can be formed.
[0295] Then, the organic film with the transferred pattern is used as a mask and the pattern is transferred to the workpiece by etching. The subsequent etching of the workpiece (the workpiece layer) can be carried out using a common method. For example, if the workpiece is SiO 2 If the substrate is a low dielectric constant insulating film of SiN or silicon dioxide, etching is performed mainly using a flon gas. If it is p-Si, Al, or W, etching is performed mainly using a chlorine or bromine gas. When the substrate is processed by etching using a flon gas, the silicon-containing resist intermediate film pattern and the substrate are simultaneously stripped. On the other hand, when the substrate is processed by etching using a chlorine or bromine gas, in order to strip the silicon-containing resist intermediate film pattern, dry etching stripping using a flon gas is required after the substrate is processed.
[0296] The organic film obtained by using the organic film-forming composition of the present invention can be an organic film having excellent etching resistance when etching the above-mentioned object to be processed.
[0297] [Four-layer resist method using a silicon-containing resist interlayer and an organic antireflection film]
[0298] In addition, the present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the organic film forming composition of the present invention, forming a silicon-containing resist intermediate film on the aforementioned organic film using a silicon-containing resist intermediate film material, forming an organic anti-reflective film (BARC) on the aforementioned silicon-containing resist intermediate film, forming a resist upper film on the aforementioned BARC using a photoresist composition, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film with the circuit pattern formed as a mask and sequentially transferring the pattern of the BARC and the aforementioned silicon-containing resist intermediate film by etching, using the aforementioned silicon-containing resist intermediate film with the pattern transferred as a mask and transferring the pattern of the organic film by etching, and using the aforementioned organic film with the pattern transferred as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.
[0299] This method can be carried out in the same manner as the above-mentioned three-layer resist method using the silicon-containing resist interlayer film, except that an organic antireflection film (BARC) is formed between the silicon-containing resist interlayer film and the resist upper layer film.
[0300] The organic anti-reflection film (BARC) may be formed using a known organic anti-reflection film material by spin coating.
[0301] [Three-layer resist method using an inorganic hard mask]
[0302] In addition, the present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the organic film forming composition of the present invention, forming an inorganic hard mask selected from silicon oxide film, silicon nitride film, silicon oxide nitride film, titanium oxide film, and titanium nitride film on the aforementioned organic film, forming a resist upper film on the aforementioned inorganic hard mask using a photoresist composition, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film with the circuit pattern formed as a mask and transferring the pattern to the aforementioned inorganic hard mask by etching, using the aforementioned inorganic hard mask with the pattern formed as a mask and transferring the pattern to the aforementioned organic film by etching, and using the aforementioned organic film with the pattern formed as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.
[0303] This method can be carried out in the same manner as the above-mentioned three-layer resist method using the silicon-containing resist interlayer film, except that an inorganic hard mask is formed on the organic film instead of the silicon-containing resist interlayer film.
[0304] The inorganic hard mask selected from silicon oxide film, silicon nitride film, and silicon oxide nitride film (SiON film) can be formed by CVD method, ALD method, etc. As for the formation method of silicon nitride film, it is described in Japanese Patent Publication No. 2002-334869, International Publication No. 2004 / 066377 Pamphlet, etc. The film thickness of the inorganic hard mask is preferably 5 to 200 nm, and more preferably 10 to 100 nm. As for the inorganic hard mask, it is most preferable to use SiON film which has a high effect as an anti-reflective film. The substrate temperature when forming the SiON film is 300 to 500°C, so the lower film needs to withstand a temperature of 300 to 500°C. The organic film formed using the organic film forming composition of the present invention has high heat resistance and can withstand high temperatures of 300 to 500°C, so it can be a combination of an inorganic hard mask formed by CVD method or ALD method and an organic film formed by spin coating method.
[0305] [Four-layer resist method using an inorganic hard mask and an organic antireflective film]
[0306] In addition, the present invention provides a pattern forming method, comprising the following steps: forming an organic film on a workpiece using the organic film forming composition of the present invention, forming an inorganic hard mask selected from silicon oxide film, silicon nitride film, silicon oxide nitride film, titanium oxide film, and titanium nitride film on the aforementioned organic film, forming a BARC on the aforementioned inorganic hard mask, forming a resist upper film on the aforementioned BARC using a photoresist composition, forming a circuit pattern on the aforementioned resist upper film, using the aforementioned resist upper film with the circuit pattern formed as a mask and sequentially transferring the pattern of the BARC and the aforementioned inorganic hard mask by etching, using the aforementioned inorganic hard mask with the pattern formed as a mask and transferring the pattern of the aforementioned organic film by etching, and using the aforementioned organic film with the pattern formed as a mask and etching the aforementioned workpiece to form a pattern on the aforementioned workpiece.
[0307] This method can be implemented in the same manner as the above-mentioned three-layer resist method using an inorganic hard mask, except that an organic antireflection film (BARC) is formed between the inorganic hard mask and the resist upper layer film.
[0308] In particular, when a SiON film is used as an inorganic hard mask, the two-layer antireflection film of the SiON film and the BARC can suppress reflection even in high NA immersion exposure with an NA exceeding 1.0. Another benefit of forming the BARC is that it has the effect of reducing the tailing of the resist upper film pattern directly above the SiON film.
[0309] Here, an example of a pattern forming method using the three-layer resist method of the present invention is shown. Figure 2 (A) to (F). In the case of the three-layer resist method, Figure 2As shown in (A), an organic film 3 is formed on a workpiece layer 2 formed on a substrate 1 using the composition for forming an organic film of the present invention, a silicon-containing resist intermediate film 4 is formed, and a resist upper film 5 is formed thereon. Figure 2 As shown in (B), the exposed portion 6 of the resist upper film 5 is exposed and PEB (post-exposure baking) is performed. Figure 2 As shown in (C), development is performed to form a resist upper film pattern 5a. Figure 2 As shown in (D), the resist upper film pattern 5a is used as a mask, and the silicon-containing resist intermediate film 4 is dry-etched using a fluorine-based gas to form a silicon-containing resist intermediate film pattern 4a. Figure 2 As shown in (E), after the resist upper film pattern 5a is removed, the organic film 3 is subjected to oxygen plasma etching using the silicon-containing resist intermediate film pattern 4a as a mask to form an organic film pattern 3a. Figure 2 As shown in (F), after the resist intermediate film pattern 4a containing silicon is removed, the processed layer 2 is etched using the organic film pattern 3a as a mask to form a pattern 2a.
[0310] When forming an inorganic hard mask, the silicon-containing resist intermediate film 4 may be replaced with an inorganic hard mask, and when forming a BARC, the BARC may be formed between the silicon-containing resist intermediate film 4 and the resist upper film 5. The etching of the BARC may be continuously performed before the etching of the silicon-containing resist intermediate film 4, or the etching of the silicon-containing resist intermediate film 4 may be performed after only the etching of the BARC is performed, and then the etching device or the like is changed to perform the etching of the silicon-containing resist intermediate film 4.
[0311] As described above, according to the pattern forming method of the present invention, a fine pattern can be formed on a workpiece with high precision using a multilayer resist method.
[0312] [Example]
[0313] Hereinafter, the present invention is described in more detail by exemplifying synthesis examples, comparative synthesis examples, embodiments, and comparative examples, but the present invention is not limited thereto. In addition, with regard to molecular weight and dispersity, the weight average molecular weight (Mw) and number average molecular weight (Mn) calculated using polystyrene by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as eluent are obtained, and dispersity (Mw / Mn, also referred to as molecular weight distribution) is obtained.
[0314] [Synthesis Example: Synthesis of Polymer]
[0315] The following compound group B: (B1) to (B16) and compound group C: (C1) to (C4) were used for the synthesis of polymers (A1) to (A18).
[0316] Compound Group B:
[0317] [Chemistry 50]
[0318]
[0319] Compound Group C:
[0320] [Chemistry 51]
[0321]
[0322] [Synthesis Example 1] Synthesis of Compound (A1)
[0323] 50.5 g of compound (B1), 50.0 g of compound (C1), and 400 g of 1,2-dichloroethane were prepared into a suspension at an internal temperature of 50°C under a nitrogen environment. 20.0 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 1000 g of toluene was added, and the organic layer was washed 6 times with 300 g of pure water, and then the organic layer was dried under reduced pressure. 300 g of THF was added to the residue to make a uniform solution, and the polymer was reprecipitated with 1000 g of methanol. The precipitated polymer was separated by filtration, washed twice with 600 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A1).
[0324] When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=2320 and Mw / Mn=1.85.
[0325] [Chemistry 52]
[0326]
[0327] [Synthesis Examples 2 to 18] Synthesis of Polymers (A2) to (A18)
[0328] The polymers (A2) to (A18) shown in Table 2 were obtained as products under the same reaction conditions as in Synthesis Example 1 except that the compound group B and compound group C shown in Table 1 were used.
[0329] [Table 1]
[0330]
[0331] [Synthesis Example 19] Synthesis of Compound (A19)
[0332] 32.4 g of 5,11-dihydroindole[3,2-b]carbazole, 50.0 g of compound (C2), and 400 g of 1,2-dichloroethane were prepared into a suspension at an internal temperature of 50°C under a nitrogen atmosphere. 20.0 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to an internal temperature of 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 1000 g of toluene was added, and the organic layer was washed 6 times with 300 g of pure water, and then the organic layer was dried under reduced pressure. 300 g of THF was added to the residue to make a uniform solution, and the polymer was reprecipitated with 1000 g of methanol. The precipitated polymer was separated by filtration, washed twice with 600 g of methanol, and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A19). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=2430 and Mw / Mn=1.65.
[0333] [Chemistry 53]
[0334]
[0335] [Synthesis Example 20] Synthesis of Compound (A20)
[0336] 22.3 g of carbazole, 50.0 g of compound (C3), and 400 g of 1,2-dichloroethane were prepared into a suspension at an internal temperature of 50°C under a nitrogen atmosphere. 20.0 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 1000 g of toluene was added, and the organic layer was washed 6 times with 300 g of pure water, and then the organic layer was dried under reduced pressure. 300 g of THF was added to the residue to make a uniform solution, and the polymer was reprecipitated with 1000 g of methanol. The precipitated polymer was separated by filtration, washed twice with 600 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A20). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were obtained by GPC, Mw=2270 and Mw / Mn=1.68.
[0337] [Chemistry 54]
[0338]
[0339] [Synthesis Example 21] Synthesis of Compound (A21)
[0340] 20.0 g of the polymer (A20) synthesized in Synthesis Example 20, 0.5 g of tetrabutylammonium iodide, 8.4 g of a 25% aqueous sodium hydroxide solution, and 100 g of toluene were prepared into a uniform dispersion at an internal temperature of 50°C under a nitrogen environment. A mixed solution of 1.3 g of butyl bromide and 2.6 g of propargyl bromide was slowly dripped into the dispersion, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 200 g of toluene was added and the water layer was removed. The organic layer was then washed twice with 60 g of a 3.0% aqueous nitric acid solution and five times with 60 g of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue, and the polymer was reprecipitated with 400 g of methanol. The precipitated polymer was separated by filtration, washed twice with 300 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A21). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=2670 and Mw / Mn=1.74.
[0341] [Chemistry 55]
[0342]
[0343] [Synthesis Example 22] Synthesis of Compound (A22)
[0344] 20.0 g of the polymer (A20) synthesized in Synthesis Example 20, 0.5 g of tetrabutylammonium iodide, 8.4 g of a 25% aqueous sodium hydroxide solution, and 100 g of toluene were prepared into a uniform dispersion at an internal temperature of 50°C under a nitrogen environment. 4.3 g of butyl bromide was slowly dripped into the dispersion, and the reaction was carried out at an internal temperature of 50°C for 24 hours. After cooling to room temperature, 200 g of toluene was added and the water layer was removed. The organic layer was then washed twice with 60 g of a 3.0% aqueous nitric acid solution and five times with 60 g of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue, and the polymer was reprecipitated with 400 g of methanol. The precipitated polymer was separated by filtration, washed twice with 300 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A22). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=2650 and Mw / Mn=1.77.
[0345] [Chemistry 56]
[0346]
[0347] [Synthesis Example 23] Synthesis of Compound (A23)
[0348] 21.0 g of 2,7-dihydroxynaphthalene, 50.0 g of compound (C2), and 400 g of 1,2-dichloroethane were prepared into a suspension at an internal temperature of 50°C under a nitrogen environment. 20.0 g of methanesulfonic acid was slowly added, and after confirming that the heat generation had stopped, the temperature was raised to 70°C and the reaction was carried out for 8 hours. After cooling to room temperature, 1000 g of toluene was added, and the organic layer was washed 6 times with 300 g of pure water, and then the organic layer was dried under reduced pressure. After adding 300 g of THF to the residue to make a uniform solution, the polymer was reprecipitated using 800 g of diisopropyl ether. The precipitated polymer was separated by filtration, washed twice with 500 g of diisopropyl ether and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A23).
[0349] When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=2370 and Mw / Mn=1.82.
[0350] [Chemistry 57]
[0351]
[0352] [Synthesis Example 24] Synthesis of Compound (A24)
[0353] 20.00 g of compound (A23), 8.7 g of potassium carbonate, and 80 g of dimethylformamide were made into a uniform dispersion at an internal temperature of 50°C under a nitrogen environment. 5.2 g of propargyl bromide was slowly added dropwise, and the reaction was carried out at an internal temperature of 50°C for 16 hours. After cooling to room temperature, 200 g of methyl isobutyl ketone and 100 g of pure water were added and homogenized, and then the water layer was removed. The organic layer was then washed twice with 60 g of 3.0% nitric acid aqueous solution and five times with 60 g of pure water, and the organic layer was dried under reduced pressure. 100 g of THF was added to the residue, and the polymer was reprecipitated with 400 g of methanol. The precipitated polymer was separated by filtration, washed twice with 300 g of methanol and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A24). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were determined by GPC, Mw=2580 and Mw / Mn=1.89.
[0354] [Chemistry 58]
[0355]
[0356] [Synthesis Example 25] Synthesis of Compound (A25)
[0357] 60.0 g of carbazole, 40.0 g of 9-fluorenone, 5 ml of 3-mercaptopropionic acid, and 300 ml of 1,2-dichloroethane were mixed under nitrogen atmosphere at an internal temperature of 70°C to form a uniform solution, and then 10 ml of methanesulfonic acid was slowly added, and the reaction was carried out at an internal temperature of 70°C for 24 hours. After cooling to room temperature, 500 g of methyl isobutyl ketone was added, and the organic layer was washed 5 times with 100 g of pure water, and then the organic layer was dried under reduced pressure. 200 g of THF was added to the residue to form a uniform solution, and the polymer was reprecipitated with 1000 g of methanol. The precipitated polymer was separated by filtration, washed twice with 600 g of methanol, and recovered. The recovered polymer was vacuum dried at 70°C to obtain (A25). When the weight average molecular weight (Mw) and the degree of dispersion (Mw / Mn) were obtained by GPC, Mw=2880 and Mw / Mn=2.29.
[0358] [Chemistry 59]
[0359]
[0360] [Synthesis Example 26] Synthesis of Compound (A26)
[0361] Under a nitrogen environment, 15.0 g of 2-acetyl-9-ethylcarbazole, 14.9 g of thionyl chloride, and 2.8 g of ethanol were added, and the reaction was carried out at 80°C for 8 hours. After cooling to room temperature, 50 g of pure water and 50 g of dichloromethane were added to the reaction solution, and the liquid was separated and washed with water, and then the organic layer was dried under reduced pressure. 50 g of THF was added to the residue to make a uniform solution, and then crystallized using 200 g of methanol. The precipitated crystals were separated by filtration, washed twice with 100 g of methanol and recovered. The recovered crystals were vacuum dried at 70°C to obtain (A26). When the weight average molecular weight (Mw) and dispersity (Mw / Mn) were obtained by GPC, Mw=690 and Mw / Mn=1.03.
[0362] [Chemistry 60]
[0363]
[0364] [Synthesis Example 27] Synthesis of Compound (A27)
[0365] Under a nitrogen environment, 17.8 g of N-ethylcarbazole-3-carboxaldehyde, 25.6 g of 2,6-dihydroxynaphthalene, 3.9 g of p-toluenesulfonic acid, and 100 g of 1,4-dioxane were added, and the reaction was carried out at 90°C for 6 hours. After cooling to room temperature, 200 g of methyl isobutyl ketone was added, and the organic layer was washed 5 times with 50 g of pure water, and then the organic layer was dried under reduced pressure. After adding 100 g of THF to the residue to make a uniform solution, crystallization was carried out using 400 g of heptane. The crystals after precipitation were separated by filtration, washed twice with 200 g of heptane and recovered. The recovered crystals were vacuum dried at 70°C to obtain (A27). When the weight average molecular weight (Mw) and dispersity (Mw / Mn) were obtained by GPC, Mw=540 and Mw / Mn=1.02.
[0366] [Chemistry 61]
[0367]
[0368] Table 2 shows the structural formula, weight average molecular weight (Mw) and dispersity (Mw / Mn) of the polymers and compounds obtained above.
[0369] [Table 2]
[0370]
[0371]
[0372]
[0373]
[0374]
[0375]
[0376] [Preparation of organic film-forming compositions (UDL-1 to 23, comparative UDL 1 to 14)]
[0377] The above-mentioned polymers or compounds (A1) to (A27), crosslinking agents (CR1, CR2) as additives, an acid generator (AG1), and high boiling point solvents (S1) 1,6-diacetoxyhexane: boiling point 260°C, (S2) γ-butyrolactone: boiling point 204°C, and (S3) tripropylene glycol monomethyl ether: boiling point 242°C were used and dissolved in a solvent containing 0.1% by mass of FC-4430 (manufactured by Sumitomo 3M Co., Ltd.) propylene glycol monomethyl ether acetate (PGMEA) and / or cyclohexanone (CyHO), and filtered using a 0.1 μm fluororesin filter to prepare organic film-forming compositions (UDL-1 to 23, comparative UDL-1 to 14).
[0378] [Table 3]
[0379]
[0380] The cross-linking agents (CR1), (CR2) and the acid generator (AG1) used are shown below.
[0381] [Chemistry 62]
[0382]
[0383] [Example 1 Solvent resistance measurement (Examples 1-1 to 1-23, Comparative Examples 1-1 to 1-14)]
[0384] The organic film-forming composition prepared above (UDL-1 to 23, comparison UDL-1 to 14) was coated on a silicon substrate and calcined at 400°C for 60 seconds under a nitrogen flow with an oxygen concentration controlled at less than 0.2%. The film thickness was measured, a PGMEA solvent was dispensed thereon, the mixture was left for 30 seconds and spin dried, and the mixture was baked at 100°C for 60 seconds to evaporate PGMEA. The film thickness was measured, and the difference in film thickness before and after PGMEA treatment was calculated.
[0385] [Table 4]
[0386]
[0387] As shown in Table 4, the residual film rate of the organic film-forming composition of the present invention (Examples 1-1 to 1-23) after PGMEA treatment is more than 99%, and a cross-linking reaction will occur even in a nitrogen environment and sufficient solvent resistance will be exhibited. In contrast, in Comparative Examples 1-1 to 1-14, the residual film rates of Comparative Examples 1-1 to 1-7, which do not add a cross-linking agent and a thermal acid generator, after PGMEA treatment are all less than 50%, and sufficient solvent resistance is not exhibited. In order to exhibit solvent resistance, cross-linking agents and thermal acid generators must be added as in Comparative Examples 1-8 to 1-14. From this result, it can be seen that the polymer of the present invention causes a thermal curing reaction due to the triple-bond substituent, exhibits solvent resistance, and forms a cured film.
[0388] [Example 2 Evaluation of heat resistance characteristics (Examples 2-1 to 2-23, Comparative Examples 2-1 to 2-14)]
[0389] The above-mentioned organic film-forming compositions (UDL-1 to 23, comparative UDL-1 to 14) were coated on silicon substrates, respectively, and fired at 180°C for 60 seconds in air to form a 200 nm coating film, and the film thickness was measured. The substrate was then fired at 450°C for 10 minutes under a nitrogen flow with an oxygen concentration of 0.2% or less, and the film thickness was measured. These results are shown in Table 5.
[0390] [Table 5]
[0391]
[0392] As shown in Table 5, in Examples 2-1 to 2-23 using the organic film-forming composition of the present invention, the film thickness reduction is less than 1% even after calcination at 450°C, and the film thickness is maintained even after calcination at 450°C, indicating high heat resistance. In contrast, Comparative Examples 2-1 to 2-14 caused a greater film thickness reduction than the organic film-forming composition of the present invention, especially in Comparative Examples 2-6 and 2-7 using a monomolecular compound, resulting in a greater film thickness reduction due to sublimation. In addition, even in Comparative Examples 2-8 to 2-14 in which a crosslinking agent was added and cured, the film thickness reduction due to thermal decomposition could not be suppressed, resulting in a film thickness reduction of more than 10%. In Examples 2-1 to 2-23 using the organic film-forming composition of the present invention, after calcination at 450°C in a nitrogen environment, the film thickness after calcination at 180°C was maintained, indicating that excellent heat resistance was exhibited under an inert gas.
[0393] [Evaluation of landfill characteristics in Example 3 (Examples 3-1 to 3-23, Comparative Examples 3-1 to 3-14)]
[0394] The above-mentioned organic film-forming compositions (UDL-1 to 23, comparative UDL-1 to 14) were applied to Figure 3SiO2 generally has a dense hole pattern (hole diameter 0.16μm, hole depth 0.50μm, and the distance between the centers of two adjacent holes is 0.32μm). 2 On the wafer substrate, an organic film 8 was formed by calcining at 450° C. for 60 seconds under a nitrogen flow with an oxygen concentration controlled at 0.2% or less using a hot plate. Figure 3 The base substrate 7 (SiO2) with a dense hole pattern shown in (G) (top view) and (H) (cross-sectional view) 2 Wafer substrate). The cross-sectional shape of each wafer substrate obtained was observed using a scanning electron microscope (SEM) to confirm whether the pores were filled with organic films without voids. The results are shown in Table 6. When an organic film material with poor filling characteristics was used, voids were generated inside the pores in this evaluation. When an organic film-forming composition with good filling characteristics was used, voids were generated inside the pores in this evaluation. Figure 3 As shown in (I), the inside of the hole is filled with the organic film 8 without any gaps.
[0395] [Table 6]
[0396] Organic film forming composition Is there any gap Example 3-1 UDL-1 none Example 3-2 UDL-2 none Example 3-3 UDL-3 none Embodiment 3-4 UDL-4 none Embodiment 3-5 UDL-5 none Embodiment 3-6 UDL-6 none Embodiment 3-7 UDL-7 none Embodiment 3-8 UDL-8 none Embodiment 3-9 UDL-9 none Embodiment 3-10 UDL-10 none Example 3-11 UDL-11 none Example 3-12 UDL-12 none Example 3-13 UDL-13 none Embodiment 3-14 UDL-14 none Example 3-15 UDL-15 none Example 3-16 UDL-16 none Example 3-17 UDL-17 none Example 3-18 UDL-18 none Example 3-19 UDL-19 none Example 3-20 UDL-20 none Example 3-21 UDL-21 none Example 3-22 UDL-22 none Example 3-23 UDL-23 none Comparative Example 3-1 Compare UDL-1 have Comparative Example 3-2 Compare UDL-2 have Comparative Example 3-3 Compare UDL-3 have Comparative Examples 3-4 Compare UDL-4 have Comparative Examples 3-5 Compare UDL-5 have Comparative Examples 3-6 Compare UDL-6 have Comparative Examples 3-7 Compare UDL-7 have Comparative Examples 3-8 Compare UDL-8 have Comparative Examples 3-9 Compare UDL-9 have Comparative Examples 3-10 Compare UDL-10 have Comparative Example 3-11 Compare UDL-11 have Comparative Example 3-12 Compare UDL-12 have Comparative Example 3-13 Compare UDL-13 have Comparative Examples 3-14 Compare UDL-14 have
[0397] As shown in Table 6, the organic film-forming composition of the present invention (Examples 3-1 to 3-23) can fill the hole pattern without generating voids, and it can be confirmed that it has good filling characteristics. On the other hand, in Comparative Examples 3-1 to 3-14, it can be confirmed that voids are generated, and the filling characteristics are poor. From this result, it can be seen that the organic film-forming composition of the present invention ensures heat resistance due to the thermal curing reaction caused by the action of the substituent containing triple bonds, and can implement filling without generating voids. On the other hand, in Comparative Examples 3-1 to 3-14, even if a cross-linking agent is used to form a cured film, the heat resistance is still insufficient under a nitrogen environment, so voids are generated and good filling characteristics cannot be obtained.
[0398] [Example 4 Evaluation of Flattening Characteristics (Examples 4-1 to 4-23, Comparative Examples 4-1 to 4-12)]
[0399] The organic film-forming compositions (UDL-1 to 23, comparative UDL-1 to 5, and 8 to 14) were applied to the surfaces having a giant isolated groove pattern ( Figure 4 (J), groove width 10 μm, groove depth 0.10 μm) base substrate 9 (SiO 2 The organic film 10 was placed on a wafer substrate and calcined at 450°C for 60 seconds under a nitrogen flow with an oxygen concentration of less than 0.2%. The height difference between the groove portion and the non-groove portion of the organic film 10 was observed using an NX10 atomic force microscope (AFM) manufactured by Park Systems. Figure 4(K) in delta 10). The results are shown in Table 7. In this evaluation, the smaller the height difference, the better the planarization characteristics. In addition, in this evaluation, the groove pattern with a depth of 0.10 μm is usually planarized using an organic film-forming composition with a film thickness of about 0.2 μm, which becomes a more stringent evaluation condition in order to evaluate the quality of the planarization characteristics. In addition, for the comparison of UDL-6 and 7, the film thickness after baking was too large, so the evaluation of the planarization characteristics could not be implemented.
[0400] [Table 7]
[0401] Organic film forming composition Height difference(nm) Example 4-1 UDL-1 60 Example 4-2 UDL-2 45 Example 4-3 UDL-3 40 Example 4-4 UDL-4 50 Embodiment 4-5 UDL-5 40 Embodiment 4-6 UDL-6 60 Embodiment 4-7 UDL-7 50 Embodiment 4-8 UDL-8 55 Embodiment 4-9 UDL-9 35 Embodiment 4-10 UDL-10 45 Embodiment 4-11 UDL-11 35 Embodiment 4-12 UDL-12 35 Embodiment 4-13 UDL-13 40 Embodiment 4-14 UDL-14 35 Embodiment 4-15 UDL-15 30 Embodiment 4-16 UDL-16 40 Example 4-17 UDL-17 35 Embodiment 4-18 UDL-18 40 Embodiment 4-19 UDL-19 30 Example 4-20 UDL-20 35 Example 4-21 UDL-21 30 Example 4-22 UDL-22 25 Example 4-23 UDL-23 20 Comparative Example 4-1 Compare UDL-1 95 Comparative Example 4-2 Compare UDL-2 90 Comparative Example 4-3 Compare UDL-3 95 Comparative Example 4-4 Compare UDL-4 90 Comparative Examples 4-5 Compare UDL-5 90 Comparative Examples 4-6 Compare UDL-8 90 Comparative Examples 4-7 Compare UDL-9 90 Comparative Examples 4-8 Compare UDL-10 95 Comparative Examples 4-9 Compare UDL-11 95 Comparative Examples 4-10 Compare UDL-12 95 Comparative Examples 4-11 Compare UDL-13 85 Comparative Examples 4-12 Compare UDL-14 85
[0402] As shown in Table 7, it is confirmed that the organic film-forming composition of the present invention (Examples 4-1 to 4-23) has a smaller height difference between the groove part and the non-groove part of the organic film than Comparative Examples 4-1 to 4-12, and has excellent planarization characteristics. In Comparative Examples 4-1 to 4-12, the film loss caused by high-temperature baking is large, so the film thickness difference between the upper part of the height difference and the lower part of the height difference is more obvious, and the flatness is deteriorated, resulting in the above-mentioned results. In addition, in Comparative Examples 4-11 and 4-12, even if it is a single-molecule compound, the thermal fluidity is hindered by the addition of a cross-linking agent, and a good planarization result cannot be obtained. If Examples 4-21 to 4-23 to which a high boiling point solvent is added are compared with Examples 4-5, 4-9, and 4-15 to which no high boiling point solvent is added, it can be seen that the addition of a high boiling point solvent further improves the flatness.
[0403] [Example 5 Pattern Formation Test (Examples 5-1 to 5-23, Comparative Examples 5-1 to 5-7)]
[0404] The organic film-forming compositions (UDL-1 to 23, comparative UDL-8 to 14) were applied to SiO2 films having a thickness of 300 nm. 2 On a silicon wafer substrate with a film, an organic film (resist intermediate film) was formed by calcining at 450°C for 60 seconds under a nitrogen flow in which the oxygen concentration was controlled to be less than 0.2%. A CVD-SiON hard mask was formed thereon, and an organic antireflection film material (ARC-29A: manufactured by Nissan Chemical Co., Ltd.) was further applied thereon, and baked at 210°C for 60 seconds to form an organic antireflection film with a film thickness of 80 nm. A single-layer resist for ArF, which was a resist upper layer film material, was applied thereon, and baked at 105°C for 60 seconds to form a photoresist film with a film thickness of 100 nm. An immersion protective film material (TC-1) was applied on the photoresist film, and baked at 90°C for 60 seconds to form a protective film with a film thickness of 50 nm. In addition, as for comparisons UDL-1 to UDL-7, solvent resistance could not be ensured, the subsequent pattern formation test could not be performed.
[0405] The resist upper film material (single-layer resist for ArF) is prepared by dissolving 100 parts by mass of a polymer (RP1) represented by the following formula, 6.6 parts by mass of an acid generator (PAG1) represented by the following formula, and 0.8 parts by mass of a basic compound (Amine1) represented by the following formula in 2500 parts by mass of PGMEA containing 0.1% by mass of FC-430 (manufactured by Sumitomo 3M Co., Ltd.), and filtering the mixture with a 0.1 μm fluororesin filter.
[0406] [Chemistry 63]
[0407]
[0408] The wet protective film material (TC-1) was prepared by dissolving 100 parts by mass of a protective film polymer (PP1) represented by the following formula in an organic solvent consisting of 2700 parts by mass of diisoamyl ether and 270 parts by mass of 2-methyl-1-butanol, and filtering the solution with a 0.1 μm fluororesin filter.
[0409] [Chemistry 64]
[0410]
[0411] Then, exposure was performed using an ArF immersion exposure device (manufactured by Nikon Co., Ltd.; NSR-S610C, NA1.30, σ0.98 / 0.65, 35 degree dipole s-polarized illumination, 6% halftone phase shift mask) while changing the exposure amount, and the film was baked (PEB) at 100°C for 60 seconds and developed for 30 seconds using a 2.38 mass % tetramethylammonium hydroxide (TMAH) aqueous solution to obtain a line and space pattern.
[0412] Then, using a Telius etching apparatus manufactured by Tokyo Electron, the organic antireflection film and the CVD-SiON hard mask were etched by dry etching using the resist pattern as a mask to form a hard mask pattern, the organic film was etched using the obtained hard mask pattern as a mask to form an organic film pattern, and the SiO 2 The film was etched and the etching conditions were as follows.
[0413] Transfer conditions of resist pattern to SiON hard mask.
[0414] Chamber pressure 10.0Pa
[0415] RF power 1,500W
[0416] CF 4 Gas flow rate 75sccm
[0417] O 2Gas flow rate 15sccm
[0418] Time 15 sec
[0419] Transfer conditions for transferring the hard mask pattern to the organic film.
[0420] Chamber pressure 2.0Pa
[0421] RF power 500W
[0422] Ar gas flow rate: 75 sccm
[0423] O 2 Gas flow rate 45sccm
[0424] Time: 120 seconds
[0425] Transfer of organic film pattern to SiO 2 Membrane transfer conditions.
[0426] Chamber pressure 2.0Pa
[0427] RF power 2,200W
[0428] C 5 F 12 Gas flow rate 20sccm
[0429] C 2 F 6 Gas flow rate 10sccm
[0430] Ar gas flow rate 300 sccm
[0431] O 2 Gas flow rate 60sccm
[0432] Time 90 sec
[0433] Table 8 shows the results of observing the pattern cross section using an electron microscope (S-4700) manufactured by Hitachi, Ltd.
[0434] [Table 8]
[0435]
[0436] As shown in Table 8, the results of the organic film-forming composition of the present invention (Examples 5-1 to 5-23) confirmed that in any case, the resist upper film pattern can be finally transferred to the substrate well, and the organic film-forming composition of the present invention can be preferably used for microfabrication using a multilayer resist method. Although the heat resistance of Comparative Examples 5-1 to 5-7 is insufficient, patterns can be formed.
[0437] [Example 6 Pattern Formation Test (Examples 6-1 to 6-23, Comparative Examples 6-1 to 6-7)]
[0438] The organic film-forming compositions (UDL-1 to 23, comparative UDL-8 to 14) were applied to SiO2 sheets having a groove pattern (groove width 10 μm, groove depth 0.10 μm). 2 The wafer substrate was calcined at 450°C for 60 seconds under a nitrogen flow with an oxygen concentration of less than 0.2%. The coating film was formed in the same manner as in Example 5, and patterning and dry etching were performed. The shape of the completed pattern was observed. The results are shown in Table 9.
[0439] [Table 9]
[0440]
[0441] As shown in Table 9, it can be confirmed that the organic film-forming composition of the present invention (Examples 6-1 to 6-23) can finally transfer the resist upper film pattern to the substrate well, and the organic film-forming composition of the present invention can be preferably used for micro-processing using a multilayer resist method. On the other hand, in Comparative Examples 6-1 to 6-7, although solvent resistance can be obtained by adding a crosslinking agent and a cured film can be formed, the pattern is poorly embedded due to insufficient heat resistance, so pattern collapse occurs during pattern processing, and ultimately a good pattern cannot be obtained.
[0442] [Example 8 Coating Test (Examples 7-1 to 7-23, Comparative Examples 7-1 to 7-4)]
[0443] The above-mentioned organic film-forming compositions (UDL-1 to 23, comparative UDL-6, 7, 13, 14) were coated on the bare-Si substrate, the substrate treated with hexamethyldisilazane (HMDS), and the substrate treated with SiON shown in Table 10, respectively, and calcined at 400°C for 60 seconds under a nitrogen flow with an oxygen concentration of 0.2% or less to form an organic film with a film thickness of 200 nm. The formed organic film was observed using an optical microscope (ECLIPSE L200 manufactured by Nikon Corporation) to see if there was any coating abnormality. The confirmation results are shown in Table 10.
[0444] [Table 10]
[0445] Organic film forming composition Bare-Si substrate HMDS treated substrate SiON Handled Substrates Example 7-1 UDL-1 No abnormality No abnormality No abnormality Example 7-2 UDL-2 No abnormality No abnormality No abnormality Example 7-3 UDL-3 No abnormality No abnormality No abnormality Example 7-4 UDL-4 No abnormality No abnormality No abnormality Example 7-5 UDL-5 No abnormality No abnormality No abnormality Example 7-6 UDL-6 No abnormality No abnormality No abnormality Example 7-7 UDL-7 No abnormality No abnormality No abnormality Embodiment 7-8 UDL-8 No abnormality No abnormality No abnormality Embodiment 7-9 UDL-9 No abnormality No abnormality No abnormality Examples 7-10 UDL-10 No abnormality No abnormality No abnormality Embodiment 7-11 UDL-11 No abnormality No abnormality No abnormality Examples 7-12 UDL-12 No abnormality No abnormality No abnormality Embodiment 7-13 UDL-13 No abnormality No abnormality No abnormality Embodiment 7-14 UDL-14 No abnormality No abnormality No abnormality Embodiment 7-15 UDL-15 No abnormality No abnormality No abnormality Embodiment 7-16 UDL-16 No abnormality No abnormality No abnormality Example 7-17 UDL-17 No abnormality No abnormality No abnormality Examples 7-18 UDL-18 No abnormality No abnormality No abnormality Embodiment 7-19 UDL-19 No abnormality No abnormality No abnormality Embodiment 7-20 UDL-20 No abnormality No abnormality No abnormality Example 7-21 UDL-21 No abnormality No abnormality No abnormality Example 7-22 UDL-22 No abnormality No abnormality No abnormality Example 7-23 UDL-23 No abnormality No abnormality No abnormality Comparative Example 7-1 Compare UDL-6 No abnormality Pinhole defect Pinhole defect Comparative Example 7-2 Compare UDL-7 No abnormality Pinhole defect Pinhole defect Comparative Example 7-3 Compare UDL-13 No abnormality Pinhole defect Pinhole defect Comparative Example 7-4 Compare UDL-14 No abnormality Pinhole defect Pinhole defect
[0446] As shown in Table 10, the organic film formed by the composition for forming an organic film of the present invention (Examples 7-1 to 7-23) has no substrate dependence, and a uniform organic film without coating abnormality can be formed. In contrast, in Comparative Examples 7-1 to 7-4, in which a monomolecular compound is used to form an organic film, aggregation is easily caused depending on the substrate due to the use of a monomolecular compound, and a large number of pinhole-shaped coating defects that are considered as shrinkage cavities are observed. By using the polymer of the present invention, a uniform coating film can be formed without substrate dependence, and it can be seen that a good organic film can be formed without substrate dependence.
[0447] From the above, it can be seen that if the organic film forming composition of the present invention contains the polymer of the present invention, it will have heat resistance of more than 400°C and a high degree of filling / planarization characteristics even under an inert gas that does not contain oxygen. Therefore, it is extremely effective as an organic film material used in a multilayer resist method. In addition, if the pattern forming method of the present invention uses the organic film forming composition, even if the processed body is a substrate with a height difference, a fine pattern can be formed with high precision.
[0448] The present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and achieving the same functions and effects as the technical concept described in the claims of the present invention are all included in the technical scope of the present invention.
[0449] Description of Reference Numerals
[0450] 1: Substrate
[0451] 2: Processing layer
[0452] 2a: Pattern (pattern formed on the processed layer)
[0453] 3: Organic film
[0454] 3': Organic film-forming composition
[0455] 3a: Organic film pattern
[0456] 4: Silicon-containing resist interlayer
[0457] 4a: Silicon-containing resist interlayer pattern
[0458] 5: Resist upper film
[0459] 5a: Resist upper film pattern
[0460] 6: Exposure part
[0461] 7: Base substrate with dense hole pattern
[0462] 8: Organic film
[0463] 9: Base substrate with giant isolated groove patterns
[0464] 10: Organic film
[0465] delta10: The height difference between the organic film 10 in the groove part and the non-groove part
Claims
1. A composition for forming an organic film, characterized in that it contains: A polymer having a partial structure represented by the following general formula (1) as a repeating unit, and Organic solvents; In the general formula (1), AR1 and AR2 are benzene rings or naphthalene rings which may be substituted, W1 is any one of the following general formulas (2), (4), and (6), and two or more W1s may be used in combination, and the divalent organic group represented by W2 is any one of the following; In the general formula (2), AR3, AR4, and AR5 are benzene rings or naphthalene rings optionally having substituents, and AR3 and AR4 or AR4 and AR5 are optionally connected to each other via carbon atoms bonded to hydrogen atoms on the aromatic rings to form a bridged structure with the aromatic rings; Y is a substituent represented by the following general formula (3); R3 is a single bond or a divalent organic group having 20 or less carbon atoms, and R4 is hydrogen or a monovalent organic group having 20 or less carbon atoms; In the general formula (4), AR6 and AR7 are benzene rings or naphthalene rings optionally having substituents, n1 is 0 or 1, and when n1=0, AR6 and AR7 do not form a bridged structure between the aromatic rings via Z, and when n1=1, AR6 and AR7 form a bridged structure via Z, and Z is a single bond or any one of the following general formulas (5); Y is a substituent represented by the general formula (3); AR8 in the general formula (6) is a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, or a pyrene ring, Y is a substituent represented by the general formula (3), and n2 and n3 are integers satisfying the relationship of 0≤n2≤4, 0≤n3≤4, and 1≤n2+n3≤4.
2. The composition for forming an organic film according to claim 1, wherein The weight average molecular weight of the polymer is 1000-5000.
3. The composition for forming an organic film according to claim 1 or 2, wherein The organic solvent is a mixture of one or more organic solvents having a boiling point lower than 180 degrees and one or more organic solvents having a boiling point higher than 180 degrees.
4. The composition for forming an organic film according to claim 1 or 2, wherein The organic film-forming composition further contains one or more of a surfactant and a plasticizer.
5. A substrate for manufacturing a semiconductor device, characterized in that: An organic film formed by curing the organic film-forming composition according to any one of claims 1 to 4 is formed on a substrate.
6. A method for forming an organic film, which is suitable for use in a manufacturing step of a semiconductor device, and which comprises the following steps: The organic film-forming composition according to any one of claims 1 to 4 is spin-coated on a substrate to be processed, and The substrate to be processed coated with the organic film-forming composition is subjected to heat treatment in an inert gas environment at a temperature of 50° C. to 600° C. for 10 to 7200 seconds to obtain a cured film.
7. A method for forming an organic film, which is suitable for use in a manufacturing step of a semiconductor device, and which comprises the following steps: The organic film-forming composition according to any one of claims 1 to 4 is spin-coated on a substrate to be processed, The substrate to be processed coated with the composition for forming an organic film is heat-treated in air at a temperature of 50° C. to 250° C. for 5 to 600 seconds to form a coating film, and A cured film is obtained by applying heat treatment at a temperature of 200° C. or higher and 600° C. or lower within a range of 10 seconds to 7200 seconds in an inert gas environment.
8. The method for forming an organic film according to claim 6 or 7, wherein: The oxygen concentration in the inert gas is set to be 1% or less.
9. The method for forming an organic film according to claim 6 or 7, wherein: The substrate to be processed uses a substrate to be processed having a structure with a height of 30 nm or more or a height difference.
10. A pattern forming method, characterized by comprising the following steps: An organic film is formed on a workpiece using the organic film-forming composition according to any one of claims 1 to 4, forming a silicon-containing resist interlayer film on the organic film using a silicon-containing resist interlayer film material, forming a resist upper film on the silicon-containing resist intermediate film using a photoresist composition, forming a circuit pattern on the resist upper film, The resist upper layer film having the circuit pattern formed thereon is used as a mask and the pattern of the resist intermediate film containing silicon is transferred by etching. The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film having the transferred pattern as a mask, and The pattern is formed on the object to be processed by etching using the organic film to which the pattern is transferred as a mask.
11. A method for forming a pattern, comprising the following steps: An organic film is formed on a workpiece using the organic film-forming composition according to any one of claims 1 to 4, forming a silicon-containing resist interlayer film on the organic film using a silicon-containing resist interlayer film material, forming an organic anti-reflection film on the silicon-containing resist intermediate film, A photoresist composition is used on the organic anti-reflective film to form a resist upper film. forming a circuit pattern on the resist upper film, The resist upper layer film having the circuit pattern formed thereon is used as a mask and the organic anti-reflection film and the silicon-containing resist intermediate film are pattern-transferred by etching in sequence. The pattern is transferred to the organic film by etching using the silicon-containing resist intermediate film having the transferred pattern as a mask, and The object to be processed is etched using the organic film to which the pattern is transferred as a mask, thereby forming a pattern on the object to be processed.
12. A method for forming a pattern, comprising the following steps: An organic film is formed on a workpiece using the organic film-forming composition according to any one of claims 1 to 4, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxide nitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming a resist upper film on the inorganic hard mask using a photoresist composition, forming a circuit pattern on the resist upper film, The resist upper layer film having the circuit pattern formed thereon is used as a mask and the inorganic hard mask is pattern-transferred by etching. The inorganic hard mask having the pattern is used as a mask and the pattern is transferred to the organic film by etching, and The object to be processed is etched using the patterned organic film as a mask to form a pattern on the object to be processed.
13. A method for forming a pattern, comprising the following steps: An organic film is formed on a workpiece using the organic film-forming composition according to any one of claims 1 to 4, forming an inorganic hard mask selected from a silicon oxide film, a silicon nitride film, a silicon oxide nitride film, a titanium oxide film, and a titanium nitride film on the organic film, forming an organic anti-reflection film on the inorganic hard mask, A photoresist composition is used on the organic anti-reflective film to form a resist upper film. forming a circuit pattern on the resist upper film, The resist upper layer film having the circuit pattern formed thereon is used as a mask and the organic anti-reflection film and the inorganic hard mask are sequentially pattern-transferred by etching, The inorganic hard mask having the pattern is used as a mask and the pattern is transferred to the organic film by etching, and The object to be processed is etched using the patterned organic film as a mask to form a pattern on the object to be processed.
14. The pattern forming method according to claim 12 or 13, wherein: The inorganic hard mask is formed by a CVD method or an ALD method.
15. The pattern forming method according to any one of claims 10 to 13, wherein: The method of forming the circuit pattern on the resist upper layer film is to use optical lithography with a wavelength of 10 nm to 300 nm, direct writing by electron beam, nanoimprinting, or a combination thereof.
16. The pattern forming method according to any one of claims 10 to 13, wherein: The developing method is development using an alkali or an organic solvent.
17. The pattern forming method according to any one of claims 10 to 13, wherein: The workpiece is a semiconductor device substrate or a semiconductor device substrate on which a metal film, a metal carbide film, a metal oxide film, a metal nitride film, a metal oxide carbide film, and a metal oxide nitride film are formed.
18. The pattern forming method according to claim 17, wherein: The metal used may be silicon, titanium, tungsten, hafnium, zirconium, chromium, germanium, copper, silver, gold, aluminum, indium, gallium, arsenic, palladium, iron, tantalum, iridium, cobalt, manganese, molybdenum, or an alloy thereof.
19. A polymer having a partial structure represented by the following general formula (1) as a repeating unit; In the general formula (1), AR1 and AR2 are benzene rings or naphthalene rings which may be substituted, W1 is any one of the following general formulas (2), (4), and (6), and two or more W1s may be used in combination, and the divalent organic group represented by W2 is any one of the following; In the general formula (2), AR3, AR4, and AR5 are benzene rings or naphthalene rings optionally having substituents, and AR3 and AR4 or AR4 and AR5 are optionally connected to each other via carbon atoms bonded to hydrogen atoms on the aromatic rings to form a bridged structure with the aromatic rings; Y is a substituent represented by the following general formula (3); R3 is a single bond or a divalent organic group having 20 or less carbon atoms, and R4 is hydrogen or a monovalent organic group having 20 or less carbon atoms; In the general formula (4), AR6 and AR7 are benzene rings or naphthalene rings optionally having substituents, n1 is 0 or 1, and when n1=0, AR6 and AR7 do not form a bridged structure between the aromatic rings via Z, and when n1=1, AR6 and AR7 form a bridged structure via Z, and Z is a single bond or any one of the following general formulas (5); Y is a substituent represented by the general formula (3); AR8 in the general formula (6) is a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, or a pyrene ring, Y is a substituent represented by the general formula (3), and n2 and n3 are integers satisfying the relationship of 0≤n2≤4, 0≤n3≤4, and 1≤n2+n3≤4.
Citation Information
Patent Citations
Method and device for forming silicon nitride film, and method for preprocessing of cleaning thereof
JP2002334869A
Material for forming photoresist lower layer film and method for forming pattern
JP2005128509A
Resist lower layer film material and pattern forming method
JP2006285095A
Photoresist undercoat-forming material and patterning process
JP2006293298A
Photoresist underlayer film forming material and pattern forming method
JP2007199653A