A nano-fluorination catalyst for preparing R152a and a preparation method thereof

By preparing nanofluorination catalysts with high specific surface area and pore volume, the problems of insufficient conversion rate and selectivity of existing catalysts in the preparation of R152a are solved, achieving more efficient catalytic reactions and longer service life.

CN112264057BActive Publication Date: 2024-10-08NORTH & SOUTH BROTHER PHARMACY INVESTMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011074805.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-09
Publication Date
2024-10-08
Estimated Expiration
2040-10-09

AI Technical Summary

Technical Problem

In the process of preparing R152a, the conversion rate and selectivity of existing catalysts are low, and the specific surface area and pore volume are insufficient, which affects the reaction efficiency.

Method used

Nanofluorination catalysts prepared from metal chromium salts, metal cobalt salts, metal zinc salts, metal lanthanum salts, complexing agents and surfactants are used to form a nanofluorination catalyst with high specific surface area and pore volume through specific molar ratios and preparation methods. catalyst, and improve the activity of the catalyst through spray drying and roasting.

Benefits of technology

The specific surface area and pore volume of the catalyst are significantly increased, the catalytic activity and selectivity are enhanced, the service life of the catalyst is extended, and the preparation process is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002716300400000061
    Figure BDA0002716300400000061
Patent Text Reader

Abstract

The present invention relates to a nano-fluorination catalyst for preparing R152a and a preparation method thereof; specifically, the present invention relates to a nano-catalyst for catalytically preparing R152a and a preparation method thereof; the precursor of the nano-fluorination catalyst is prepared from a metal chromium salt, a metal cobalt salt, a metal zinc salt, a metal lanthanum salt, a complexing agent and a surfactant, wherein the molar ratio of the metal chromium salt, the metal cobalt salt, the metal zinc salt and the metal lanthanum salt is 1:(0.10-0.20):(0.05-0.18):(0.20-0.30); the specific surface area of ​​the nano-fluorination catalyst is 465-500m 2 / g, and the pore volume is 0.7-0.9mL / g; the nano-fluorination catalyst of the present invention has higher catalytic activity and service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a nano-fluorination catalyst for preparing R152a and a preparation method and application thereof, and in particular to a catalyst for gas phase fluorination reaction of halogenated hydrocarbons and hydrogen fluoride, in particular to a nano-fluorination catalyst for catalytically preparing R152a and a preparation method thereof. Background Art

[0002] R152a (HFC-152a, F152a, molecular structure CH3-CHF2) is an important fluorine-containing organic compound, with an ozone depletion potential of OPD = 0 and a global warming coefficient of GWP = 0.03. It is an excellent variety among the two-carbon substitutes for Freon. R152a is generally mixed with other refrigerants to form a mixed refrigerant, which is widely used in refrigeration systems.

[0003] The main synthetic routes of R152a are as follows: (1) gas phase fluorination with vinyl chloride as raw material; (2) liquid phase fluorination with vinyl chloride as raw material; (3) gas phase fluorination with acetylene as raw material; (4) liquid phase fluorination with acetylene as raw material. Catalysts play an important role in the synthesis of R152a, affecting reaction conditions, conversion rate, selectivity, etc.

[0004] For example, CN1931431A discloses a catalyst for the gas phase production of 1,1-difluoroethane, which is prepared by coprecipitation and includes chromium, other metal bases, fluorine and oxygen elements. The other metal bases are one or two elements of Co, Mn, Zn, Fe, Mg, Al and Ni, and the molar ratio of chromium to other metal elements is 1:0.001-0.6. However, the specific surface area of ​​the catalyst is 260m 2 / g or less, the pore volume is below 0.4mL / g, and in the reaction of vinyl chloride and HF to produce 1,1-difluoroethane, the maximum yield of R152a is only 73.7%.

[0005] Therefore, there is an urgent need for a catalyst with a simple preparation method and high conversion rate, high selectivity and long life in the preparation of R152a. Summary of the invention

[0006] In order to solve at least one of the above problems, the present invention provides a nano-fluorination catalyst for preparing R152a, characterized in that the precursor of the nano-fluorination catalyst is prepared from a metal chromium salt, a metal cobalt salt, a metal zinc salt, a metal lanthanum salt, a complexing agent and a surfactant, wherein the molar ratio of the metal chromium salt, the metal cobalt salt, the metal zinc salt and the metal lanthanum salt is 1: (0.10-0.20): (0.05-0.18): (0.20-0.30); the specific surface area of ​​the nano-fluorination catalyst is 465-500m 2 / g, and the pore volume is 0.7-0.9mL / g.

[0007] In some embodiments, the specific surface area of ​​the nano-fluorination catalyst is 480-500m 2 / g, and the pore volume is 0.8-0.9mL / g.

[0008] In other embodiments, the specific surface area of ​​the nano-fluorination catalyst is 480-500 m 2 / g, and the pore volume is 0.85-0.9mL / g.

[0009] In other embodiments, the molar ratio of the metal chromium salt, the metal cobalt salt, the metal zinc salt and the metal lanthanum salt is 1:0.12:0.08:0.30, 1:0.15:0.12:0.28, 1:0.15:0.15:0.23, 1:0.2:0.18:0.25 or 1:0.2:0.05:0.2.

[0010] In some embodiments, the complexing agent is selected from one or more of EDTA, maleic acid, glycine, citric acid, ammonium citrate, oxalic acid, ammonium oxalate, ethanolamine, diethanolamine or triethanolamine.

[0011] In other embodiments, the complexing agent is selected from EDTA.

[0012] In some embodiments, the surfactant is selected from one or more of polyvinyl pyrrolidone, polyethylene glycol (PEG), cyclodextrin, and cetyltrimethylammonium bromide (CTAB).

[0013] In some other embodiments, the surfactant is selected from two or more of polyvinyl pyrrolidone, polyethylene glycol, cyclodextrin or cetyltrimethylammonium bromide; preferably, the surfactant is polyethylene glycol and cetyltrimethylammonium bromide, and the molar ratio of polyethylene glycol to cetyltrimethylammonium bromide is (0.8-0.85): (0.2-0.15).

[0014] In some embodiments, the molar ratio of the metal chromium salt to the surfactant in the precursor of the nano-fluorination catalyst is 1:(0.01-0.02).

[0015] By adding a surfactant, a protective layer is formed on the surface of the precipitated particles to prevent the precipitated particles from agglomerating and growing, and the prepared nanoparticles have a small particle size and a narrow particle size distribution range. In the present application, preferably, the surfactant is selected from one or more of polyvinyl pyrrolidone, polyethylene glycol (PEG), cyclodextrin, and cetyltrimethylammonium bromide (CTAB); more preferably, the surfactant is polyethylene glycol and cetyltrimethylammonium bromide, and the molar ratio of polyethylene glycol to cetyltrimethylammonium bromide is (0.8-0.85): (0.2-0.15); wherein the molar ratio of the metal chromium salt and the surfactant in the precursor of the nano-fluorination catalyst is 1: (0.01-0.02).

[0016] In some embodiments, the metal chromium salt may be a nitrate, sulfate, acetate or chloride of chromium. Such examples include, but are not limited to, Cr(NO3)3, Cr(NO3)3·9H2O, CrCl3, CrCl3·6H2O, Cr2(SO4)3, Cr2(SO4)3·5H2O, Cr2(SO4)3·6H2O or (CH3COO)3Cr.

[0017] In some embodiments, the metal cobalt salt may be a nitrate, sulfate or chloride of cobalt. Such examples include, but are not limited to, Co(NO3)2, Co(NO3)2·6H2O, CoSO4, CoSO4·7H2O, CoCl2 or CoCl2·6H2O.

[0018] In some embodiments, the metal zinc salt can be a nitrate, sulfate or chloride of zinc. Such examples include, but are not limited to, ZnCl2, ZnSO4, ZnSO4·7H2O, Zn(NO3)2 or Zn(NO3)2·6H2O.

[0019] In some embodiments, the metal lanthanum salt can be lanthanum nitrate, sulfate or chloride of lanthanum. Such examples include, but are not limited to, La(NO3)3, La(NO3)3·6H2O, LaCl3, LaCl3·7H2O, La2(SO4)3 or La2(SO4)3·8H2O.

[0020] In some embodiments, the molar ratio of the metal chromium salt, the metal cobalt salt, the metal zinc salt and the metal lanthanum salt is 1:(0.12-0.20):(0.05-0.18):(0.20-0.30).

[0021] In other embodiments, the molar ratio of the metal chromium salt, the metal cobalt salt, the metal zinc salt and the metal lanthanum salt is 1:(0.12-0.15):(0.08-0.12):(0.28-0.30).

[0022] In the field of gas phase fluorination reaction of halogenated hydrocarbons and fluorinated hydrocarbons, a catalyst for the reaction needs to be specially designed for different reactions of halogenated hydrocarbons and fluorinated hydrocarbons. In the present application, the types of metals constituting the catalyst are optimized. The present application preferably uses metal chromium salts, metal cobalt salts, metal zinc salts and metal lanthanum salts. Combinations of other metals such as chromium / cobalt / aluminum / lanthanum, chromium / cobalt / iron / lanthanum, chromium / cobalt / magnesium / aluminum, chromium / aluminum / zinc / lanthanum, chromium / cobalt / zinc / nickel, etc., cannot obtain the effect of the fluorination catalyst of the present application; further, the molar ratio of metal chromium salts, metal cobalt salts, metal zinc salts and metal lanthanum salts is also optimized. Generally speaking, an increase in chromium content usually increases the specific surface area and pore volume of the catalyst, thereby improving the reaction activity; however, when the chromium content reaches a certain range, the specific surface area and pore volume decrease due to the formation of chromate polymers and other reasons, and the activity decreases instead. The addition of Zn, Co, and La can improve the catalyst activity within an appropriate range. Preferably, the molar ratio of the metal chromium salt, the metal cobalt salt, the metal zinc salt and the metal lanthanum salt is 1: (0.12-0.20): (0.05-0.18): (0.20-0.30). Within this ratio range, the catalyst has high activity, increased strength, and improved catalyst life and selectivity.

[0023] On the other hand, the present invention provides a method for preparing the above-mentioned nano-fluorination catalyst for preparing R152a, comprising the following steps:

[0024] S1. Preparation of mixed solution: adding metal chromium salt, metal cobalt salt, metal zinc salt and metal lanthanum salt to water, and then adding surfactant, stirring to dissolve;

[0025] S2, preparation of nano-fluorination catalyst precursor: adding the complexing agent and the precipitating agent dropwise to the mixed solution prepared in S1, reacting, aging after forming a gel, and spray drying; calcining the spray-dried mixture, pressing into tablets, and obtaining a nano-fluorination catalyst precursor;

[0026] S3. Preparation of nano-fluorination catalyst: The precursor obtained in S2 is loaded into a reactor, and a mixed gas of nitrogen and HF is introduced for fluorination to obtain a nano-fluorination catalyst.

[0027] In some embodiments, the precipitant in S2 is an alkaline solution; the alkaline solution is one or more of aqueous ammonia, ammonium carbonate solution, sodium hydroxide solution, sodium carbonate solution, sodium bicarbonate solution or potassium carbonate solution.

[0028] Preferably, the precipitant in S2 is aqueous ammonia.

[0029] In some embodiments, the reaction temperature in S2 is 40-70°C.

[0030] Specifically, the reaction temperature in S2 is 40°C, 50°C, 60°C or 70°C.

[0031] In some of the embodiments, there is no specific requirement for the reaction time in S2, and the reaction time can be as long as the gel is completely formed.

[0032] In some embodiments, the spray drying conditions in S2 are: inlet temperature 150-200°C, outlet temperature 80-120°C, gas flow rate 4-8m 3 / h; the specific inlet temperature is 150℃, 160℃, 170℃, 180℃, 190℃ or 200℃; the specific outlet temperature is 80℃, 90℃, 95℃, 100℃, 110℃ or 120℃; the specific gas flow rate is 4m 3 / h、5m 3 / h、6m 3 / h、7m 3 / h or 8m 3 / h.

[0033] By introducing spray drying, re-granulation was carried out, and the particle size of the spherical mixture was 3.0μm≤D 50 ≤4.0μm, and the mixture is loose and porous, with an increased specific surface area.

[0034] In some embodiments, the calcination temperature in S2 is 450-600°C; specifically, the calcination temperature is 450°C, 500°C, 550°C or 600°C.

[0035] In some of the embodiments, the roasting time in S2 is 2-6 h; specifically, the roasting time is 2 h, 2.5 h, 3 h, 3.5 h, 4 h, 4.5 h, 5 h or 6 h.

[0036] In some of the embodiments, a graphite additive is added to the powder during tableting in S2, wherein the mass of the graphite is 1-5% of the total mass; specifically, the mass of the graphite is 1%, 2%, 3%, 4% or 5% of the total mass.

[0037] In some embodiments, the fluorination temperature in S3 is 200-400°C; specifically, the fluorination temperature in S3 is 200°C, 230°C, 250°C, 280°C, 300°C, 320°C, 350°C or 400°C.

[0038] Preferably, the present invention provides a nano-fluorination catalyst for preparing R152a, wherein the precursor of the nano-fluorination catalyst is prepared from a metal chromium salt, a metal cobalt salt, a metal zinc salt, a metal lanthanum salt, a complexing agent and a surfactant, wherein the molar ratio of the metal chromium salt, the metal cobalt salt, the metal zinc salt and the metal lanthanum salt is 1: (0.10-0.20): (0.05-0.18): (0.20-0.30); the specific surface area of ​​the nano-fluorination catalyst is 465-500m 2 / g, pore volume is 0.7-0.9mL / g; the complexing agent is selected from EDTA; the surfactant is polyethylene glycol and hexadecyltrimethylammonium bromide, and the molar ratio of polyethylene glycol to hexadecyltrimethylammonium bromide is (0.8-0.85):(0.2-0.15); the molar ratio of metal chromium salt and surfactant in the precursor of the nano-fluorination catalyst is 1:(0.01-0.02); the preparation method of the nano-fluorination catalyst comprises the following steps:

[0039] S1. Preparation of mixed solution: adding metal chromium salt, metal cobalt salt, metal zinc salt and metal lanthanum salt to water, and then adding surfactant, stirring to dissolve;

[0040] S2, preparation of nano-fluorination catalyst precursor: adding the complexing agent and the precipitating agent dropwise to the mixed solution prepared in S1, reacting at 40-70°C, aging after forming a gel, and spray drying; calcining and tableting the spray-dried mixture to obtain a nano-fluorination catalyst precursor;

[0041] S3. Preparation of nano-fluorination catalyst: The precursor obtained in S2 is loaded into a reactor, and a mixed gas of nitrogen and HF is introduced for fluorination to obtain a nano-fluorination catalyst.

[0042] In another aspect, the present invention provides the use of the nano-fluorination catalyst of the present invention in catalyzing the preparation of hydrofluorocarbons, especially in the fluorination reaction of catalyzing the preparation of R152a; preferably, in the fluorination reaction of catalyzing the preparation of R152a by vinyl chloride.

[0043] Compared with the prior art, the present invention has the following beneficial effects: (1) the nano-fluorination catalyst has a higher specific surface area and pore volume; (2) the reasonable ratio of chromium, zinc, cobalt and lanthanum makes the catalyst have higher catalytic activity and longer service life; (3) the preparation method is simple and time-saving, and by introducing spray drying, the mixture before calcination has acquired porous and larger specific surface area properties. DETAILED DESCRIPTION

[0044] The present invention will be better understood through the following examples, but the present invention is by no means limited to the following examples.

[0045] Example 1

[0046] In 200 mL of water, 0.1 mol Cr(NO3)3·9H2O, 0.012 mol Co(NO3)2·6H2O, 0.008 mol Zn(NO3)2·6H2O and 0.030 mol La(NO3)3·6H2O were added respectively, and 0.0008 mol PEG4000 and 0.0002 mol hexadecyltrimethylammonium bromide were added, and the mixture was stirred and dissolved to obtain a mixed salt solution.

[0047] 100 g of 0.5 mol / L EDTA aqueous solution and 4.5 g of 25% ammonia water were added dropwise at 40 °C while stirring. After the gel was formed, it was aged at room temperature for 4 h, the clear liquid was removed by filtration, and the mixture was washed with water twice and spray dried. The inlet temperature was set at 200 °C, the outlet temperature was 100 °C, and the gas flow rate was 5 m 3 / h.

[0048] The spray-dried mixture was calcined at 550° C. for 2 h to obtain a mixed nano powder, 1% graphite was added and mixed evenly, and the mixture was pressed into tablets to obtain a nano fluorination catalyst precursor.

[0049] According to the transmission electron microscope photos, the grain size of the mixed nano powder is 25-40nm, with little agglomeration and good dispersibility.

[0050] Then the nano-fluorination catalyst precursor is loaded into a reactor, and a mixed gas of nitrogen and HF is introduced to perform fluorination at 320° C. to prepare a nano-fluorination catalyst.

[0051] The specific surface area of ​​the nano-fluorination catalyst was analyzed by the specific surface area and pore structure tester and was found to be 495.87 m 2 / g, and the pore volume is 0.89mL / g.

[0052] A similar method to that of Example 1 was adopted, with other conditions unchanged, and the amount of metal salt was changed to prepare the nano-fluorination catalysts of Examples 2-5 and the catalysts of Comparative Examples 1-4.

[0053] Table 1 Catalysts prepared by using different amounts of mixed metal salts

[0054] Examples Cr salt Co salt Zn salt La Salt Specific surface area Kong Rong Example 2 0.1mol 0.015mol 0.012mol 0.028mol <![CDATA[481.31m 2 / g]]> 0.89mL / g Example 3 0.1mol 0.015mol 0.015mol 0.023mol <![CDATA[477.19m 2 / g]]> 0.83mL / g Example 4 0.1mol 0.020mol 0.018mol 0.025mol <![CDATA[473.56m 2 / g]]> 0.78mL / g Example 5 0.1mol 0.020mol 0.005mol 0.020mol <![CDATA[469.27m 2 / g]]> 0.76mL / g Comparative Example 1 0.05mol 0.012mol 0.008mol 0.030mol <![CDATA[423.76m 2 / g]]> 0.56mL / g Comparative Example 2 0.1mol 0.012mol 0.008mol 0.035mol <![CDATA[410.84m 2 / g]]> 0.65mL / g Comparative Example 3 0.1mol 0.030mol 0.008mol 0.030mol <![CDATA[429.25m 2 / g]]> 0.58mL / g Comparative Example 4 0.1mol 0.012mol 0.001mol 0.030mol <![CDATA[423.16m 2 / g]]> 0.51mL / g

[0055] As can be seen from Table 1, a catalyst having a higher specific surface area and a larger pore volume is obtained by a suitable molar ratio of the metal chromium salt, the metal cobalt salt, the metal zinc salt and the metal lanthanum salt.

[0056] A similar method to that of Example 1 was adopted, with other conditions unchanged, and the type of metal salt was changed to prepare catalysts of Comparative Examples 5-10.

[0057] Table 2 Catalysts prepared from different types of mixed metal salts

[0058]

[0059] A similar method to that of Example 1 was adopted, with the amount of metal salt remaining unchanged and the type and amount of surfactant being changed, to prepare the nano-fluorination catalysts of Examples 6-8 and the catalysts of Comparative Examples 11-12.

[0060] Table 3 Catalysts prepared by different surfactant types and dosages

[0061] Examples Surfactants Dosage Example 6 PEG+CTAB 0.00085mol+0.00015mol Example 7 PEG+CTAB 0.00083mol+0.00017mol Example 8 PEG+CTAB 0.00082mol+0.00018mol Comparative Example 11 PEG 0.001mol Comparative Example 12 CTAB 0.001mol

[0062] A similar method to that of Example 1 was adopted, with the amount of metal salt remaining unchanged and the reaction conditions changed, to prepare the nano-fluorination catalysts of Examples 9-14 and the catalysts of Comparative Examples 13-14.

[0063] Table 4 Catalysts prepared under different reaction conditions

[0064] Example Reaction temperature Calcination temperature / time Example 9 40℃ 450℃,2.5h Example 10 40℃ 500℃,2.5h Embodiment 11 40℃ 600℃,2.5h Example 12 50℃ 600℃,3h Example 13 60℃ 600℃,3h Embodiment 14 70℃ 600℃,3h Comparative Example 13 20℃ 600℃,3h Comparative Example 14 85℃ 600℃,3h

[0065] Catalyst performance characterization

[0066] The catalysts of Examples 1-14 and Comparative Examples 1-14 were used to synthesize R152a: 100 mL of catalyst was loaded into a self-made fixed bed, and the reaction temperature was controlled at 150-200°C. Vinyl chloride and HF were introduced into the reactor, with a vinyl chloride flow rate of 20 g / h and a HF flow rate of 48 g / h. Vinyl chloride and HF were mixed and then introduced into the reactor, and the product was washed with water and alkali, and analyzed by gas chromatography.

[0067] Table 5 Conversion rate of vinyl chloride and selectivity of R152a

[0068] Example Vinyl chloride conversion rate R152a Selectivity Comparative Example Vinyl chloride conversion rate R152a Selectivity Example 1 96.3% 87.2% Comparative Example 1 74.7% 68.4% Example 2 96.4% 86.5% Comparative Example 2 76.5% 65.3% Example 3 94.1% 85.6% Comparative Example 3 70.2% 68.2% Example 4 94.2% 84.8% Comparative Example 4 73.8% 60.3% Example 5 94.0% 84.2% Comparative Example 5 74.0% 64.0% Example 6 95.8% 87.3% Comparative Example 6 58.8% 58.2% Example 7 95.5% 87.3% Comparative Example 7 65.3% 60.1% Example 8 95.6% 87.5% Comparative Example 8 75.6% 66.8% Example 9 94.4% 86.8% Comparative Example 9 68.9% 59.9% Example 10 94.2% 88.2% Comparative Example 10 73.0% 63.2% Embodiment 11 95.1% 86.7% Comparative Example 11 69.1% 59.7% Example 12 94.0% 86.9% Comparative Example 12 72.7% 68.8% Example 13 94.8% 85.9% Comparative Example 13 65.4% 60.5% Embodiment 14 96.6% 86.7% Comparative Example 14 70.8% 64.3%

[0069] It can be seen from Table 5 that the nano-fluorination catalyst prepared in the present application has a higher specific surface area and a larger pore volume; when synthesizing R152a in the gas phase, the vinyl chloride conversion rate is higher and the R152a selectivity is higher.

[0070] In addition, after the nano-fluorination catalyst prepared in Example 1-5 was continuously reacted for 600 hours, the conversion rate of vinyl chloride was still maintained at about 80%, indicating that the prepared catalyst still maintained a relatively high catalytic activity.

[0071] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0072] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0073] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A nano-fluorination catalyst for preparing R152a, It is characterized in that The precursor of the nano-fluorination catalyst is prepared from metal chromium salt, metal cobalt salt, metal zinc salt, metal lanthanum salt, a complexing agent and a surfactant, wherein the molar ratio of the metal chromium salt, the metal cobalt salt, the metal zinc salt and the metal lanthanum salt is 1: (0.10-0.20): (0.05-0.18): (0.20-0.30); the specific surface area of ​​the nano-fluorination catalyst is 465-500m 2 / g, pore volume is 0.7-0.9mL / g; The surfactant is polyethylene glycol and hexadecyltrimethylammonium bromide, and the molar ratio of the polyethylene glycol to the hexadecyltrimethylammonium bromide is (0.8-0.85): (0.2-0.15); Wherein, the precursor of the nano-fluorination catalyst is prepared by the following method: Add metal chromium salt, metal cobalt salt, metal zinc salt and metal lanthanum salt into water, then add surfactant, stir and dissolve to obtain a mixed solution; Adding the complexing agent and the precipitating agent dropwise to the mixed solution to react, forming a gel, aging the gel, and spray drying the gel; calcining the spray-dried mixture, pressing the mixture into tablets, and obtaining a nano-fluorination catalyst precursor; The reaction temperature is 40-70°C.

2. The nano-fluorination catalyst for preparing R152a according to claim 1, It is characterized in that The complexing agent is selected from EDTA.

3. The nano-fluorination catalyst for preparing R152a according to claim 1, It is characterized in that The molar ratio of the metal chromium salt to the surfactant in the precursor of the nano-fluorination catalyst is 1:(0.01-0.02).

4. The method for preparing a nano-fluorination catalyst for preparing R152a according to any one of claims 1 to 3, It is characterized in that The following steps are involved: S1. Preparation of a mixed solution: adding metal chromium salt, metal cobalt salt, metal zinc salt and metal lanthanum salt to water, and then adding a surfactant, stirring and dissolving; wherein the surfactant is polyethylene glycol and hexadecyltrimethylammonium bromide, and the molar ratio of the polyethylene glycol to the hexadecyltrimethylammonium bromide is (0.8-0.85): (0.2-0.15); S2, preparation of nano-fluorination catalyst precursor: adding the complexing agent and the precipitating agent dropwise to the mixed solution prepared in S1, reacting, aging after forming a gel, and spray drying; calcining and tableting the spray-dried mixture to obtain a nano-fluorination catalyst precursor; the reaction temperature in S2 is 40-70°C; S3. Preparation of nano-fluorination catalyst: The precursor obtained in S2 is loaded into a reactor, and a mixed gas of nitrogen and HF is introduced for fluorination to obtain a nano-fluorination catalyst.

5. The preparation method according to claim 4, It is characterized in that Graphite additive is added to the powder during tableting, wherein the mass of the graphite accounts for 1-5% of the total mass.

6. The preparation method according to claim 4, It is characterized in that The precipitant in S2 is one or more of ammonia water, ammonium carbonate solution, sodium hydroxide solution, sodium carbonate solution, sodium bicarbonate solution or potassium carbonate solution.

7. The preparation method according to claim 4, It is characterized in that The spray drying conditions in S2 are: inlet temperature 150-200°C, outlet temperature 80-120°C, gas flow rate 4-8m 3 / h.

8. The preparation method according to claim 4, It is characterized in that The calcination temperature in S2 is 450-600°C, and the calcination time is 2-6h.

9. The preparation method according to claim 4, It is characterized in that The fluorination temperature in S3 is 200-400°C.

10. The use of any one of claims 1 to 3 for preparing R152a nano-fluorination catalyst, It is characterized in that Used in the fluorination reaction for catalytic preparation of R152a.