Method for recycling spent lithium-ion battery cells

By heating under hydrogen and treating aqueous media, the complexity and high energy consumption of the transition metal recycling process in waste lithium-ion batteries are solved, and efficient recycling and purification of nickel, cobalt, manganese and lithium are achieved.

CN112400029BActive Publication Date: 2024-12-03BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980045758.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-07-10
Filing Date
2019-07-09
Publication Date
2024-12-03
Estimated Expiration
2039-07-09

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently recover and purify transition metals such as nickel, cobalt and manganese in waste lithium-ion batteries, and often require mechanical separation and high temperature treatment, resulting in complex processes and high energy consumption.

Method used

The lithium-containing transition metal oxide material was heated to 200-900°C in the presence of hydrogen, followed by treatment with an aqueous medium and solid-solid separation, Li and Ni were recovered, and Ni and Co were extracted by acid treatment.

Benefits of technology

It realizes efficient recycling of nickel, cobalt, manganese and lithium, reduces energy consumption and steps, and improves the purity of recycled products, which is especially suitable for the recycling of low-content precious metals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005038696670000241
    Figure GDA0005038696670000241
  • Figure GDA0005038696670000251
    Figure GDA0005038696670000251
  • Figure GDA0005038696670000261
    Figure GDA0005038696670000261
Patent Text Reader

Abstract

A method for recovering transition metals from spent lithium-ion batteries containing nickel, wherein the method comprises the following steps: (a) heating a lithium-containing transition metal oxide material to a temperature in the range of 200 to 900° C. in the presence of H2, (b) treating the product obtained in step (a) with an aqueous medium, (c) solid-solid separation for removing Ni from the solid residue of step (b), (d) recovering Li as a hydroxide or salt from the solution obtained in step (b), (e) extracting Ni and, if applicable, Co from the solid Ni-concentrate obtained in step (c).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for recovering transition metals from spent lithium-ion batteries containing nickel, the method comprising the following steps:

[0002] (a) heating a lithium-containing transition metal oxide material to a temperature in the range of 200 to 900° C. in the presence of H 2 , said material comprising typical impurities such as fluorine compounds (e.g. inorganic fluorides) and / or phosphorus compounds,

[0003] (b) treating the product obtained in step (a) with an aqueous medium,

[0004] (c) solid-solid separation for removing Ni from the solid residue of step (b),

[0005] (d) recovering Li as hydroxide or salt from the solution obtained in step (b), and optionally further

[0006] (e) extracting Ni and, if applicable, Co from the solid Ni-concentrate obtained in step (c).

[0007] Storing electrical energy is a subject of growing interest. Efficient electrical energy storage will allow electrical energy to be generated when it is advantageous and used when and where it is needed. Secondary electrochemical cells are very suitable for this purpose due to their rechargeability. Secondary lithium batteries are of particular interest for energy storage because they provide a high energy density due to the small atomic weight and large ionization energy of lithium, and they have been widely used as power sources for many portable electronic devices (such as mobile phones, laptop computers, miniature cameras, etc.), but also for power sources for electric vehicles. In particular, the growing demand for raw materials such as cobalt and nickel will cause challenges in the future.

[0008] The life of lithium-ion batteries is not infinite. Therefore, it is expected that there will be an increasing number of spent lithium-ion batteries. Since spent lithium-ion batteries contain important transition metals such as, but not limited to, cobalt and nickel and also lithium, spent lithium-ion batteries may become a valuable source of raw materials for new generations of lithium-ion batteries. For this reason, increased research efforts have been carried out with the goal of recycling transition metals and optionally even lithium from used lithium-ion batteries.

[0009] Lithium-ion batteries or parts of lithium-ion batteries that do not meet specifications and requirements (so-called off-spec materials and production waste) may also be a source of raw materials.

[0010] Raw material recovery goes through two main processes. One main process is based on smelting the corresponding battery waste, followed by hydrometallurgical processing of the metal alloy (matte) obtained from the smelting process. Another main process is direct hydrometallurgical processing of battery waste materials. The principle has been disclosed in WO 2017 / 091562 and Power Sources, 2014, 262, 255ff. Such a hydrometallurgical process will be supplied as an aqueous solution or in a precipitated form, such as a transition metal as a hydroxide, either alone or in the required stoichiometric amount for making new cathode active materials. In the latter case, the composition of the metal salt solution can be adjusted to the required stoichiometry by adding a single metal component.

[0011] In WO 2017 / 091562, the coprecipitation of transition metals is described. In WO 2014 / 180743, a coprecipitation process is described in which ammonia or amines are used.

[0012] Starting with conversion experiments with model substances such as LiCoO2, JP 2012-229481 discloses a method for recovering metals from spent lithium-ion batteries, which method includes a preliminary impregnation step, followed by high-temperature oxidation, reduction roasting, aqueous treatment with filtration and recovery of lithium carbonate from the filtrate and transition metals from the residue.

[0013] Known methods for recovering such valuable materials are generally faced with the following problems: waste batteries, i.e. battery cells in which most of these materials are contained, must be disassembled to mechanically separate components such as electrodes and electrolytes, or contain high levels of impurities such as fluorine and / or phosphorus compounds, which must be removed to allow the required materials to be recovered in purity for the production of new battery cells (battery-grade materials). Therefore, the object of the present invention is to provide a method that allows easy recovery of nickel and, if present, cobalt and manganese. Another object of the present invention is to provide a method for recovering further valuable elements contained in battery waste, i.e. lithium and carbon as graphite. Another object of the present invention is to provide an economical method that reduces the number of expensive and / or energy-consuming steps. A specific object of the present invention is to provide a method that allows efficient recovery of nickel, optionally cobalt and manganese and lithium. Another object of the present invention is to provide a method for recovering the transition metals and lithium in high purity, especially with low content of copper and precious metals such as Ag, Au and platinum group metals.

[0014] Thus, it has been found that the process as defined at the outset is also referred to hereinafter as the process of the invention or the recycling process of the invention. The process of the invention comprises the following steps defined in more detail, also referred to hereinafter as step (a), step (b), step (c), etc.:

[0015] (a) heating a lithium-containing transition metal oxide material to a temperature in the range of 200 to 900° C. in the presence of H 2 , said material originating from a lithium ion battery and containing a fluorine compound and / or a phosphorus compound as an impurity,

[0016] (b) treating the product obtained in step (a) with an aqueous medium,

[0017] (c) a solid-solid separation for removing Ni and, if applicable, Co from the solid residue of step (b),

[0018] (d) recovering Li as hydroxide or salt from the solution obtained in step (b), and

[0019] (e) extracting Ni and, if applicable, Co from the solid Ni-concentrate obtained in step (c).

[0020] Therefore, a typical method of the present invention comprises the following steps:

[0021] (a) heating a lithium-containing transition metal oxide material to a temperature in the range of 200 to 900° C. in the presence of H 2 ,

[0022] (b) treating the product obtained in step (a) with an aqueous medium,

[0023] (c) solid-solid separation for removing Ni from the solid residue of step (b),

[0024] (d) recovering Li as hydroxide or salt from the solution obtained in step (b),

[0025] (e) extracting Ni and, if applicable, Co from the solid Ni-concentrate obtained in step (c);

[0026] The lithium-containing transition metal oxide material heated in step (a) originates from a lithium-ion battery and contains fluorine in a range of 0.5 to 8, typically 1 to 8 and in particular 2 to 8% by weight and / or phosphorus in a range of 0.2% to 2% by weight, relative to the weight of the lithium-containing transition metal oxide material.

[0027] However, steps (a) to (c) may also be performed in the following order (step (a), step (c), and then step (b)). In a preferred embodiment of the present invention, steps (a) to (c) are performed in the above alphabetical order, followed by steps (d) and (e).

[0028] Step (a) comprises heating the lithium-containing transition metal oxide material to a temperature in the range of 200-900° C., preferably 300 to 600° C., more preferably 350 to 500° C. Since strong heating, especially under oxidizing conditions (but also to a lesser extent under reducing atmospheres), tends to increase the formation of insoluble species (such as LiMnO2), it is preferred that the lithium-containing transition metal oxide material is generally not exposed to temperatures of 500° C. or higher (e.g., temperatures above 450° C.). Therefore, it is preferred to keep the temperature below 500° C. or even below 450° C. during the preparation of the lithium-containing transition metal oxide material and also in step (a), and preferably to keep the material at a temperature in the range of 350 to 450° C., especially 380 to 440° C. in this step.

[0029] The atmosphere for carrying out the reduction comprises 0.1% to 100% hydrogen by volume. In one embodiment, it comprises 3% to 50% hydrogen by volume, the remainder being a non-oxidizing gas, preferably nitrogen, argon, steam, carbon monoxide, carbon dioxide or a mixture of at least two of these gases. Preferred non-oxidizing gases are nitrogen and steam and a mixture of nitrogen and steam. In a preferred embodiment, step (a) of the method is carried out mainly under hydrogen, for example in an atmosphere comprising 35 to 100%, preferably 50 to 100%, hydrogen by volume (normal conditions), the remainder, if present, being a non-oxidizing gas.

[0030] In one embodiment of the invention, step (a) has a duration in the range of 10 minutes to 30 hours, preferably 20 minutes to 8 hours, more preferably 30 minutes to 4 hours. Of particular technical interest is a duration of step (a) of 20 to 90 minutes, especially 30-60 minutes.

[0031] The concentration of hydrogen in the reducing atmosphere and the reaction time are dependent on each other. Generally, a lower concentration of hydrogen requires a longer reduction time, and vice versa.

[0032] In a preferred method of the invention, step (a) is therefore carried out by heating the lithium-containing transition metal oxide material to a temperature in the range of 350 to 450° C. in the presence of more than 35%, in particular 50-100%, by volume of H2 and for a period of 20 to 90 minutes. In the present invention, a particularly preferred method uses the following to carry out step (a) to recover Li in a particularly efficient manner: a temperature between 400 and 420° C. for up to 2.5 hours (in particular about 30 to 60 minutes) and 35 volume-% or more of hydrogen; applying too high a temperature may lead to lower yields, longer durations do not lead to negative effects, but tend to reduce the space-time yield, while a H2 concentration of ≥35 vol-% translates into a short reaction time of ≤2.5 h and is therefore advantageous; the use of pure hydrogen can achieve the best space-time yield.

[0033] In one embodiment of the invention, the reduction conditions with respect to the hydrogen concentration and duration of step (a) are selected such that at least a portion of the lithium-containing transition metal oxide material comprises a paramagnetic, ferromagnetic or ferrimagnetic component separable by application of a magnetic field. The formation of a ferromagnetic or ferrimagnetic component resulting from at least partial reduction of the lithium-containing transition metal material is preferred. With respect to nickel contained in the lithium-containing transition metal material, the degree of reduction may vary in the range between 1 and 100%, preferably in the range of 80 to 100%.

[0034] The lithium-containing transition metal oxide material is a material derived from a lithium-ion battery or a part of a lithium-ion battery. Typically, the lithium-containing transition metal oxide material is obtained after mechanical removal of the housing, wiring or circuit, and thus typically consists mainly of battery cell materials. For safety reasons, such lithium-ion batteries are completely discharged, for example by immersion in a dry conductive bath, such as metal fragments, or by feeding the current into the power grid in a controlled manner, for example via an inverter. Otherwise, a short circuit may occur, constituting a fire and explosion hazard. Such lithium-ion batteries can be disassembled, perforated, ground, for example in a hammer mill, or shredded, for example in an industrial pulverizer.

[0035] It is advantageous to at least partially remove the electrolyte, especially an electrolyte comprising an organic solvent or a mixture of organic solvents, before starting step (a), for example by drying, for example at a temperature in the range of 50 to 250° C. at or below atmospheric pressure. As mentioned above, the lithium-containing transition metal oxide material is preferably not exposed to high temperatures (especially 400° C. or more) under oxidizing conditions before subjecting it to this step (a).

[0036] In one embodiment of the present invention, the lithium-containing transition metal oxide material is derived from battery waste. In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material is derived from mechanically processed battery waste, such as battery waste processed in a hammer mill or an industrial pulverizer. Such lithium-containing transition metal oxide material may have an average particle size (D50) in the range of 1 μm to 1 cm.

[0037] In one embodiment of the present invention, step (a1) is performed before step (a), and the step (a1) includes removing, for example, carbon or organic polymers by a solid-solid separation method. Examples of such solid-solid separation methods are electrical sorting, screening, magnetic separation or other classification methods. Solid-solid separation can be performed dry or in the presence of a suitable dispersion medium, preferably water.

[0038] In one embodiment of the present invention, the mechanically treated battery waste is ground before step (a). Such grinding is preferably carried out in a ball mill or an agitated ball mill. The grinding can be carried out under wet or dry conditions, preferably dry conditions.

[0039] In one embodiment of the invention, the mechanically treated battery waste is subjected to a solvent treatment to dissolve and separate the polymer binder used to bind the lithium transition metal oxide to the current collector film. Suitable solvents are N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and N-ethylpyrrolidone, dimethyl sulfoxide, hexamethylphosphoramide, tetramethylurea, trimethyl phosphate and triethyl phosphate in their pure form or as a mixture.

[0040] The solvent treatment described above can be carried out in a continuous step with one or more solvents or in a single step using a solvent capable of dissolving the electrolyte components and the binder polymer. The solvent is applied at a temperature ranging from 10°C to 200°C. In particular, the dissolution of the polymer may require an elevated temperature ranging from 50 to 200°C, preferably between 100 and 150°C. Unless a pressure above 1 bar is applied, the upper temperature limit is usually limited by the boiling point of the solvent.

[0041] In one embodiment, the washing of the mechanically treated battery waste with an aprotic solvent is performed in the absence of humidity, for example, under a dry gas such as dry air, dry nitrogen.

[0042] In one embodiment of the present invention, the lithium-containing transition metal oxide material does not contain a significant amount of impurities, such as but not limited to other parts or materials from parts of a lithium-ion battery. Such lithium-containing transition metal oxide materials may include substandard materials.

[0043] However, the lithium-containing transition metal oxide material preferably contains compounds other than nickel compounds (such as nickel / cobalt components or nickel / cobalt / manganese or nickel / cobalt / aluminum compounds) in the range of 0.1 to 80% by weight and, if applicable, in extreme cases, valuable materials as minority components. Examples of such components are carbon in conductive form, also referred to as conductive carbon hereinafter, such as graphite, soot and graphene. Further examples of impurities are copper and its compounds, aluminum and aluminum compounds, such as aluminum oxide, iron and iron compounds, zinc and zinc compounds, silicon and silicon compounds, such as silicon dioxide and silicon oxide SiO with zero < y ≤ 2. y , tin, silicon-tin alloys, and organic polymers such as polyethylene, polypropylene and fluorinated polymers, for example polyvinylidene fluoride, tetrafluoroethylene polymers, etc. Additional impurities include fluorine compounds, such as inorganic fluorides, and phosphorus compounds, which may originate from liquid electrolytes, such as in the widely used LiPF6 and from the products of hydrolysis of LiPF6. Battery waste used as starting material for the method of the present invention may originate from a variety of sources, and therefore in most embodiments, the lithium-containing transition metal oxide material contains compounds other than nickel / cobalt compounds or nickel / cobalt / manganese or nickel / cobalt / aluminum components, if applicable, one of such components is carbon in a conductive form in the range of 2 to 65% by weight relative to the entire lithium-containing transition metal oxide material.

[0044] In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material comprises copper as a metal or in the form of one or more of its compounds in the range of 20 ppm to 3% by weight.

[0045] In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material contains aluminum as a metal or in the form of one or more of its compounds in the range of 100 ppm to 15% by weight.

[0046] In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material contains iron as a metal or an alloy or in the form of one or more of its compounds in the range of 100 ppm to 5% by weight.

[0047] In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material contains zinc as a metal or an alloy or in the form of one or more of its compounds in the range of 20 ppm to 2% by weight.

[0048] In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material contains zirconium as a metal or an alloy or in the form of one or more of its compounds in the range of 20 ppm to 2% by weight.

[0049] In a preferred embodiment of the invention, the lithium-containing transition metal oxide material contains fluorine in the range of 0.5 to 8, typically 1 to 8 and especially 2 to 8% by weight, calculated as the sum of organic fluorides (e.g., bound in a polymer) and inorganic fluorides (as one or more of their inorganic fluorides).

[0050] In a preferred embodiment of the present invention, the lithium-containing transition metal oxide material contains phosphorus in the range of 0.2% to 2% by weight. The phosphorus may be present in one or more inorganic compounds.

[0051] Each of the percentages given above is by weight of the dry material (ie, the lithium-containing transition metal oxide material).

[0052] The lithium-containing transition metal oxide material comprises nickel and cobalt. Examples of lithium-containing transition metal oxide materials may be based on lithiated nickel cobalt manganese oxide ("NCM") or lithiated nickel cobalt aluminum oxide ("NCA") or mixtures thereof.

[0053] Examples of layered nickel-cobalt-manganese oxides are those of the general formula Li 1+x (Ni a Co b Mn c M 1 d ) 1-x O2 compounds, where M 1 is selected from the group consisting of Mg, Ca, Ba, Al, Ti, Zr, Zn, Mo, V and Fe, and the additional variables are defined as follows:

[0054] Zero ≤ x ≤ 0.2

[0055] 0.1≤a≤0.8,

[0056] Zero ≤ b ≤ 0.99; usually zero ≤ b ≤ 0.5, preferably 0.05 <b≤0.5,

[0057] zero ≤ c ≤ 0.6,

[0058] Zero≤d≤0.1, and a+b+c+d=1.

[0059] In a preferred embodiment, in the compound according to general formula (I)

[0060] Li (1+x) [Ni a Co b Mn c M 1 d ] (1-x) O2

[0061] (I)

[0062] M 1 is selected from Ca, Mg, Zr, Al and Ba,

[0063] and the additional variables are as defined above.

[0064] An example of a lithiated nickel-cobalt aluminum oxide is a compound of the general formula Li[Ni h Co i Al j ]O 2+r Typical values ​​of r, h, i and j are:

[0065] h is in the range of 0.8 to 0.90,

[0066] i is in the range of 0.15 to 0.19,

[0067] j is in the range of 0.01 to 0.05, and

[0068] r is in the range of zero to 0.4.

[0069] Particularly preferred is Li (1+x) [Ni 0.33 Co 0.33 Mn 0.33 ] (1-x) O2、Li (1+x) [Ni 0.5 Co 0.2 Mn 0.3 ] (1-x) O2、Li (1+x) [Ni 0.6 Co 0.2 Mn 0.2 ] (1-x) O2、Li (1+x) [Ni 0.7 Co 0.2 Mn 0.1 ] (1-x) O2、Li (1+x) [Ni 0.8 Co 0.1 Mn 0.1 ] (1-x) O2 (each with x as defined above) and Li[Ni 0.85 Co 0.13 Al 0.02 ]O2.

[0070] The lithium-containing transition metal oxide material may have a regular shape, but it generally has an irregular shape. Although, it is preferred to remove light parts such as housing parts from organic plastics and aluminum or copper foils as much as possible, for example in a forced air flow.

[0071] In one embodiment, the composition of the atmosphere is changed during step (a), for example, in case volatile organic compounds are present in the feed, this can be done by removing the volatile organic compounds under an inert atmosphere and then switching the atmosphere to one containing hydrogen.

[0072] In one embodiment, an oxidizing atmosphere at a temperature ranging between 20 and 350° C. is used in step (a) prior to reduction with a hydrogen-containing atmosphere. By this embodiment, some impurity components, i.e. organic components, or dry materials can be burned off (especially using temperatures up to 250° C. as further described above. The preferred oxidizing gas is oxygen or a gas containing oxygen, such as air. The steps of the method are preferably carried out without subjecting the material containing lithium, transition metal oxides and further fluorine and / or phosphorus compounds originating from spent lithium-ion battery cells to oxidation above 350° C.

[0073] In one embodiment, a non-oxidizing and non-reducing atmosphere is used in step (a) at a temperature in the range of 20 to 900° C., in particular 20 to 450° C., before the reduction with a hydrogen-containing atmosphere. Thus, volatile compounds can be removed. Preferred gases are inert gases, such as nitrogen and argon or carbon dioxide.

[0074] In one embodiment of the invention, step (a) is carried out in the presence of steam at a temperature range between 100 and 900° C., such as the temperature range specified above for step (a). Steam may also be added when removing volatile organic compounds prior to reduction under a hydrogen-containing atmosphere.

[0075] In one embodiment of the invention, step (a) is carried out in the presence of lime, quartz or one or more silicates or silicon dioxide or a mixture thereof, preferably lime and silicon dioxide. The lime may be selected from slaked lime and quicklime or burnt lime. In a preferred embodiment of the invention, step (a) is carried out in the presence of 2 to 40% by weight of lime or quartz or silicate or silicon dioxide relative to the lithium-containing transition metal oxide material. When such compounds are used, a heat treatment may be advantageous before the reduction with a hydrogen-containing atmosphere as described above. Such a heat treatment may be carried out in any of the atmospheres mentioned above, preferably an inert gas which may also contain steam.

[0076] Step (a) can be carried out in any type of oven that allows the introduction of hydrogen or different gases. These ovens can be operated in batches or continuously. Preferred ovens are rotary kilns and fluidized bed reactors. These reactors can be operated continuously. Different gas compositions can be applied in successive ovens or kilns or in successive sections of a kiln. In the latter case, the gases are introduced in a manner that the reactive gases cannot intermix.

[0077] After step (a) has been performed, the heat-treated lithium-containing transition metal oxide material is cooled, for example to room temperature or slightly above room temperature, for example 25 to 90°C.

[0078] In one embodiment of the present invention, step (b1) is carried out before step (b), and the step (b1) includes removing such as carbon or organic polymer by dry solid-solid separation method. The example of such dry solid-solid separation method is electric sorting, screening, magnetic separation or other classification methods. Step (b1) is introduced here as an additional step. As mentioned above, dry solid-solid separation can be enough to separate the solid material containing Ni from the solid residue obtained in step (a). In this case, the order of steps (b) and (c) is reversed, and the solid residue containing Ni obtained after aqueous treatment is directly leached to extract Ni and other transition metals if applicable.

[0079] Step (b) of the process of the present invention comprises treating the heat-treated lithium-containing transition metal oxide material (the material obtained in step (a) or the corresponding part of step (b1)) with an aqueous medium capable of selectively dissolving the Li component formed in step (a) without dissolving the transition metal contained in the heat-treated material. This treatment can be carried out at ambient temperature or at a higher temperature, for example in the range of between 20 and 150° C. When a temperature above the boiling point of water is used, the treatment is carried out at an elevated pressure.

[0080] In one embodiment of the invention, the aqueous medium used comprises a weak acid such as carbonic acid (which is obtained by dissolving carbon dioxide in water at atmospheric pressure or higher pressure), formic acid, acetic acid or sulfurous acid. These acids are used in a concentration of 0.1 to 10w% in water, preferably a concentration of 1 to 10w%. When carbonic acid is used, it is preferably used under a carbon dioxide pressure of 10 to 150 bar. In a specific embodiment of technical interest, the aqueous medium of step (b) contains neither a weak acid nor carbon dioxide or carbonic acid.

[0081] In one embodiment of the present invention, the aqueous medium used in step (b) is water, such as deionized water. In one embodiment of the present invention, the aqueous medium used in step (b) is an aqueous formic acid solution.

[0082] In one embodiment of the present invention, the solid residue from step (a) or the lithium-containing transition metal material portion obtained in step (b1) is first treated with water and then treated with a dilute weak acid as described above after solid-liquid separation, such as filtration after water treatment. The two extracts can be kept separately to separate the different dissolved Li species.

[0083] In one embodiment of the present invention, step (b) has a duration ranging from 20 minutes to 10 hours, preferably from 1 to 3 hours.

[0084] In one embodiment, step (b) is performed at least twice to achieve optimal recovery of lithium hydroxide or lithium salts. A solid-liquid separation is performed between each treatment. The lithium salt solutions obtained can be treated uniformly or individually to recover solid lithium salts. In the case of different lithium salts of different solubility, the latter can be advantageous. In this case, the first extract will mainly contain highly soluble lithium salts, while the successive extracts will contain lower concentrations of sparingly soluble salts.

[0085] In one embodiment of the present invention, the ratio of the aqueous medium to the material obtained in step (a) or (b1) is in the range of 1:1 to 99:1, preferably 2:1 to 9:1 by weight.

[0086] In one embodiment of the invention, the material obtained from step (a) or (b1) is ground before step (b) to deagglomerate different solid particles from each other in the case where these materials are agglomerated in some way, for example by residual binder polymer. Such grinding is preferably carried out in a ball mill or a stirred ball mill. Grinding can be carried out under dry or wet conditions. Preferably, grinding is also carried out in the aqueous medium used in the continuous step (b).

[0087] If applicable, the pressure can be released at the end of step (b).An aqueous solution comprising LiOH, LiHCO3 and / or Li2CO3 or a Li salt of the acid used in step (b) is obtained.

[0088] The solid residue is contained in the aqueous solution, forming a suspension. In case the one or more Li compounds are extracted in two or more steps as described above, the solid residue will be contained in the slurry of the second or last step, respectively.

[0089] In a preferred embodiment of the invention, the solid residue obtained from step (b) dispersed in the Li salt solution is recovered by a solid-liquid separation step. This can be a filtration or centrifugation, or a sedimentation and decantation type. In order to recover such fine particles of solid material, for example with an average diameter of 50 μm or less, a flocculant, such as a polyacrylate, can be added. The solid residue obtained by solid-liquid separation is dispersed in water.

[0090] The solid residue dispersed in an aqueous medium, for example in a Li salt solution or water as described above, is then treated according to step (c).By carrying out step (c), nickel and if applicable Co are recovered as a nickel (and if applicable cobalt) containing solid.

[0091] Step (c) of the present invention includes a solid-solid separation step. In a preferred embodiment, it is a wet solid-solid separation step. This solid-solid separation step is used to separate insoluble components, such as carbon and polymers or insoluble inorganic components, such as metal particles or metal oxide particles, from the metal or metal oxide components of the transition metal oxide material containing lithium. After the solid-solid separation of step (c), a solid concentrate portion is obtained, which contains most of the Ni and, if applicable, Co in an enriched form. Such a solid-solid separation step can be performed by mechanical, column or pneumatic or mixed flotation. In many embodiments, a collector compound is added to the slurry, which makes the target component hydrophobic. Typical collector compounds for carbon and polymer particles are hydrocarbons or fatty alcohols, which are introduced in an amount of 1g to 50kg / t of the heat-treated transition metal oxide material containing lithium from step (a). Flotation can also be performed in reverse, that is, the initial hydrophilic component is converted into a strong hydrophobic component by a specific collector substance, such as a fatty alcohol sulfate or an ester-based quaternary ammonium salt. Preferred is the direct flotation using hydrocarbon collectors such as mineral oil, kerosene or diesel. In order to improve the selectivity of flotation to carbon and polymer particles, inhibitors can be added, which reduce the amount of metal and metal oxide components entrained in the foam phase. The reagent that can be used can be an acid or base for controlling the pH value in the range of 3 to 9. It can also be an ionic component adsorbed on the surface of the metal or metal oxide, such as sodium silicate or a bipolar component, such as an amino acid. In order to improve the flotation efficiency, it can be advantageous to add carrier particles that form agglomerates with hydrophobic target particles such as polymer particles, carbonaceous particles such as graphite or coal. By using magnetic carrier particles, magnetic agglomerates that can be separated magnetically can be formed. In the case where the target component is paramagnetic, ferrimagnetic or ferromagnetic, these components can also be separated by magnetic separation using a high intensity magnetic separator ("WHIMS"), a medium intensity magnetic separator ("MIMS") or a low intensity magnetic separator ("LIMS"). Other solid-solid separation techniques utilize the density difference of solid components, such as the density difference between graphite and metal or metal oxides. These techniques include floatation and sinking using a fluid with a density between the density of the solid components to be separated. Another such technique is heavy medium separation. Additional separation techniques based on density differences are spiral separators and hydrocyclones.

[0092] Likewise, a combination of at least two of the solid-solid separation techniques described above may be used.

[0093] In a preferred embodiment, the solid-solid separation in step (c) is magnetic separation.

[0094] In one embodiment of the invention, the material obtained from step (b) is ground before step (c) to release different solid particles from each other in the case where these materials are agglomerated in some way, for example by residual binder polymer. Such grinding is preferably carried out in a ball mill or a stirred ball mill.

[0095] In one embodiment of the invention, step (c) is a wet solid-solid separation using an aqueous medium, preferably water as a fluid. The ratio of the fluid medium to the solid material obtained in step (b) is in the range of 1:1 to 99:1, preferably 2:1 to 9:1 by weight.

[0096] From the wet solid-solid separation of step (c), two slurries are obtained, one comprising a solid material containing the target transition metal, and one comprising other components, such as carbonaceous materials and polymers and, if applicable, some inorganic compounds. By suitable selection and, if necessary, a combination of solid-solid separation steps, at least 60% of Ni is obtained and concentrated into a portion. Preferably, at least 80 to 99% of Ni is separated.

[0097] In one embodiment of the invention, the liquid phase of the slurry fed to step (c) contains dissolved lithium. In this case, one or the other or both slurries obtained from the solid-solid separation in step (c) are subjected to solid-liquid separation to recover the lithium solution. The lithium solution is then further processed in step (d).

[0098] In step (d) the solution comprising lithium obtained from any of the preceding steps is treated to recover the lithium as a hydroxide or a salt in the form of a solid material.

[0099] In one embodiment of the invention, the Li salt or LiOH is recovered by evaporating the water contained in the solution. Advantageously, the residual acid is neutralized by adding a stoichiometric amount of LiOH or Li2CO3 or by adding ammonia.

[0100] In one embodiment of the invention, Li is recovered from the Li salt solution by precipitation by addition of sodium carbonate or ammonium carbonate, or by carbonic acid formed by dissolving carbon dioxide, preferably under pressure, as Li carbonate.

[0101] In a preferred embodiment of the present invention, Li is recovered as LiOH.

[0102] The obtained solid Li salt and / or LiOH can be further purified by dissolution and recrystallization, as known in the art.

[0103] Subjecting the solid Ni-concentrate obtained from step (c) to step (e) allows extraction of the Ni and if applicable Co and if applicable other valuable metals such as lithium contained in the Ni-concentrate. For the extraction, a furnace or an acid or ammonium carbonate may be applied.

[0104] In one embodiment of the present invention, such step (e) may be pyrometallurgically carried out by smelting the solid Ni-concentrate obtained in step (c) as such or as a co-feed in a furnace dedicated to Ni-concentrate from mining production.

[0105] During step (e), the transition metal material is treated with a leaching agent, which is preferably an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid and citric acid or a combination of at least two of the foregoing, such as a combination of nitric acid and hydrochloric acid. In another preferred form, the leaching agent is

[0106] -- inorganic acids, such as sulfuric acid, hydrochloric acid, nitric acid,

[0107] - organic acids, such as methanesulfonic acid, oxalic acid, citric acid, aspartic acid, malic acid, ascorbic acid or glycine,

[0108] - a base, such as ammonia, an amine, an aqueous solution of ammonia, ammonium carbonate or a mixture of ammonia and carbon dioxide, or

[0109] -- Chelating agents, such as EDTA or dimethylglyoxime.

[0110] In one form, the leaching agent comprises an aqueous acid solution, such as an aqueous inorganic or organic acid solution. In another form, the leaching agent comprises a base, preferably ammonia or an amine. In another form, the leaching agent comprises a complex former, preferably a chelating agent. In another form, the leaching agent comprises an inorganic acid, an organic acid, a base or a chelating agent.

[0111] The concentration of the leaching agent can vary in a wide range, for example 0.1 to 98% by weight, and preferably in a range between 10 and 80%. A preferred example of an aqueous acid solution is an aqueous sulfuric acid solution, for example a concentration in the range of 10 to 98% by weight. Preferably, the aqueous acid solution has a pH value in the range of -1 to 2. The amount of acid is adjusted to maintain an excess of acid (relative to the transition metal). Preferably, at the end of step (e), the pH value of the resulting solution is in the range of -0.5 to 2.5. A preferred example of an alkali as a leaching agent is an aqueous ammonia solution having a molar ratio of NH3 to metal (Ni, Co) of 1:1 to 6:1, preferably 2:1 to 4:1, preferably also in the presence of carbonate or sulfate ions. Suitable chelating agents such as EDTA or dimethylglyoxime are generally applied in a molar ratio of 1:1 to 3:1.

[0112] Leaching can be carried out in the presence of an oxidizing agent. Preferred oxidizing agents are oxygen as a pure gas or in a mixture with an inert gas such as nitrogen or as air. Other oxidizing agents are oxidizing acids such as nitric acid.

[0113] In one embodiment of the present invention, such step (e) may be performed by dissolving the solid Ni-concentrate obtained in step (c) in an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid and citric acid.

[0114] In one embodiment of the present invention, such step (e) can be carried out by treating the solid Ni-concentrate obtained in step (c) with an aqueous solution of ammonium carbonate or ammonium bicarbonate. Such aqueous solution may contain additional ammonia.

[0115] In one embodiment of the invention, the Ni-concentrate obtained from step (c) is treated in step (e) with an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid and citric acid or a combination of at least two of the foregoing, such as a combination of nitric acid and hydrochloric acid. In the case of an aqueous acid solution, the concentration of the acid may vary over a wide range, such as 0.1 to 99% by weight, preferably between 10 and 96%. The amount of acid is adjusted to maintain an excess of acid. Preferably, at the end of step (e), the pH value of the resulting solution is in the range of -0.5 to 2.

[0116] A preferred example of an aqueous acid solution is an aqueous sulfuric acid solution, for example in a concentration ranging from 10 to 98% by weight.

[0117] The treatment according to step (e) can be carried out at a temperature in the range of 20 to 200° C., in particular 20 to 130° C. If a temperature above 100° C. is required, step (e) is carried out at a pressure above 1 bar. Otherwise, normal pressure is preferred. In the context of the present invention, normal pressure means 1 atm or 1013 mbar. "Normal conditions" means normal pressure and 20° C.

[0118] In one embodiment of the invention, step (e) is carried out in a container protected from strong acids, such as a molybdenum and copper rich steel alloy, a nickel based alloy, a duplex stainless steel or a glass lined or enameled or titanium coated steel. Further examples are polymer liners and polymer containers derived from acid resistant polymers, such as polyethylene, such as HDPE and UHMPE, fluorinated polyethylene, perfluoroalkoxyalkanes ("PFA"), polytetrafluoroethylene ("PTFE"), PVdF and FEP. FEP stands for fluorinated ethylene propylene polymer (copolymer of tetrafluoroethylene and hexafluoropropylene).

[0119] The slurry obtained in step (e) may be stirred, agitated or subjected to a grinding treatment, for example in a ball mill or an agitated ball mill. Such a grinding treatment generally results in better access of water or acid to the particulate transition metal material.

[0120] In one embodiment of the invention, step (e) has a duration in the range of 10 minutes to 10 hours, preferably 1 to 3 hours. For example, the reaction mixture in step (e) is stirred with a power of at least 0.1 W / l or circulated by pumping to achieve good mixing and avoid sedimentation of insoluble components. Shearing can be further improved by using baffles. All these shearing devices need to apply sufficient corrosion resistance and can be produced by materials and coatings similar to those described for the container itself.

[0121] Step (e) can be carried out under an air atmosphere or under air diluted with N2. However, it is preferred to carry out step (e) under an inert atmosphere such as nitrogen or a rare gas such as Ar.

[0122] The treatment according to step (e) results in the dissolution of metal compounds originating from the cathode active material, such as the dissolution of the NCM or NCA including impurities other than carbon and organic polymers. In most embodiments, a slurry is obtained after performing step (e). Residual lithium and transition metals, such as but not limited to nickel, cobalt, copper and, if applicable, manganese, are generally in dissolved form when leached, for example in the form of their salts.

[0123] In one embodiment of the invention, step (e) is carried out in the presence of a reducing agent. Examples of reducing agents are organic reducing agents such as methanol, ethanol, sugars, ascorbic acid, urea, bio-based materials containing starch or cellulose, and inorganic reducing agents such as hydrazine and its salts such as sulfates and hydrogen peroxide. Preferred reducing agents for step (e) are those that do not leave impurities based on metals other than nickel, cobalt or manganese. Preferred examples of reducing agents in step (e) are methanol and hydrogen peroxide. With the aid of a reducing agent, for example, Co 3+ Reduction to Co 2+ Or Mn(+IV) or Mn 3+ Reduction to Mn 2+ .

[0124] In a preferred embodiment of the invention, an excess of reducing agent is used relative to the amount of Co and, if applicable, Mn. In the presence of Mn, this excess is advantageous.

[0125] In a preferred embodiment of the present invention, relative to Co 3+ amount, use an excess of reducing agent.

[0126] In one embodiment of the invention, the ratio of extraction medium, such as acid solution and if applicable reducing agent, to the Ni-concentrate obtained in step (c) is in the range of 1:1 to 99:1, preferably 2:1 to 9:1 by weight.

[0127] In the embodiment where a so-called oxidizing acid has been used in step (e), it is preferred to add a reducing agent to remove unused oxidizing agent. Examples of oxidizing acids are nitric acid and a combination of nitric acid and hydrochloric acid. In the context of the present invention, hydrochloric acid, sulfuric acid and methanesulfonic acid are preferred examples of non-oxidizing acids.

[0128] The leachate obtained in step (e) may have a transition metal concentration in the range of 1 to 20% by weight, preferably 3 to 15% by weight, depending on the concentration of the acid used.

[0129] In one embodiment, step (e) is performed under an inert gas such as nitrogen or argon.

[0130] In one embodiment of the invention, the Ni concentrate obtained from step (c) is ground before step (e) to release different solid particles from each other in the case where these Ni concentrates are agglomerated in some way, for example, by residual binder polymer. Such grinding is preferably carried out in a ball mill or a stirred ball mill.

[0131] The liquid phase obtained in step (e) may have a transition metal concentration in the range of 1 to 25% by weight, preferably 6 to 15% by weight, depending on the concentration and amount of the aqueous acid solution used in step (e). The transition metal concentration depends on the solubility of the corresponding salt of the acid used. Preferably, step (e) is performed so that the transition metal concentration of the main metal, such as Ni and optionally Co and Mn, is slightly below the solubility limit of the most insoluble salt to ensure a high metal concentration in the solution.

[0132] The optional step that can be carried out after step (e) is to remove undissolved solids, such as carbonaceous materials and polymers produced by the battery shell. The step can be carried out by filtering centrifugation or sedimentation and decantation with or without adding a flocculant. The solid residue obtained can be washed with water and can be further processed so as to separate carbonaceous and polymer components, for example, by a solid-solid separation method as described above.

[0133] In one embodiment of the present invention, step (e) and the removal of undissolved solids are performed sequentially in a continuous operation mode.

[0134] In the continuous step (e1), the Ni-concentrate in step (e) is dissolved, and the pH of the above slurry or solution can be adjusted to 2.5 to 8, preferably 5.5 to 7.5 and even more preferably 6 to 7. The pH value can be determined by conventional means, such as by potentiometric titration, and refers to the pH value of the continuous liquid phase at 20°C. The pH value is adjusted by diluting with water or by adding a base or by a combination thereof. Examples of suitable bases are ammonia and alkali metal hydroxides, such as LiOH, NaOH or KOH, in solid form, for example as pellets, or preferably as an aqueous solution. A combination of at least two of the aforementioned is also feasible, such as a combination of ammonia and caustic soda solution.

[0135] Preferably, the optional step (e2) comprises removing a precipitate of carbonates, oxides, phosphates, hydroxides or oxyhydroxides of Al, Cu, Fe, Zr, Zn, Zn, a combination of at least two of the foregoing formed in the optional step (e1). The precipitate may be formed during the pH adjustment. The phosphate may be a stoichiometric or alkaline phosphate. Without wishing to be bound by any theory, the phosphate may be generated when the phosphate is formed by hydrolysis of the hexafluorophosphate formed during step (a) or its decomposition products. The precipitate may be removed by filtration or by means of a centrifuge or by sedimentation. Preferred filters are belt filters, plate and frame filter presses, suction filters and cross-flow filters. Filter aids and / or flocculants may be added to improve solid-liquid separation.

[0136] In a preferred embodiment of the present invention, step (e2) comprises an optional step (e3). Step (e3) comprises treating the solution obtained after step (e1) or step (e2) with metallic nickel, metallic cobalt or metallic manganese or any combination of at least two of the foregoing.

[0137] In optional step (e3), the solution obtained after step (e2) is contacted with metallic nickel, cobalt or manganese or a combination of at least two of the foregoing, for example in a column. In such an embodiment, it is advantageous to provide a column filled with metallic nickel, metallic cobalt or metallic manganese or a combination of at least two of the foregoing in the form of blocks or particles, for example as a fixed bed, and allow the solution to flow through such a column.

[0138] In one embodiment of the present invention, step (e3) is carried out under normal pressure.

[0139] In one embodiment of the invention, step (e3) has a duration ranging from 30 minutes to 5 hours. If step (e1 ) is carried out in a column, the duration corresponds to the mean residence time.

[0140] In one embodiment of the present invention, step (e3) is performed at a pH range of 1 to 6, preferably pH 2 to 5. The lower the pH in step (e1), the higher the amount of metal selected from Ni, Co and Mn dissolved under hydrogen formation.

[0141] Step (e3) is particularly useful for removing traces of copper. By carrying out step (e3), no new impurities requiring additional purification steps are introduced into the solution of transition metals. Even if the metals nickel, cobalt or manganese contain traces of copper, they will not dissolve.

[0142] Optional step (f) comprises precipitation of the transition metal as a mixed hydroxide or mixed carbonate, preferably as a mixed hydroxide.

[0143] In a preferred embodiment of the present invention, step (f) is carried out by adding ammonia or an organic amine such as dimethylamine or diethylamine, preferably ammonia and at least one inorganic base such as lithium hydroxide, sodium hydroxide, potassium hydroxide, sodium carbonate, sodium bicarbonate, potassium carbonate or potassium bicarbonate or a combination of at least two of the foregoing. Preference is given to adding ammonia and sodium hydroxide.

[0144] In one embodiment of the invention, step (f) is carried out at a temperature in the range of 10 to 85°C, preferably 20 to 50°C. In one embodiment of the invention, the concentration of the organic amine or ammonia is in the range of 0.05 to 1 mol / l, preferably 0.1 to 0.7 mol / l. In this context, the term "ammonia concentration" includes the concentration of ammonia and ammonium. Particular preference is given to Ni 2+ and Co 2+ The amount of ammonia whose solubility in the mother liquor is each not more than 1000 ppm, more preferably each not more than 500 ppm.

[0145] In one embodiment of the invention, mixing is effected during step (f) of the process of the invention, for example with a stirrer, a rotor stator mixer or a ball mill. Preference is given to introducing at least 1 W / l, preferably at least 3 W / l and more preferably at least 5 W / l of the stirrer output into the reaction mixture. In one embodiment of the invention, no more than 25 W / l of the stirrer output may be introduced into the reaction mixture.

[0146] The optional step (f) of the process of the present invention may be carried out in the presence or absence of one or more reducing agents. Examples of suitable reducing agents are hydrazine, primary alcohols such as, but not limited to, methanol or ethanol, furthermore ascorbic acid, glucose and alkali metal sulfites. It is preferred that no reducing agent is used in step (f). In cases where a large amount of manganese is present in the transition metal oxide material, for example, at least 3 mol-% relative to the transition metal portion of the corresponding cathode active material, the use of a reducing agent or an inert atmosphere or a combination of both is preferred.

[0147] Step (f) of the process of the present invention may be carried out under an atmosphere of an inert gas such as nitrogen or argon or carbon dioxide.

[0148] In one embodiment of the present invention, step (f) is carried out at a pH value in the range of 9 to 13.5, preferably a pH value of 11 to 12.5 in the case of hydroxides, and a pH value in the range of 7.5 to 8.5 in the case of carbonates. The pH value refers to the pH value in the mother liquor measured at 23°C.

[0149] Step (f) can be carried out in a batch reactor, or preferably continuously, for example in a continuous stirred tank reactor, or in two or more cascades, for example two or three continuously stirred tank reactors.

[0150] Step (f) of the process according to the invention can be carried out under air, under an inert gas atmosphere, for example under a noble gas or nitrogen atmosphere, or under a reducing atmosphere. An example of a reducing gas is, for example, SO2. Preference is given to carrying out the process under an inert gas atmosphere, in particular under nitrogen.

[0151] For further purification purposes, the solid recovered in step (f) may be dissolved in an acid, such as hydrochloric acid, or more preferably sulfuric acid.

[0152] By carrying out the process of the invention, transition metals nickel and cobalt and, if applicable, manganese can be recovered from cathode materials comprising nickel and cobalt and, if applicable, also manganese in a form in which they can be very easily converted into cathode active material. In particular, the process of the invention allows the recovery of transition metals, such as nickel and cobalt, and optionally manganese, containing only tolerable trace impurities such as copper, iron and zinc, for example with less than 10 ppm of copper (preferably even less, for example 1 to 5 ppm).

[0153] In one embodiment of the invention, the solid Ni-concentrate obtained in step (c) is treated with ammonium carbonate (bicarbonate) in an aqueous solution at a concentration of 0.2 to 30 wt %, preferably 1 to 20 % by weight. The slurry can be heated to a temperature of 30 to 150° C. The heating is carried out under pressure at a temperature above the boiling point of the mixture. Below the boiling point, applying pressure is beneficial to maintain sufficient ammonia and carbon dioxide in the system.

[0154] The treatment with ammonium (bi)carbonate may be carried out under an inert atmosphere or in the presence of oxygen, for example under air. The leach or solution may also contain additional ammonia and / or hydrogen peroxide.

[0155] By the ammonium (bi)carbonate treatment, Ni and, if applicable, Co and Cu will be dissolved as ammonium complexes. The concentration of the metal ammonium complexes in the leachate may be in the range of 0.2 to 30 wt%, preferably 1-15 wt%, calculated as metal. The solution obtained by this treatment is subjected to solid-liquid separation to obtain a solution comprising mainly Ni and, if applicable, Co and Cu ammonium complexes and a separate solid residue comprising mainly other transition metals, if applicable, namely Mn and Fe.

[0156] The solution obtained can be heated, and ammonia can be removed by purging with carbon dioxide.By this first carbonate Ni and through longer processing, advantageously at elevated temperatures, carbonate Co as precipitate will also be obtained.This allows two kinds of metal separation.In one embodiment of the present invention, Ni and Co carbonate are not separated from each other.From mother liquor, separate the mixed Ni / Co carbonate of precipitation and can be dissolved by sulfuric acid or other acids to obtain the solution of corresponding Ni and if applicable Co salt.This solution can also include a small amount of Cu salt, and as mentioned above, these cupric salts can be removed by processing with metal Ni, Co or Mn.Similarly as described above, other impurities such as Fe or Al that can be included in low concentration can be removed by hydroxide or carbonate precipitation under the pH value between 2.5 and 8.

[0157] Ni and Co hydroxides can be co-precipitated from purified Ni and, if applicable, Co salt solutions.

[0158] In one embodiment of the invention, the solution is further processed to extract the Ni and Co salts separately, for example by solvent extraction methods. Pure metals can be recovered from the separated Ni and Co salts via electrochemical methods known in the art.

[0159] The present invention is further illustrated by working examples.

[0160] Metallic impurities and phosphorus were determined by elemental analysis using ICP-OES (Inductively Coupled Plasma-Emission Spectrometry) or ICP-MS (Inductively Coupled Plasma-Mass Spectrometry). After combustion, total carbon was determined using a thermal conductivity detector (CMD). Total fluorine after combustion or fluorine from ionic fluoride after distillation of H3PO4 was detected using an ion sensitive electrode (ISE). The phase composition of the solid was determined using powder x-ray diffraction (PXRD).

[0161] Nl: Normal liters, liters under normal conditions (1atm, 20℃).

[0162] Unless specifically defined otherwise, percentages refer to % by weight. The expressions % by weight and wt% can be used interchangeably. Wherever mentioned, the terms "room temperature" and "ambient temperature" refer to a temperature between about 18 and 25°C.

[0163] Embodiment 1:

[0164] Step (a.1) Heat treatment in the presence of H2

[0165] A quantity of 60 g of mechanically treated battery waste comprising:

[0166] 32.8 g of spent cathode active material containing nickel, cobalt and manganese in similar molar amounts,

[0167] 17.5 g of organic carbon in the form of graphite and soot and residual electrolyte, and

[0168] 9.7 g of additional impurities, including Al (0.6 g), Cu (0.5 g), F (total: 2.2 g), Fe (0.55 g), P (0.3 g), Zn (0.04 g), Zr (0.15 g), Mg (2 mg), Ca (6 mg)

[0169] Placed in a graphite crucible in a tube furnace and heated to 400° C. in 45 minutes under argon flow (20 Nl / h). The temperature was kept constant for 7.5 hours under a flow of 10 wt % hydrogen in argon (22 Nl / h) until the hydrogen flow was stopped and the furnace was cooled to ambient temperature under argon flow. 50.1 g of the heat-treated material was recovered from the crucible, showing XRD signals of Ni / Co alloy, graphite and LiOH.

[0170] Step (b.1) Aqueous treatment of the product obtained in step (a.1)

[0171] 5.5 g of the material obtained in step (a.1) was slurried in 53 mL of deionized water and stirred at ambient temperature for 30 min and then filtered. The clear filtrate was found to contain 133 mg Li +, 212 mg hydroxide anions, 93 mg carbonate ions and 13 mg fluoride ions. This corresponds to a lithium leaching efficiency of 46% where 65% of the lithium is present as LiOH.

[0172] Step (c.1) is used to remove Ni from the solid residue of step (b.1) by solid-solid separation

[0173] The hydrogen-treated material obtained from step (a.1) in an amount of 12 g was slurried in 100 ml of deionized water and dispersed at 800 rpm for 10 minutes with a paddle stirrer assisted by a sonotrode. The slurry was introduced into a laboratory-scale L-series 4-type high-intensity wet magnetic separator from Eriez Magnetics Europe Ltd. Steel wool was placed between the poles of the separator in the tank. The feed slurry was pumped into the matrix within 5 min while the matrix was magnetized to 1 Tesla. The attached solids were rinsed with deionized water until a clear and colorless solution was obtained from the outlet to fully recover the non-magnetic part. After removing the electric field, the magnetic part was removed from the tank by rinsing with deionized water again. The two recovered slurries were filtered and dried in an oven to obtain 9.0 g of a magnetic part and 1.25 g of a non-magnetic part. The non-magnetic part contained 86 wt% of carbon and less than 0.2 wt% of inorganic and organic fluorine. The metal content of Ni, Co and Mn in the magnetic part was 52 wt%.

[0174] Step (d.1): Recovering Li salt from the solution obtained in step (b.1)

[0175] Under reduced pressure, 31.5 g of the clear filtrate obtained in step (b) containing a total amount of 79 mg of lithium ions was concentrated to dryness. The flask was refilled with dry nitrogen and transferred to a glove box filled with argon. 215 mg of solid material was recovered, showing X-ray diffraction signals of mainly LiOH and trace amounts of Li2CO3.

[0176] Step (e.1): Acidic extraction of Ni and Co from the solid Ni-concentrate obtained in step (c.1)

[0177] In a stirred 250 mL batch reactor, 3.0 g of the material obtained as the magnetic part from step (c.1) was suspended in 50 g of deionized water and heated to 40° C. A mixture of 33.4 g H2SO4 (96% H2SO4) in 20.0 g of deionized water was slowly added, followed by a mixture of 3.62 g H2SO4 (96% H2SO4), 1.2 g of aqueous hydrogen peroxide solution (30% H2O2) in 3.47 g of deionized water. Slow gas evolution was observed with only a small amount of foam formation. The resulting slurry was stirred at 60° C. for 3 hours and then cooled to ambient temperature. The resulting mixture was filtered with a glass frit and the solid residue was washed with 62.2 g of deionized water. 111.4 g of a red clear filtrate was recovered, which contained 535 mg Ni, 535 mg Co, 423 mg Mn, corresponding to leaching efficiencies of greater than 95% for each Ni, Co and Mn.

[0178] Alternative step (e.1): Ammonia extraction of Ni and Co from the solid Ni-concentrate obtained in step (c.1)

[0179] In a stirred 250 mL batch reactor, 3.0 g of the material obtained as the magnetic part from step (c.1) was suspended in a mixture of 117 g of 25% aqueous ammonia solution and 20 g of ammonium carbonate and 9 g of deionized water and heated to 60° C. under stirring. 40.1 g of aqueous hydrogen peroxide solution (30% H2O2) was added under stirring over a period of 5 h. The reaction was exothermic with gas evolution. The resulting slurry was stirred at 60° C. for 3 hours and then cooled to ambient temperature. The resulting mixture was filtered with a glass frit and the solid residue was washed with 60.3 g of deionized water. 204.7 g of dark clear combined filtrate was recovered, which contained 534 mg Ni, 520 mg Co, 2 mg Mn, corresponding to leaching efficiencies of 95% and 94% for Ni and Co, respectively, and only 0.5% for Mn. Such ammonia leaching method may be advantageous in cases where Mn may interfere with subsequent separation steps.

[0180] Example 2: Heat treatment in the presence of H2 in step (a.1)

[0181] An amount of 20 g of mechanically treated battery waste comprising 55 wt.-% spent cathode active material comprising nickel, cobalt and manganese in similar molar amounts, 29 wt.-% organic carbon in the form of graphite and soot and residual electrolyte, and 16 wt.-% further impurities including Al (1 wt.-%), Cu (0.8 wt.-%), F (total: 3.7 wt.-%), Fe (0.9 wt.-%), P (0.5 wt.-%), Zn (0.07 wt.-%), Zr (0.3 wt.-%), Mg (<0.01 wt.-%), Ca (0.01 wt.-%) were placed in a rotary furnace and heated to 400, 410, 420, 430, 450, 470, 500° C., respectively, during 45 minutes under a flow of argon (20 Nl / h). At each temperature, the temperature was kept constant for another 45 min under the flow of hydrogen (100%, 20 Nl / h). Afterwards, the flow of hydrogen was stopped and the furnace was cooled to ambient temperature under the flow of argon. The heat-treated material was recovered from the oven, showing XRD signals of Ni / Co alloy, graphite and LiOH. The amount of Li in the heated material was determined after each heating experiment.

[0182] Step (b.1) Aqueous treatment of the product obtained in step (a.1)

[0183] 5 g of the material obtained in step (a.1) was slurried in 50 mL of deionized water and stirred for 30 min at ambient temperature and then filtered. The clear filtrate was found to contain lithium, hydroxide, carbonate and fluoride in the concentrations listed below (Table 1).

[0184] Table 1 : Experimental conditions during thermal treatment under H2 and analysis of the leaching filtrate.

[0185]

[0186] Similar to Example 1, steps (c1), (d1) and (e1) were carried out.

[0187] Example 3: Heat treatment in the presence of H2 in step (a.1)

[0188] An amount of 20 g of mechanically treated battery waste comprising 55 wt.-% of spent cathode active material comprising nickel, cobalt and manganese in similar molar amounts, 29 wt.-% of organic carbon in the form of graphite and soot and residual electrolyte, and 16 wt.-% of further impurities, including Al (1 wt.-%), Cu (0.8 wt.-%), F (in total: 3.7 wt.-%), Fe (0.9 wt.-%), P (0.5 wt.-%), Zn (0.07 wt.-%), Zr (0.3 wt.-%), Mg (<0.01 wt.-%), Ca (0.01 wt.-%) were placed in a rotary furnace and heated to 400° C. under a flow of argon (20 Nl / h) during 45 minutes. As shown in Table 2, the temperature was kept constant for 15, 30, 45, 60, 150 or 450 min under the flow of hydrogen (100%, 20 Nl / h). Afterwards, the flow of hydrogen was stopped and the furnace was cooled to ambient temperature under the flow of argon. The heat-treated material was recovered from the oven, showing XRD signals of Ni / Co alloy, graphite and LiOH. The amount of Li in the heated material was determined after each heating experiment.

[0189] Step (b.1) Aqueous treatment of the product obtained in step (a.1)

[0190] 5 g of the material obtained in step (a.1) was slurried in 50 mL of deionized water and stirred for 30 min at ambient temperature and then filtered. The clear filtrate was found to contain lithium, hydroxide, carbonate and fluoride in the concentrations listed below (Table 2).

[0191] Table 2 : Heating duration under H2 atmosphere and analysis of the leaching filtrate.

[0192]

[0193] Similar to Example 1, steps (c1), (d1) and (e1) were carried out.

[0194] Embodiment 4:

[0195] Step (a.3) Solvent treatment before heat treatment

[0196] An amount of 750 g of mechanically treated battery waste containing: 55 wt.-% of spent cathode active material containing nickel, cobalt and manganese in similar molar amounts, 29 wt.-% of organic carbon in the form of graphite and soot and residual electrolyte, and 16 wt.-% of additional impurities including Al (1 wt.-%), Cu (0.8 wt.-%), F (total: 3.7 wt.-%), Fe (0.9 wt.-%), P (0.5 wt.-%), Zn (0.07 wt.-%), Zr (0.3 wt.-%), Mg (<0.01 wt.-%), Ca (0.01 wt.-%) were mixed with 2.5 L of water, stirred at ambient temperature for 60 min, and then filtered.

[0197] Step (a.1) Heat treatment in the presence of H2

[0198] The material obtained in step (a.3) in an amount of 20 g is placed in a rotary furnace and heated to 400° C. in a flow of argon (20 Nl / h) over the course of 45 minutes. The temperature is kept constant for several hours under a flow of a hydrogen / argon mixture (20 Nl / h); the hydrogen concentration is 3, 5, 7, 10, 14, 25, 35 or 100 vol-%, respectively, as shown in Table 3 below. Afterwards, the flow of hydrogen is stopped and the furnace is cooled to ambient temperature under a flow of argon. The heat-treated material is recovered from the oven, showing XRD signals of Ni / Co alloy, graphite and LiOH. The amount of Li in the heated material is determined after each heating experiment.

[0199] Step (b.1) Aqueous treatment of the product obtained in step (a.1)

[0200] 5 g of the material obtained in step (a.1) was slurried in 50 mL of deionized water and stirred for 30 min at ambient temperature and then filtered. The clear filtrate was found to contain lithium, hydroxide, carbonate and fluoride in the concentrations listed below (Table 3).

[0201] Table 3 : H2 concentration during heating and analysis of the leaching filtrate.

[0202]

[0203] Similar to Example 1, steps (c1), (d1) and (e1) were carried out.

Claims

1. A method for recovering transition metals from spent lithium-ion batteries containing nickel, wherein: The method comprises the following steps: (a) heating a lithium-containing transition metal oxide material to a temperature in the range of 200 to 900° C. in the presence of H 2 , said material originating from a lithium ion battery and containing a fluorine compound and / or a phosphorus compound as an impurity, (b) treating the product obtained in step (a) with an aqueous medium, (c) solid-solid separation for removing Ni from the solid residue of step (b), (d) recovering Li as hydroxide or salt from the solution obtained in step (b), and (e) extracting Ni and optionally Co from the solid Ni-concentrate obtained in step (c), wherein the lithium-containing transition metal oxide material used in step (a) is obtained after mechanical removal of a casing, wiring or circuit from a lithium-ion battery and discharge, and wherein the material is not exposed to a temperature of 400° C. or more under oxidative conditions before subjecting the material to this step (a).

2. The method according to claim 1, wherein: The heating temperature in step (a) is in the range of 350 to 500°C.

3. The method according to claim 2, wherein: 35% by volume or more of hydrogen is present in step (a), and the heating temperature in step (a) is in the range of 350 to 450°C.

4. The method according to claim 1, wherein: Step (e) includes one or more of the following: - smelting the solid Ni-concentrate obtained in step (c); - treating the solid Ni-concentrate obtained in step (c) with an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid, citric acid or a combination of at least two thereof; - treating the Ni-concentrate obtained in step (c) with ammonium (bi)carbonate.

5. The method according to claim 2, wherein: Step (e) includes one or more of the following: - smelting the solid Ni-concentrate obtained in step (c); - treating the solid Ni-concentrate obtained in step (c) with an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid, citric acid or a combination of at least two thereof; - treating the Ni-concentrate obtained in step (c) with ammonium (bi)carbonate.

6. The method according to claim 3, wherein: Step (e) includes one or more of the following: - smelting the solid Ni-concentrate obtained in step (c); - treating the solid Ni-concentrate obtained in step (c) with an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid, citric acid or a combination of at least two thereof; - treating the Ni-concentrate obtained in step (c) with ammonium (bi)carbonate.

7. The method according to claim 1, wherein: Step (e) comprises treating the Ni-concentrate obtained in step (c) with a base.

8. The method according to claim 2, wherein: Step (e) comprises treating the Ni-concentrate obtained in step (c) with a base.

9. The method according to claim 3, wherein: Step (e) comprises treating the Ni-concentrate obtained in step (c) with a base.

10. The method according to claim 7, wherein: The base is ammonia, an amine, an aqueous solution of ammonia, ammonium carbonate, or a mixture of ammonia and carbon dioxide.

11. The method according to any one of claims 4 to 9, wherein: The solution containing Ni and optionally Co salts is treated with ammonia or an alkali metal hydroxide to obtain a solution having a pH in the range of 2.5 to 8.

12. The method according to any one of claims 4 to 9, wherein: The solution containing Ni and optionally Co salts is treated with metallic nickel, metallic cobalt, metallic manganese or any combination of at least two thereof.

13. The method according to any one of claims 1 to 10, wherein: Prior to step (b), carbon or organic polymers are removed by a dry solid-solid separation method.

14. The method according to claim 11, wherein: Prior to step (b), carbon or organic polymers are removed by a dry solid-solid separation method.

15. The method according to claim 12, wherein: Prior to step (b), carbon or organic polymers are removed by a dry solid-solid separation method.

16. The method according to any one of claims 1 to 10, comprising wherein: In step (d), the lithium is recovered as lithium hydroxide.

17. The method according to any one of claims 1 to 10, comprising wherein: In step (d), the lithium is recovered as carbonate by means of precipitation.

18. A process according to any one of claims 1 to 10, comprising an additional step (f), wherein step (f) comprises precipitating the nickel and optionally cobalt and / or manganese as hydroxides, oxyhydroxides or carbonates.

19. A process according to claim 18, wherein nickel and optionally cobalt and / or manganese are precipitated as hydroxides, oxyhydroxides or carbonates by raising the pH to a value greater than 8.

20. The method of claim 18, wherein step (f) is performed by adding at least one reagent selected from the group consisting of lithium hydroxide, sodium hydroxide, ammonia and potassium hydroxide.

21. The method according to any one of claims 1 to 10, wherein: Step (a) is carried out in the presence of steam.

22. The method according to any one of claims 1 to 10, wherein: Step (a) is carried out in the presence of lime, quartz, silicon dioxide or a silicate.

23. The method according to any one of claims 1 to 10, comprising an additional step before step (a), wherein the additional step comprises contacting the material from the spent lithium ion battery with water and / or an organic solvent, followed by a solid-liquid separation step.

24. A method for recovering transition metals from spent lithium-ion batteries containing nickel, wherein: The method comprises the following steps: (a) heating a lithium-containing transition metal oxide material to a temperature in the range of 200 to 900° C. in the presence of H 2 , (b) treating the product obtained in step (a) with an aqueous medium, (c) solid-solid separation for removing Ni from the solid residue of step (b), (d) recovering Li as hydroxide or salt from the solution obtained in step (b), and (e) extracting Ni and optionally Co from the solid Ni-concentrate obtained in step (c), wherein the lithium-containing transition metal oxide material heated in step (a) originates from a lithium-ion battery and contains fluorine in the range of 2 to 8% by weight and / or phosphorus in the range of 0.2 to 2% by weight, relative to the weight of the lithium-containing transition metal oxide material, wherein the lithium-containing transition metal oxide material used in step (a) is obtained after mechanical removal of the casing, wiring or circuitry from a lithium-ion battery and discharge, and wherein the material is not exposed to a temperature of 400° C. or higher under oxidative conditions before subjecting the material to this step (a).

25. The method according to claim 24, wherein: The heating temperature in step (a) is in the range of 350 to 500°C.

26. The method according to claim 25, wherein: 35% by volume or more of hydrogen is present in step (a), and the heating temperature in step (a) is in the range of 350 to 450°C.

27. The method according to claim 24, wherein: Step (e) includes one or more of the following: - smelting the solid Ni-concentrate obtained in step (c); - treating the solid Ni-concentrate obtained in step (c) with an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid, citric acid or a combination of at least two thereof; - treating the Ni-concentrate obtained in step (c) with ammonium (bi)carbonate.

28. The method according to claim 25, wherein: Step (e) includes one or more of the following: - smelting the solid Ni-concentrate obtained in step (c); - treating the solid Ni-concentrate obtained in step (c) with an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid, citric acid or a combination of at least two thereof; - treating the Ni-concentrate obtained in step (c) with ammonium (bi)carbonate.

29. The method according to claim 26, wherein: Step (e) includes one or more of the following: - smelting the solid Ni-concentrate obtained in step (c); - treating the solid Ni-concentrate obtained in step (c) with an acid selected from the group consisting of sulfuric acid, hydrochloric acid, nitric acid, methanesulfonic acid, oxalic acid, citric acid or a combination of at least two thereof; - treating the Ni-concentrate obtained in step (c) with ammonium (bi)carbonate.

30. The method of claim 24, wherein: Step (e) comprises treating the Ni-concentrate obtained in step (c) with a base.

31. The method of claim 25, wherein: Step (e) comprises treating the Ni-concentrate obtained in step (c) with a base.

32. The method of claim 26, wherein: Step (e) comprises treating the Ni-concentrate obtained in step (c) with a base.

33. The method of claim 30, wherein: The base is ammonia, an amine, an aqueous solution of ammonia, ammonium carbonate, or a mixture of ammonia and carbon dioxide.

34. The method according to any one of claims 27 to 32, wherein: The solution containing Ni and optionally Co salts is treated with ammonia or an alkali metal hydroxide to obtain a solution having a pH in the range of 2.5 to 8.

35. The method according to any one of claims 27 to 32, wherein: The solution containing Ni and optionally Co salts is treated with metallic nickel, metallic cobalt, metallic manganese or any combination of at least two thereof.

36. The method of claim 33, wherein: The solution containing Ni and optionally Co salts is treated with metallic nickel, metallic cobalt, metallic manganese or any combination of at least two thereof.

37. The method of claim 34, wherein: The solution containing Ni and optionally Co salts is treated with metallic nickel, metallic cobalt, metallic manganese or any combination of at least two thereof.

38. The method according to any one of claims 24 to 32, wherein: Prior to step (b), carbon or organic polymers are removed by a dry solid-solid separation method.

39. The method of claim 33, wherein: Prior to step (b), carbon or organic polymers are removed by a dry solid-solid separation method.

40. The method of claim 34, wherein: Prior to step (b), carbon or organic polymers are removed by a dry solid-solid separation method.

41. A method according to any one of claims 24 to 32, comprising wherein: In step (d), the lithium is recovered as lithium hydroxide.

42. A method according to any one of claims 24 to 32, comprising wherein: In step (d), the lithium is recovered as carbonate by means of precipitation.

43. A process according to any one of claims 24 to 32 comprising the additional step (f), wherein step (f) comprises precipitating the nickel and optionally cobalt and / or manganese as hydroxides, oxyhydroxides or carbonates.

44. A process according to claim 43 wherein nickel and optionally cobalt and / or manganese are precipitated as hydroxides, oxyhydroxides or carbonates by raising the pH to greater than 8.

45. The method of claim 43, wherein step (f) is performed by adding at least one reagent selected from the group consisting of lithium hydroxide, sodium hydroxide, ammonia and potassium hydroxide.

46. ​​A method according to any one of claims 24 to 32, wherein: Step (a) is carried out in the presence of steam.

47. A method according to any one of claims 24 to 32, wherein: Step (a) is carried out in the presence of lime, quartz, silicon dioxide or a silicate.

48. A method according to any one of claims 24 to 32, comprising an additional step before step (a), wherein the additional step comprises contacting the material from the spent lithium ion battery with water and / or an organic solvent, followed by a solid-liquid separation step.