Methods, apparatus and procedures for nondestructive testing of elastomeric cable insulation sheaths
The non-destructive testing of nuclear cable insulation sheath through proton nuclear magnetic resonance technology solves the destructive problem of nuclear cable aging detection, realizes reliable monitoring and prediction of cable life, and reduces detection costs.
Patent Information
- Application Number
- CN201980049059.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-05-23
- Filing Date
- 2019-05-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-05-21
AI Technical Summary
The prior art aging detection of nuclear cables requires destructive testing, resulting in high cost of sampling and replacement of cables and inability to achieve lossless monitoring.
The insulating sheath of the cable was tested by using proton nuclear magnetic resonance technology. By measuring the elastic active chain parameters of the macromolecular network of the elastomeric polymer, it evaluates its comparison with the set threshold to determine the end of the cable's life.
Non-destructive testing of nuclear cables is achieved, reducing cable sampling and replacement costs, and providing reliable monitoring and prediction of cable aging status.
Smart Images

Figure CN112469995B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for non-destructive testing of an insulating sheath of a cable, in particular a nuclear cable.
[0002] One field of application of the invention relates to cables for nuclear power plants for generating electricity. Background Art
[0003] In a nuclear power plant for generating electricity, an average of 1500 km of cables are installed per nuclear unit (including 50 km in the reactor building). In use, the installed cables are subject to aging phenomena, i.e. degradation.
[0004] Understanding and monitoring this degradation is critical to ensuring the proper functioning of these cables.
[0005] The ageing state of a nuclear cable is determined from the elongation at break value of its insulation. This characteristic is measured in the laboratory by a mechanical uniaxial tensile test, which is a destructive test that requires sampling of at least 50cm of the entire cable. Therefore, cable sampling campaigns are periodically arranged in the field, and these cables are then analyzed in the laboratory, allowing to argue the end of their life.
[0006] The disadvantage of this test that requires cable sampling is first of all its destructive nature. In other words, the sampled cable will not be restored to service, and replacing the cable involves a lot of costs. Summary of the invention
[0007] The invention aims at obtaining a non-destructive testing method (without requiring replacement of the cable) which allows conclusions to be drawn about the durability of the cable.
[0008] To this end, a first subject of the invention is a method for non-destructive testing of an insulating sheath of an electric cable made of at least one elastomeric polymer material,
[0009] Characterized in that the method comprises the following steps: performing a measurement using proton nuclear magnetic resonance on the insulating sheath in order to measure at least one first parameter characterizing the elastic active chains of the macromolecular network of the elastomeric polymer,
[0010] And includes an evaluation step, which includes comparing a first parameter characterizing the elastic active chain and / or a second parameter that has been determined based on the first parameter characterizing the elastic active chain with at least one specified evaluation threshold to determine that when the first parameter and / or the second parameter is below the specified evaluation threshold, the cable is at the end of its life.
[0011] According to one embodiment of the present invention, the first parameter comprises the fraction of elastic active chains of the macromolecular network of the elastomeric polymer and / or the average molar mass of the elastic active chains of the macromolecular network of the elastomeric polymer.
[0012] According to one embodiment of the invention, the first parameter comprises the fraction of elastic active chains of the macromolecular network of the elastomeric polymer,
[0013] The evaluation step includes comparing the fraction of elastic active chains of the macromolecular network of the elastomeric polymer to a specified evaluation threshold to determine that the cable is at the end of life when the fraction of elastic active chains of the macromolecular network of the elastomeric polymer is below the specified evaluation threshold.
[0014] According to one embodiment of the invention, the measuring step comprises measuring transverse proton relaxation using proton nuclear magnetic resonance on the insulating sheath in order to determine at least from this measurement the fraction of elastically active chains of the macromolecular network of the elastomeric polymer.
[0015] According to one embodiment of the present invention, the first parameter comprises the average molar mass of the elastic active chains of the macromolecular network of the elastomeric polymer,
[0016] The second parameter includes the elongation at break which has been determined based on the average molar mass of the elastic living chains,
[0017] The evaluation step includes comparing the elongation at break to a specified evaluation threshold value to determine that the cable is at the end of its life when the elongation at break is below the specified evaluation threshold value.
[0018] According to one embodiment of the invention, the measuring step comprises measuring the increase in proton double quantum coherence using proton nuclear magnetic resonance on the insulating sheath in order to determine at least from the measurement the average molar mass of the elastically active chains of the macromolecular network of the elastomeric polymer.
[0019] According to one embodiment of the present invention, the average molar mass of the elastic active chains is calculated based on the residual dipole coupling measured by measuring the increase in proton double quantum coherence using proton nuclear magnetic resonance.
[0020] According to one embodiment of the present invention, the average molar mass of the elastic active chains is calculated to be proportional to the inverse of the residual dipole coupling measured by measuring the increase in proton double quantum coherence using proton nuclear magnetic resonance.
[0021] According to one embodiment of the present invention, the average molar mass M of the elastic active chain is c Calculated by the following equation:
[0022] M c =(D stat / k).3 / 5.r 2 / D res
[0023] in
[0024] D statis the predetermined static dipole coupling,
[0025] D res The residual dipole coupling is measured by measuring the increase in proton double quantum coherence using proton nuclear magnetic resonance.
[0026] k is a predetermined parameter for the local coupling topology and the motion between material segments,
[0027] r is a predetermined ratio between the end-to-end chain length of a portion of the chains between the topological constraints and the average value of the end-to-end chain length when the material is in equilibrium.
[0028] According to one embodiment of the invention, the method comprises the step of sampling the insulating sheath of the cable, and the step of performing measurements using proton nuclear magnetic resonance on the sample.
[0029] According to one embodiment of the invention, during the sampling step, the sample mass taken of the insulating sheath of the cable is 20 mg to 40 mg.
[0030] According to one embodiment of the present invention, the method comprises the step of bringing an apparatus for measuring using proton nuclear magnetic resonance into contact with the insulating sheath of the cable, the measuring step being performed by the apparatus for measuring using proton nuclear magnetic resonance.
[0031] A second subject of the invention is a computer program comprising code instructions for implementing the above method when it is executed on a computer.
[0032] A third subject of the invention is a device for non-destructive testing of an insulating sheath of an electric cable made of at least one elastomeric polymer material,
[0033] Characterized in that the device comprises: a device for measuring on the insulating sheath using proton nuclear magnetic resonance to measure at least one first parameter characterizing the elastic active chains of the macromolecular network of the elastomeric polymer,
[0034] And comprises: a computer for implementing an evaluation step, which includes comparing a first parameter characterizing the elastic active chain and / or a second parameter determined from the first parameter characterizing the elastic active chain with at least one specified evaluation threshold value, so as to determine that when the first parameter and / or the second parameter is below the specified evaluation threshold value, the cable is at the end of its life. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The invention will be better understood on reading the following description given purely by way of non-limiting example with reference to the accompanying drawings, in which:
[0036] - Figure 1 and Figure 2 Schematic representation of the molecular network of the elastomer of the cable jacket,
[0037] - Figure 3 Schematically represents a transverse relaxation signal of an elastomeric network of a cable jacket, which signal can be used according to one embodiment of the present invention,
[0038] - Figure 4 The module block diagram of the nondestructive testing method according to an embodiment of the present invention is schematically shown. DETAILED DESCRIPTION
[0039] Reference below Figure 4 A method for nondestructive testing of an insulating sheath G of a cable CB according to an embodiment of the present invention is described. The insulating sheath G of the cable CB is made of an electrical insulating material including at least one elastomeric polymer. The material may be, for example, made of EPDM or other materials. The cable CB may be, for example, a cable installed in a nuclear power plant for power generation or other. Figure 4 As shown, in such a nuclear power plant, the cable CB and its insulating sheath G can withstand high stress, especially ionizing radiation, which may be 0.1Gy.h -1 (h means hours), and temperature, which may be 50°C, which may lead to accelerated aging of the cable CB and its insulating sheath G. The invention is equally applicable to any cable comprising an insulating sheath. The invention is also applicable to any elastomeric polymer material, such as, for example, seals, pipes, base elements, any sealing elements, tires.
[0040] According to one embodiment of the invention, the method comprises a first step E1 of sampling the insulating sheath G of the cable CB. This can be done by taking one or more microsamples (a few milligrams) of the material of the sheath G, which do not affect the function of the cable C and do not damage it. This sample is very small. For example, the mass of the sample taken of the insulating sheath G of the cable CB during the sampling step E1 is 20 mg to 40 mg. This low mass represents about (2 x 5 x 5) mm 3 For example, the maximum length of insulation that can be collected from a live cable at the end of the cable without affecting the cable functionality is estimated to be 1 cm. This places no restrictions on the shape of the sample to be collected. The sample preferably always has the same shape, more precisely a symmetrical shape (for example like a washer), so that the magnetic field of the magnet is always changed in the same way when the sample is inserted into the spectrometer of the measuring device during the measurement step E2 described below. This step E1 is fast and simpler to implement. Therefore, this ensures non-destructive monitoring of the cable CB in terms of its functionality, so that the cable CB can be maintained on site for continued operation.
[0041] In a variant, in addition to or instead of the first step E1 of sampling the insulating sheath of the cable, a first step E1bis may be provided of bringing the device for measuring using proton nuclear magnetic resonance into contact with the sheath G of the cable CB, for example at the location where the cable CB is installed on site, in the case where the measuring device is portable and is brought to that location. Likewise, the step E1bis of bringing the device for measuring using proton nuclear magnetic resonance into contact with the sheath G ensures non-destructive monitoring of the functionality of the cable CB, so that the cable CB can be maintained on site to continue working.
[0042] After the first step E1 and / or E1bis, a second step E2 is performed on the insulating sheath G: using solid-state proton nuclear magnetic resonance (abbreviated as: 1 H NMR) in order to measure at least one first parameter P1 of the elastic active chains A of the macromolecular network of the elastomeric polymer of the insulating sheath G of the cable CB. This second measurement step E2 can be carried out by means of a device for measuring by proton nuclear magnetic resonance (which, in the case of step E1, has been brought to the location of the cable) and / or on a sample taken from the sheath G of the cable CB in a laboratory by means of a device for measuring by proton nuclear magnetic resonance.
[0043] According to one embodiment of the present invention, the first parameter P1 comprises: the fraction FCEA of the elastic active chains A of the macromolecular network of the elastomeric polymer, which is calculated based on measurements performed using proton nuclear magnetic resonance; and / or the average molar mass M of the elastic active chains A of the macromolecular network of the elastomeric polymer c , which is calculated from measurements using proton nuclear magnetic resonance.
[0044] The topology (chemical properties) of the macromolecular network is related to the mechanical properties of the polymeric material of the sheath G. Indeed, the relevant macromolecular material parameters reflect the state of the cable CB. According to one embodiment of the invention, these parameters include the proportions of the macromolecular chains (elastic active chains A, pendant chains B, extractables C) of the network, FCEA and / or the molar mass distribution M between the crosslinking nodes. c. Preferably, these two analyses explicitly concern the elastic active chains A for which a threshold S is applied. They are directly related to the mechanical strength of the insulating sheath G, which influences the lifetime of the cable C. The lifetime of the cable CB and its functionality are linked to the integrity of the insulating sheath G. This integrity is described by the mechanical properties of the material. In the case of implementation of the above-mentioned step E1, the study of the macromolecular network of the polymer insulation of the sheath G requires only microsampling, allowing non-destructive testing of the cable, or no sampling in the case of implementation of the above-mentioned step E1bis. It should be noted that the term "elastic active chains A" is a term specific to the elastomer family. For other polymer families, it is simply called macromolecular chains.
[0045] Solid-state proton nuclear magnetic resonance (SPR) 1 H NMR) is a technique for the physicochemical analysis of polymers. It is a non-destructive technique that allows the characterization of macromolecular networks. It can be used as a primary tool to monitor changes in materials during aging.
[0046] After the second measurement step E2, a third step E3 is performed: evaluating the aging state of the cable CB according to the first parameter P1 and / or the second parameter P2 determined by the first parameter characterizing the elastic active chain A. This third evaluation step E3 comprises comparing the first parameter P1 and / or the second parameter with at least one prescribed evaluation threshold S, and determining that the cable CB is at the end of its life when the first parameter P1 and / or the second parameter P2 is less than the prescribed evaluation threshold S.
[0047] Use of the elastic active chain A fraction FCEA:
[0048] A first series of embodiments of the method using the first parameter P1 is described below.
[0049] According to one embodiment, the first parameter P1 comprises the fraction FCEA of elastic active chains A of the macromolecular network of the elastomeric polymer. The evaluation step E3 comprises: a comparison E31 of the fraction FCEA of elastic active chains A of the macromolecular network of the elastomeric polymer with a prescribed evaluation threshold S, the evaluation threshold S being a threshold value A of the fraction of elastic active chains. THRESHOLD This threshold A THRESHOLD It is determined according to the type of material. When the fraction FCEA of the elastically active chains A of the macromolecular network of the elastomeric polymer falls below a specified evaluation threshold S, the cable CB is determined to be at the end of its life.
[0050] According to one embodiment, the measurement step E2 comprises a measurement E21 of transverse proton relaxation using proton nuclear magnetic resonance on the insulating sheath G. The fraction FCEA of elastically active chains A of the macromolecular network of the elastomeric polymer is determined at least by this measurement E21 .
[0051] According to one embodiment, the measurement of the transverse proton relaxation E21 allows obtaining 1 The H transverse relaxation signal can be obtained using 3 complementary experiments: solid echo (short time) and Hahn / CARR-Purcell-Meiboom-Gill echo (CPMG) (intermediate and long time). This measurement E21 allows to measure 1 The H transverse relaxation signal is used to obtain the ratio of network components. These experiments provide important information about the mobility of protons in the network. Figure 1 and Figure 2 As shown, due to the large differences in dynamics within the polymer network, three macromolecular chain populations of the network can be identified.
[0052] exist Figure 1 and Figure 2 In the example, the elastically active chains A are chains that are crosslinked or entangled at both ends. The side chains B are chains that are crosslinked or entangled at only one end or chain ends. The extractables C are non-crosslinked chains / free chains in the macromolecular network. The side chains B and extractables C do not participate in the elasticity: they are elastically inactive. The mechanical properties are then mainly determined by the elastically active chains A. 1 Analysis of the H transverse relaxation signal allows the determination of the fractions of different parts of the network, namely chain A, chain B and chain C.
[0053] According to one embodiment, firstly 1 H transverse relaxation measurements were performed to determine the mole fraction of side chains B and the mole fraction of extractables C in the network. The fraction B and the fraction C were obtained from 1 The H transverse relaxation signal M(t) is obtained, which has been determined by measuring E21 with the help of the following fitting analysis:
[0054] M(t)=B exp(-t / T2b)+C exp(-t / T2c)
[0055] Where M(t) is the magnetization,
[0056] T2b is obtained from M(t) and is related to the proton of the side chain B 1 H transverse relaxation time,
[0057] T2c is obtained from M(t) and is related to the protons of extractable C 1 H transverse relaxation time.
[0058] Figure 3 Schematically represented is the transverse relaxation signal M(t) / M0 (logarithmic scale) on the ordinate as a function of time t on the abscissa for an elastomeric network consisting of three relaxation components A, B and C, where M0 is a defined constant. Figure 3As shown, these extractables C (indicated by dashed lines) correspond to points of M(t) that are located after the components associated with the protons of the elastic active chains A (the elastic active chains A are the first relaxing components) disappear.
[0059] Simple subtraction FCEA = 1 – BC gives the fractional FCEA of elastically active chains A in the network.
[0060] Determining the fraction of elastic active chains A by NMR FCEA can tell the relative threshold A THRESHOLD Condition:
[0061] - If FCEA>A THRESHOLD , the mechanical strength of the material is considered to be satisfactory.
[0062] - If FCEA THRESHOLD , the material is considered to have degraded and can no longer ensure good strength.
[0063] Furthermore, if there is a dynamic evolution of the fraction FCEA of elastically active chains A (for example, by carrying out accelerated aging tests), the remaining lifetime of the material can be determined.
[0064] Therefore, the measured value of the fraction of elastically active chains A by FCEA is below the threshold A THRESHOLD , which indicates that the cable CB is at the end of its useful life and therefore the cable CB is in a very advanced state of ageing and must be replaced with a new cable CB on site.
[0065] The method according to the invention therefore allows obtaining reliable information about the wear of the cable CB, based on which maintenance operations on the cable can be decided.
[0066] The average molar mass M of the elastic active chain A c Use:
[0067] A second series of embodiments of the method using the second parameter P2 is described below.
[0068] According to one embodiment, the second parameter P2 comprises the elongation at break ε r , which has been calculated based on the average molar mass M of the elastic active chain A of the first parameter P1 c Sure.
[0069] According to one embodiment, the evaluation step E3 comprises the elongation at break ε r The comparison E32 is made with the prescribed evaluation threshold S, which is the threshold S2 of the elongation at break. r When it falls below a prescribed evaluation threshold value S2, it is determined that the cable CB is at the end of its life.
[0070] According to one embodiment, the measurement step E2 comprises a measurement E22 of the increase in proton double quantum coherence using solid-state proton nuclear magnetic resonance on the insulating sheath G. From at least this measurement E22 the average molar mass M of the elastic active chains A of the macromolecular network of the elastomeric polymer is determined. c .
[0071] According to one embodiment, based on Improved Baum & Pines sequence acquisition 1 H Measurement of the increase in double quantum coherence E22.
[0072] This analysis allows obtaining the experimental curve I DQ , the curve shows 1 The amplitude of H double quantum coherence varies with the excitation time t DQ evolution.
[0073] right 1 H Coherence increase curve I DQ The analytical description of the network gives the residual coupling D according to the following formula res The distribution value of:
[0074]
[0075] Among them, D stat is the distribution constant defined,
[0076] P(D res ) is the defined distribution density.
[0077] D res (in Hz) corresponds to the residual dipole coupling measured by NMR experiments. It is the average dipole coupling of the segments between topological constraints in the network. The farther the topological constraints are, the smaller D res The weaker it is, because it is averaged over more molecular motions.
[0078] D stat (in Hz) corresponds to the static dipole coupling and is the value measured for protons in the absence of molecular motion (to obtain this value it is necessary to measure the polymer at very low temperatures). stat Is static 1 H- 1 The value of H dipole coupling can be obtained from the 1 H- 1 H distance calculation D stat , without taking into account any molecular motion.
[0079] k is a unitless parameter that allows to take into account additional averaging effects originating from motions within the Kuhn segment (motions, vibrations and conformational jumps of the order of a few hundred picoseconds). k is specific to each polymer.
[0080] P(D res ) is a function of the residual dipole coupling distribution for the material under investigation. For some materials, P(D res ) can be a Gaussian probability density. For EPDM, in order to describe the heterogeneity at the P(Dres) level, P(D res ) is calculated from an asymmetric probability density called the "lognormal" as shown below:
[0081]
[0082] Where μ and σ are two adjustable parameters.
[0083] From the distribution P(D) determined for crosslinked, unfilled EPDM (μ = 0.752; σ = 0.506) res ) parameters, the distribution of residual dipole coupling in the network before aging can be plotted.
[0084] f(t DQ ,D res ) is the reaction curve I DQ (t DQ ) growth core function, which is achieved through DQ 1 H double quantum measurement is obtained if there is only one residual dipole coupling in the network. In other words, this equation allows describing the increase in coherence for a perfect single-mode network without the help of any distribution.
[0085] For elastomeric polymers, the function f(t DQ ,D res ) can be of the following types:
[0086]
[0087] Among them, Q and U are the first predetermined coefficient and the second predetermined coefficient.
[0088] For example, for the above EPDM material, Q = 0.378 and U = 0.583 and the function f(t DQ ,D res )for:
[0089]
[0090] Of course, the function f(t DQ ,D res ) may be different from another elastomeric polymer or another polymer.
[0091] According to the following equation, D res The distribution of can be converted into the average molar mass M between macromolecular chains (including topological constraints of entanglements and cross-linking nodes) c Distribution:
[0092]
[0093] where N is the number of Khun segments between crosslink nodes, which is related to the average molar mass of the polymer, M c Proportional,
[0094] r and k are material-dependent parameters and can be determined by molecular dynamics.
[0095] r2 corresponds to the end-to-end vector (or end-to-end chain length) of the partial chains between topological constraints (R 2 ) and the average value of the vector (or end-to-end chain length) in equilibrium (average R 2 ). r2 is usually a Gaussian distribution. res Depends on the average molar mass M c The reciprocal of the average molar mass M of the entangled chain e The reciprocal of .
[0096] Dres∝1 / Mc+1 / Me
[0097] D res This distribution of can be viewed as the molar mass distribution (M) between topological constraints.
[0098] Assume 1 / M e Much smaller than 1 / M c (Ignore tangles).
[0099] M c It can be calculated by the above equation, which is factored by G = (D stat / k).3 / 5.r 2 D res With molar mass M c So we can calculate:
[0100] D res =(D stat / k).3 / 5.r 2 / M c
[0101] The following therefore applies:
[0102] M c =(D stat / k).3 / 5.r 2 / D res
[0103] The following therefore applies:
[0104] M c =G / D res
[0105] The main parameter determining the mechanical properties and their degradation is the elastic active chain, whose molar mass (M c ) is a good indicator and is related to the elongation at break ε r is directly related to the evolution of .
[0106] Understand the average molar mass M of the elastic active chain A c , M c Connection to elongation at break ε r The multi-scale relationship of can predict the elongation at break ε of the analyzed material r , and thus draw conclusions about the degradation state relating to the critical threshold value S2.
[0107] Therefore, the average molar mass (M c : the average molar mass of the chains between cross-link nodes, and M e The measurement of ε: the average molar mass of the entangled chains) will give the elongation at break ε r For example, the elongation at break ε r The value of is less than 50% of the absolute value of the elongation at break threshold S2, which indicates that the cable has exceeded the limit of its service life.
[0108] If there is a material M c If the dynamic evolution of the strain is determined (for example, accelerated aging tests are performed), the elongation at break ε can be determined due to the multiscale relationship. r This method allows the remaining lifetime of the material to be determined.
[0109] The average molar mass M of the elastic active chain A is described below c and elongation at break ε r An example of the relationship between .
[0110] Macromolecular size (M c ) and macroscopic scale (ε r ) using a methodology based on fracture mechanics and the concept of intrinsic defects to predict the fracture of elastomers for materials where post-crosslinking is the dominant process during aging.
[0111] The input data is:
[0112] - Tear energy J of unaged material obtained on a broken test piece: test piece SENT (single notch) c0 The value of
[0113] - Elongation at break of tensile test pieces versus stress as a function of deformation for unaged material. (□ c0 ,W0=f(□)), index 0 refers to the unaged material.
[0114] Based on these input data, the inherent defect a can be calculated th Size:
[0115]
[0116] in
[0117] Among them, a th is the theoretical size of the inherent defect,
[0118] J c0 is the tearing energy of the unaged material,
[0119] k(λ) is the scaling factor in the case of the test piece DENT.
[0120] In the case of EPDM, it was found that the intrinsic defect length (2a th ) is equal to 0.5 mm (the diameter of the imaginary circular defect in the uniaxial tensile test piece) and is used for any other EPDM.
[0121] M c =f(t×a T ): molar mass M c With the reduction of time t×a T The evolution of is:
[0122]
[0123] It is obtained by time-temperature equivalence.
[0124] t×a T It means t multiplied by a T .
[0125] a T is the sliding factor of the time-temperature equivalence curve.
[0126] a1, a2 are constants obtained by least squares regression,
[0127] M c1 are the parameters obtained through least squares regression,
[0128] t is the time in hours.
[0129] The output data is J c and W c .
[0130] J c It is the critical rupture and tearing energy.
[0131] W c is the deformation energy density at fracture.
[0132] J c =f(Mc): for a given molar mass M c Value J c The values are:
[0133]
[0134] For EPDM: A = 125 kJ / m 2 and M c0 =678 g / mol (indicating a threshold lower than the material with zero tearing energy).
[0135] W c =f(Mc): corresponding deformation energy density W c The value of .
[0136] As a first approximation, a Gaussian model is assumed which allows writing:
[0137]
[0138] where R and T are the gas constant and absolute temperature, respectively, ρ is the density, and f is a functional factor that depends on the number of segments starting from the cross-link node.
[0139] W is the deformation energy density,
[0140] λ1, λ2, λ3 are the eigenvalues of the deformation gradient tensor.
[0141] For a given M c The corresponding Jc can be derived from equation 3, and in the case of uniaxial tension, from equation 4 with λ2=λ3=λ1 -1 / 2 The corresponding deformation energy density W calculated by numerical method c .
[0142] Known inherent defectsa th The elongation at break λ can be obtained by solving the following equation c :
[0143] J c =4k c a th W c (Equation 5)
[0144] and
[0145]
[0146] Elongation at breakε r Expressed as:
[0147] ε r =λ c –1 (Equation 7)
[0148] The molar mass between the topological constraints M obtained here means that the tangle nodes (M e ) and cross-link nodes (M c ) is the contribution of M (obtained from NMR using the previous equation) can be decomposed into:
[0149] M=M c +M e
[0150] Among them, M c is the molar mass between cross-link nodes, M e is the molar mass between entanglement nodes, M e Usually given in the data sheet.
[0151] M c =MM e
[0152] The end-of-life criterion is set at 50% of the absolute value of the elongation at break.
[0153] The described approach can be enhanced by two different applications:
[0154] -Use in knowing its M c A tool for assessing the state of a material at time t (measured by NMR),
[0155] - Use as a predictive tool: Knowing the evolution of the molar mass Mc of a material, it is possible to obtain the elongation at break ε r evolution and thus predict the end of life of the cable.
[0156] In these first and second series of embodiments, the third evaluation step E3 may implement a comparison E31 and / or a comparison E32 .
[0157] The above method can be implemented on a computer (which can be a computer, a processor, a microprocessor, etc.) used for evaluating step E3. When the above method is implemented on the computer, the computer may have been programmed by a computer program (including code instructions for implementing the method).
[0158] Of course, the above embodiments, features, possibilities and examples can be combined with one another or selected independently of one another.
Claims
1. A method for non-destructive testing of an insulating sheath (G) of a cable (CB) made of at least one elastomeric polymer material, It is characterized in that The method comprises a measuring step (E2): measuring on the insulating sheath (G) using proton nuclear magnetic resonance in order to measure at least one first parameter (P1) characterizing the elastic active chains (A) of the macromolecular network of the elastomeric polymer, The measuring step (E2) comprises measuring (E22) the increase in proton double quantum coherence using proton nuclear magnetic resonance on the insulating sheath (G) in order to determine at least from this measurement (E22) the average molar mass (M) of the elastic active chains (A) of the macromolecular network of the elastomeric polymer. c ), The first parameter (P1) comprises the average molar mass (M) of the elastic active chains (A) of the macromolecular network of the elastomeric polymer. c ), The average molar mass M of the elastic active chain (A) is c Calculated according to the following equation: Mc=(Dstat / k).3 / 5.r 2 / D res , in, D stat is the predetermined static dipole coupling, D res is the residual dipole coupling measured by measuring the increase in proton double quantum coherence using proton nuclear magnetic resonance (E22), k is a predetermined parameter for the local coupling topology and the motion between material segments, r is a predetermined ratio between the end-to-end chain length of a portion of the chains between the topological constraints and the average of said end-to-end chain lengths of the material at equilibrium, and an evaluation step (E3), the evaluation step comprising comparing a first parameter (P1) characterizing the elastic active chain (A) and / or a second parameter (P2) determined based on the first parameter (P1) characterizing the elastic active chain (A) with at least one prescribed evaluation threshold (S), so as to determine that the cable (CB) is at the end of its life when the first parameter (P1) and / or the second parameter (P2) is lower than the prescribed evaluation threshold.
2. The method according to claim 1, characterized in that: The first parameter (P1) also comprises the fraction (FCEA) of elastically active chains (A) of the macromolecular network of the elastomeric polymer, The evaluation step (E3) includes comparing (E31) the fraction (FCEA) of elastic active chains (A) of the macromolecular network of the elastomeric polymer with the specified evaluation threshold (S) so as to determine that the cable (CB) is at the end of its life when the fraction (FCEA) of elastic active chains (A) of the macromolecular network of the elastomeric polymer is lower than the specified evaluation threshold (S).
3. The method according to claim 2, characterized in that The measuring step (E2) comprises measuring (E21) transverse proton relaxation using proton nuclear magnetic resonance on the insulating sheath (G) in order to determine at least from this measurement (E21) the fraction (FCEA) of elastically active chains (A) of the macromolecular network of the elastomeric polymer.
4. The method according to any one of the preceding claims, characterized in that The second parameter (P2) comprises the elongation at break (ε) determined from the average molar mass (Mc) of the elastic active chains (A). r ), The evaluation step (E3) comprises: r ) is compared (E32) with the prescribed evaluation threshold (S), so that when the elongation at break (ε r ) is lower than the specified evaluation threshold (S), it is determined that the cable (CB) is at the end of its life.
5. The method according to any one of the preceding claims, characterized in that The method comprises a step of sampling the insulating sheath of the cable (E1), and a step of performing a measurement using proton nuclear magnetic resonance on the sample (E2).
6. The method according to claim 5, characterized in that During the sampling step (E1), the mass of the sample taken of the insulating sheath (G) of the cable (CB) is between 20 mg and 40 mg.
7. The method according to any one of the preceding claims, characterized in that The method comprises a step (E1bis) of bringing a device for measuring using proton nuclear magnetic resonance into contact with the insulating sheath (G) of the cable (CB), the measuring step (E2) being performed by the device for measuring using proton nuclear magnetic resonance.
8. A non-transitory computer-readable storage medium storing code instructions which, when executed by a processor, cause the processor to perform the method according to any one of the preceding claims.
9. A device for non-destructive testing of an insulating sheath (G) of a cable (CB) made of at least one elastomeric polymer material, It is characterized in that The device comprises a device (E1, E1bis) for measuring on the insulating sheath (G) using proton nuclear magnetic resonance in order to measure at least one first parameter (P1) characterizing the elastic active chains (A) of the macromolecular network of the elastomeric polymer, the first parameter (P1) comprising the average molar mass (M) of the elastic active chains (A) of the macromolecular network of the elastomeric polymer c ), The device (E1, E1bis) for measuring is capable of measuring (E22) the increase in proton double quantum coherence using proton nuclear magnetic resonance on the insulating sheath (G) in order to determine at least from this measurement (E22) the average molar mass (M) of the elastic active chains (A) of the macromolecular network of the elastomeric polymer c ), The average molar mass M of the elastic active chain (A) is c Calculated according to the following equation: Mc=(D stat / k).3 / 5.r 2 / D res , in, D stat is the predetermined static dipole coupling, D res is the residual dipole coupling measured by measuring the increase in proton double quantum coherence using proton nuclear magnetic resonance (E22), k is a predetermined parameter for the local coupling topology and the motion between material segments, r is a predetermined ratio between the end-to-end chain length of a portion of the chains between the topological constraints and the average of said end-to-end chain lengths of the material at equilibrium, and a computer for implementing an evaluation step (E3), the evaluation step comprising comparing a first parameter (P1) characterizing the elastic active chain (A) and / or a second parameter (P2) determined based on the first parameter (P1) characterizing the elastic active chain (A) with at least one prescribed evaluation threshold (S), so as to determine that the cable (CB) is at the end of its life when the first parameter (P1) and / or the second parameter (P2) is below the prescribed evaluation threshold.
10. The device according to claim 9, wherein: The first parameter (P1) also comprises the fraction (FCEA) of elastically active chains (A) of the macromolecular network of the elastomeric polymer, The computer is capable of executing the evaluation step (E3), which includes comparing (E31) the fraction (FCEA) of elastic active chains (A) of the macromolecular network of the elastomeric polymer with the specified evaluation threshold (S) so as to determine that the cable (CB) is at the end of its life when the fraction (FCEA) of elastic active chains (A) of the macromolecular network of the elastomeric polymer is lower than the specified evaluation threshold (S).
11. The device according to claim 9 or 10, wherein: The device (E1, E1bis) for measuring is capable of measuring (E21) transverse proton relaxation using proton nuclear magnetic resonance on the insulating sheath (G) in order to determine at least from this measurement (E21) the fraction (FCEA) of elastically active chains (A) of the macromolecular network of the elastomeric polymer.
12. The device according to any one of claims 9 to 11, wherein: The computer is capable of determining the second parameter (P2), which comprises the elongation at break (ε) determined from the average molar mass (Mc) of the elastic active chains (A). r ), The computer is capable of executing the evaluation step (E3), which includes converting the elongation at break (ε r ) is compared (E32) with the prescribed evaluation threshold (S), so that when the elongation at break (ε r ) is lower than the specified evaluation threshold (S), it is determined that the cable (CB) is at the end of its life.