A high-mobility flexible low-voltage organic thin film transistor and a preparation method thereof
By mixing C8-BTBT with polymer and combining it with PVA/P (VDF-TrFE-CFE) dual dielectric layer, using high-speed center spin coating method, the difficulty of spin coating of C8-BTBT precursor solution and the problem of orthogonal solvent selection are solved , achieving flexible organic thin film transistors with high mobility and low-voltage operation, with significantly improved mobility and switching ratio.
Patent Information
- Application Number
- CN201910914422.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-09-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-09-24
AI Technical Summary
In the existing technology, 2,7-Dioctyl[1]benzothieno[3,2-b][1]benzothiophene (C8-BTBT) is a high-mobility P-type semiconductor material. The viscosity of the precursor solution is too low to be spin-coated. Moreover, the preparation of top-deleted structure transistors is difficult, resulting in difficulty in selecting orthogonal solvents.
The organic small molecule C8-BTBT is mixed with polymer, combined with high-speed center spin coating method and PVA/P (VDF-TrFE-CFE) double dielectric layer to form a high mobility flexible low-voltage organic thin film transistor. Through vertical phase separation and The design of the modified layer solves the problems of solvent selection and polarization.
A high-performance flexible low-voltage organic thin film transistor with a device mobility of 3.18cm2·V-1·s-1 and a switching ratio of up to 106 at an operating voltage of 5V has been achieved, solving the difficult problems of precursor solution spin coating and orthogonal solvent selection. .
Smart Images

Figure CN112635673B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optoelectronic components, and in particular to a high-mobility flexible low-voltage organic thin-film transistor and a preparation method thereof. Background Art
[0002] Thin film transistors are important electronic components in the field of electronic displays, and their performance directly determines the development of display technology. Therefore, the continuous development and innovation of thin film transistors is a necessity for the current social and technological development. Organic small molecule semiconductors have attracted extensive attention from researchers due to their high mobility. 2,7-Dioctyl[1]benzothieno[3,2-b][1]benzothiophene (C8-BTBT), as a high-mobility P-type semiconductor, is currently a widely studied organic small molecule semiconductor material, but there are also some problems, such as the viscosity of the precursor solution is too low to be spin-coated on the substrate.
[0003] In recent years, researchers have mixed organic small molecule semiconductors with polymers, using the excellent solution processing properties of polymers to assist the small molecules in film formation on the substrate, and prepare high-performance organic thin film transistors through vertical phase separation. However, due to the general solubility of organic small molecules in organic solvents, the preparation of top-gate structure transistors is difficult. Currently, the medium used in top-gate structure transistors based on organic small molecule semiconductors is mostly CYTOP. Here we use the water-soluble polymer PVA as a modification layer to solve the problem of difficulty in selecting orthogonal solvents. The gate dielectric layer is selected to have a high dielectric constant relaxor ferroelectric polymer Poly (vinylidene fluoride-trifluoroethylene-chlorofloroethylene) (P (VDF-TrFE-CFE)). This double dielectric layer top-gate structure organic thin film transistor was prepared on a flexible PET substrate, and a high-mobility flexible low-voltage organic thin film transistor was obtained. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a method for preparing a high-mobility flexible low-voltage organic thin film transistor. The flexible thin film transistor prepared by combining the organic small molecule C8BTBT with a polymer mixed semiconductor layer and a double dielectric layer provided by the present invention has the advantages of high mobility and low-voltage operation.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] A thin film transistor mixed with organic small molecules and polymers comprises a substrate, a mixed system of organic small molecules 2,7-Dioctyl[1]benzothieno[3,2-b][1]benzothiophene (C8-BTBT) and an inert polymer, a double dielectric layer, a high-speed center spin coating method, and a pair of metal electrodes arranged in sequence.
[0007] Preferably, the dual dielectric layer is PVA / P(VDF-TrFE-CFE).
[0008] Preferably, the substrate comprises a flexible plastic substrate such as PET.
[0009] Preferably, the distance between the metal electrode pairs is 50-150 nm.
[0010] The present invention also provides a method for preparing the high-mobility flexible low-voltage organic thin film transistor described in the above technical solution, comprising the following steps:
[0011] Providing a substrate, a C8-BTBT and polymer mixed precursor solution, and a double dielectric layer, wherein the C8-BTBT and polymer mixed precursor solution is a C8BTBT / PMMA mixed precursor solution, and the double dielectric layer is PVA / P (VDF-TrFE-CFE);
[0012] (1) covering the flexible substrate with metal electrodes to form source and drain electrodes;
[0013] (2) high-speed center spin coating of a C8-BTBT and polymer mixed precursor solution on the flexible substrate coated with the electrode to form a C8-BTBT semiconductor layer;
[0014] (3) Preparing a PVA modification layer and a P(VDF-TrFE-CFE) insulating layer on the C8-BTBT semiconductor layer
[0015] (4) Covering a metal gate electrode at a fixed position on the surface of the P(VEF-TrFE-CFE) to obtain a high-mobility, flexible, low-voltage organic thin film transistor.
[0016] Preferably, the spin coating in step (2) is carried out in a nitrogen glove box, and after obtaining the C8-BTBT mixed semiconductor layer, the step further includes: heating the mixed semiconductor layer in the nitrogen glove box, the heating temperature is 60-80° C., and the heating time is 15 minutes.
[0017] Preferably, the spin coating in step (3) is performed in a nitrogen glove box, and the PVA layer and the high-k P (VDF-TrFE-CFE) layer are heated at 70° C. for 2 hours respectively.
[0018] The present invention provides a high-mobility flexible low-voltage organic thin film transistor and a preparation method thereof, which belongs to the field of optoelectronic components. It includes a substrate, an organic small molecule C8-BTBT and an inert polymer mixed system, a high-speed center spin coating method, a PVA / P (VDF-TrFE-CFE) double dielectric layer and a metal gate electrode arranged in sequence. The present invention controls the ratio of the mixed system by using a high-speed center spin coating method to prepare a hybrid semiconductor film with uniform performance that can be manufactured on a large area. By equipping the PVA / P (VDF-TrFE-CFE) double dielectric layer, low-voltage operation can be achieved without sacrificing mobility. The introduction of PVA solves the problem of difficulty in selecting orthogonal solvents on the one hand, and weakens the strong polarization effect of the high-k gate dielectric layer P (VDF-TrFE-CFE) on the other hand. The flexible low-voltage organic thin film transistor prepared by us has a device mobility of 3.18cm at an operating voltage of 5V. 2 ·V -1 ·s -1 , on / off ratio up to 10 6 . BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0020] Figure 1 This is a device structure diagram of a flexible low-voltage organic thin film transistor in Example 1 of the present invention;
[0021] Figure 2 is the transfer characteristic curve of the device in Example 1 of the present invention;
[0022] Figure 3 is the output characteristic curve of the device in Example 1 of the present invention; DETAILED DESCRIPTION
[0023] The present invention provides a method for preparing a high-mobility flexible low-voltage organic thin film transistor, comprising a substrate, an organic small molecule C8-BTBT and an inert polymer mixed system, high-speed central spin coating, a PVA / P (VDF-TrFE-CFE) double dielectric layer, and a metal electrode pair which are arranged in sequence.
[0024] In the present invention, the high-mobility flexible low-voltage organic thin film transistor is characterized in that the substrate comprises a flexible plastic substrate such as PET, and the substrate preferably has a planar structure.
[0025] In the present invention, the high mobility flexible low voltage organic thin film transistor is characterized in that the organic small molecule C8-BTBT and the polymer mixed system, the polymer accounts for a small proportion, preferably 5% to 20%.
[0026] In the present invention, the high-speed center spin coating is characterized in that the high-speed center spin coating is for the organic small molecule C8-BTBT and the polymer mixed semiconductor layer, and the spin coating speed is preferably 4000r / min to 7000r / min
[0027] In the present invention, the high-mobility flexible low-voltage organic thin film transistor is characterized in that the double dielectric layer is a water-soluble PVA modification layer and a high-kP (VDF-TrFE-CFE) insulating layer.
[0028] The present invention uses organic small molecule C8-BTBT as semiconductor material and polymer as blending material to improve solution processing performance. After high-speed center spin coating, a thin film with uniform performance is prepared through vertical phase separation. By equipping with PVA / P (VDF-TrFE-CFE) double dielectric layers, low-voltage operation can be achieved without sacrificing mobility. The introduction of PVA solves the problem of difficulty in selecting orthogonal solvents on the one hand, and weakens the strong polarization effect of the high-k gate dielectric layer P (VDF-TrFE-CFE) on the other hand. The flexible low-voltage organic thin film transistor prepared by us has a device mobility of 3.18 cm at an operating voltage of 3V. 2 ·V -1 ·s -1 , on / off ratio up to 10 6 .
[0029] The present invention also provides a method for preparing a thin film transistor of a mixture of organic small molecules and polymers according to the above technical solution, comprising the following steps:
[0030] (1) providing a flexible substrate, a C8-BTBT and polymer mixed precursor solution, and a double dielectric layer, wherein the C8-BTBT and polymer mixed precursor solution is a C8BTBT / PMMA mixed precursor solution; and the double dielectric layer is PVA / P(VDF-TrFE-CFE);
[0031] (2) covering the flexible substrate with a metal counter electrode to form a source-drain electrode;
[0032] (3) spin coating a C8-BTBT and polymer mixed precursor solution at a high speed center on the low surface energy polymer interface to form a C8-BTBT semiconductor layer;
[0033] (4) preparing a PVA / P (VDF-TrFE-CFE) double dielectric layer on the mixed semiconductor layer;
[0034] (5) evaporating a metal gate electrode at a fixed position on the dielectric layer;
[0035] The present invention provides a PET substrate. In the present invention, the pretreatment method of the PET substrate is not particularly limited, as long as the substrate can be cleaned.
[0036] The present invention provides a C8-BTBT and polymer mixed precursor solution. In the present invention, the C8BTBT / PMMA precursor solution preferably includes C8BTBT, PMMA and chlorobenzene. In the present invention, the molar ratio of C8BTBT and PMMA to chlorobenzene is 5 mol: 1 mol: 1 ml, and simple mixing and dissolving can be done. In the present invention, the C8BTBT, PMMA and chlorobenzene can be commercially available products known to those skilled in the art. In the present invention, the purity of C8BTBT is preferably 99%, and the purity of PMMA (M w =996 kDa) and chlorobenzene were purchased from Sigma-Aldrich.
[0037] In the present invention, the spin coating is preferably performed on a coater. In the present invention, the rotation speed of the coater is preferably 4000-7000 r / min, more preferably 5500 r / min; the rotation time is preferably 20-40 s, more preferably 30 s.
[0038] After the mixed semiconductor film is obtained, a PVA modification layer and a P (VDF-TrFE-CFE) dielectric layer are prepared on the semiconductor film by spin coating.
[0039] In the present invention, the spin coating is preferably performed on a coater. In the present invention, the rotation speed of the coater is preferably 2000-4000 r / min, more preferably 3000 r / min; the rotation time is preferably 50-70 s, more preferably 60 s.
[0040] In the present invention, the spin coating is preferably performed in a nitrogen glove box, and after obtaining the electrode layers, the layers are heated at 70° C. for 2 hours.
[0041] After preparing the double dielectric layer, the present invention covers the metal gate electrode at a fixed position on the surface of the dielectric layer. The present invention has no special limitation on the operation of covering the metal electrode pair, and the technical scheme for preparing electrodes well known to those skilled in the art can be used. In the present invention, the method of covering the metal electrode pair is preferably evaporation, and more preferably vacuum evaporation. In the present invention, the temperature of the vacuum evaporation is preferably 1000-1200°C, more preferably 1050-1150°C; the time of the vacuum evaporation is preferably 20-30min, more preferably 24-26min; the vacuum degree of the vacuum evaporation is preferably 3-4×10 -4 Pa. In the present invention, the target material during the evaporation is preferably aluminum.
[0042] In the present invention, the thin film transistor mixed with organic small molecules and polymers is preferably used under an inert condition without water and oxygen. The present invention has no special limitation on the connection method of the thin film transistor mixed with organic small molecules and polymers, and the connection method with a power source well known to those skilled in the art can be used.
[0043] The high-mobility flexible low-voltage organic thin film transistor and the preparation method thereof provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0044] Example 1
[0045] 25 mg C8BTBT and 5 mg PMMA were placed in a sample bottle with 5 ml chlorobenzene, and stirred to obtain a C8BTBT / PMMA mixed precursor solution. 20 mg PVA was placed in a sample bottle with 5 ml deionized water, and stirred to obtain a PVA precursor solution. 160 mg P(VDF-TrFE-CFE) was placed in a sample bottle with 4 ml butanone, and stirred to obtain a P(VDF-TrFE-CFE) precursor solution. In the present invention, the sample bottle needs to be cleaned with acetone, isopropanol and deionized water before use. The present invention uses acetone, isopropanol and deionized water once each in sequence.
[0046] Gold electrodes were evaporated on a clean PET substrate to serve as source and drain electrodes.
[0047] The obtained C8BTBT / PMMA mixed precursor solution is spin-coated on a PET substrate covered with source and drain electrodes in a nitrogen glove box by a spin coater to obtain a mixed semiconductor layer. The rotation speed of the spin coater is preferably 5000 rpm, and the rotation time is preferably 30 s. The mixed semiconductor layer is heated in a nitrogen glove box, and the heating temperature is preferably 70° C., and the heating time is preferably 15 minutes.
[0048] After heating, the mixture is cooled to room temperature, and the PVA precursor solution is spin-coated on the mixed semiconductor layer by a coating machine to obtain a PVA modified layer. In the present invention, the PVA precursor spin coating speed is preferably 3000 rpm, and the spin coating time is preferably 60 s. Then, the mixture is annealed at 70° C. for 2 hours in a glove box.
[0049] On the PVA modified layer, the P(VDF-TrFE-CFE) precursor solution is spin-coated on the PVA modified layer by a coating machine to obtain a P(VDF-TrFE-CFE) dielectric layer. In the present invention, the spin coating speed of the P(VDF-TrFE-CFE) precursor is preferably 3000 rpm, and the spin coating time is preferably 60 s. Then, annealing is performed at 70° C. for 2 hours in a glove box.
[0050] The obtained dielectric layer is attached to a mask of a specific shape, and a 30nm thick aluminum electrode is deposited by vacuum evaporation. The mask is removed to obtain a high-mobility, flexible, low-voltage organic thin-film transistor.
[0051] The structure of the flexible low-voltage organic thin film transistor in this embodiment is shown in FIG. Figure 1 shown.
[0052] The performance of the flexible low-voltage organic thin film transistor in this embodiment is as follows: Figure 2 , as shown in 3, from Figure 3 It can be obtained that the mobility of the flexible low-voltage organic thin film transistor is 3.18 cm at an operating voltage of 5V. 2 / Vs, switching ratio exceeds 10 5 .
[0053] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A top-gate organic thin film transistor combining a mixed semiconductor layer of an organic small molecule C8-BTBT and an inert polymer PMMA with a double dielectric layer, comprising a flexible substrate and a source and a drain, a semiconductor layer, a dielectric layer and a gate arranged on the substrate; the semiconductor layer is obtained by vertical phase separation of the organic small molecule C8-BTBT and the inert polymer PMMA; the dielectric layer adopts a low-k / high-k double dielectric layer of PVA / P (VDF-TrFE-CFE).
2. The method for preparing an organic thin film transistor according to claim 1, comprising the following steps: (1) providing a flexible PET substrate, a C8-BTBT and polymer mixed precursor solution, wherein the C8-BTBT and polymer mixed precursor solution is a C8-BTBT / PMMA mixed precursor solution, a PVA precursor solution, and a P(VDF-TrFE-CFE) precursor solution; (2) covering the substrate with a metal electrode to form a source electrode; (3) spin coating a C8-BTBT / PMMA mixed precursor solution on the substrate covered with the source and drain electrodes to form a semiconductor film; (4) spin coating a PVA precursor solution on the semiconductor film to form a PVA modification layer; (5) Spin coating a P(VDF-TrFE-CFE) precursor solution on the PVA modified layer to form a dielectric layer.