Low temperature, high quality dielectric film

By using precursor-containing gas mixtures and RF bias technology to deposit dielectric films, the need for low resistivity and low dielectric constant materials in integrated circuit manufacturing is addressed, achieving high density and high refractive index. dielectric film deposition that meets stringent thermal budgets and high-density requirements.

CN112437971BActive Publication Date: 2024-10-11APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980047986.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-07-19
Filing Date
2019-07-15
Publication Date
2024-10-11
Estimated Expiration
2039-07-15

AI Technical Summary

Technical Problem

In integrated circuit manufacturing, as integrated circuit component sizes decrease, low resistivity conductive materials and low dielectric constant insulating materials are required to obtain suitable electrical properties, while pattern size decreases result in the thickness of energy-sensitive resists must be reduced, and many applications in industry have very low thermal budgets, making it difficult to deposit high-quality dielectric films to meet stringent thermal budgets and high-density requirements.

Method used

By forming a film on a substrate, a gas mixture containing a precursor is flowed in a processing chamber positioned on an electrostatic chuck, an RF bias is applied to generate a plasma, and a dielectric film is deposited, the dielectric film having a thickness of 1.5 to 3 refractive index and are deposited under low temperature conditions (approximately -50°C to 150°C) and low pressure conditions (0.1mTorr to 10Torr).

Benefits of technology

It achieves the deposition of high-density, high-refractive-index dielectric films at low temperature and low pressure, with high etch selectivity and low stress. It is suitable for patterning and other applications with strict thermal budgets, and the process is compatible with existing integration solutions. Allow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112437971B_ABST
    Figure CN112437971B_ABST
Patent Text Reader

Abstract

A technique for depositing a high density dielectric film for patterning applications is described. More specifically, a method for processing a substrate is provided. The method includes flowing a gas mixture containing a precursor into a processing volume of a processing chamber having a substrate positioned on an electrostatic chuck. The substrate is maintained at a pressure between about 0.1 mTorr and about 10 Torr. A dielectric film is deposited on the substrate by applying a first RF bias to the electrostatic chuck to generate a plasma at the level of the substrate. The dielectric film has a refractive index in the range of about 1.5 to about 3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present disclosure relate to the field of electronic component manufacturing, and in particular, to integrated circuit (IC) manufacturing. More particularly, embodiments of the present disclosure provide methods of depositing dielectric films that can be used for patterning applications. Background Art

[0002] Integrated circuits have evolved into complex components that may include millions of transistors, capacitors, and resistors on a single wafer. Advances in wafer design continue to require faster circuitry and greater circuit density. The demand for faster circuits with greater circuit density places corresponding demands on the materials used to manufacture such integrated circuits. Specifically, as the size of integrated circuit components decreases, low resistivity conductive materials and low dielectric constant insulating materials must be used to obtain suitable electrical properties from such components.

[0003] The demand for greater integrated circuit density also places demands on the process sequences used in manufacturing integrated circuit components. For example, in a process sequence using conventional photolithography, an energy-sensitive resist layer is formed over a stack of material layers disposed on a substrate. The energy-sensitive resist layer is exposed to a pattern image to form a photoresist mask. Thereafter, an etching process is used to transfer the mask pattern to one or more material layers of the stack. The chemical etchant used in the etching process is selected to have a greater etching selectivity to the material layers of the stack than the mask of the energy-sensitive resist. That is, the chemical etchant etches one or more layers of the material stack at a much faster rate than the energy-sensitive resist. The etching selectivity of the resist to the one or more material layers of the stack prevents the energy-sensitive resist from being consumed before the pattern transfer is completed.

[0004] As pattern size decreases, the thickness of the energy sensitive resist must be correspondingly reduced in order to control pattern resolution. Many new applications in the industry have very low thermal budgets, below 400°C (e.g., cross-point memory flows). Therefore, there is a need to deposit high quality dielectric films for patterning and other applications that meet this stringent thermal budget without sacrificing film quality. Summary of the invention

[0005] Apparatus and methods for manufacturing integrated circuits are described. In one or more embodiments, a method of forming a film on a substrate is described. In one embodiment, a film is formed on a substrate by flowing a gas mixture containing a precursor into a processing volume of a processing chamber having a substrate positioned on an electrostatic chuck. The substrate is maintained at a pressure in a range of about 0.1 mTorr and about 10 Torr and at a temperature in a range of about -50°C to about 150°C. A dielectric film is deposited on the substrate by applying a first RF bias to the electrostatic chuck to generate a plasma at the level of the substrate, the dielectric film having a refractive index in a range of about 1.5 to about 3.

[0006] In one or more embodiments, a method of forming a film on a substrate is described. In one embodiment, the film is formed on the substrate by flowing a gas mixture containing a precursor into a processing volume of a processing chamber having the substrate positioned on an electrostatic chuck, wherein the gas mixture containing the precursor comprises one or more precursors selected from the group consisting of silane (SiH4), triethoxysilane (SiH(OEt)3), tetraethoxysilane (tetraethyl orthosilicate; Si(OEt)4 or TEOS), disilane (Si2H6), SiH(CH3)3, dimethylsilane (SiH2(CH3)2), methylsilane (SiH3CH3), dichlorosilane (SiH2Cl2), silicon tetrachloride (SiCl4), silicon tetrafluoride (SiF4), trichlorosilane (HSiCl3), methylsilane (CH3SiH3), trimethylsilane (C3H 10 Si), 1,1,3,3-tetramethyldisiloxane (TMDZ), 1,3,5-trisilapentane (TSP), (bis(tert-butylamino)silane (BTBAS), (bis(diethylamino)silane (BDEAS), tris(dimethylamino)silane (TDMAS), (Si[N(tBu)CH=CHN(tBu)](OEt)2(Si-TBES), Si[N(tBu)CH=CHN(tBu)](H)NH2(Si-TBAS), germane The method comprises the steps of: applying a first RF bias and a second RF bias to an electrostatic chuck to generate a plasma at a substrate level, and depositing a dielectric film on the substrate, the dielectric film having a refractive index in a range of about 1.5 to about 3.

[0007] In one or more embodiments, a method of forming a film on a substrate is described. In one embodiment, a film is formed on a substrate by flowing a gas mixture containing a precursor into a processing volume of a processing chamber having a substrate positioned on an electrostatic chuck. The processing volume is maintained at a pressure in the range of about 0.1 mTorr to about 10 Torr. A dielectric film is deposited on the substrate by applying a first RF bias and a second RF bias to the electrostatic chuck to generate a plasma at the level of the substrate, the dielectric film having a refractive index in the range of about 1.5 to about 3. A patterned photoresist layer is formed on the dielectric film. The dielectric film is etched in a pattern corresponding to the patterned photoresist layer. The pattern is etched into the substrate. Material is deposited into the etched portion of the dielectric film. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] In order to be able to understand in detail the manner in which the above-mentioned features of the present disclosure are used, a more specific description of the present disclosure briefly summarized above may be made with reference to embodiments, some of which are shown in the accompanying drawings. However, it should be noted that the accompanying drawings only illustrate typical embodiments of the present disclosure and are not to be considered as limiting the scope thereof, as the present disclosure may allow for other equally effective embodiments. The embodiments as described herein are shown by way of example and are not limited to the figures of the accompanying drawings, in which the same references indicate similar elements.

[0009] Figure 1A shows a schematic cross-sectional view of a deposition system that can be used to practice the embodiments described herein;

[0010] Figure 1B depicts a schematic cross-sectional view of another deposition system that may be used to practice embodiments described herein;

[0011] Figure 2 Describes the Figure 1A and Figure 1B A schematic cross-sectional view of an electrostatic chuck in an apparatus for practicing embodiments described herein;

[0012] Figure 3 A flow chart depicting a method for forming a dielectric film on a substrate according to one or more embodiments; and

[0013] FIG. 4A to FIG. 4B One embodiment of a sequence for forming a dielectric film on a film stack formed on a substrate in accordance with one or more embodiments is depicted. DETAILED DESCRIPTION

[0014] Before describing several exemplary embodiments of the present disclosure, it will be understood that the present disclosure is not limited to the details of construction or process steps set forth in the following description. The present disclosure is capable of other embodiments and of being practiced or carried out in various ways.

[0015] The numerous details, dimensions, angles and other features illustrated in the figures illustrate only specific embodiments. Thus, other embodiments may have other details, components, dimensions, angles and features without departing from the spirit or scope of the present disclosure. In addition, other embodiments of the present disclosure may be practiced without some of the details described below.

[0016] As used herein, "substrate", "substrate surface", etc. refer to any substrate or material surface formed on a substrate on which processing is performed. For example, depending on the application, the substrate surface on which processing can be performed includes, but is not limited to, materials such as silicon, silicon oxide, strained silicon, silicon on insulator (SOI), carbon-doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other materials such as metals, metal nitrides, metal alloys and other conductive materials. Substrates include, but are not limited to, semiconductor wafers. The substrate may be exposed to a pretreatment process to polish, etch, reduce, oxidize, hydroxylate (or otherwise generate or graft a target chemical moiety to impart chemical functionality), anneal, and / or bake the substrate surface. In addition to processing directly on the surface of the substrate itself, in the present disclosure, as disclosed in more detail below, any film processing step disclosed may also be performed on an underlying layer formed on the substrate, and the term "substrate surface" is intended to include such an underlying layer as indicated by the context. Thus, for example, in the case where a film / layer or a portion of a film / layer has been deposited onto a substrate surface, the exposed surface of the newly deposited film / layer becomes the substrate surface. The materials contained on a given substrate surface will depend on the materials being deposited, as well as the specific chemistry used.

[0017] As used in this specification and the appended claims, the terms "reactive compound," "reactive gas," "reactive substance," "precursor," "process gas," and the like are used interchangeably to mean a substance having a species capable of reacting with a substrate surface or a material on a substrate surface in a surface reaction (e.g., chemisorption, oxidation, reduction). For example, a first "reactive gas" may simply adsorb onto a substrate surface and be available for further chemical reaction with a second reactive gas.

[0018] As used in this specification and the appended claims, the terms "precursor," "reactant," "reactive gas," and the like are used interchangeably to refer to any gas species that can react with a substrate surface.

[0019] As used herein, "chemical vapor deposition" refers to a process that exposes a substrate surface to precursors and / or co-reactants simultaneously or substantially simultaneously. As used herein, "substantially simultaneously" refers to co-flow or overlap of the majority of the exposures to the precursors.

[0020] Plasma enhanced chemical vapor deposition (PECVD) is widely used to deposit films due to cost efficiency and film quality versatility. In the PECVD process, a hydrocarbon source (such as vapor of a gaseous or liquid hydrocarbon) already carried in a carrier gas is introduced into the PECVD chamber. A plasma-induced gas (usually helium) is also introduced into the chamber. The plasma is then induced in the chamber to produce excited CH radicals. The excited CH radicals chemically bond to the surface of a substrate positioned in the chamber, thereby forming a desired amorphous carbon film thereon. The embodiments described herein with reference to the PECVD process can be performed using any suitable thin film deposition system. Any device description described herein is illustrative and should not be understood or interpreted as limiting the scope of the embodiments described herein.

[0021] Numerous applications in the semiconductor industry have very low thermal budgets of less than 400° C., and even in some cases less than 300° C. Typically, in PECVD processes, film quality suffers drastically at low temperatures. The embodiments described herein advantageously provide methods for depositing high quality dielectric films for patterning and other applications that meet this stringent thermal budget without sacrificing film quality.

[0022] Embodiments described herein include improved methods of manufacturing dielectric films having high density (e.g., >1.8 g / cc), high refractive index (e.g., >1.5), and low stress (e.g., <-500 MPa). In one or more embodiments, the density and stress depend on the specific film being manufactured, but the films of one or more embodiments have similar or improved density and stress when compared to films manufactured at very high temperatures. The dielectric films manufactured according to the embodiments described herein are amorphous in nature and have higher etch selectivity, as well as very large density (e.g., >1.8 g / cc) and lower stress (<-500 MPa) compared to existing patterned films. In general, the deposition processes described herein are also fully compatible with existing integration schemes for hard mask applications.

[0023] In some embodiments, the dielectric films described herein can be formed by a chemical vapor deposition (plasma enhanced and / or thermal) process using a precursor-containing gas mixture, wherein the precursor-containing gas mixture includes one or more precursors selected from the group consisting of silane (SiH4), triethoxysilane (SiH(OEt)3), tetraethoxysilane (tetraethyl orthosilicate; Si(OEt)4 or TEOS), disilane (Si2H6), SiH(CH3)3, dimethylsilane (SiH2(CH3)2), methylsilane (SiH3CH3), dichlorosilane (SiH2Cl2), silicon tetrachloride (SiCl4), silicon tetrafluoride (SiF4), trichlorosilane (HSiCl3), methylsilane (CH3SiH3), trimethylsilane (C3H 10Si), 1,1,3,3-tetramethyldisiloxane (TMDZ), 1,3,5-trisilopentane (TSP), (bis(tert-butylamino)silane (BTBAS), (bis(diethylamino)silane (BDEAS), tris(dimethylamino)silane (TDMAS), (Si[N(tBu)CH=CHN(tBu)](OEt)2(Si-TBES), Si[N(tBu)CH=CHN(tBu)](H)NH2(Si-TBAS), germane (GeH4), germanium tetrachloride (GeCl4), germanium tetrafluoride (GeF4), tert-butylgermane (GeH(CH3)3), N2O, O2, NH3, N2, H2, C2H2, or C3H6.

[0024] The deposition process may be performed at a temperature ranging from about -50°C to about 150°C, including about -50°C, about -45°C, about -40°C, about -35°C, about -30°C, about -25°C, about -20°C, about -15°C, about -10°C, about -5°C, about 0°C, about 5°C, about 10°C, about 15°C, about 20°C, about 25°C, about 30°C, about 35°C, about 40°C, about 45°C, about 50°C, about 55°C, about 60°C, about 65°C, about 70°C, about 75°C, about 80°C, about 85°C, about 90°C, about 95°C, about 100°C, about 105°C, about 110°C, about 115°C, about 120°C, about 125°C, about 130°C, about 135°C, about 140°C, about 145°C, and about 150°C.

[0025] The deposition process may be performed in the process volume at pressures varying from 0.1 mTorr to 10 Torr, including pressures of about 0.1 mTorr, about 1 mTorr, about 10 mTorr, about 100 mTorr, about 500 mTorr, about 1 Torr, about 2 Torr, about 3 Torr, about 4 Torr, about 5 Torr, about 6 Torr, about 7 Torr, about 8 Torr, about 9 Torr, and about 10 Torr.

[0026] The precursor-containing gas mixture may further include one or more diluent gases selected from the group consisting of helium (He), argon (Ar), xenon (Xe), nitrogen (N2), or hydrogen (H2). The diluent gas of some embodiments includes a compound that is an inert gas relative to the reactants and substrate materials.

[0027] The gas mixture containing the precursor may further include an etchant gas such as Cl2, CF4 or NF3 for improving the film quality.

[0028] Plasma (e.g., capacitively coupled plasma) can be formed from top and bottom electrodes or side electrodes. The electrodes can be formed from a single powered electrode, dual powered electrodes, or more electrodes with multiple frequencies (such as but not limited to 350 KHz, 2 MHz, 13.56 MHz, 27 MHz, 40 MHz, 60 MHz, and 100 MHz) used alternately or simultaneously in a CVD system with any or all of the reactant gases listed herein to deposit dielectric films. In some embodiments, the plasma is a capacitively coupled plasma (CCP). In some embodiments, the plasma is an inductively coupled plasma (ICP). In some embodiments, the plasma is a microwave plasma.

[0029] In some embodiments, dielectric films are deposited in a chamber with a substrate pedestal maintained at 10° C. and a pressure maintained at 2 mTorr, where plasma is generated at wafer level (i.e., direct plasma) by applying a bias of 2500 Watts (13.56 MHz) to an electrostatic chuck. In some embodiments, an additional RF power of 1000 Watts at 2 MHz is also delivered to the electrostatic chuck, thereby generating a dual bias plasma at wafer level.

[0030] Figure 1A A schematic illustration of a substrate processing system 132 that can be used to perform dielectric film deposition according to embodiments described herein is depicted. The substrate processing system 132 includes a process chamber 100 coupled to a gas panel 130 and a controller 110. The process chamber 100 generally includes a top wall 124, a side wall 101, and a bottom wall 122 that define a processing volume 126. A substrate support assembly 146 is provided in the processing volume 126 of the process chamber 100. The substrate support assembly 146 generally includes an electrostatic chuck 150 supported by a rod 160. The electrostatic chuck 150 can be generally made of aluminum, ceramic, or other suitable materials. The electrostatic chuck 150 can be moved in a vertical direction inside the process chamber 100 using a shift mechanism (not shown).

[0031] The vacuum pump 102 is coupled to a port formed in the bottom of the process chamber 100. The vacuum pump 102 is used to maintain a desired gas pressure in the process chamber 100. The vacuum pump 102 also evacuates post-process gases and process byproducts from the process chamber 100.

[0032] The substrate processing system 132 may further include additional equipment for controlling chamber pressure, such as valves (eg, throttle valves and isolation valves) positioned between the process chamber 100 and the vacuum pump 102 to control the chamber pressure.

[0033] A gas distribution assembly 120 having a plurality of holes 128 is disposed on top of the process chamber 100 above the electrostatic chuck 150. The holes 128 of the gas distribution assembly 120 are used to introduce process gases into the process chamber 100. The holes 128 may have different sizes, numbers, distributions, shapes, designs, and diameters to facilitate the flow of various process gases for different process requirements. The gas distribution assembly 120 is connected to a gas panel 130 that allows the various gases to be supplied to the processing volume 126 during processing. A plasma is formed from the process gas mixture exiting the gas distribution assembly 120 to enhance thermal decomposition of the process gases, thereby causing material to be deposited on a surface 191 of the substrate 190.

[0034] The gas distribution assembly 120 and the electrostatic chuck 150 may form a pair of spaced apart electrodes in the processing volume 126. One or more RF power supplies 140 provide a bias potential to the gas distribution assembly 120 via an optional matching network 138 to facilitate the generation of a plasma between the gas distribution assembly 120 and the electrostatic chuck 150. Alternatively, the RF power supply 140 and the optional matching network 138 may be coupled to the gas distribution assembly 120, the electrostatic chuck 150, or to both the gas distribution assembly 120 and the electrostatic chuck 150, or to an antenna (not shown) disposed external to the process chamber 100. In some embodiments, the RF power supply 140 may generate power at a frequency of 350 KHz, 2 MHz, 13.56 MHz, 27 MHz, 40 MHz, 60 MHz, or 100 MHz. In one embodiment, the RF power supply 140 may provide between about 100 watts and about 3000 watts at a frequency of about 50 kHz to about 13.56 MHz. In another embodiment, the RF power 140 may be provided at between about 500 Watts and about 1800 Watts at a frequency of about 50 kHz to about 13.56 MHz.

[0035] The controller 110 includes a central processing unit (CPU) 112, a memory 116, and support circuits 114 for controlling the process sequence and regulating the gas flow from the gas panel 130. The central processing unit (CPU) 112 can be any form of general-purpose computer processor that can be used in an industrial environment. Software routines can be stored in the memory 116, such as a random access memory, read-only memory, a floppy disk, or a hard disk drive, or other form of digital storage. The support circuits 114 are conventionally coupled to the central processing unit (CPU) 112 and may include caches, clock circuits, input / output systems, power supplies, etc. Bidirectional communication between the controller 110 and the various components of the substrate processing system 132 is handled via a number of signal cables, collectively referred to as a signal bus 118, some of which are in Figure 1A Shown in.

[0036] Figure 1B A schematic cross-sectional view of another substrate processing system 180 that can be used to practice the embodiments described herein is depicted. The substrate processing system 180 is similar to Figure 1A The substrate processing system 132 is different in that the substrate processing system 180 is configured to flow the processing gas from the gas panel 130 across the surface 191 of the substrate 190 through the sidewall 101. Figure 1A The gas distribution assembly 120 depicted in FIG. 1 is replaced with an electrode 182. The electrode 182 can be configured for secondary electron generation. In one embodiment, the electrode 182 is a silicon-containing electrode.

[0037] Figure 2 Depicted are embodiments that can be used to practice the embodiments described herein. Figure 1A and Figure 1B Schematic cross-sectional view of a substrate support assembly 146 used in a processing system of FIG. Figure 2 , the electrostatic chuck 150 may include an embedded heater element 170 adapted to control the temperature of a substrate 190 supported on an upper surface 192 of the electrostatic chuck 150. The electrostatic chuck 150 may be resistively heated by applying an electric current from a heater power supply 106 to the heater element 170. The heater power supply 106 may be coupled via an RF filter 216. The RF filter 216 may be used to protect the heater power supply 106 from RF energy. The heater element 170 may be made of a nickel-iron-chromium alloy (e.g., ) sheath. The current supplied from the heater power supply 106 is regulated by the controller 110 to control the heat generated by the heater element 170, thereby maintaining the substrate 190 and the electrostatic chuck 150 at a substantially constant temperature during film deposition. The supplied current can be adjusted to selectively control the temperature of the electrostatic chuck 150 between about -50°C and about 150°C.

[0038] See also Figure 1A and Figure 1B A temperature sensor 172, such as a thermocouple, may be embedded in the electrostatic chuck 150 to monitor the temperature of the electrostatic chuck 150 in a conventional manner. The measured temperature is used by the controller 110 to control the power supplied to the heater element 170 to maintain the substrate at a desired temperature.

[0039] See also Figure 2 The electrostatic chuck 150 includes a chucking electrode 210, which may be a mesh of conductive material. The chucking electrode 210 may be embedded in the electrostatic chuck 150. The chucking electrode 210 is coupled to a chucking power source 212, which, when energized, electrostatically chucking the substrate 190 to the upper surface 192 of the electrostatic chuck 150.

[0040] The chuck electrode 210 may be configured as a monopolar electrode or a bipolar electrode, or have another suitable arrangement. The chuck electrode 210 may be coupled to a chuck power supply 212 via an RF filter 214, which provides direct current (DC) power to electrostatically fix the substrate 190 to the upper surface 192 of the electrostatic chuck 150. The RF filter 214 prevents the RF power used to form the plasma in the process chamber 100 from damaging electrical equipment or presenting an electrical hazard outside the chamber. The electrostatic chuck 150 may be made of a ceramic material, such as AlN or Al2O3. Alternatively, the electrostatic chuck 150 may be made of a polymer, such as polyimide, polyetheretherketone (PEEK), polyaryletherketone (PAEK), etc.

[0041] The power application system 220 is coupled to the substrate support assembly 146. The power application system 220 may include the heater power supply 106, the clamping power supply 212, the first radio frequency (RF) power supply 230, and the second RF power supply 240. Embodiments of the power application system 220 may additionally include the controller 110, and a sensor device 250 in communication with both the controller 110 and the first and second RF power supplies 230, 240.

[0042] The controller 110 may also be used to control plasma from the process gas by applying RF power from a first radio frequency (RF) power source 230 and a second RF power source 240 to deposit a material layer on the substrate 190 .

[0043] As described above, the electrostatic chuck 150 includes a clamping electrode 210, which can be used to clamp the substrate 190 in one aspect and also serves as a first RF electrode. The electrostatic chuck 150 may also include a second RF electrode 260, and together with the clamping electrode 210, RF power can be applied to tune the plasma. A first radio frequency (RF) power source 230 can be coupled to the second RF electrode 260, and a second RF power source 240 can be coupled to the clamping electrode 210. A first matching network and a second matching network for the first radio frequency (RF) power source 230 and the second RF power source 240, respectively, can be provided. The second RF electrode 260 can be a solid metal plate of a conductive material as shown in the figure. Alternatively, the second RF electrode 260 can be a mesh of a conductive material.

[0044] The first RF power source 230 and the second RF power source 240 may generate power at the same frequency or at different frequencies. In some embodiments, one or both of the first RF power source 230 and the second RF power source 240 may independently generate power at a frequency in the range of about 350 KHz to about 100 MHz (including but not limited to 350 KHz, 2 MHz, 13.56 MHz, 27 MHz, 40 MHz, 60 MHz, or 100 MHz). In some embodiments, the first RF power source 230 may generate power at a frequency of 13.56 MHz and the second RF power source 240 may generate power at a frequency of 2 MHz, or vice versa. The RF power from one or both of the first RF power source 230 and the second RF power source 240 may be changed to tune the plasma. For example, the sensor device 250 may be used to monitor the RF energy from one or both of the first RF power source 230 and the second RF power source 230. Data from the sensor device 250 may be communicated to the controller 110 , and the controller 110 may be used to vary the power applied by the first radio frequency (RF) power source 230 and the second RF power source 240 .

[0045] In general, the following exemplary deposition process parameters can be used to form a freshly deposited dielectric film. The wafer temperature may vary from about -50°C to about 150°C, including but not limited to from about 10°C to about 100°C, or from about 10°C to about 50°C. The chamber pressure may vary from a chamber pressure in the range of about 0.1mTorr to about 10Torr, including but not limited to from about 2mTorr to about 50mTorr, or from about 2mTorr to about 10mTorr. The flow rate of the gas mixture containing the precursor may be in the range of from about 10sccm to about 1000sccm, including but not limited to from about 100sccm to about 200sccm, or from about 150sccm to about 200sccm. The flow rate of the dilution gas may vary independently from 50sccm to about 50000sccm, including but not limited to from about 50sccm to about 1000sccm, or from about 50sccm to about 100sccm.

[0046] The dielectric film can be deposited to about to about The thickness range includes about to about range, approx. to about range, or approximately to about range.

[0047] The deposited dielectric film may have a refractive index or n value (n(at 633 nm)) greater than about 1.5, for example, about 1.6 to about 3.0, including about 1.5, about 1.6, about 1.7, about 1.8, about 1.9, about 2.0, about 2.1, about 2.2, about 2.3, about 2.4, about 2.5, about 2.6, about 2.7, about 2.8, about 2.9, or about 3.0. In one or more embodiments, the film is silicon oxide and the refractive index is about 1.5. In yet another embodiment, the film is silicon nitride and the refractive index is about 1.9 to about 2.0. The methods of one or more embodiments advantageously enable the manufacture of high quality films and low temperatures that have properties similar to or improved upon those of films prepared by high temperature CVD or high temperature PECVD. The deposited dielectric film may have an extinction coefficient or k value (k(at 633 nm)) greater than 0.1, for example, from about 0.2 to about 0.3, including about 0.2, about 0.21, about 0.22, about 0.23, about 0.24, about 0.25, about 0.26, about 0.27, about 0.28, about 0.29, and about 0.30. The deposited dielectric film may have a stress (MPa) of less than about -300 MPa, for example, from about -600 MPa to about -300 MPa, from about -600 MPa to about -500 MPa, including about -600 MPa, about -575 MPa, about -550 MPa, about -525 MPa, about -500 mPa, about -475 MPa, about -450 MPa, about -425 MPa, about -400 MPa, about -375 MPa, about -350 MPa, about -325 MPa, or about -300 MPa.

[0048] In one or more embodiments, the density of the dielectric film is greater than 1.8 g / cc, including greater than 1.9 g / cc, and including greater than 2.0 g / cc. In one or more embodiments, the density of the dielectric film is about 2.1 g / cc. In one or more embodiments, the density of the dielectric film is in the range of about greater than 1.8 g / cc to about 2.2 g / cc. In one or more embodiments, the density of the dielectric film is greater than about 2.2 g / cc.

[0049] Another advantage of the method of one or more embodiments is that lower temperature processes can be used to produce dielectric films with desired density and transparency. In general, higher substrate temperatures during deposition are process parameters used to promote the formation of higher density films. When the precursors and methods of one or more embodiments are used together, surprisingly, the substrate temperature can be reduced during deposition, for example, as low as about less than -40°C, and less than about 0°C, less than about 10°C, less than about room temperature, or less than about 22°C to about 26°C, and still produce a film of desired density, that is, a dielectric film having a density greater than about 1.8 g / cc, including greater than about 1.9 g / cc, and including greater than about 2.0 g / cc. Therefore, the method of one or more embodiments can produce relatively high density films, particularly high density carbon films, wherein the absorption coefficient is as low as about 0.04.

[0050] Figure 3 A flow chart of a method 300 for forming a dielectric film on a film stack disposed on a substrate according to one embodiment of the present disclosure is depicted. For example, the dielectric film formed on the film stack may be used as an insulating layer in the film stack.

[0051] FIG. 4A to FIG. 4B A schematic cross-sectional view of a sequence for forming a dielectric film on a film stack disposed on a substrate according to method 300 is shown. Although method 300 is described below with reference to a dielectric layer that may be formed on a film stack for fabricating staircase-like structures in a film stack for use in a three-dimensional semiconductor device, method 300 may also be used to advantage in other device fabrication applications. In addition, it should also be understood that in Figure 3 The operations depicted in the examples may be performed simultaneously and / or in parallel. Figure 3 The order in which they are depicted is different from the order in which they are executed.

[0052] Method 300 begins at operation 310 by placing a substrate (such as Figure 4A The substrate 400 depicted in FIG. 1 is positioned in a process chamber, such as in Figure 1A or Figure 1B The process chamber 100 is depicted in FIG. The substrate 400 may be Figure 1A , Figure 1B and Figure 2 190 is depicted in FIG. The substrate 400 may be positioned on an electrostatic chuck (e.g., an upper surface 192 of the electrostatic chuck 150). The substrate 400 may be a silicon-based material or any suitable insulating or conductive material as desired, having a film stack 404 disposed thereon, the substrate 400 being operable to form a structure 402, such as a staircase-like structure, in the film stack 404.

[0053] As in Figure 4AAs shown in the exemplary embodiment depicted in , the substrate 400 may have a substantially flat surface, a non-uniform surface, or a substantially flat surface with a structure formed thereon. A film stack 404 is formed on the substrate 400. In one embodiment, the film stack 404 may be used to form a gate structure, a contact structure, or an interconnect structure in a front-end process or a back-end process. The method 300 may be performed on the film stack 404 to form a staircase-like structure used in a memory structure (such as a NAND structure) therein. In one embodiment, the substrate 400 may be a material such as crystalline silicon (e.g., Si(100) or Si(111)), silicon oxide, strained silicon, silicon germanium, doped or undoped polysilicon, doped or undoped silicon substrate, and patterned or unpatterned substrate silicon on insulator (SOI), carbon-doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, sapphire. The substrate 400 may have various sizes, such as 200 mm, 300 mm, and 450 mm, or other diameter substrates, and rectangular or square panels. Unless otherwise mentioned, the embodiments and examples described herein are performed on a substrate having a 200 mm diameter, a 300 mm diameter, or a 450 mm diameter substrate. In embodiments where an SOI structure is used for substrate 400, substrate 400 may include a buried dielectric layer disposed on a silicon crystalline substrate. In the embodiments depicted herein, substrate 400 may be a crystalline silicon substrate.

[0054] In one embodiment, the film stack 404 disposed on the substrate 400 may have a plurality of vertically stacked layers. The film stack 404 may include a pair including a first layer (illustrated as 408) repeatedly formed in the film stack 404. a1 ,408 a2 ,408 a3 ,……,408 an ) and the second floor (shown as 408 b1 ,408 b2 ,408 b3 ,……,408 bn The pairs include alternating first layers (shown as 408) that are repeatedly formed until a predetermined number of pairs of first layers and second layers are reached. a1 ,408 a2 ,408 a3 ,……,408 an ) and the second floor (shown as 408 b1 ,408 b2 ,408 b3 ,……,408 bn ).

[0055] The film stack 404 may be part of a semiconductor chip, such as a three-dimensional memory chip. FIG. 4A to FIG. 4B The first layer (shown as 408a1 ,408 a2 ,408 a3 ,……,408 an ) and the second floor (shown as 408 b1 ,408 b2 ,408 b3 ,……,408 bn ), but note that any desired number of repeating pairs of the first and second layers may be utilized as desired.

[0056] In one embodiment, the film stack 404 may be used to form multiple gate structures of a three-dimensional memory wafer. The first layer 408 formed in the film stack 404 a1 ,408 a2 ,408 a3 ,……,408 an may be a first dielectric layer according to one or more embodiments, and the second layer 408 b1 ,408 b2 ,408 b3 ,……,408 bn A suitable dielectric film according to one or more embodiments may be used to form the first layer 408. a1 ,408 a2 ,408 a3 ,……,408 an and / or second layer 408 b1 ,408 b2 ,408 b3 ,……,408 bn , including but not limited to one or more of the following: silicon, silicon nitride, silicon carbide, silicon oxide, silicon oxycarbide, silicon oxycarbon nitride, silicon oxynitride, titanium nitride, or a composite of oxide and nitride (at least one or more oxide layers are sandwiched between nitride layers), and combinations thereof, etc.

[0057] In some embodiments, the dielectric layer may have a high dielectric constant material having a dielectric constant greater than 4. Suitable examples of high dielectric constant materials include, but are not limited to, hafnium oxide (HfO2), zirconium oxide (ZrO2), hafnium silicon oxide (HfSiO2), hafnium aluminum oxide (HfAlO), zirconium silicon oxide (ZrSiO2), tantalum dioxide (TaO2), aluminum oxide, aluminum-doped hafnium dioxide, bismuth strontium titanium (BST), and platinum zirconium titanium (PZT), among others.

[0058] In one specific example, the first layer 408 a1 ,408 a2 ,408 a3 ,……,408 an is a silicon oxide layer, and the second layer 408b1 ,408 b2 ,408 b3 ,……,408 bn It is on the first floor 408 a1 ,408 a2 ,408 a3 ,……,408 an In one embodiment, the first layer 408 a1 ,408 a2 ,408 a3 ,……,408 an The thickness can be controlled at about About Between, such as about , and each second layer 408 b1 ,408 b2 ,408 b3 ,……,408 bn The thickness can be controlled at about About Between, such as about The membrane stack 404 may have a About In one embodiment, the total thickness of the film stack 404 is about 3 microns to about 10 microns, and will change as technology advances.

[0059] The dielectric film of one or more embodiments may be formed on any surface or any portion of the substrate 400 with or without the film stack 404 on the substrate 400 .

[0060] At operation 320, a chucking voltage is applied to the electrostatic chuck to chuck the substrate 400 to the electrostatic chuck. In some embodiments where the substrate 400 is positioned on the upper surface 192 of the electrostatic chuck 150, the upper surface 192 provides support and chucking of the substrate 400 during processing. The electrostatic chuck 150 is more tightly pressed against the upper surface 192 to flatten the substrate 400, thereby preventing backside deposition. An electrical bias is provided to the substrate 400 via the chucking electrode 210. The chucking electrode 210 may be in electronic communication with a chucking power supply 212, which supplies a bias voltage to the chucking electrode 210. In one embodiment, the chucking voltage is between about 10 volts and about 3000 volts. In one embodiment, the chucking voltage is between about 100 volts and about 2000 volts. In one embodiment, the chucking voltage is between about 200 volts and about 1000 volts.

[0061] During operation 320, several process parameters may be adjusted. In one embodiment suitable for processing 300 mm substrates, the process pressure in the processing volume may be maintained at about 0.1 mTorr to about 10 Torr, including about 2 mTorr to about 50 mTorr, or about 5 mTorr to about 20 mTorr. In one embodiment suitable for processing 300 mm substrates, the process temperature and / or substrate temperature may be maintained at about -50°C to about 250°C, including about 0°C to about 50°C; or about 10°C to about 20°C.

[0062] In one embodiment, a constant chucking voltage is applied to the substrate 400. In one embodiment, the chucking voltage may be pulsed to the electrostatic chuck 150. In some embodiments, a backside gas may be applied to the substrate 400 while the chucking voltage is applied to control the substrate temperature. The backside gas may include, but is not limited to, helium (He), argon (Ar), etc.

[0063] In operation 330, plasma is generated at the substrate level by applying a first RF bias to the electrostatic chuck. The plasma generated at the substrate level may be generated in a plasma region between the substrate and the electrostatic chuck. The first RF bias may be from about 10 watts to about 3000 watts at a frequency in the range of about 350 KHz to about 100 MHz (including but not limited to 350 KHz, 2 MHz, 13.56 MHz, 27 MHz, 40 MHz, 60 MHz, or 100 MHz). In one embodiment, the first RF bias is provided at a power between about 2500 watts and about 3000 watts at a frequency of about 13.56 MHz. In one embodiment, the first RF bias is provided to the electrostatic chuck 150 via the second RF electrode 260. The second RF electrode 260 may be in electronic communication with the first radio frequency (RF) power supply 230, which supplies a bias voltage to the second RF electrode 260. In one embodiment, the bias power is between about 10 watts and about 3000 watts. In one embodiment, the bias power is between about 2000 Watts and about 3000 Watts. In one embodiment, the bias power is between about 2500 Watts and about 3000 Watts. The first radio frequency (RF) power source 230 may generate power at a frequency in a range from about 350 KHz to about 100 MHz, including but not limited to 350 KHz, 2 MHz, 13.56 MHz, 27 MHz, 40 MHz, 60 MHz, or 100 MHz.

[0064] In some embodiments, operation 330 further includes applying a second RF bias to the electrostatic chuck. At a frequency ranging from about 350KHz to about 100MHz (including but not limited to 350KHz, 2MHz, 13.56MHz, 27MHz, 40MHz, 60MHz, or 100MHz), the second RF bias may be from about 10 watts to about 3000 watts. In one embodiment, at a frequency of about 2MHz, the second RF bias is provided at a power between about 800 watts and about 1200 watts. In one embodiment, the second RF bias is provided to the substrate 400 via the clamping electrode 210. The clamping electrode 210 may be in electronic communication with the second RF power supply 240, which supplies the bias voltage to the clamping electrode 210. In one embodiment, the bias power is between about 10 watts and about 3000 watts. In one embodiment, the bias power is between about 500 watts and about 1500 watts. In one embodiment, the bias power is between about 800 watts and about 1200 watts. The second RF power source 240 may generate power at a frequency ranging from about 350 KHz to about 100 MHz, including but not limited to 350 KHz, 2 MHz, 13.56 MHz, 27 MHz, 40 MHz, 60 MHz, or 100 MHz. In one embodiment, the clamping voltage supplied in operation 320 is maintained during operation 330 .

[0065] In some embodiments, during operation 330, a first RF bias is provided to the substrate 400 via the chuck electrode 210, and a second RF bias may be provided to the substrate 400 via the second RF electrode 260. In one embodiment, the first RF bias is about 2500 Watts (13.56 MHz), and the second RF bias is about 1000 Watts (2 MHz).

[0066] During operation 340, a gas mixture containing precursors flows into the processing volume 126 to form a dielectric film on the film stack. The gas mixture containing the precursors may flow into the processing volume 126 through the gas distribution assembly 120 or from the gas panel 130 via the sidewall 101. The gas mixture containing the precursors may include one or more precursors as described herein. The gas mixture containing the precursors may further include an inert gas, a diluent gas, a nitrogen-containing gas, an etchant gas, or a combination thereof. The precursor may be a liquid or a gas, although a preferred precursor will be a vapor at room temperature to simplify the hardware required for material metering, control, and delivery to the chamber. In some embodiments, the clamping voltage supplied during operation 320 is maintained during operation 340. In some embodiments, the process conditions established during operation 320 and the plasma formed during operation 330 are maintained during operation 340.

[0067] In some embodiments, the gas mixture containing the precursor further includes one or more diluent gases. If desired, a suitable diluent gas (such as helium (He), argon (Ar), xenon (Xe), hydrogen (H2), nitrogen (N2), ammonia (NH3) or a combination thereof, etc.) can be added to the gas mixture. Argon (Ar), helium (He) and nitrogen (N2) are used to control the density and deposition rate of the dielectric film. In some cases, as discussed below, the addition of N2 and / or NH3 can be used to control the hydrogen ratio of the dielectric film. Alternatively, no diluent gas may be used during deposition.

[0068] In some embodiments, the precursor-containing gas mixture further comprises one or more nitrogen-containing gases. For example, suitable nitrogen-containing compounds include pyridine, aliphatic amines, amines, nitriles, ammonia, and the like.

[0069] In some embodiments, the gas mixture containing the precursor further includes an inert gas. In some embodiments, an inert gas such as argon (Ar) and / or helium (He) may be supplied to the processing volume 126 together with the gas mixture containing the precursor. Other inert gases such as nitrogen (N2) and nitric oxide (NO) may also be used to control the density and deposition rate of the dielectric film. In addition, various other processing gases may be added to the gas mixture containing the precursor to modify the properties of the dielectric film material. In one embodiment, the other processing gas may be a reactive gas such as hydrogen (H2), ammonia (NH3), a mixture of hydrogen (H2) and nitrogen (N2), or a combination thereof. Adding H2 and / or NH3 may be used to control the hydrogen ratio of the deposited dielectric film. The hydrogen ratio present in the dielectric film provides control over layer properties such as reflectivity.

[0070] In some embodiments, the precursor-containing gas mixture further includes an etchant gas. Suitable etchant gases include chlorine (Cl2), carbon tetrafluoride (CF4), nitrogen trifluoride (NF3), or a combination thereof.

[0071] In some embodiments, the dielectric film 412 is exposed to hydrogen radicals after the dielectric film 412 is formed on the substrate during operation 340. In some embodiments, the dielectric film 412 is exposed to hydrogen radicals during the deposition process of operation 340. In some embodiments, the hydrogen radicals are formed in the RPS and delivered to the processing region.

[0072] At operation 350, after the dielectric film 412 is formed on the substrate, the substrate is de-chucked. During operation 350, the chuck voltage is turned off. The reactive gases are turned off and optionally purged from the process chamber. In one embodiment, during operation 350, the RF power is reduced (e.g., ~200 W). Optionally, the controller 110 monitors the impedance change to determine whether the electrostatic charge is dissipated to ground via the RF path. Once the substrate is de-chucked from the electrostatic chuck, the remaining gases are purged from the process chamber. The process chamber is evacuated and the substrate is moved upward on the lift pins and transferred out of the chamber.

[0073] After dielectric film 412 is formed on the substrate, dielectric film 412 can be used as a patterned mask in an etching process to form a three-dimensional structure, such as a staircase-like structure. Dielectric film 412 can be patterned using standard photoresist patterning techniques. A patterned photoresist (not shown) can be formed above dielectric film 412. Dielectric film 412 can be etched in a pattern corresponding to the patterned photoresist layer, and then the pattern is etched into substrate 400. Material can be deposited into the etched portion of dielectric film 412. Dielectric film 412 can be removed using a solution including hydrogen peroxide and sulfuric acid. An exemplary solution including hydrogen peroxide and sulfuric acid is known as Piranha solution or Piranha etchant. Dielectric film 412 can also be removed using etching chemicals containing oxygen and halogens (including but not limited to chlorine (Cl), fluorine (F), iodine (I), bromine (Br), and astatine (At)). For example, the dielectric film 412 may be removed using an etching chemistry containing Cl2 / O2, CF4 / O2, or Cl2 / O2 / CF4. The dielectric film 412 may be removed by a chemical mechanical polishing (CMP) process.

[0074] The process may be typically stored in a memory as a software routine that, when executed by a processor, causes the process chamber to perform the process of the present disclosure. The software routine may also be stored and / or executed by a second processor (not shown) that is located at the far end of the hardware controlled by the processor. Some or all of the methods of the present disclosure may also be performed in hardware. Therefore, the process may be implemented in software and executed in hardware using a computer system, as, for example, an application specific integrated circuit or other type of hardware implementation, or as a combination of software and hardware. When executed by a processor, the software routine converts a general purpose computer into a special purpose computer (controller) that controls the chamber operation so that the process is performed.

[0075] The present disclosure is now described with reference to the following examples. Before describing several exemplary embodiments of the present disclosure, it will be understood that the present disclosure is not limited to the details of the construction or process steps set forth in the following description. The present disclosure is capable of other embodiments and of being practiced or carried out in various ways.

[0076] Example

[0077] Example 1

[0078] Low temperature, high quality silicon nitride dielectric films were made by flowing 30 sccm SiH4, 100 sccm NH3, and N2 as process gases at 100°C, 400 mTorr pressure, applying 200 Watts of RF (13.56 MHz) power through the substrate pedestal (electrostatic chuck) in a CVD reactor with Ar(g) and He(g) as diluent gases. The resulting dielectric film had a refractive index (RI) of 1.82 (633 nm), which is much higher than dielectric films formed by PECVD at the same temperature. The RI was improved by adjusting the power (higher) and voltage (lower). The primary and secondary RF can be any combination of 350 KHz, 2 MHz, 13.56 MHz, 27 MHz, 40 MHz, 60 MHz, 100 MHz.

[0079] Unless otherwise indicated herein or clearly contradicted by context, the use of the terms "a" and "an" and "the" and similar references in the context of describing the materials and methods discussed herein (especially in the context of the appended claims) will be understood to cover the singular and the plural. Unless otherwise indicated herein, the recitation of the value range herein is intended only as a shorthand method of independently referring to each individual value falling into this range, and each individual value is incorporated into this specification as if it were independently recorded herein. Unless otherwise indicated herein or clearly contradicted by context, all methods described herein can be performed in any suitable order. The use of any and all examples, or exemplary language (e.g., "such as") provided herein is intended to only better illustrate the materials and methods, and no limitation on the scope is proposed unless otherwise claimed. No language in this specification should be understood to indicate that any unclaimed element is important for practicing the materials and methods of the disclosed content.

[0080] References throughout this specification to "one embodiment," "certain embodiments," "one or more embodiments," or "an embodiment" mean that a particular feature, structure, material, or characteristic described in conjunction with the embodiment is included in at least one embodiment of the present disclosure. Thus, the appearance of phrases such as "in one or more embodiments," "certain embodiments," "in one embodiment," or "in an embodiment" in various places throughout this specification do not necessarily refer to the same embodiment of the present disclosure. Furthermore, the particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0081] Although the disclosure herein has been described with reference to specific embodiments, it will be understood that these embodiments are merely illustrative of the principles and applications of the disclosure. It will be appreciated by those skilled in the art that various modifications and variations may be made to the methods and apparatus of the disclosure without departing from the spirit and scope of the disclosure. Therefore, the disclosure is intended to include modifications and variations within the scope of the appended claims and their equivalents.

Claims

1. A method for processing a substrate, the method comprising: flowing a gas mixture containing a precursor into a processing volume of a processing chamber having a substrate positioned on an electrostatic chuck; maintaining the substrate at a pressure in a range of 0.1 mTorr and 10 Torr and at a temperature in a range of -50°C to 150°C; as well as depositing a dielectric film on the substrate by applying a first RF bias to the electrostatic chuck to generate a plasma at the substrate level, the dielectric film having a refractive index in the range of 1.5 to 3 at 633 nm, The dielectric film includes one or more of the following: silicon, silicon nitride, silicon carbide, silicon oxide, silicon oxycarbide, silicon oxynitride-carbon oxynitride, silicon oxynitride, titanium nitride, or a composite of the above oxides and nitrides.

2. The method of claim 1, further comprising: A second RF bias is applied to the electrostatic chuck to generate the plasma at the substrate level.

3. The method of claim 2, wherein the second RF bias is provided at a power in the range of 10 Watts to 3000 Watts and at a frequency in the range of 350 KHz to 100 MHz.

4. The method of claim 3, wherein the second RF bias is provided at a power in the range of 800 Watts to 1200 Watts at a frequency of 2 MHz.

5. The method of claim 1, wherein the first RF bias is provided at a power in the range of 10 Watts to 3000 Watts and at a frequency in the range of 350 KHz to 100 MHz.

6. The method of claim 5, wherein the first RF bias is provided at a power in the range of 2500 Watts to 3000 Watts at a frequency of 13.56 MHz.

7. The method of claim 1, further comprising: A chucking voltage is applied to the substrate positioned on the electrostatic chuck.

8. The method of claim 1, wherein the precursor-containing gas mixture comprises one or more precursors selected from the group consisting of silane (SiH4), triethoxysilane (SiH(OEt)3), tetraethoxysilane (tetraethyl orthosilicate; Si(OEt)4 or TEOS), disilane (Si2H6), SiH(CH3)3, dimethylsilane (SiH2(CH3)2), methylsilane (SiH3CH3), dichlorosilane (SiH2Cl2), silicon tetrachloride (SiCl4), silicon tetrafluoride (SiF4), trichlorosilane (HSiCl3), methylsilane (CH3SiH3), trimethylsilane (C3H 10 Si), 1,1,3,3-tetramethyldisiloxane (TMDZ), 1,3,5-trisilapentane (TSP), (bis(tert-butylamino)silane (BTBAS), (bis(diethylamino)silane (BDEAS), tris(dimethylamino)silane (TDMAS), (Si[N(tBu)CH=CHN(tBu)](OEt)2(Si-TBES), Si[N(tBu)CH=CHN(tBu)](H)NH2(Si-TBAS), germane (GeH4), germanium tetrachloride (GeCl4), germanium tetrafluoride (GeF4), tert-butylgermane (GeH(CH3)3), N2O, O2, NH3, N2, H2, C2H2 or C3H6.

9. The method of claim 1, wherein the precursor-containing gas mixture comprises one or more diluent gases selected from the group consisting of helium (He), argon (Ar), xenon (Xe), krypton (Kr), nitrogen (N2), or hydrogen (H2).

10. The method of claim 1, wherein the dielectric film has a density greater than 1.8 g / cc.

11. A method for processing a substrate, the method comprising: A precursor-containing gas mixture is flowed into a processing volume of a processing chamber having a substrate positioned on an electrostatic chuck, wherein the precursor-containing gas mixture includes one or more precursors selected from the group consisting of silane (SiH4), triethoxysilane (SiH(OEt)3), tetraethoxysilane (tetraethyl orthosilicate; Si(OEt)4 or TEOS), disilane (Si2H6), SiH(CH3)3, dimethylsilane (SiH2(CH3)2), methylsilane (SiH3CH3), dichlorosilane (SiH2Cl2), silicon tetrachloride (SiCl4), silicon tetrafluoride (SiF4), trichlorosilane (HSiCl3), methylsilane (CH3SiH3), trimethylsilane (C3H 10 Si), 1,1,3,3-tetramethyldisiloxane (TMDZ), 1,3,5-trisilapentane (TSP), (bis(tert-butylamino)silane (BTBAS), (bis(diethylamino)silane (BDEAS), tris(dimethylamino)silane (TDMAS), (Si[N(tBu)CH=CHN(tBu)](OEt)2(Si-TBES), Si[N(tBu)CH=CHN(tBu)](H)NH2(Si-TBAS), germanium (GeH4), germanium tetrachloride (GeCl4), germanium tetrafluoride (GeF4), tert-butylgermane (GeH(CH3)3), N2O, O2, NH3, N2, H2, C2H2 or C3H6; maintaining the substrate at a pressure in a range of 0.1 mTorr to 10 Torr and at a temperature in a range of -50°C to 150°C; as well as A dielectric film having a refractive index in the range of 1.5 to 3 at 633 nm is deposited on the substrate by applying a first RF bias and a second RF bias to the electrostatic chuck to generate plasma at a substrate level.

12. The method of claim 11, wherein the first RF bias is provided at a power in the range of 2500 Watts to 3000 Watts at a frequency of 13.56 MHz.

13. The method of claim 11, wherein the second RF bias is provided at a power in the range of 800 Watts to 1200 Watts at a frequency of 2 MHz.

14. A method for processing a substrate, the method comprising: flowing a gas mixture containing a precursor into a processing volume of a processing chamber having a substrate positioned on an electrostatic chuck; maintaining the process volume at a pressure in a range of 0.1 mTorr to 10 Torr and at a temperature in a range of -50°C to 150°C; depositing a dielectric film on the substrate by applying a first RF bias and a second RF bias to the electrostatic chuck to generate a plasma at the substrate level, the dielectric film having a refractive index in the range of 1.5 to 3 at 633 nm, wherein the dielectric film comprises one or more of silicon, silicon nitride, silicon carbide, silicon oxide, silicon oxycarbide, silicon oxycarbonitride, silicon oxynitride, titanium nitride, or a composite of the above oxides and nitrides; forming a patterned photoresist layer over the dielectric film; etching the dielectric film in a pattern corresponding to the patterned photoresist layer to provide etched portions of the dielectric film; etching the pattern into the substrate; as well as A material is deposited into the etched portion of the dielectric film.

15. The method of claim 14, wherein the first RF bias is provided at a power in the range of 10 Watts to 3000 Watts at a frequency of 350 KHz to 100 MHz.

16. The method of claim 14, wherein the second RF bias is provided at a frequency in the range of 350 KHz to 100 MHz at a power in the range of 10 Watts to 3000 Watts.

17. The method of claim 14, further comprising: A chucking voltage is applied to the substrate positioned on the electrostatic chuck.

18. The method of claim 14, wherein the precursor-containing gas mixture comprises one or more precursors selected from the group consisting of silane (SiH4), triethoxysilane (SiH(OEt)3), tetraethoxysilane (tetraethyl orthosilicate; Si(OEt)4 or TEOS), disilane (Si2H6), SiH(CH3)3, dimethylsilane (SiH2(CH3)2), methylsilane (SiH3CH3), dichlorosilane (SiH2Cl2), silicon tetrachloride (SiCl4), silicon tetrafluoride (SiF4), trichlorosilane (HSiCl3), methylsilane (CH3SiH3), trimethylsilane (C3H 10 Si), 1,1,3,3-tetramethyldisiloxane (TMDZ), 1,3,5-trisilapentane (TSP), (bis(tert-butylamino)silane (BTBAS), (bis(diethylamino)silane (BDEAS), tris(dimethylamino)silane (TDMAS), (Si[N(tBu)CH=CHN(tBu)](OEt)2(Si-TBES), Si[N(tBu)CH=CHN(tBu)](H)NH2(Si-TBAS), germane (GeH4), germanium tetrachloride (GeCl4), germanium tetrafluoride (GeF4), tert-butylgermane (GeH(CH3)3), N2O, O2, NH3, N2, H2, C2H2 or C3H6.

19. The method of claim 14, wherein the precursor-containing gas mixture comprises one or more diluent gases selected from the group consisting of helium (He), argon (Ar), xenon (Xe), krypton (Kr), nitrogen (N2) or hydrogen (H2).